Method for manufacturing electrode and its catalytic layer

By using a mixture of large-particle and small-particle catalysts in the electrode catalytic layer of an oxygen generator, combined with conductive agents and binders, a multi-layer electrode structure is formed, which solves the problem of low redox reaction efficiency caused by the electrode catalytic layer structure and achieves a more efficient oxygen production effect.

CN116022737BActive Publication Date: 2026-11-24TAIWAN CARBON NANO TECHNOLOGY CORPORATION
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202211329505.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-10-27
Filing Date
2022-10-27
Publication Date
2026-11-24
Estimated Expiration
2042-10-27

AI Technical Summary

Technical Problem

The electrode catalyst layer structure of existing oxygen generators results in low redox reaction efficiency, which affects oxygen production efficiency.

Method used

A multilayer electrode is formed by mixing large-particle and small-particle catalysts, combining them with conductive agents and binders, and forming a catalyst layer through stirring and rolling. This layer is then pressed together with a conductive current collector and a gas diffusion membrane.

Benefits of technology

This increased the reaction area and oxygen production efficiency of the electrodes, thereby improving the oxygen production efficiency of the oxygen generator.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116022737B_ABST
    Figure CN116022737B_ABST
Patent Text Reader

Abstract

The present invention provides a method for manufacturing an electrode, the steps of which include: mixing a first catalyst having a first average particle size, a second catalyst having a second average particle size, a first conductive agent, a first binder, and a solvent to form a first mixture, wherein the weight ratio of the first catalyst to the second catalyst is 5:1 to 1:5; obtaining a second mixture by stirring the first mixture; rolling the second mixture into a catalyst layer; and pressing the catalyst layer with a conductive current collector and a gas diffusion membrane to obtain the electrode.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for manufacturing an electrode and its catalytic layer, and more particularly to a method for manufacturing an electrode for generating oxygen and its catalytic layer. Background Technology

[0002] Common oxygen generators are continuous oxygen supply devices. Their principle involves using an electric motor (or air compressor) to draw air from the atmosphere into the machine. The air passes through a molecular sieve to separate oxygen and nitrogen, thus producing a high concentration of oxygen. Because this type of oxygen generator operates on the principle of a metal-air electrochemical cell, where oxidation-reduction reactions occur at the electrodes, the consumption of oxygen from the external air at the cathode leads to a decrease in oxygen production efficiency. Therefore, the material of the electrodes and their manufacturing process are key factors affecting oxygen production efficiency.

[0003] To achieve more efficient redox reactions, the selection of the appropriate catalyst for the electrode's catalytic layer has become a key research focus in this field, as the catalyst's activity significantly impacts the performance of the air electrode. Typically, an air electrode consists of a catalytic layer containing the catalyst, a conductive current collector, and a gas diffusion film. The inventors of this invention focus on improving the catalytic layer to enhance the oxygen production efficiency of an oxygen generator. Summary of the Invention

[0004] The purpose of this invention is to provide a method for manufacturing an electrode to improve the structure of the electrode catalyst layer, increase the reaction area, and improve oxygen production efficiency.

[0005] Based on the above concept, a method for manufacturing an electrode is proposed, comprising the following steps: mixing a first catalyst having a first average particle size, a second catalyst having a second average particle size, a first conductive agent, a first binder, and a solvent to form a first mixture, wherein the weight ratio of the first catalyst to the second catalyst is 5:1 to 1:5; obtaining a second mixture by stirring the first mixture; rolling the second mixture into a catalyst layer; and pressing the catalyst layer with a conductive current collector and a gas diffusion membrane to obtain the electrode.

[0006] Based on the above concept, a method for manufacturing an electrode is proposed, the steps of which include: mixing a catalyst, a first conductive agent, a first binder and a solvent to form a first mixture, wherein the catalyst includes: a large-particle-size catalyst and a small-particle-size catalyst; obtaining a second mixture by stirring the first mixture; rolling the second mixture into a catalyst layer; and pressing the catalyst layer with a conductive current collector and a gas diffusion membrane to obtain the electrode.

[0007] Based on the above concept, a catalytic layer for an electrode is proposed, comprising: a large-particle-size catalyst, a small-particle-size catalyst, a conductive agent, and a binder, wherein: the large-particle-size catalyst and the small-particle-size catalyst have a first average particle size and a second average particle size, respectively; and the first average particle size is greater than the second average particle size. Attached Figure Description

[0008] The above-described objects and advantages of the present invention will become more immediately apparent to those skilled in the art upon reading the following detailed description and accompanying drawings.

[0009] [ Figure 1 [This is an enlarged schematic diagram showing the structure of the catalyst layer of an electrode according to one embodiment of the present invention.]

[0010] [ Figure 2 [This image shows a flowchart illustrating the manufacturing process of an electrode containing a catalyst layer according to one embodiment of the present invention.]

[0011] [ Figure 3A [This image shows a schematic diagram of an electrode structure according to one embodiment of the present invention.]

[0012] [ Figure 3B [This image shows a schematic diagram of an electrode structure according to another embodiment of the present invention.]

[0013] [ Figure 4 [This represents a schematic diagram of the oxygen generation device used to configure the electrodes of Examples 1-5 and the comparative examples for testing.]

[0014] [ Figure 5 The graph shows the change in unit area current density versus time for Embodiments 1-5 and the comparative examples of the present invention. Detailed Implementation

[0015] The invention presented in this case will be fully understood by the following embodiments, which will enable those skilled in the art to carry it out. However, the implementation of this case is not limited to the following embodiments. Those skilled in the art can still deduce other embodiments based on the spirit of the disclosed embodiments, and such embodiments should all fall within the scope of this invention.

[0016] Figure 1 This is an enlarged schematic diagram showing the structure of the catalyst layer of a cathode according to one embodiment of the present invention. Figure 1In this catalyst layer 100, the catalyst mainly comprises a conductive agent 101, a binder 102, a large-particle-size catalyst 103, and a small-particle-size catalyst 104. The conductive agent 101 is uniformly distributed in the binder 102 and on the surfaces of the large-particle-size catalyst 103 and the small-particle-size catalyst 104. The binder 102 also fixes the large-particle-size catalyst 103 and the small-particle-size catalyst 104 together. Even so, fluid channels 105 still exist in the catalyst layer 100 between the large-particle-size catalyst 103, between the small-particle-size catalyst 104, and between the large-particle-size catalyst 103 and the small-particle-size catalyst 104, and the fluid channels 105 also vary in size. In the embodiments of the present invention, the catalyst layer 100, through this structure of catalysts with mixed particle sizes, uses large-particle-size catalysts to create large fluid channels and small-particle-size catalysts to create small fluid channels, so that the fluid channels are closely distributed in the catalyst layer, thereby increasing the surface area of ​​the catalyst, improving the reaction efficiency, and thus improving the oxygen production efficiency.

[0017] In the embodiments of the present invention, the catalyst layer 100 is mainly composed of a large-particle-size catalyst 103 and a small-particle-size catalyst 104, where "particle size" refers to "average particle size". The "average particle size" refers to the D50 value (i.e., the median particle size distribution) or arithmetic mean calculated using, for example, a laser particle size analyzer known in the art. This "average particle size" can be determined by those skilled in the art based on specific requirements. For example, to ensure product quality stability, catalyst particles of appropriate size are screened using sieves of a specific mesh size as needed. Furthermore, since the shape of catalyst particles is not fixed, the particle size is calculated based on the major axis of the particle. The large-particle-size catalyst 103 of the present invention uses an average particle size range of 150–270 μm, and the small-particle-size catalyst 104 uses an average particle size range of 5–50 μm. The average particle size of the large-particle-size catalyst 103 is 3–54 times that of the small-particle-size catalyst 104.

[0018] Furthermore, the materials of the large-particle-size catalyst 103 and the small-particle-size catalyst 104 in the catalyst layer 100 of the present invention are selected from the group consisting of ruthenium dioxide, iridium dioxide, manganese dioxide, cobalt oxide, cobalt tetroxide, nickel hydroxide, nickel oxide, iron oxide, tungsten trioxide, vanadium pentoxide and palladium oxide.

[0019] The adhesive 102 is made of polytetrafluoroethylene (PTFE), perfluoroethylene propylene copolymer (FEP), or polyvinylidene fluoride (PVDF). The conductive agent 101 is made of carbon black, acetylene black, or carbon nanofibers.

[0020] Figure 2This diagram illustrates the manufacturing process of an electrode comprising a catalyst layer 100 according to an embodiment of the present invention. The manufacturing method includes the following steps: Step S1, mixing a large-particle-size catalyst, a small-particle-size catalyst, a conductive agent, a binder, and a solvent to form a first mixture; then Step S2, stirring the first mixture to obtain a second mixture; and Step S3, rolling the second mixture into a catalyst layer to obtain the catalyst layer 100. Furthermore, the solvent is water, an alcohol, or a combination thereof. Then, in order to further fabricate the catalyst layer 100 into an electrode, the solvent evaporates during the electrode manufacturing process, thereby facilitating the formation of fluid channels 105, such as pores, in the catalyst layer 100. Finally, in Step S4, the catalyst layer 100 is pressed together with a conductive current collector and a gas diffusion film to obtain the electrode.

[0021] The amount of conductive agent added in step S1 above shall not exceed half the total weight of the first mixture, preferably in the range of 20% to 50%, and more preferably 28% to 46%. This is because while conductive agents can enhance electrode conductivity, excessive addition of conductive agent will reduce the catalyst content and decrease the reactivity. The catalyst added in step S1 above, wherein the weight ratio of the large-particle-size catalyst to the small-particle-size catalyst is 10:1 to 1:10, preferably 5:1 to 1:5.

[0022] The difference between the mixing and stirring in steps S1 and S2 lies in the fact that step S1 is a general mixing process that does not require high homogeneity, while step S2 is performed to achieve high homogeneity of the mixture. Therefore, the stirring process in step S1 can be set at a speed of 50–800 rpm, preferably 100–700 rpm, and more preferably 150–600 rpm, using a commonly used mixer (blade shear mixer) to produce the first mixture. The stirring in step S2 is preferably performed using a planetary mixer (also known as a gravity centrifugal mixer), with a speed set in the range of 200–2000 rpm, preferably 400–1900 rpm, and more preferably 500–1400 rpm, to produce the second mixture. Furthermore, step S2 is not limited to using a planetary mixer; a blade shear mixer can also be used, as long as the uniform distribution of materials is achieved.

[0023] The rolling process in step S3 above uses a rolling mill commonly used by those skilled in the art, with the rotation speed set between 1 and 30 rpm, preferably between 2 and 28 rpm, more preferably between 4 and 26 rpm, and the roller temperature set below 150°C, preferably between 15 and 100°C, more preferably between 20 and 80°C.

[0024] Figure 3A A schematic diagram showing an electrode structure according to one embodiment of the present invention. Figure 3BA schematic diagram showing an electrode structure according to another embodiment of the present invention. (See attached diagram.) Figure 3A As shown, cathode 113 is formed by pressing conductive current collector 112 onto catalyst layer 100, and gas diffusion film 111 is pressed onto conductive current collector 112. Alternatively, it can be as follows... Figure 3B As shown, a first gas diffusion film 111a is pressed onto the catalyst layer 100, then a conductive current collector 112 is pressed onto the first gas diffusion film 111a, and finally a second gas diffusion film 111b is pressed onto the conductive current collector 112. This four-layer electrode structure provides a more stable reaction than a three-layer structure because the gas diffusion film 111 has a better bond with the conductive current collector 112.

[0025] The conductive current collector 112 functions to concentrate current, fix the catalyst layer, and support the electrode structure. It is made of a mesh or foam material, such as stainless steel, nickel, titanium, or copper. The gas diffusion membranes 111, 111a, and 111b function to allow oxygen to pass through and prevent electrolyte leakage. They are made of materials similar to the conductive agent 101 and adhesive 102 described above. Specifically, the gas diffusion membranes 111, 111a, and 111b are made by mixing, stirring, and rolling a conductive agent (e.g., carbon black, acetylene black, and carbon nanofibers) and an adhesive (e.g., polytetrafluoroethylene (PTFE), perfluoroethylene propylene copolymer (FEP), and polyvinylidene fluoride (PVDF)). The steps are similar to steps S1 to S3 described above, except that a catalyst is not added. The mixing ratio can be adjusted by those skilled in the art as needed, but it is preferable that the proportion of conductive agent 101 is higher than that of adhesive 102. In the gas diffusion membrane 111, the proportion of adhesive is higher than that of the catalyst layer 100.

[0026] Based on the above-described method for manufacturing the catalyst layer 100 of the present invention, the following embodiments are proposed.

[0027] Table 1

[0028]

[0029] In Example 1 of this invention, the preparation was carried out according to the proportions shown in Table 1 above. Specifically, 45 grams of MnO2 with an average particle size of 270 μm, 9 grams of MnO2 with an average particle size of 5 μm, 103.5 grams of XC72R, 67.5 grams of PTFE, 112 grams of 95% ethanol, and 665 grams of water were mixed and stirred at 200 rpm for 10 minutes using a DLH DC stirrer (YOTEC, model: MRB-3500L) to produce a gel-like first mixture. This gel-like first mixture was then stirred at 1900 rpm for 5 minutes using a Thinky planetary stirrer to obtain a lumpy second mixture. The lumpy second mixture was then rolled into a catalyst layer with a thickness of 0.78 mm using a rolling mill (Yezhong, EKT-2100SLM) at 25°C and 50 rpm. Finally, the catalyst layer is pressed together with a conductive current collector and a gas diffusion film (1.2 mm thick) to obtain an electrode (or cathode) with a thickness of 1.87 mm.

[0030] Table 2

[0031]

[0032] Regarding Example 2 of the present invention, the preparation was carried out according to the proportions shown in Table 2 above. Specifically, 78.75 g of MnO2 with an average particle size of 270 μm, 15.75 g of MnO2 with an average particle size of 50 μm, 56.25 g of XC72R, 6.75 g of VGCF-H, 67.5 g of PTFE, 112 g of 95% ethanol, and 665 g of water were mixed and stirred at 200 rpm for 10 minutes using a DLH DC stirrer (YOTEC, model: MRB-3500L) to produce a gel-like first mixture. This gel-like first mixture was then stirred at 1900 rpm for 5 minutes using a Thinky planetary stirrer to obtain a lumpy second mixture. Then, the lumpy second mixture was rolled into a catalyst layer with a thickness of 0.78 mm using a rolling mill (Yezhong, EKT-2100SLM) at 25°C and 50 rpm. Finally, the catalyst layer is pressed together with a conductive current collector and a gas diffusion film (1.2 mm thick) to obtain an electrode (or cathode) with a thickness of 1.87 mm.

[0033] Table 3

[0034]

[0035] Regarding Example 3 of the present invention, the preparation was carried out according to the proportions shown in Table 3 above. Specifically, 78.75 g of MnO2 with an average particle size of 150 μm, 15.75 g of MnO2 with an average particle size of 5 μm, 85.5 g of XC72R, 45 g of PTFE, 114 g of 95% ethanol, and 662 g of water were mixed and stirred at 200 rpm for 10 minutes using a DLH DC stirrer (YOTEC, model: MRB-3500L) to produce a gel-like first mixture. This gel-like first mixture was then stirred at 1900 rpm for 5 minutes using a Thinky planetary stirrer to obtain a lumpy second mixture. Then, the lumpy second mixture was rolled into a catalyst layer with a thickness of 0.78 mm using a rolling mill (Yezhong, EKT-2100SLM) at 25°C and 50 rpm. Finally, the catalyst layer is pressed together with a conductive current collector and a gas diffusion film (1.2 mm thick) to obtain an electrode (or cathode) with a thickness of 1.87 mm.

[0036] Table 4

[0037]

[0038] Example 4 of the present invention was prepared according to the proportions shown in Table 4 above. Specifically, 67.5 g of MnO2 with an average particle size of 150 μm, 13.5 g of MnO2 with an average particle size of 50 μm, 99 g of XC72R, 45 g of PTFE, 114 g of 95% ethanol, and 662 g of water were mixed and stirred at 200 rpm for 10 minutes using a DLH DC stirrer (YOTEC, model: MRB-3500L) to produce a gel-like first mixture. This gel-like first mixture was then stirred at 1900 rpm for 5 minutes using a Thinky planetary stirrer to obtain a lumpy second mixture. The lumpy second mixture was then rolled into a catalyst layer with a thickness of 0.78 mm using a rolling mill (Yezhong, EKT-2100SLM) at 25°C and 50 rpm. Finally, the catalyst layer is pressed together with a conductive current collector and a gas diffusion film (1.2 mm thick) to obtain an electrode (or cathode) with a thickness of 1.87 mm.

[0039] Table 5

[0040]

[0041] Example 5 of the present invention was prepared according to the proportions shown in Table 5 above. Specifically, 13.5 g of MnO2 with an average particle size of 150 μm, 67.5 g of MnO2 with an average particle size of 50 μm, 69.75 g of XC72R, 6.75 g of VGCF-H, 67.5 g of PTFE, 112 g of 95% ethanol, and 665 g of water were mixed and stirred at 200 rpm for 10 minutes using a DLH DC stirrer (YOTEC, model: MRB-3500L) to produce a gel-like first mixture. This gel-like first mixture was then stirred at 1900 rpm for 5 minutes using a Thinky planetary stirrer to obtain a lumpy second mixture. The lumpy second mixture was then rolled into a catalyst layer with a thickness of 0.78 mm using a rolling mill (Yezhong, EKT-2100SLM) at 25°C and 50 rpm. Finally, the catalyst layer is pressed together with a conductive current collector and a gas diffusion film (1.2 mm thick) to obtain an electrode (or cathode) with a thickness of 1.87 mm.

[0042] Table 6

[0043]

[0044] The comparative example of the single average particle size of the present invention was prepared according to the proportions shown in Table 6 above. Specifically, 45.0 g of manganese dioxide with a single average particle size of 150 μm (as in Examples 1-5 above, this single average particle size refers to the D50 value calculated using a laser particle size analyzer known in the art), 112.5 g of XC72R, 67.5 g of PTFE, 112 g of 95% ethanol, and 665 g of water were mixed and stirred at 200 rpm for 10 minutes using a DLH DC stirrer (YOTEC, model: MRB-3500L) to produce a gel-like first mixture. This gel-like first mixture was then stirred at 1900 rpm for 5 minutes using a Thinky planetary stirrer to obtain a lumpy second mixture. The lumpy second mixture was then rolled into a catalyst layer with a thickness of 0.78 mm using a rolling mill (Yezhong, EKT-2100SLM) at 25°C and 50 rpm. Finally, the catalyst layer is pressed together with a conductive current collector and a gas diffusion film (1.2 mm thick) to obtain an electrode (or cathode) with a thickness of 1.87 mm.

[0045] Figure 4 This diagram illustrates the structure of the oxygen generation device used to configure the electrodes of Examples 1-5 and the comparative examples for testing. To test the performance of electrodes made of different materials, a simplified oxygen generation device 200 is proposed. Figure 4As shown, a portion of the cathode 113, manufactured according to the steps of the above-described embodiments and comparative examples, is placed in a container 116 containing electrolyte 115 (30% sodium hydroxide), along with a nickel mesh serving as the anode 114. Inside the container 116, the catalyst layer 100 of the cathode 113 and the anode 114 are immersed in the electrolyte 115. The gas diffusion layer 111 of the cathode 113 is disposed outside the container 116, while the catalyst layer 100 is inside the container 116, allowing atmospheric oxygen to enter the container 116 through the gas diffusion layer 111. When a voltage is applied, atmospheric oxygen is generated through an electrochemical reaction between the catalyst layer 100 and the anode 114, concentrating the atmospheric oxygen concentration of only 19% to a concentration greater than 80% within the device assembly. The surface area of ​​the cathode 113 and the anode 114 is 100 cm². 2 It can be used in portable oxygen generation devices. During testing, a 1V voltage is applied to the electrodes to measure the current value. Dividing the current value by the area yields the current density value, as shown below. Figure 5 As shown.

[0046] Please see Figure 5 The graph shows the change in current density per unit area versus time for Examples 1-5 and the Comparative Examples of the present invention. A higher current density per unit area indicates better electrochemical reaction capability, which can be used to evaluate the electrode oxygen production efficiency of the embodiments of the present invention. This test was conducted using the cathodes of Examples 1-5, in conjunction with a potassium hydroxide electrolyte and an anode Ni mesh. Figure 5 It can be seen that the current density per unit area exhibited by Examples 1-5, which use a dual average particle size catalyst mixture of the present invention, is greater than that of the comparative examples using a single average particle size catalyst. Although Example 1 performed worse than the comparative examples in the first hour, its effect gradually increased after one hour, and by three hours it was close to the performance of Examples 4 and 5. In other words, because the ratio of binder to catalyst was different, the initial values ​​of each example were also different, but the final results were still better than those of catalysts with a single average particle size range. Figure 5 It is clear that Example 3 performs the best.

[0047] Although the invention has been described with reference to embodiments currently considered to be the most practical and preferred, it should be understood that the invention is not limited to the disclosed embodiments. Rather, it is intended to cover various modifications and similar configurations included within the spirit and scope of the appended claims, and these modifications and similar configurations should be consistent with the broadest interpretation to cover all such modifications and similar structures.

[0048] Explanation of reference numerals in the attached figures

[0049] 100 catalyst layers

[0050] 101 conductive agent

[0051] 102 adhesive

[0052] 103 Large Particle Size Catalyst

[0053] 104 small particle size catalyst

[0054] 105 fluid channels

[0055] 111 Gas Diffusion Membrane

[0056] 111a First Gas Diffusion Membrane

[0057] 111b Second Gas Diffusion Membrane

[0058] 112 conductive current collector

[0059] 113 cathode

[0060] 114 anode

[0061] 115 electrolyte

[0062] 116 containers

[0063] 200 oxygen production unit

[0064] Steps S1 to S4

Claims

1. A method for manufacturing an electrode, comprising the steps of: A first catalyst having a first average particle size, a second catalyst having a second average particle size, a first conductive agent, a first binder, and a solvent are mixed to form a gel-like first mixture, wherein the weight ratio of the first catalyst to the second catalyst is 5:1 to 1:5, wherein each of the first catalyst and the second catalyst is manganese dioxide, the first average particle size is 150 to 270 µm, and the second average particle size is 5 to 50 µm; The first mixture is stirred to obtain a lumpy second mixture; The lumpy second mixture is rolled into a catalyst layer; as well as The catalyst layer is pressed together with a conductive current collector and a gas diffusion membrane to obtain the electrode, which is used in an oxygen generation device.

2. The method for manufacturing an electrode as claimed in claim 1, wherein the gas diffusion film comprises a second conductive agent and a second adhesive; The first conductive agent and the second conductive agent are carbon black, acetylene black or carbon nanofibers; The first adhesive and the second adhesive are polytetrafluoroethylene (PTFE), perfluoroethylene propylene copolymer (FEP), or polyvinylidene fluoride (PVDF). The solvent is water, an alcohol, or a combination thereof; and The conductive current collector is a mesh or foam material made of stainless steel, nickel, titanium, or copper.

3. The method for manufacturing an electrode as claimed in claim 1, wherein the rotational speed in the mixing step and the stirring step is 100 to 2000 rpm; The mixing step includes at least gravity centrifugal mixing and blade shear mixing; and The pressing step uses a roller device, and the rolling speed is below 30 rpm and the temperature is below 150°C.

4. The method for manufacturing an electrode as claimed in claim 1, wherein the first average particle size is 3 to 54 times the second average particle size.

5. A method for manufacturing an electrode, comprising the steps of: A first mixture of a catalyst, a first conductive agent, a first binder, and a solvent is formed into a gel-like first mixture, wherein the catalyst comprises: a large-particle-size catalyst; And a small-particle-size catalyst, wherein each of the large-particle-size catalyst and the small-particle-size catalyst is manganese dioxide, wherein the first average particle size of the large-particle-size catalyst is 150 to 270 µm, the second average particle size of the small-particle-size catalyst is 5 to 50 µm, and the weight ratio of the large-particle-size catalyst and the small-particle-size catalyst is 5:1 to 1:

5. The first mixture is stirred to obtain a lumpy second mixture; The lumpy second mixture is rolled into a catalyst layer; as well as The catalyst layer is pressed together with a conductive current collector and a gas diffusion membrane to obtain the electrode, which is used in an oxygen generation device.

6. The method for manufacturing an electrode as claimed in claim 5, wherein the gas diffusion film comprises a second conductive agent and a second adhesive; The first conductive agent and the second conductive agent are carbon black, acetylene black or carbon nanofibers; The first adhesive and the second adhesive are polytetrafluoroethylene (PTFE), perfluoroethylene propylene copolymer (FEP), or polyvinylidene fluoride (PVDF). The solvent is water, an alcohol, or a combination thereof; and The conductive current collector is a mesh or foam material made of stainless steel, nickel, titanium, or copper.

7. The method for manufacturing an electrode as claimed in claim 5, wherein the rotation speed during the mixing step and the stirring step is 100 to 2000 rpm; The mixing step includes at least gravity centrifugal mixing and blade shear mixing; and The rotational speed in this rolling step is below 30 rpm and the temperature is below 150°C.

8. The method for manufacturing an electrode as described in claim 5, wherein the average particle size of the large-particle catalyst is 3 to 54 times the average particle size of the small-particle catalyst.

9. A catalyst layer for an electrode, comprising: The catalyst comprises a large-particle-size catalyst, a small-particle-size catalyst, a conductive agent, and a binder, wherein the conductive agent is carbon black, acetylene black, or carbon nanofibers, and the binder is polytetrafluoroethylene (PTFE), perfluoroethylene-propylene copolymer (FEP), or polyvinylidene fluoride (PVDF). The large-particle-size catalyst and the small-particle-size catalyst each have a first average particle size and a second average particle size. The first average particle size of the large-particle-size catalyst is 150–270 µm, and the second average particle size of the small-particle-size catalyst is 5–50 µm. The first average particle size is 3–54 times the second average particle size. The weight ratio of the large-particle-size catalyst to the small-particle-size catalyst is 5:1 to 1:5, and each of the large-particle-size catalyst and the small-particle-size catalyst is manganese dioxide.

10. The catalyst layer of claim 9, wherein the catalyst layer is used to manufacture the electrode.

Citation Information

Patent Citations

  • Catalyst for electrochemical oxygen reduction and / or oxygen generation

    JP2015192986A

  • Catalyst layer

    US20170033369A1

  • catalyst

    US20200321622A1