A catalytic cracking reaction method, a catalytic cracking reaction aid and a preparation method thereof, and a catalytic cracking catalyst

By using copper-containing oxide additives for self-heating and pretreatment in the catalytic cracking reaction, the problems of insufficient catalyst heat capacity and molecular sieve damage are solved, the reaction temperature and the yield of high-value products are increased, and the catalyst activity is maintained.

CN116023979BActive Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111256530.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-27
Publication Date
2024-10-15
Estimated Expiration
2041-10-27

Smart Images

  • Figure CN116023979B_ABST
    Figure CN116023979B_ABST
Patent Text Reader

Abstract

The present disclosure relates to a method for catalytic cracking reaction, a catalytic cracking reaction aid, a preparation method thereof and a catalytic cracking catalyst, wherein the crude oil is contacted with the catalytic cracking aid and the catalytic cracking main agent in a catalytic cracking reactor to carry out a catalytic cracking reaction; wherein, based on the total weight of the catalytic cracking aid, the catalytic cracking aid comprises 20-60% by weight of a first carrier, 10-40% by weight of a first binder and 1-40% by weight of a copper-containing oxide in terms of weight percentage. The above method uses a catalytic cracking aid using a copper-containing oxide as a heat-generating material, and the catalytic cracking aid can self-heat by self-oxidation and reduction of copper, provide heat for the catalytic cracking reaction, increase the catalytic cracking reaction temperature, and increase the yield of high-value products, and avoids catalyst damage caused by the molecular sieve and the heat-generating material being in the same particle.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the field of catalytic cracking, and in particular, to a catalytic cracking reaction method, a catalytic cracking reaction aid and a preparation method thereof, and a catalytic cracking catalyst. Background Art

[0002] The catalytic cracking unit is the core equipment of the secondary processing of the refinery. It is a process that converts the distillate oil or residual oil obtained from the atmospheric and vacuum tower into fuels such as liquefied gas, gasoline, diesel, or chemical raw materials such as ethylene, propylene, butene, BTX, etc. under the action of catalysts and high temperature. The catalyst is not only the reaction active center of the catalytic cracking reaction, but also the heat and mass transfer carrier of the catalytic cracking regeneration system. The catalyst enters the reactor from the high-temperature regenerator and brings in a large amount of heat, which promotes the occurrence of catalytic cracking reaction. The coke generated by the reaction is loaded on the surface of the catalyst. Then, when entering the regenerator, it burns with oxygen in the air to generate a large amount of heat, completing the transfer and generation of heat.

[0003] With the heavy and inferior processing raw materials, and the requirement for the transformation of oil refining equipment to chemical type, the reaction conditions are more stringent. However, the heat capacity of the catalyst is limited, resulting in limited heat provided to the reaction part, so the reaction temperature is difficult to further increase; at the same time, in order to transfer more heat, the catalyst-oil ratio also increases, which will bring some adverse effects. For this reason, some studies have used heat-generating materials to increase the conversion depth without increasing the catalyst-oil ratio.

[0004] So far, the existing heat-generating materials cannot achieve satisfactory reaction effects when used in catalytic cracking. Summary of the invention

[0005] The purpose of the present disclosure is to provide a catalytic cracking reaction method, a catalytic cracking reaction aid and a preparation method thereof, and a catalytic cracking catalyst. The catalytic cracking aid has a higher calorific value and avoids catalyst damage caused by the molecular sieve and the heat-generating material being in the same particle.

[0006] In order to achieve the above object, the present disclosure provides a method for catalytic cracking reaction in a first aspect, the method comprising:

[0007] The crude oil is brought into contact with a catalytic cracking aid and a catalytic cracking main agent in a catalytic cracking reactor to carry out a catalytic cracking reaction;

[0008] Wherein, based on the total weight of the catalytic cracking aid, the catalytic cracking aid comprises, by weight percentage, 20-60% by weight of a first carrier, 10-40% by weight of a first binder and 1-40% by weight of a copper-containing oxide.

[0009] Optionally, the first carrier comprises one or more of kaolin, montmorillonite, diatomaceous earth, attapulgite, sepiolite, halloysite, hydrotalcite, bentonite and rectorite;

[0010] The first binder includes one or more of aluminum oxide, silicon oxide and aluminum phosphate;

[0011] The copper-containing oxide is copper oxide and / or cuprous oxide.

[0012] Optionally, the method further comprises: before the contacting, subjecting the catalytic cracking aid to reduction pretreatment to obtain a catalytic cracking aid in a reduced state;

[0013] Optionally, the reduction pretreatment comprises: contacting the catalytic cracking aid with a reducing gas, the time of the reduction pretreatment is 0.5-3 minutes, the temperature of the reduction pretreatment is 650-700°C; the reducing gas comprises one or more of hydrogen, ethylene and methane.

[0014] Optionally, based on the weight of copper element, the low-valent copper on the surface of the reduced catalytic cracking aid accounts for more than 70% of the total weight of the surface copper element, and the low-valent copper is +1-valent copper.

[0015] Optionally, the temperature of the catalytic cracking reaction is 450-650°C, and the catalyst-oil ratio is 5-20;

[0016] The weight ratio of the catalytic cracking aid to the catalytic cracking main agent is 0.01-0.5.

[0017] Optionally, the method comprises:

[0018] Separating reaction oil gas and spent catalytic material from a product mixture obtained by catalytic cracking reaction, and obtaining a regenerated catalytic material after regenerating the spent catalytic material;

[0019] Optionally, the regeneration process comprises the following steps:

[0020] a. allowing the catalytic material to be regenerated to enter a regenerator for regeneration treatment to obtain a regenerated catalytic material comprising a regenerated catalyst and an oxidized catalytic cracking aid;

[0021] b. returning the regenerated catalytic material to the catalytic cracking reactor for continued use or returning the regenerated catalytic material to the catalytic cracking reactor for continued use after reduction.

[0022] A second aspect of the present disclosure provides a catalytic cracking catalyst, the catalytic cracking catalyst comprising catalytic particles and heat-generating particles;

[0023] Based on the total weight of the heat-generating particles, the heat-generating particles include 20-60 wt % of the second carrier, 10-40 wt % of the second binder and 1-40 wt % of the copper-containing oxide.

[0024] Optionally, based on the total weight of the catalytic particles, the catalytic particles contain 10-40 wt % of the molecular sieve, 30-60 wt % of the third carrier and 20-40 wt % of the third binder in terms of weight percentage;

[0025] Optionally, the molecular sieve includes one or more of a FAU structure molecular sieve, an MFI structure molecular sieve and a BEA structure molecular sieve;

[0026] The copper-containing oxide includes copper oxide and / or cuprous oxide;

[0027] The second binder and the third binder are the same or different and independently include one or more of aluminum oxide, silicon oxide and aluminum phosphate;

[0028] The second carrier and the third carrier are the same or different, and independently include one or more of kaolin, montmorillonite, diatomaceous earth, attapulgite, sepiolite, halloysite, hydrotalcite, bentonite and rectorite;

[0029] Optionally, the weight ratio of the heat-generating particles to the catalytic particles is 0.01-0.5.

[0030] A third aspect of the present disclosure provides a catalytic cracking reaction aid, which comprises, based on the total weight of the catalytic cracking reaction aid, 20-60 wt % of a fourth carrier, 10-40 wt % of a fourth binder and 1-40 wt % of a copper-containing oxide in terms of weight percentage.

[0031] Optionally, the copper-containing oxide includes copper oxide and / or cuprous oxide;

[0032] The fourth carrier comprises one or more of kaolin, montmorillonite, diatomite, attapulgite, sepiolite, halloysite, hydrotalcite, bentonite and rectorite;

[0033] The fourth binder includes one or more of aluminum oxide, silicon oxide and aluminum phosphate.

[0034] Optionally, based on the weight of copper element, the low-valent copper on the surface of the catalytic cracking reaction aid accounts for more than 70% of the total weight of the surface copper element, and the low-valent copper is +1-valent copper.

[0035] The fourth aspect of the present disclosure provides a method for preparing the catalytic cracking reaction aid according to the third aspect of the present disclosure, the method comprising the following steps:

[0036] S1, mixing the copper-containing material, the fifth binder and the fourth carrier to obtain a mixed slurry;

[0037] S2, spray drying the mixed slurry and then calcining;

[0038] Wherein, based on the total dry weight of the mixed slurry, the mixed slurry includes, by weight percentage, 1-40 weight % of the copper-containing substance, 1-40 weight % of the fifth binder and 20-60 weight % of the fourth carrier, the content of the copper-containing substance is calculated by the weight of copper oxide, the content of the fifth binder is calculated by the weight of metal oxide, and the copper-containing substance includes copper oxide and / or copper salt.

[0039] Optionally, the copper-containing oxide includes copper oxide and / or cuprous oxide;

[0040] The copper salt includes one or more of copper sulfate, copper chloride, copper nitrate and copper carbonate;

[0041] The fifth binder includes one or more of aluminum sol, silica sol, phosphate aluminum sol and peptized pseudo-boehmite. The solid content of the fifth binder is 20-90% by weight based on metal oxide.

[0042] Optionally, the calcination conditions are: temperature of 500-700° C. and time of 2-5 h.

[0043] Through the above technical scheme, the method of catalytic cracking reaction of the present application uses a catalytic cracking aid with a copper-containing oxide as a heat-generating material, and the catalytic cracking aid can generate heat by self-oxidation and reduction, provide heat for the catalytic cracking reaction, increase the catalytic cracking reaction temperature, and increase the yield of high-value products. Compared with the method in which the copper-containing oxide and the molecular sieve are in the same particle, the method of the present application avoids direct contact between the alkaline copper-containing oxide and the acidic molecular sieve, and can avoid damage to the molecular sieve while ensuring a high calorific value, thereby avoiding the influence on the catalytic activity of the catalyst.

[0044] Other features and advantages of the present disclosure will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] The accompanying drawings are used to provide a further understanding of the present disclosure and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present disclosure but do not constitute a limitation of the present disclosure. In the accompanying drawings:

[0046] Figure 1 This is the H2-TPR curve of the catalytic cracking reaction aid Z-15-1 of Example 6 of the present application. DETAILED DESCRIPTION

[0047] The specific implementation of the present disclosure is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described herein is only used to illustrate and explain the present disclosure, and is not used to limit the present disclosure.

[0048] A first aspect of the present disclosure provides a method for catalytic cracking reaction, the method comprising:

[0049] The crude oil is brought into contact with a catalytic cracking aid and a catalytic cracking main agent in a catalytic cracking reactor to carry out a catalytic cracking reaction;

[0050] Wherein, based on the total weight of the catalytic cracking aid, the catalytic cracking aid comprises, by weight percentage, 20-60% by weight of a first carrier, 10-40% by weight of a first binder and 1-40% by weight of a copper-containing oxide.

[0051] In the present disclosure, the catalytic cracking aid is reduced by the dry gas produced by the catalytic cracking reaction after entering the reactor, and the dry gas includes reducing gases such as hydrogen and ethylene. At this time, the copper element in the catalytic cracking aid is converted into a reduced state under the action of the reducing gas.

[0052] In one embodiment of the present disclosure, the method further includes: before contacting, subjecting the catalytic cracking aid to reduction pretreatment to obtain a reduced catalytic cracking aid; the reduction pretreatment includes: contacting the catalytic cracking aid with a reducing gas, the reduction pretreatment time is 0.5-3 minutes, and the reduction pretreatment temperature is 650-700°C; the reducing gas includes one or more of hydrogen, ethylene and methane. When the catalytic cracking aid that has undergone reduction pretreatment is used in a catalytic cracking reaction, it is beneficial to optimize the product distribution and further improve the yield of high-value products.

[0053] In the present disclosure, the low-valent copper on the surface of the reduced catalytic cracking aid accounts for more than 70% of the total weight of the surface copper element, measured by the weight of the copper element, and the low-valent copper is +1-valent copper. When the catalytic cracking aid meeting the above low-valent copper content is used in a catalytic cracking reaction, the product distribution is good and the yield of high-value products is high. The above content is tested by XPS.

[0054] In one embodiment of the present disclosure, the temperature of the catalytic cracking reaction is 450-650°C, preferably 500-600°C; the catalyst-oil ratio is 5-20, preferably 5-15; the weight ratio of the catalytic cracking aid to the catalytic cracking reaction catalyst is 0.01-0.5, preferably 0.01-0.2.

[0055] In the present disclosure, the agent-oil ratio refers to the mass ratio of the total mass of the catalytic cracking main agent and the catalytic cracking auxiliary agent to the mass ratio of the feedstock oil.

[0056] In one embodiment of the present disclosure, the weight ratio of the catalytic cracking aid to the catalytic cracking main agent is 0.01-0.5.

[0057] In one embodiment of the present disclosure, the method includes:

[0058] Reaction oil and gas and catalytic material to be regenerated are separated from the product mixture obtained from the catalytic cracking reaction, and the catalytic material to be regenerated is obtained after the catalytic material to be regenerated.

[0059] In one embodiment of the present disclosure, the regeneration process comprises the following steps:

[0060] a. allowing the catalytic material to be regenerated to enter a regenerator for regeneration treatment to obtain a regenerated catalytic material comprising a regenerated catalyst and an oxidized catalytic cracking aid;

[0061] b. Returning the regenerated catalytic material to the catalytic cracking reactor for continued use;

[0062] The temperature of the regeneration treatment is 650-750°C, preferably 670-730°C.

[0063] In the present disclosure, the regeneration method may be, for example, introducing oxygen into the regenerator to oxidize the copper element in the catalytic material to be regenerated.

[0064] In the present disclosure, the type of feedstock oil used in the catalytic cracking reaction is conventional in the art and is not specifically required. The feedstock oil may include, for example, one or more of hydrotreated oil, atmospheric residue oil, hydrogenated residue oil, coker wax oil, and vacuum residue oil. Specifically, the feedstock oil may be hydrogenated residue oil.

[0065] A second aspect of the present disclosure provides a catalytic cracking catalyst, the catalytic cracking catalyst comprising catalytic particles and heat-generating particles;

[0066] Based on the total weight of the heat-generating particles, the heat-generating particles include 20-60 wt % of the second carrier, 10-40 wt % of the second binder and 1-40 wt % of the copper-containing oxide.

[0067] In one embodiment of the present disclosure, based on the total weight of the catalytic particles, the catalytic particles comprise 10-40 wt% of the molecular sieve, 30-60 wt% of the third carrier and 20-40 wt% of the third binder in terms of weight percentage.

[0068] In one embodiment of the present disclosure, the weight ratio of the heat generating particles to the catalytic particles is 0.01-0.5, preferably 0.01-0.2.

[0069] In one embodiment of the present disclosure, the molecular sieve includes one or more of a FAU structure molecular sieve, an MFI structure molecular sieve and a BEA structure molecular sieve. For example, it can be one or more of a Y molecular sieve, a ZSM-5 molecular sieve, and a β molecular sieve. Further, the Y molecular sieve includes one or more of HY, REY, REHY, USY, and a Y molecular sieve containing phosphorus elements and rare earth elements. The ZSM-5 molecular sieve includes one or more of HZSM-5, a ZSM-5 molecular sieve containing phosphorus elements and transition metal elements, and a ZRP molecular sieve, and the transition metal may include one or more of Fe elements, Co elements, Ni elements, Mn elements, Ti elements, Zn elements, Cu elements, Ga elements, and Re elements.

[0070] In the present disclosure, the average particle size of the catalytic particles is 70-90 μm.

[0071] A third aspect of the present disclosure provides a catalytic cracking reaction aid, which comprises, based on the total weight of the catalytic cracking reaction aid, 20-60 wt % of a fourth carrier, 10-40 wt % of a fourth binder and 1-40 wt % of a copper-containing oxide in terms of weight percentage.

[0072] The catalytic cracking reaction aid disclosed in the present invention uses copper-containing oxide as a heat-generating material and generates heat by self-heating through the following redox reaction cycle to provide heat for the catalytic cracking reaction.

[0073] 2Cu+O2→2CuO ΔH=-156KJ / mol=1914J / g

[0074] CuO+2H2→Cu+2H2O ΔH=-95KJ / mol=1190J / g

[0075] In one embodiment of the present disclosure, the low-valent copper on the surface of the catalytic cracking reaction aid accounts for more than 70% of the total weight of the surface copper element, based on the weight of the copper element, and the low-valent copper is +1-valent copper. The above content is tested by XPS.

[0076] The fourth aspect of the present disclosure provides a method for preparing the catalytic cracking reaction aid according to the third aspect of the present disclosure, the method comprising the following steps:

[0077] S1, mixing the copper-containing material, the fifth binder and the fourth carrier to obtain a mixed slurry;

[0078] S2, drying and then calcining the mixed slurry;

[0079] Wherein, based on the total dry weight of the mixed slurry, the mixed slurry includes, by weight percentage, 1-40 weight % of the copper-containing substance, 1-40 weight % of the fifth binder and 20-60 weight % of the fourth carrier, the content of the copper-containing substance is calculated by the weight of copper oxide, the content of the fifth binder is calculated by the weight of metal oxide, and the copper-containing substance includes copper oxide and / or copper salt.

[0080] In the present disclosure, copper-containing oxides include copper oxide and / or cuprous oxide; copper salts include one or more of copper sulfate, copper chloride, copper nitrate and copper carbonate; preferably, copper-containing substances include copper sulfate and / or copper chloride. Further, no matter which copper-containing substance is selected, after drying and roasting, the copper element mainly exists in the form of copper oxide.

[0081] In one embodiment of the present disclosure, the fifth binder includes one or more of aluminum sol, silica sol, phosphate aluminum sol and peptized pseudo-boehmite, and the solid content of the fifth binder is 20-90% by weight, such as 20-40% by weight, calculated as metal oxide.

[0082] In one embodiment of the present disclosure, the calcination conditions are: temperature of 500-700° C. and time of 2-5 h.

[0083] In the present disclosure, the method for preparing a catalytic cracking reaction aid further comprises treating the catalytic cracking reaction aid pre-product obtained after roasting with an ammonium sulfate solution, wherein the ratio of ammonium sulfate, the catalytic cracking reaction aid pre-product on a dry basis and water is (0.3-0.7):1:(8-12), and then rinsing with deionized water, filtering, drying and secondary roasting to obtain the catalytic cracking reaction aid. The secondary roasting temperature is 600-800°C and the time is 3-6h.

[0084] In the present disclosure, the first carrier, the second carrier, the third carrier and the fourth carrier are the same or different, and independently include one or more of kaolin, montmorillonite, diatomaceous earth, attapulgite, sepiolite, halloysite, hydrotalcite, bentonite and rectorite; the first binder, the second binder, the third binder and the fourth binder are the same or different, and independently include one or more of alumina, silicon oxide and aluminum phosphate.

[0085] The catalytic cracking main agent used in the first aspect of the present disclosure is conventional in the art, for example, having the same composition and structure as the catalytic particles in the second aspect of the present disclosure.

[0086] The present invention will be further described below by way of examples, but the present invention is not limited thereto. The instruments and reagents used in the examples and comparative examples of the present invention are commonly used by those skilled in the art unless otherwise specified.

[0087] In the present disclosure, the content of the carrier, the content of the binder and the content of the copper-containing oxide are calculated based on the feed amount.

[0088] The FAU structure molecular sieve used in the examples and comparative examples is DASY2.0, and the catalytic cracking main agent is COKC-1, both of which are products of Sinopec Catalyst Company.

[0089] Examples 1-4

[0090] On a dry basis, the components were weighed according to the ratio shown in Table 1, and the catalytic cracking reaction aid was prepared according to the following steps.

[0091] The fourth carrier kaolin is prepared into a slurry with a solid content of 30 wt% with decationized water, and the slurry is stirred evenly. The pH of the slurry is adjusted to 2.5 with hydrochloric acid, and the pH value is maintained. After standing and aging at 50°C for 1 hour, aluminum sol (alumina content is 21.5 wt%) is added, and stirred for 1 hour to form a colloid. Copper chloride is added to form a mixed slurry.

[0092] After continued stirring, the mixed slurry was spray dried to prepare a microsphere catalytic cracking reaction aid precursor. The microsphere catalytic cracking reaction aid precursor was then calcined at 500°C for 1 hour to obtain a catalytic cracking reaction aid pre-product. It was then washed with an ammonium sulfate solution at 60°C (the mass ratio of ammonium sulfate, catalytic cracking reaction aid pre-product on a dry basis and water was 0.5:1:10) until the sodium oxide content was less than 0.25% by weight. After that, it was rinsed with deionized water and filtered, dried, and calcined at 650°C for 3h to obtain catalytic cracking reaction aids Z-12 to Z-15. XPS was used to test the proportion of low-valent copper on the surface of catalytic cracking reaction aids Z-12 to Z-15 to the total weight of copper elements on the surface area, and the results are listed in Table 2.

[0093] Example 5

[0094] On a dry basis, each component was weighed according to the ratio shown in Table 1, and a catalytic cracking reaction aid Z-16 was prepared according to the steps of Example 1, except that copper sulfate was used instead of copper chloride as the copper-containing substance. XPS was used to test the ratio of low-valent copper on the surface of the catalytic cracking reaction aid Z-16 to the total weight of copper elements on the surface area, and the results are listed in Table 2.

[0095] Example 6

[0096] Before entering the reactor, 20% hydrogen (the rest is nitrogen) by mass was used as a reducing gas to reduce the catalytic cracking reaction aid Z-15 prepared in Example 4, and the pre-reduction treatment was carried out at 650° C. for 2 minutes to obtain the catalytic cracking reaction aid Z-15-1. XPS was used to test the proportion of low-valent copper on the surface of the catalytic cracking reaction aid Z-15-1 to the total weight of copper elements on the surface area, and the results are listed in Table 2. Figure 1 This is the H2-TPR curve of the catalytic cracking reaction aid Z-15-1 of Example 6.

[0097] The H2-TPR curve was measured by the ChemBetPulsar TPR / TPD produced by Micromertics, USA. The test method is as follows: the sample mass is 10 mg, placed in a U-shaped quartz tube, heated to 200°C at 10°C / min in He gas, kept constant at 200°C for 30 minutes, then cooled to 100°C, and reduced gas was introduced at a gas flow rate of 120 cm / min. 3 / min, and then heated to 1000℃ at a rate of 10℃ / min.

[0098] The instrument model for testing the proportion of low-priced copper is ESCALab250 X-ray photoelectron spectrometer.

[0099] Examples 7-12

[0100] Catalytic cracking catalysts A-12 to A-16 and A-15-1 were obtained by mixing catalytic cracking reaction aids Z-12 to Z-16 and Z-15-1 with a catalytic cracking agent at a weight ratio of 1:19, and aging them at 800°C with 100% steam for 12 hours. The catalytic cracking agent was a fresh industrial agent. Based on the total weight of the catalytic cracking agent, the catalytic cracking agent contained 28% by weight of alumina, 40% by weight of kaolin and 32% by weight of a FAU structured molecular sieve. The properties of the catalytic cracking agent are listed in Table 3.

[0101] Comparative Example 1

[0102] On a dry basis, each component was weighed according to the ratio shown in Table 1, and a catalytic cracking reaction aid Z-1 was prepared according to the steps of Example 1, except that the catalytic cracking reaction main agent of Comparative Example 1 did not contain a copper-containing substance. XPS was used to test the ratio of low-valent copper on the surface of the catalytic cracking reaction aid Z-1 to the total weight of copper elements on the surface area, and the results are listed in Table 2.

[0103] Table 1

[0104]

[0105] Comparative Example 2

[0106] Catalytic cracking catalyst D was prepared by the method of Example 1, except that the copper-containing oxide and the molecular sieve were in the same particle, and based on the total weight of the catalytic cracking catalyst, the catalytic cracking catalyst contained 1 wt% of the copper-containing oxide, 30.4 wt% of the FAU structure molecular sieve, 27.6 wt% of alumina and 41 wt% of kaolin in terms of weight ratio. XPS was used to test the ratio of low-valent copper on the surface of the catalytic cracking catalyst D to the total weight of copper elements on the surface area, and the results are listed in Table 2.

[0107] Comparative Example 3

[0108] The catalytic cracking catalyst A-1 was prepared by the method of Example 7, except that the catalytic cracking aid Z-1 prepared in Comparative Example 1 was used as the catalytic cracking aid.

[0109] Table 3

[0110] Analyze Project Industrial freshener Elemental composition, weight % - <![CDATA[Na2O]]> 0.14 <![CDATA[Al2O3]]> 55.7 <![CDATA[SiO2]]> 36.8 <![CDATA[RE2O3,%]]> 2.7 Apparent bulk density / (g / mL) 0.79 Drip hole / (mL / g) 0.37 <![CDATA[BET specific surface area, m 2 / g]]> 237 <![CDATA[Matrix area, m 2 / g]]> 89 <![CDATA[Micropore area, m 2 / g]]> 149 Total pore volume, mL / g 0.18 Micropore volume, mL / g 0.069 Particle size distribution, % - 0-20μm 1.9 0-40μm 17.2 0-80μm 61.7 0-105μm 79.8 0-149μm 94.8 APS 68.3

[0111] Test Example 1

[0112] The catalytic cracking reaction catalysts A-12 to A-16, A-15-1, A-1, and D prepared above were subjected to the ACE evaluation of the feedstock oil. The properties of the evaluated feedstock oil are shown in Table 4 below.

[0113] Table 4

[0114]

[0115]

[0116] The catalytic cracking catalysts prepared in Examples 7-12 and Comparative Examples 2 and 3 were fed into a catalytic cracking fixed fluidized bed micro-ACE reactor for catalytic cracking reaction. The reaction starting temperature was set at 530°C, the catalyst-oil ratio was 5, the measurement point of the bed temperature after the reaction was in the middle of the bed of the reactor, and the end of the reaction was 70s after the feed oil was introduced. The reaction temperature control point was in the middle of the reactor. The reaction temperature changes were recorded and listed in Table 2.

[0117] Table 2

[0118]

[0119] Since the heat generated during the reduction of copper is not included in Table 2, the temperature change value of the reduced additive Z-15-1 is small. In actual production, the heat generated by this part of the reduction can be used.

[0120] The low-valent copper ratio in Table 2 refers to the ratio of +1-valent copper on the surface of the catalytic cracking aid to the total amount of copper elements on the surface.

[0121] According to the data in Table 2, the catalytic cracking reaction aid using the copper-containing oxide of the present application as a heat-generating material is used for a catalytic cracking reaction, and when it is in different particles from the molecular sieve, its heat-generating effect is significant compared to the catalytic cracking reaction aid without the copper-containing oxide.

[0122] Test Example 2

[0123] The distribution of catalytic cracking products of catalytic cracking catalysts A-1, A-15, A-15-1 and D was analyzed by Agilent 6890GC (TCD detector) online composition analysis; liquid products were collected and weighed offline, and simulated distillation analysis and PONA analysis were performed; ACE device was equipped with a CO2 converter and an online CO2 infrared detector for online analysis of the total amount of coke generated; the mass of all products was normalized and the material balance was calculated, and the results are listed in Table 5. Among them, the conversion rate refers to the conversion rate calculated for products other than slurry oil and diesel.

[0124] Table 5

[0125] Catalyst No. A-1 A-15 A-15-1 D Additive No. Z-1 Z-15 Z-15-1 - Yield / wt% - - - - Dry gas 4.92 5.18 4.65 5.62 Liquefied gas 25.54 22.62 24.36 19.63 Coke 7.29 11.58 8.34 16.57 gasoline 24.42 22.24 23.86 18.9 diesel fuel 16.63 15.93 17.18 17.45 Oil slurry 21.19 22.46 21.61 21.83 Conversion rate / wt% 62.18 61.62 61.21 60.72

[0126] According to the data of Tables 2 and 5, the catalytic cracking catalyst A-1 that does not contain copper oxides, although the yield of high-value products such as liquefied gas and gasoline is high, its heating effect is not good; the catalyst A-15-1 that has been pretreated by reduction, relative to the catalyst A-15 that has not been pretreated by reduction, can maintain a better product distribution while ensuring the heating effect, and the yield of high-value products such as liquefied gas and gasoline is high. In addition, according to the data of catalyst D, when the heating material and the molecular sieve are in different particles, the catalytic performance of the main agent is less affected, the coke is lower, and the yield of high-value products such as gasoline and liquefied gas is higher. Therefore, before carrying out the catalytic cracking reaction, the catalytic cracking reaction aid of the present application is pretreated by reduction, and the heating material and the molecular sieve are in different particles, so as to achieve the effect of optimizing the product distribution while maintaining a high calorific value.

[0127] The preferred embodiments of the present disclosure are described in detail above in conjunction with the accompanying drawings; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.

[0128] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.

[0129] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.

Claims

1. A method for catalytic cracking reaction, characterized in that: The method includes: The crude oil is brought into contact with a catalytic cracking aid and a catalytic cracking main agent in a catalytic cracking reactor to carry out a catalytic cracking reaction; Wherein, based on the total weight of the catalytic cracking aid, the catalytic cracking aid comprises, by weight percentage, 20-60% by weight of the first carrier, 10-40% by weight of the first binder and 1-40% by weight of the copper-containing oxide; The method further comprises: before the contacting, subjecting the catalytic cracking aid to reduction pretreatment to obtain a reduced catalytic cracking aid; Calculated by the weight of copper element, the low-valent copper on the surface of the reduced catalytic cracking aid accounts for more than 70% of the total weight of the surface copper element, and the low-valent copper is +1-valent copper.

2. The method according to claim 1, wherein: The first carrier comprises one or more of kaolin, montmorillonite, diatomaceous earth, attapulgite, sepiolite, halloysite, hydrotalcite, bentonite and rectorite; The first binder includes one or more of aluminum oxide, silicon oxide and aluminum phosphate; The copper-containing oxide is copper oxide and / or cuprous oxide.

3. The method according to claim 1, wherein: The reduction pretreatment comprises: contacting the catalytic cracking aid with a reducing gas, the time of the reduction pretreatment is 0.5-3 minutes, the temperature of the reduction pretreatment is 650-700° C.; the reducing gas comprises one or more of hydrogen, ethylene and methane.

4. The method according to claim 1, wherein: The temperature of the catalytic cracking reaction is 450-650°C, and the catalyst-oil ratio is 5-20; The weight ratio of the catalytic cracking aid to the catalytic cracking main agent is 0.01-0.

5.

5. The method according to claim 1, wherein: The method includes: Reaction oil and gas and catalytic material to be regenerated are separated from the product mixture obtained from the catalytic cracking reaction, and the catalytic material to be regenerated is obtained after the catalytic material to be regenerated.

6. The method according to claim 5, wherein: The regeneration process comprises the following steps: a. allowing the catalytic material to be regenerated to enter a regenerator for regeneration treatment to obtain a regenerated catalytic material comprising a regenerated catalyst and an oxidized catalytic cracking aid; b. returning the regenerated catalytic material to the catalytic cracking reactor for continued use or returning the regenerated catalytic material to the catalytic cracking reactor for continued use after reduction.

7. A catalytic cracking catalyst, characterized in that: The catalytic cracking catalyst comprises a catalytic cracking main agent and a catalytic cracking auxiliary agent; Based on the total weight of the catalytic cracking aid, the catalytic cracking aid comprises, by weight percentage, 20-60% by weight of a first carrier, 10-40% by weight of a first binder and 1-40% by weight of a copper-containing oxide; Calculated by the weight of copper element, the low-valent copper on the surface of the catalytic cracking aid accounts for more than 70% of the total weight of the surface copper element, and the low-valent copper is +1-valent copper.

8. The catalytic cracking catalyst according to claim 7, wherein Based on the total weight of the catalytic cracking main agent, the catalytic cracking main agent comprises 10-40 wt % of molecular sieve, 30-60 wt % of the second carrier and 20-40 wt % of the second binder in terms of weight percentage.

9. The catalytic cracking catalyst according to claim 8, wherein The molecular sieve includes one or more of a FAU structure molecular sieve, an MFI structure molecular sieve and a BEA structure molecular sieve; The copper-containing oxide includes copper oxide and / or cuprous oxide; The first binder and the second binder are the same or different, and independently include one or more of aluminum oxide, silicon oxide and aluminum phosphate; The first carrier and the second carrier are the same or different, and independently include one or more of kaolin, montmorillonite, diatomaceous earth, attapulgite, sepiolite, halloysite, hydrotalcite, bentonite and rectorite.

10. The catalytic cracking catalyst according to claim 8, wherein The weight ratio of the catalytic cracking aid to the catalytic cracking main agent is 0.01-0.

5.

11. A catalytic cracking reaction aid, characterized in that: Based on the total weight of the catalytic cracking reaction aid, the catalytic cracking reaction aid comprises, by weight percentage, 20-60% by weight of a first carrier, 10-40% by weight of a first binder and 1-40% by weight of a copper-containing oxide; Calculated by the weight of copper element, the low-valent copper on the surface of the catalytic cracking reaction aid accounts for more than 70% of the total weight of the surface copper element, and the low-valent copper is +1-valent copper.

12. The method for preparing the catalytic cracking reaction aid according to claim 11, characterized in that: The method comprises the following steps: S1, mixing a copper-containing material, a first binder precursor and a first carrier to obtain a mixed slurry; S2, spray drying the mixed slurry and then calcining; Wherein, based on the total dry weight of the mixed slurry, the mixed slurry includes, by weight percentage, 1-40 weight % of the copper-containing substance, 1-40 weight % of the fifth binder and 20-60 weight % of the first carrier, the content of the copper-containing substance is calculated by the weight of copper oxide, the content of the first binder precursor is calculated by the weight of metal oxide, and the copper-containing substance includes copper oxide and / or copper salt.

13. The method according to claim 12, wherein: The copper-containing oxide includes copper oxide and / or cuprous oxide; The copper salt includes one or more of copper sulfate, copper chloride, copper nitrate and copper carbonate; The first binder precursor comprises one or more of aluminum sol, silica sol, phosphate aluminum sol and peptized pseudo-boehmite. The solid content of the first binder precursor is 20-90% by weight based on metal oxide.

14. The method according to claim 12, wherein: The calcination conditions are: temperature of 500-700° C. and time of 2-5 hours.