Three-dimensional stacked integrated circuit of two-dimensional semiconductor thin film and method for manufacturing the same

By using modular two-dimensional semiconductor circuit layers with nanoimprint stacking and external lead interconnection, the problems of process complexity and long processing time in the three-dimensional stacking scheme of two-dimensional semiconductor circuits are solved, achieving efficient integration improvement and simplified processing.

CN116017983BActive Publication Date: 2026-11-24NANJING UNIV OF AERONAUTICS & ASTRONAUTICS
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202211491595.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-25
Publication Date
2026-11-24
Estimated Expiration
2042-11-25

AI Technical Summary

Technical Problem

Existing three-dimensional stacking schemes for two-dimensional semiconductor circuits are complex to process and take a long time when integrated over a large area, making it difficult to further improve the integration density.

Method used

Two-dimensional semiconductor circuit layers with functional modularity are stacked using nanoimprinting, and the layers are interconnected through external leads. This nanoimprinting technology enables three-dimensional integration, reducing process complexity and processing time.

Benefits of technology

This greatly improves integration, reduces process complexity and processing time, enhances processing tolerance and yield, and promotes the application of two-dimensional semiconductor thin film materials in the integrated circuit industry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116017983B_ABST
    Figure CN116017983B_ABST
Patent Text Reader

Abstract

This invention discloses a three-dimensional stacked integrated circuit based on a two-dimensional semiconductor thin film and its fabrication method, belonging to the field of semiconductor device technology. Taking advantage of the ease of transfer of two-dimensional materials, this invention significantly increases the integration density of functionally modular two-dimensional semiconductor circuits through three-dimensional stacking, greatly reducing process complexity and processing time. The three-dimensional integrated circuit of this invention is constructed by stacking modular single-layer two-dimensional semiconductor thin film circuits. Each stack can realize a specific logic function, and the stacks are separated by insulating layers and connected through a common lead. The single-layer circuit is fabricated based on a two-dimensional semiconductor thin film. This invention features a simple process, low cost, and the resulting circuit device has advantages such as multi-functional integration, shortened interconnections, and high integration density, which can promote the application of two-dimensional semiconductor thin film materials in the integrated circuit industry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of semiconductor device technology, specifically relating to a three-dimensional stacked integrated circuit of two-dimensional semiconductor thin films and its fabrication method. Background Technology

[0002] With the continuous development of the integrated circuit industry, the method of improving integration by shrinking device size has reached a bottleneck. Researchers in the industry are trying to find breakthroughs in materials and integration methods, such as replacing traditional silicon-germanium materials with new two-dimensional semiconductor materials and replacing planar structures with three-dimensional stacked structures.

[0003] Novel two-dimensional semiconductor materials (represented by phosphorene and transition metal chalcogenides) possess atomically thin single-crystal structures compared to traditional silicon and germanium materials. Their band structures are tunable with the number of layers, and they exhibit higher electron mobility, making them ideal materials for constructing high-performance integrated circuits. Furthermore, current research on surface two-dimensional materials demonstrates good compatibility with traditional MOS and CMOS technologies. Based on traditional techniques, researchers have utilized MoS2 to construct various combinational logic gates and sequential circuits (AND, OR, NAND, NOR, XNOR, latches, edge-triggered registers) (Design, Modeling and Fabrication of CVD GrownMoS2 Circuits with E-Mode FETs for Large-Area Electronics, Lili Yu, Dina El-Damak, Nano Lett 2016, 16 (6349-6356), and found that it has stable and good performance. Furthermore, taking advantage of the atomic thinness and easy transfer characteristics of two-dimensional materials, a three-dimensional stacked integration scheme has been proposed: for example, using two-dimensional chalcogenides (WSe2, MoS2) to realize three-dimensional logic gate circuits and adder circuits (Monolithic 3D CMOS Using Layered Semiconductors, AB Sachid, M. Tosun, SB Desai, Adv. Mater. 2016, 28 ,2547-2554) Three-dimensional stacking of two-dimensional semiconductor circuits is an ideal solution to the current limitations in circuit integration. To date, proposed three-dimensional stacked circuits have all focused on single gate circuits, making large-area integration processes extremely complex; furthermore, processing time increases exponentially with the number of stacked layers. Therefore, there is still significant room for research into three-dimensional stacking schemes for two-dimensional materials. Summary of the Invention

[0004] This invention provides a three-dimensional stacked integrated circuit of two-dimensional semiconductor thin films and its fabrication method. Taking advantage of the ease of transfer of two-dimensional materials, the functionally modular two-dimensional semiconductor circuit is integrated by three-dimensional stacking to significantly increase its integration density, thereby greatly reducing process complexity and processing time.

[0005] To achieve the above objectives, the present invention adopts the following technical solution: A three-dimensional stacked integrated circuit of a two-dimensional semiconductor thin film includes a substrate and multiple functionally modular two-dimensional semiconductor circuit layers; each functionally modular two-dimensional semiconductor circuit layer is stacked by nanoimprinting and interconnected by external leads; each functionally modular two-dimensional semiconductor circuit layer can realize a complex logic function. The modular two-dimensional semiconductor circuit layer consists of a device array, an insulating layer, circuit logic connections, and lead-out layers. The device array is constructed on the surface of the insulating layer and connected by circuit logic connections and lead-out layers to form a complete circuit. Each layer of the circuit logic connections and lead-out layers is separated by an insulating layer and encapsulated at the top by an insulating layer. The device array includes active devices and passive devices. The circuit logic connections and lead-out layers refer to the interconnection of the device array through circuit design to realize specific logic functions, and the lead-out of the power bus and data transmission bus to the external lead-out terminals for inter-layer interconnection. The device array is fabricated based on a two-dimensional semiconductor thin film, which is selected from any one or more of the following materials: transition metal chalcogenides (TMDs), black phosphorus (BP), borophene, and tellurene. The insulating layer material is selected from any one or more of the following materials: metal oxides such as aluminum oxide and hafnium oxide, Si3N4, and SiO2. x N y The substrate material is selected from the following materials: silicon wafer (containing a thin layer of silicon oxide), sapphire, and insulating polymer; the lead-out material is a thin film material with good conductivity. The modular two-dimensional semiconductor circuit layer design method includes traditional top-gate, back-gate, novel dual-gate (simultaneously having a top gate and a back gate), and common-gate (Monolithic 3D CMOS Using Layered Semiconductors, AB Sachid, Adv. Mater. 2016, 28 Scheme 2547-2554). The specific logic functions implemented by the circuit logic connection and lead-out layer include single or multiple bit inverters, adders, latches, and decoders.

[0006] A method for fabricating a three-dimensional stacked integrated circuit based on a two-dimensional semiconductor thin film includes the following steps: (1) Substrate pretreatment: The substrate material is selected from the following: silicon wafer (containing a thin layer of silicon oxide), sapphire, and insulating polymer. The pretreatment method includes: surface cleaning and planarization, and alignment marking. The purpose of substrate surface cleaning is to remove surface residues, and ultrasonic cleaning can be performed using organic solvents, dilute acid or alkali solutions, deionized water, etc. The purpose of substrate planarization is to reduce the roughness of the substrate surface and enhance surface adhesion, and pretreatment can be performed using methods such as oven or heating table heating, plasma treatment, etc. The purpose of substrate alignment marking is for precise alignment between subsequent processes. (2) Form p-type and n-type two-dimensional semiconductor materials and lead-out materials, and pattern them: The two-dimensional semiconductor material is selected from one or more of transition metal chalcogenides (TMDs), black phosphorus (BP), borophene, and tellurene. The lead-out material is a thin film material with good conductivity, including conductive two-dimensional materials such as graphene, and metal foil; The formation methods include chemical vapor deposition (CVD), physical vapor deposition, thermal evaporation, and other methods for preparing large-area thin films. Formation can be done directly at the target location or transferred from elsewhere to the target location; the specific implementation depends on design requirements and process specifications. The methods for realizing p-type and n-type two-dimensional semiconductor material layers include: forming two types of two-dimensional semiconductors separately, or forming a single type and then modifying it to become a different type; the specific implementation depends on design requirements and process specifications. The modification methods include doping, induced phase transition, layer number modulation, and strain engineering modulation. Doping refers to inserting other atoms or molecules into the material using physical or chemical methods to change the band gap; induced phase transition refers to changing the material's band gap by altering its crystal structure using physical or chemical methods; layer number modulation utilizes the unique electrical properties of two-dimensional materials and their relationship to the number of layers to change the band gap; strain engineering modulation refers to changing the material's band gap by applying strain to the material. The purpose of the patterning process is to fabricate a two-dimensional semiconductor thin film into a channel array that meets the design requirements, and to fabricate the lead-out material into a lead-out that meets the design requirements; the processing methods include photolithography, electron beam etching, plasma etching, and reactive ion etching. (3) Based on patterned two-dimensional semiconductor materials and lead-out materials, and according to specific circuit designs, insulating layer materials, electrodes, and interconnects are formed to construct a two-dimensional semiconductor circuit stack: The insulating layer material is selected from metal oxides, such as Si3N4 and SiO2. x N yThe electrode or connecting wire is selected from one or more two-dimensional insulators such as nitrides and hexagonal boron nitride (hBN). The formation method is thermal evaporation (TE), electron beam evaporation (EBE), atomic layer deposition (ALD), magnetron sputtering, physical vapor deposition (PVD), or chemical vapor deposition (CVD). The electrode or connecting wire is selected from highly conductive metal materials such as Au and Cu, and the formation method is photolithography, thermal evaporation (TE), or magnetron sputtering. It should be emphasized that steps (2) and (3) are not sequential. The specific operation should be adjusted according to the actual circuit design. Some complex circuits may require repeating steps (2) and (3) multiple times. For example, to construct a top-gate transistor array, step (2) is required to form a patterned two-dimensional semiconductor layer first, and then the source, drain, and gate are processed on it through step (3). For a back-gate transistor array, step (3) is required to form the back gate electrode first, then step (2) is required to form a patterned two-dimensional semiconductor layer, and then step (3) is required to form the source and drain. It should be emphasized that different circuit design schemes should ensure that step (3) is performed first to form a layer of easily transferable two-dimensional insulating material (such as hBN) at the bottom layer, which can play a role in encapsulation protection and facilitate subsequent transfer and stacking. (4) The two-dimensional semiconductor circuit stack is sequentially transferred to the target location and stacked; The transfer method is as follows: dry transfer, spin-coating a polymer material as a support layer, and then accurately imprinting it onto the target position using nanoimprinting technology; the polymer material includes polyvinyl alcohol (PVA) and polydimethylsilane (PMMA); an adhesive can be coated between the two layers as needed, and the adhesive includes high-temperature resistant organic materials, such as high-temperature silicone grease; (5) Interconnection of leads; The interconnection methods are: hot rolling, welding, and lead stitching; welding can be used for metal foil leads; hot rolling can be used for two-dimensional material leads (such as graphene).

[0007] Beneficial Effects: This invention provides a three-dimensional stacked integrated circuit based on a two-dimensional semiconductor thin film and its fabrication method. It proposes a three-dimensional integration scheme that treats functionally modular two-dimensional semiconductor circuits as individual stacked layers, achieving inter-layer interconnection through external bus connections. By integrating functionally modular two-dimensional semiconductor circuits through three-dimensional stacking, the integration density is significantly increased. Compared to existing three-dimensional stacking schemes for individual gate circuits, which can only be processed linearly layer by layer, the method of this invention has low inter-layer correlation, allowing for parallel processing, followed by stacking via transfer imprinting, greatly reducing process complexity and processing time. Furthermore, modularity enhances replaceability, helping to improve processing tolerance and yield, further promoting the application of two-dimensional semiconductor thin film materials in the integrated circuit industry. Attached Figure Description

[0008] Figure 1This is a side view of a single two-dimensional material thin-film circuit structure in an embodiment of the present invention; Figure 2 This is a top view of a single two-dimensional material thin-film circuit structure in an embodiment of the present invention; Figure 3 This is a schematic diagram illustrating different stacking and interlayer connection methods in embodiments of the present invention; Figure 4 This is a schematic diagram illustrating the formation of the semiconductor material and the lead-out material in Embodiment 1 of the present invention; Figure 5 This is a schematic diagram of the semiconductor material and lead-out terminals in Embodiment 1 of the present invention; Figure 6 This is a schematic diagram of semiconductor material doping modification in Embodiment 1 of the present invention; Figure 7 This is a schematic diagram of the source, drain, and gate formation in Embodiment 1 of the present invention; Figure 8 This is a schematic diagram of the formation of the first layer of interconnect lines in Embodiment 1 of the present invention; Figure 9 This is a schematic diagram of the formation of the insulating layer and the second interconnecting line in Embodiment 1 of the present invention; Figure 10 This is a schematic diagram of the formation of the insulating layer and the third interconnecting line in Embodiment 1 of the present invention; Figure 11 This is a schematic diagram illustrating the top encapsulation and functions of each part in Embodiment 1 of the present invention; Figure 12 This is a schematic diagram of the 4-bit latch circuit stack-up design in Embodiment 1 of the present invention; Figure 13 This is a schematic diagram of the stacking process of the double-layer stacked decoding / latch unit in Embodiment 1 of the present invention; Figure 14 This is a schematic diagram of a multi-stage ring oscillator with an odd number of stacked layers in Embodiment 2 of the present invention; Figure 15 This is a schematic diagram of a single full adder circuit in Embodiment 3 of the present invention; Figure 16 This is a schematic diagram of a multi-bit adder with multiple layers stacked in Embodiment 3 of the present invention. Detailed Implementation

[0009] The present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments: Example 1

[0010] A two-layer stacked 4-bit address decoder and 4-bit latch enable selective read and write operations. The decoder circuit and latch circuit are located in two different layers and connected by leads to achieve functional integration. The specific fabrication method can be divided into two steps: fabricating a single two-dimensional thin-film circuit layer and stacking the layers.

[0011] The fabrication of a single two-dimensional thin-film circuit stack is illustrated using the construction of a decoder circuit stack as an example (e.g.) Figure 4-11 The latch circuit stack is directly provided ( Figure 12 The construction method is the same, such as Figures 4-13 As shown, the specific steps are as follows: (1) Preparation of substrate: The silicon wafer (containing a thin layer of silicon oxide) substrate was ultrasonically cleaned with acetone, isopropanol and ethanol in sequence. The cleaned and dried silicon wafer substrate was placed on a hot table at 60 °C and baked for 5 min. (2) Transfer a layer of hexagonal boron nitride on the substrate as a bottom two-dimensional insulating material layer; (3) A MoS2 thin film is transferred on the hexagonal boron nitride layer as an n-type two-dimensional semiconductor material layer, and a graphene layer is transferred at the edge of the hexagonal boron nitride layer as a lead-out terminal. Figure 4 ); (4) Using photolithography, spin-coating photoresist, exposure and development are performed to obtain the MoS2 thin film pattern and lead-out pattern of the transistor array channel region. The channel and lead-out are then etched out using CF4 gas dry etching. Figure 5 ); (5) Using photolithography, some n-type MoS2 channels are doped and modulated into p-type ( Figure 6 The doping method is 5×10 - 3 Mol / L AuCl3 dopant was spin-coated onto the film at 5500 rpm for 1 minute, and then calcined at 50 °C for 5 min. (6) Using photolithography, construct the source, drain, and gate ( Figure 7 The gate dielectric is a 20 nm hafnium oxide layer prepared by magnetron sputtering, and the metal electrode is a 35 nm Au layer prepared by magnetron sputtering. (7) Using photolithography to construct interconnects in layers ( Figure 8-11 The interconnects are 20 nm Au lines fabricated by magnetron sputtering; each pair of interconnects is separated by an insulating layer, which is a 20 nm ZrO2 layer fabricated by magnetron sputtering; the top layer needs to be an insulating layer for encapsulation and protection. (8) 4-bit latch circuit stack-up ( Figure 12 It can be constructed in the same way as steps (1)-(7) in Example 1, only the circuit design is different.

[0012] Multiple stacked structures such as Figure 13 As shown, the specific steps are as follows: (1) Substrate cleaning and marking: The sapphire substrate was ultrasonically cleaned with acetone, ethanol and deionized water in sequence. The cleaned and dried sapphire substrate was placed on a hot plate at 45°C and baked for 10 min. Alignment marking patterns were then photolithographically etched onto the substrate. (2) Place the stacked layer at the target position: spin coat a layer of PVA as a support layer on the stacked layer, dry and cure at 80°C, and use nanoimprint technology to accurately transfer the stacked layer with the support layer to the target position. Remove the PVA support layer with deionized water at 90°C. (3) Apply adhesive to the stack to prepare for bonding with the next stack: Spin-on a layer of high-temperature silicone grease as an adhesive layer on the stack, which can also serve as a heat dissipation layer; (4) Repeat steps (2) and (3) to achieve multi-layer stacking. For this embodiment, it only needs to be repeated twice. (5) Lead-out interconnection: The graphene lead-out ends that need to be connected between the two layers are pressed together by rolling, with a pressure of 0.5 MPa and a temperature of 100 ℃.

[0013] Through the above steps, the double-layer stacked decoding / latch unit is constructed. It should be noted that the leads can be further connected to other layers to achieve more complex functions. Compared with traditional planar integrated circuits, the area of ​​this circuit is reduced by about half, which effectively improves the device integration.

[0014] Example 2

[0015] Odd-layer stacked multi-stage ring oscillator Figure 14 This refers to a circuit model that can generate periodic oscillations. A single stack is a modular inverter circuit, which can be mass-produced, and its construction method is the same as in Example 1; the stacking method is as follows: (1) Substrate cleaning and marking: The silicon / silicon oxide substrate was ultrasonically cleaned with acetone, ethanol and deionized water in sequence. The cleaned and dried silicon / silicon oxide substrate was placed on a hot plate at 40°C and baked for 15 min. Alignment marking patterns were then photolithographically etched onto the substrate. (2) Place the stack A at the target position: spin coat a layer of PVA on the stack as a support layer, dry and cure at 80°C, and use nanoimprint technology to accurately transfer the stack with the support layer to the target position. Remove the PVA support layer with deionized water at 90°C. (3) Apply an insulating agent to the lead-out terminals that do not require interlayer connection, and apply PMMA as an insulating agent to the input terminals of the stacked circuit to avoid parallel connection of the input terminals of the remaining stacked circuits. (4) Mirror and flip layer A to obtain layer B, and stack layer B onto layer A in accordance with the methods (2) and (3) above; (5) Stack an odd number of layers in the ABA-… manner to form an oscillating circuit; (6) Lead-out interconnection: The graphene lead-out ends that need to be connected between the two layers are pressed together by rolling, with a pressure of 0.5 MPa and a temperature of 100℃.

[0016] Example 3

[0017] Multi-layer stacked multi-bit adders ( Figure 16 It can perform multi-bit addition operations, and a single stack is a modular full adder circuit. Figure 15 It can be mass-produced, and the construction method is the same as in Example 1. The stacking method is as follows: (1) Substrate cleaning and marking: The silicon / silicon oxide substrate was ultrasonically cleaned with acetone, ethanol and deionized water in sequence. The cleaned and dried silicon / silicon oxide substrate was placed on a hot plate at 40°C and baked for 15 min. Alignment marking patterns were then photolithographically etched onto the substrate. (2) Transfer layers 1, 3, 5... sequentially to the target position: spin coat a layer of PVA on the stack as a support layer, dry and cure at 80°C, and use nanoimprint technology to accurately transfer the stack with the support layer to the target position. Remove the PVA support layer with 90°C deionized water. (3) Interconnect the power bus leads of the stack 1, 3, 5... and press the graphene leads that need to be connected between the two layers by rolling, with a pressure of 0.5 MPa and a temperature of 100℃. (4) Transfer layers 2, 4, 6... to layers 1, 3, 5... in a staggered manner, using the same transfer method as in Example 3; (5) Interconnect the power bus leads of stack 2, 4, 6... and interconnect the carry input / output terminals of adjacent stacks. The interconnection method is the same as in Example 3.

[0018] It should be emphasized that layer 1 can be replaced with a half-adder to simplify the circuit. In addition, this staggered stacking structure (similar to brickwork) can greatly enhance the longitudinal stability of the three-dimensional structure and can be applied to stacks with higher numbers of layers.

[0019] The above are merely preferred embodiments of the present invention, which will help those skilled in the art to further understand the present invention, but do not limit the present invention in any way. It should be noted that for those skilled in the art, any modifications and improvements made without departing from the concept of the present invention are within the protection scope of the present invention.

Claims

1. A method for fabricating a three-dimensional stacked integrated circuit of a two-dimensional semiconductor thin film, characterized in that, Includes the following steps: (1) Substrate pretreatment: The substrate is cleaned, planarized, and aligned in sequence; (2) Form an easily transferable insulating material layer on the substrate surface; (3) A two-dimensional semiconductor material layer and a lead-out material layer are formed on the insulating layer and then patterned. (4) Construct source, drain, gate electrodes, interconnects, insulating separators and top insulating encapsulation layer to obtain a functional modular two-dimensional semiconductor circuit layer; (5) Spin-coating a polymer material as a support layer onto the functional modular two-dimensional semiconductor circuit layer, transferring and imprinting it to the target position using nanoimprinting technology, and then removing the support layer; (6) Apply adhesive to the stacked circuit layers and repeat steps (2)-(5) to build and stack different functional modular two-dimensional semiconductor circuit layers; (7) Interconnect the leads that need to be connected.

2. The method for fabricating a three-dimensional stacked integrated circuit of a two-dimensional semiconductor thin film according to claim 1, characterized in that, The two-dimensional semiconductor material layer mentioned in step (3) is a p-type and an n-type two-dimensional semiconductor material, which is formed directly at the target location or formed elsewhere and then transferred to the target location.

3. The method for fabricating a three-dimensional stacked integrated circuit of a two-dimensional semiconductor thin film according to claim 2, characterized in that, The methods for preparing p-type and n-type two-dimensional semiconductor materials are as follows: p-type two-dimensional semiconductor materials and n-type two-dimensional semiconductor materials are formed respectively; or, one type of two-dimensional semiconductor material is formed uniformly, and then a part of its region is modified to become another type of two-dimensional semiconductor material.

4. The method for fabricating a three-dimensional stacked integrated circuit of a two-dimensional semiconductor thin film according to claim 1, characterized in that, The polymer material mentioned in step (5) is polyvinyl alcohol or polydimethylsilane, and the adhesive mentioned in step (6) is a high-temperature resistant organic adhesive.

5. A three-dimensional stacked integrated circuit of a two-dimensional semiconductor thin film prepared by the method of any one of claims 1-4, characterized in that, It includes a substrate, multiple functionally modular two-dimensional semiconductor circuit layers, and an insulating layer; each functionally modular two-dimensional semiconductor circuit layer is stacked by nanoimprinting, and the layers are separated by an insulating layer. Each layer is interconnected through an external lead-out terminal, and each functionally modular two-dimensional semiconductor circuit layer can realize a logic function.

6. The three-dimensional stacked integrated circuit of the two-dimensional semiconductor thin film according to claim 5, characterized in that, The modular two-dimensional semiconductor circuit layer consists of a device array, an insulating layer, circuit logic connections, and a lead-out layer. The device array is constructed on the surface of the insulating layer and connected through the circuit logic connections and the lead-out layer to form a complete circuit. The device array includes active devices and passive devices; The circuit logic connection and lead-out layer interconnects the device array through circuit design to achieve specific logic functions, and leads the power bus and data transmission bus to the external lead-out terminal for inter-layer interconnection.

7. The three-dimensional stacked integrated circuit of a two-dimensional semiconductor thin film according to claim 6, characterized in that, The circuit logic connections and lead-out layers of the modular two-dimensional semiconductor circuit layers are separated by an insulating layer, and the top is encapsulated by an insulating layer.

8. The three-dimensional stacked integrated circuit of the two-dimensional semiconductor thin film according to claim 6, characterized in that, The device array is fabricated based on a two-dimensional semiconductor thin film.

9. The three-dimensional stacked integrated circuit of the two-dimensional semiconductor thin film according to claim 6, characterized in that, The device array is constructed on the surface of an insulating layer, wherein the insulating layer is one or more two-dimensional insulators selected from aluminum oxide, hafnium oxide, Si3N4, and hexagonal boron nitride.

10. The three-dimensional stacked integrated circuit of a two-dimensional semiconductor thin film according to any one of claims 5-9, characterized in that, The substrate is a silicon wafer, sapphire, or an insulating polymer; the material of the external lead-out terminal is a conductive thin film material.

Citation Information

Patent Citations

  • Two-dimensional nano sheet layer transition metal sulfide bidirectional switch device

    CN105845739A

  • Bump with nanolaminated structure, package structure of the same, and method of preparing the same

    US20120305298A1

  • Semiconductor device wafer bonding integration techniques

    WO2017052594A1