A phosphonate flame retardant, its preparation method and application
The preparation of phosphonate flame retardants by direct precipitation method solves the problems of poor dispersibility and thermal stability of alkylphosphonate flame retardants, and achieves the effects of narrow particle size distribution, good dispersibility and high thermal stability, thereby improving the flame retardant performance of polymer materials.
Patent Information
- Application Number
- CN202211731696.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-30
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2042-12-30
AI Technical Summary
Existing alkylphosphinate flame retardants suffer from poor dispersibility and thermal stability, leading to uneven processing and low thermal decomposition temperatures.
A direct precipitation method was used, in which an aqueous solution of alkyl phosphonates and an aqueous solution of soluble aluminum salts were simultaneously added to a stirred reaction vessel. After mixing and precipitation, the mixture was filtered, washed, and dried. The reaction temperature and time were controlled to obtain a phosphonate flame retardant with narrow particle size distribution, good dispersibility, and high thermal stability.
The prepared phosphonate flame retardant has a narrow particle size distribution, good dispersibility, high thermal stability, and low heat loss rate, which can significantly improve the flame retardant performance of polymer materials.
Smart Images

Figure BDA0004031792060000081 
Figure BDA0004031792060000082 
Figure BDA0004031792060000091
Abstract
Description
Technical Field
[0001] This invention relates to the field of halogen-free phosphorus flame retardant technology, and more specifically, to a phosphonate flame retardant, its preparation method, and its application. Background Technology
[0002] Flame retardants are widely used in daily life, from mobile phones and carpets to various heat insulation sheets. Their purpose is to prevent combustion or slow the spread of fire in emergencies. With increasing environmental and health awareness, flame retardants are showing a trend towards improving flame retardant performance while also prioritizing environmental protection and ecological safety. Against this backdrop, some traditional flame retardants have faced increasing pressure from stringent environmental and flame retardant regulations, prompting the emergence of new flame retardant materials with low heat release rates, low smoke production, and low toxicity. Alkyl phosphines, with their advantages of being halogen-free and environmentally friendly, and their ability to achieve high flame resistance, are becoming effective alternatives to halogenated flame retardants. Alkyl phosphines are halogen-free, low-toxicity flame retardants that have been widely adopted.
[0003] Existing methods for preparing alkylphosphinates involve adding soluble aluminum salts dropwise into an alkylphosphinate solution over a specific time period. This method has the following drawbacks: the concentration of alkylphosphinates changes continuously during the reaction; due to the extremely rapid reaction, crystal nuclei form in a very short time, inhibiting crystal growth and resulting in small crystal particles. Furthermore, crystal agglomeration leads to a wide particle size distribution, resulting in poor dispersibility of the alkylphosphinate flame retardant during polymer processing, leading to uneven feeding and poor flame retardant performance of the polymer. Additionally, after washing, filtering, and drying, the product exhibits caking, resulting in a low thermal decomposition temperature and poor thermal stability.
[0004] Therefore, it is urgent to provide an alkylphosphine salt flame retardant with narrow particle size distribution and high thermal stability. Summary of the Invention
[0005] The technical problem to be solved by the present invention is to overcome the defects and shortcomings of existing alkylphosphinates in terms of poor dispersibility and poor thermal stability, and to provide a method for preparing phosphinate flame retardants. By simultaneously adding an aqueous solution of alkylphosphinate and an aqueous solution of soluble aluminum salt into a container and stirring, mixing and precipitating, the obtained phosphinate flame retardant has high yield, narrow particle size distribution, good dispersibility, high thermal stability, resistance to yellowing and low heat loss rate.
[0006] Another object of the present invention is to provide a phosphonate flame retardant.
[0007] Another object of the present invention is to provide an application of phosphonate flame retardants in improving the flame retardant properties of polymers.
[0008] The above-mentioned objective of this invention is achieved through the following technical solution:
[0009] A method for preparing a phosphonate flame retardant includes the following steps:
[0010] S1. Prepare aqueous solutions of alkyl phosphonates and soluble aluminum salts, respectively;
[0011] S2. The aqueous solutions of alkyl phosphonates and soluble aluminum salts are simultaneously and continuously added to the reaction vessel, stirred, mixed and precipitated. After the addition is completed, the mixture is filtered, washed and dried to obtain the phosphonate flame retardant.
[0012] In S1, the mass concentration of the alkyl phosphonate aqueous solution is 25-40%; the mass concentration of the soluble aluminum salt aqueous solution is 20-40%.
[0013] In S2, the molar ratio of alkylphosphinate in the aqueous solution to soluble aluminum salt in the aqueous solution is (6-8):1.
[0014] The reaction temperature is 20–100℃, and the reaction time is 0.5–3 h.
[0015] This invention discloses a preparation process for a phosphonate flame retardant. The preparation process is a direct precipitation method, in which an aqueous solution of an alkyl phosphonate and an aqueous solution of a soluble aluminum salt are simultaneously added to a container, stirred, mixed, precipitated, filtered, washed, and dried to obtain the flame retardant. The process of this invention results in a high product yield, narrow particle size distribution, good dispersibility, high resistance to yellowing, and high thermal stability.
[0016] The process of this invention maintains stable concentration and medium conditions in the reaction system during the reaction process, resulting in stable product quality; at the same time, the process is simple and the production operation process is straightforward.
[0017] In this process, two solutions, an aqueous solution of alkylphosphinate and an aqueous solution of soluble aluminum salt, are simultaneously added dropwise to the reaction vessel in a continuous manner.
[0018] The dropping rate of the solution can be determined based on the mass concentration of the solution, ensuring that both solutions are added simultaneously.
[0019] Preferably, in S2, the reaction temperature is 40–100°C.
[0020] Preferably, in S2, the reaction temperature is 60–80°C.
[0021] Preferably, in S2, the reaction time is 0.8-2h.
[0022] Preferably, in S1, the mass concentration of the alkylphosphinate aqueous solution is 25-35%.
[0023] Preferably, in S1, the mass concentration of the soluble aluminum salt aqueous solution is 20-30%.
[0024] Preferably, in S1, the alkylphosphinate is one or more of diethylphosphinate, ethylphosphinate, butylphosphinate, methylphosphinate, cyclohexylphosphinate or ethylcyclohexylphosphinate.
[0025] More preferably, the alkylphosphinate is sodium alkylphosphinate.
[0026] More preferably, the alkylphosphinate is sodium diethylphosphinate.
[0027] Preferably, in S1, the soluble aluminum salt is one or more of aluminum sulfate, aluminum nitrate, aluminum chloride, or aluminum acetate.
[0028] More preferably, the soluble aluminum salt is aluminum sulfate.
[0029] In practical applications, some water can be added to the reaction vessel to prevent the amount of alkylphosphinate and soluble aluminum salt added at the same time from being too small to allow for sufficient stirring and reaction.
[0030] This invention also protects phosphonate flame retardants prepared by the above-described method for preparing phosphonate flame retardants.
[0031] The method for preparing the phosphonate flame retardant obtained by the present invention has excellent flame retardant properties and can be widely used in the preparation of plastic products. The present invention particularly protects the application of the method for preparing the phosphonate flame retardant in improving the flame retardant properties of polymers.
[0032] The polymer can be one or more of PBT, high-temperature nylon PA10T, PA, PPE, TPE or TPU.
[0033] Compared with the prior art, the beneficial effects of the present invention are:
[0034] This invention discloses a method for preparing a phosphonate flame retardant. The method involves simultaneously and continuously adding an aqueous solution of alkyl phosphonates and an aqueous solution of soluble aluminum salts into a reaction vessel for stirring, mixing, and precipitation. After the addition is complete, the mixture is filtered, washed, and dried to obtain the phosphonate flame retardant. The obtained phosphonate flame retardant has a high yield, narrow particle size distribution, good dispersibility, high thermal stability, resistance to yellowing, and low heat loss rate.
[0035] The phosphonate flame retardant prepared by the method of this invention exhibits good dispersibility, with a D50 of 20-45 μm, a single-peak differential distribution of 12%-30%, and an angle of repose reaching 25°-35°. The phosphonate flame retardant prepared by the method of this invention also demonstrates good thermal stability, with a thermal weight loss of <4.1% after 60 min at TG365℃, and a heat loss rate of <1.25% after baking in air at 290℃ for 120 min, with a yield greater than 97%. Detailed Implementation
[0036] The present invention will be further described below with reference to specific embodiments, but the embodiments do not limit the present invention in any way. Unless otherwise stated, the raw materials and reagents used in the embodiments of the present invention are conventionally purchased raw materials and reagents.
[0037] Example 1
[0038] A method for preparing a phosphonate flame retardant includes the following steps:
[0039] S1. Prepare aqueous solutions of alkyl phosphonates and soluble aluminum salts, respectively;
[0040] S2. The aqueous solutions of alkyl phosphonates and soluble aluminum salts are simultaneously and continuously added to the reaction vessel, stirred, mixed and precipitated. After the addition is completed, the mixture is filtered, washed and dried to obtain the phosphonate flame retardant.
[0041] In S1, the alkylphosphine salt is sodium diethylphosphine, and the mass concentration of the aqueous solution of the alkylphosphine salt is 26%.
[0042] The soluble aluminum salt is aluminum sulfate, and the mass concentration of the aqueous solution of the soluble aluminum salt is 30%.
[0043] In S2, the molar ratio of alkylphosphinate in the aqueous solution to soluble aluminum salt in the aqueous solution is 6.5:1;
[0044] The reaction temperature was 60℃ and the reaction time was 2 hours.
[0045] Example 2
[0046] A method for preparing a phosphonate flame retardant includes the following steps:
[0047] S1. Prepare aqueous solutions of alkyl phosphonates and soluble aluminum salts, respectively;
[0048] S2. The aqueous solutions of alkyl phosphonates and soluble aluminum salts are simultaneously and continuously added to the reaction vessel, stirred, mixed and precipitated. After the addition is completed, the mixture is filtered, washed and dried to obtain the phosphonate flame retardant.
[0049] In S1, the alkylphosphine salt is sodium diethylphosphine, and the mass concentration of the aqueous solution of the alkylphosphine salt is 26%.
[0050] The soluble aluminum salt is aluminum sulfate, and the mass concentration of the aqueous solution of the soluble aluminum salt is 30%.
[0051] In S2, the molar ratio of alkylphosphinate in the aqueous solution to soluble aluminum salt in the aqueous solution is 6.5:1;
[0052] The reaction temperature was 80℃ and the reaction time was 2 hours.
[0053] The difference between Example 2 and Example 1 is that in S2, the reaction temperature is 80°C.
[0054] Example 3
[0055] A method for preparing a phosphonate flame retardant is basically the same as that in Example 1.
[0056] The difference between Example 3 and Example 1 is that in S2, the reaction temperature is 100°C.
[0057] The rest is the same as in Example 1, and will not be repeated here.
[0058] Example 4
[0059] A method for preparing a phosphonate flame retardant is basically the same as that in Example 1.
[0060] The difference between Example 4 and Example 1 is that in S2, the reaction temperature is 20°C.
[0061] The rest is the same as in Example 1, and will not be repeated here.
[0062] Example 5
[0063] A method for preparing a phosphonate flame retardant is basically the same as that in Example 1.
[0064] The difference between Example 5 and Example 1 is that in S2, the reaction temperature is 40°C.
[0065] The rest is the same as in Example 1, and will not be repeated here.
[0066] Example 6
[0067] A method for preparing a phosphonate flame retardant is basically the same as that in Example 1.
[0068] The difference between Example 6 and Example 1 is that, in S2, the molar ratio of alkylphosphinate in the aqueous solution of alkylphosphinate to soluble aluminum salt in the aqueous solution of soluble aluminum salt is 6:1.
[0069] The rest is the same as in Example 1, and will not be repeated here.
[0070] Example 7
[0071] A method for preparing a phosphonate flame retardant is basically the same as that in Example 1.
[0072] The difference between Example 7 and Example 1 is that, in S2, the molar ratio of alkylphosphinate in the aqueous solution of alkylphosphinate to soluble aluminum salt in the aqueous solution of soluble aluminum salt is 8:1.
[0073] The rest is the same as in Example 1, and will not be repeated here.
[0074] Example 8
[0075] A method for preparing a phosphonate flame retardant is basically the same as that in Example 1.
[0076] The difference between Example 8 and Example 1 is that in S2, the reaction time is 0.5h.
[0077] The rest is the same as in Example 1, and will not be repeated here.
[0078] Example 9
[0079] A method for preparing a phosphonate flame retardant is basically the same as that in Example 1.
[0080] The difference between Example 9 and Example 1 is that in S2, the reaction time is 0.8h.
[0081] The rest is the same as in Example 1, and will not be repeated here.
[0082] Example 10
[0083] A method for preparing a phosphonate flame retardant is basically the same as that in Example 1.
[0084] The difference between Example 10 and Example 1 is that in S2, the reaction time is 3 hours.
[0085] The rest is the same as in Example 1, and will not be repeated here.
[0086] Example 11
[0087] A method for preparing a phosphonate flame retardant is basically the same as that in Example 1.
[0088] The difference between Example 11 and Example 1 is that in S1, the mass concentration of the alkylphosphinate aqueous solution is 35%.
[0089] The rest is the same as in Example 1, and will not be repeated here.
[0090] Example 12
[0091] A method for preparing a phosphonate flame retardant is basically the same as that in Example 1.
[0092] The difference between Example 12 and Example 1 is that in S1, the mass concentration of the alkylphosphinate aqueous solution is 40%.
[0093] The rest is the same as in Example 1, and will not be repeated here.
[0094] Example 13
[0095] A method for preparing a phosphonate flame retardant is basically the same as that in Example 1.
[0096] The difference between Example 13 and Example 1 is that in S1, the mass concentration of the soluble aluminum salt aqueous solution is 20%.
[0097] The rest is the same as in Example 1, and will not be repeated here.
[0098] Example 14
[0099] A method for preparing a phosphonate flame retardant is basically the same as that in Example 1.
[0100] The difference between Example 14 and Example 1 is that in S1, the mass concentration of the soluble aluminum salt aqueous solution is 39%.
[0101] The rest is the same as in Example 1, and will not be repeated here.
[0102] Comparative Example 1
[0103] A method for preparing a phosphonate flame retardant includes the following steps:
[0104] S1. Prepare aqueous solutions of alkyl phosphonates and soluble aluminum salts, respectively;
[0105] S2. Add the aqueous solution of alkyl phosphonates to a three-necked flask, stir and heat, and add the aqueous solution of soluble aluminum salt dropwise to the three-necked flask through a constant pressure funnel. Stir, mix and precipitate, filter, wash and dry to obtain phosphonate flame retardant.
[0106] In S1, the alkylphosphine salt is sodium diethylphosphine, and the mass concentration of the aqueous solution of the alkylphosphine salt is 26%.
[0107] The soluble aluminum salt is aluminum sulfate, and the mass concentration of the aqueous solution of the soluble aluminum salt is 30%.
[0108] The molar ratio of alkylphosphinic acid salt in aqueous solution to soluble aluminum salt in aqueous solution is 6.5:1;
[0109] In S2, the reaction temperature is 60℃ and the reaction time is 2h.
[0110] Comparative Example 2
[0111] A method for preparing a phosphonate flame retardant includes the following steps:
[0112] S1. Prepare aqueous solutions of alkyl phosphonates and soluble aluminum salts, respectively;
[0113] S2. Add the aqueous solution of alkyl phosphonates to a three-necked flask, stir and heat, and add the aqueous solution of soluble aluminum salt dropwise to the three-necked flask through a constant pressure funnel. Stir, mix and precipitate, filter, wash and dry to obtain phosphonate flame retardant.
[0114] In S1, the alkylphosphine salt is sodium diethylphosphine, and the mass concentration of the aqueous solution of the alkylphosphine salt is 26%.
[0115] The soluble aluminum salt is aluminum sulfate, and the mass concentration of the aqueous solution of the soluble aluminum salt is 30%.
[0116] The molar ratio of alkylphosphinic acid salt in aqueous solution to soluble aluminum salt in aqueous solution is 6.5:1;
[0117] In S2, the reaction temperature is 80℃ and the reaction time is 2h.
[0118] The difference between Comparative Example 2 and Comparative Example 1 is that in S2, the reaction temperature is 80℃.
[0119] Result detection
[0120] The flame retardants of each embodiment and comparative example were tested using the following test methods:
[0121] Particle size testing: The sample was dispersed in ethanol and measured using a laser particle size analyzer.
[0122] Flame retardant particle size differential distribution: Using ethanol as the dispersion medium, the flame retardant particle size differential distribution is tested using a laser particle size analyzer. The higher the distribution rate, the more uniform the particle size distribution.
[0123] Angle of repose: The test method involves pouring a powder sample into a funnel, allowing it to fall through the funnel onto a circular plate of radius r below. The powder gradually accumulates until it can no longer be piled up. The height of the accumulated powder, h, is measured, and the angle of repose α is calculated using the formula tanα = h / r. Generally, it is considered that if α is less than 30°, the powder can flow freely; if α is between 30° and 40°, the powder can meet processing requirements; however, if α exceeds 40°, the powder is difficult to process. The smaller the angle of repose, the better the flowability of the powder and the better its dispersibility during the processing of polymer materials.
[0124] Thermal stability: Thermogravimetric analysis (TGA) was used. The heating range was 40–365 °C, held for 60 min, and then further increased to 750 °C at a heating rate of 20 °C / min under N2 atmosphere. The lower the heat loss, the lower the decomposition rate of the product at high temperatures, and the higher the product stability.
[0125] Heat loss rate: In air atmosphere, baked at 290℃ for 120 min, the heat loss rate is the percentage of the difference in mass before and after baking to the mass before baking. The smaller the heat loss rate, the less weight of flame retardant is lost, and the higher the thermal stability.
[0126] Flame retardant yellowing test: Bake the flame retardant at 290℃ and normal pressure for 120 minutes and observe the color of the flame retardant. According to the RAL color chart, 9003 is signal white, 9016 is traffic white, and 1013 is a light gray that is close to white. The colors change from white to yellow in the following order: 9003, 9016, and 1013.
[0127] Yield: The percentage of the weight of the flame retardant product to the theoretical mass of the flame retardant.
[0128] The phosphonate flame retardants of Examples 1 and 2, and Comparative Examples 1 and 2 were mixed with PBT, glass fiber, and toughening agent at a weight ratio of 10:50:30:10 at 230-260°C and extruded from a twin-screw extruder to obtain flame-retardant thermoplastic polymer molding materials. Samples were prepared and their combustion performance and mechanical properties were tested.
[0129] Tensile strength: GB / T1040~1992 Test methods for tensile properties of plastics;
[0130] Bending strength: GB / T9341~2000 Test method for bending properties of plastics;
[0131] Deflection: GB / T9341~2000 Test method for bending properties of plastics;
[0132] Flame retardant rating: UL94-2018 burning 1.6mm and UL94 burning 2.5mm.
[0133] The specific test results of the flame retardants in each embodiment and comparative example are shown in Table 3 below:
[0134] Table 3
[0135]
[0136] Table 4: Application of phosphonate flame retardants in Examples 1-2 and Comparative Examples 1-2 in PBT polymer materials
[0137]
[0138]
[0139] The data above show that the phosphonate flame retardant prepared by the method of the present invention has good dispersibility, with a D50 of 20-45 μm, a single-peak differential distribution of 12%-30%, and an angle of repose of 25°-35°. The phosphonate flame retardant prepared by the method of the present invention also exhibits good thermal stability, with a thermal weight loss of <4.1% after 60 min at TG365℃, and a heat loss rate of <1.25% after baking in air at 290℃ for 120 min, with a yield greater than 97%.
[0140] The phosphonate flame retardant prepared by the method of the present invention can improve the tensile, bending and flame retardant properties of polymer materials.
[0141] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the implementation of the present invention. Those skilled in the art can make other variations or modifications based on the above description. It is neither necessary nor possible to exhaustively describe all embodiments here. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the scope of protection of the claims of the present invention.
Claims
1. A method for preparing a phosphonate flame retardant, characterized in that, Includes the following steps: S1. Prepare aqueous solutions of alkyl phosphonates and soluble aluminum salts, respectively; S2. An aqueous solution of alkyl phosphonates and an aqueous solution of soluble aluminum salts are simultaneously and continuously added to a reaction vessel for stirring, mixing, and precipitation. After the simultaneous addition is completed, the mixture is filtered, washed, and dried to obtain the phosphonate flame retardant. in, In S1, the mass concentration of the alkyl phosphonate aqueous solution is 25-40%; the mass concentration of the soluble aluminum salt aqueous solution is 20-39%. In S2, the molar ratio of alkylphosphinate in the aqueous solution to soluble aluminum salt in the aqueous solution is (6~8):1; The reaction temperature is 60~80℃, and the reaction time is 0.8~2h.
2. The method for preparing the phosphonate flame retardant as described in claim 1, characterized in that, In S1, the mass concentration of the alkylphosphinate aqueous solution is 25-35%.
3. The method for preparing the phosphonate flame retardant as described in claim 1, characterized in that, In S1, the mass concentration of the soluble aluminum salt aqueous solution is 20-30%.
4. The method for preparing the phosphonate flame retardant as described in claim 1, characterized in that, In S1, the alkylphosphonate is one or more of diethylphosphonate, ethylphosphonate, butylphosphonate, methylphosphonate, cyclohexylphosphonate, or ethylcyclohexylphosphonate.
5. The method for preparing the phosphonate flame retardant as described in claim 1, characterized in that, In S1, the soluble aluminum salt is one or more of aluminum sulfate, aluminum nitrate, aluminum chloride, or aluminum acetate.
Citation Information
Patent Citations
Coated flame retardant, preparation method and application thereof, as well as high polymer composition comprising coated flame retardant
CN104861205A
Organic aluminophosphite and preparation method and application thereof
CN107936055A