Method for manufacturing a magnetically deformable machine and deformable 3D magnetic machine

By employing a bottom-up assembly method of isomorphic voxels, the problem of manufacturing sub-millimeter-scale magnetic soft machinery in existing technologies has been solved, enabling the manufacturing of high-resolution and complex-structured magnetic soft machinery, which is applicable to biomimetic robots and minimally invasive medical devices.

CN116058112BActive Publication Date: 2026-11-20MAX PLANCK GESELLSCHAFT ZUR FOERDERUNG DER WISSENSCHAFTEN EV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202180055880.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-08-10
Filing Date
2021-08-04
Publication Date
2026-11-20
Estimated Expiration
2041-08-04

AI Technical Summary

Technical Problem

Existing technologies struggle to integrate various material compositions with arbitrary 3D magnetic setups and geometries at the sub-millimeter scale. Furthermore, existing methods are limited by the selection of materials, geometries, and magnetization profiles, making it impossible to fabricate complex magnetic soft machinery structures.

Method used

By employing a bottom-up assembly method, heterogeneous voxels are gradually bonded together to form magnetic deformable machines. By defining deformation characteristics, creating blueprints, selecting appropriate voxels, and using adhesives for curing, composite 3D micro wireless magnetic soft machines with arbitrary multi-material combinations, arbitrary 3D geometry, and arbitrary configurable 3D magnetization profiles can be realized.

Benefits of technology

It enables high-resolution fabrication of complex magnetic soft machinery at the sub-millimeter scale, improving design flexibility and functional versatility, and is applicable to biomimetic robots, micro-factories, and minimally invasive medical devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116058112B_ABST
    Figure CN116058112B_ABST
Patent Text Reader

Abstract

The invention relates to a method of manufacturing a magnetically deformable machine comprising isomorphic voxels and a deformable 3D magnetic machine having a size of less than 10000 mm, the magnetic machine comprising a plurality of voxels, at least some of the plurality of voxels being magnetic, wherein at least some of the voxels have a Young's modulus of less than 500 MPa, the plurality of voxels being bonded to each other with a bonding agent, wherein each voxel has a predefined shape, size, has predefined magnetic properties and predefined material properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for manufacturing a magnetic deformable machine comprising isomeric voxels and a deformable 3D magnetic machine having a size of less than 10,000 mm. The magnetic machine comprises a plurality of voxels, at least some of which are magnetic, wherein at least one of the voxels has a Young's modulus of less than 500 MPa. The plurality of voxels are bonded together with an adhesive, wherein each voxel has a predefined shape, size, predefined magnetic properties, and predefined material properties. Background Technology

[0002] Small, soft machines that respond to external stimuli hold promise for breakthrough applications in biomimetic robotics, microfabrication, and minimally invasive medical devices. External magnetic fields have emerged as a promising stimulus option for the safe, rapid, precise, dexterous, and wireless actuation of soft machines. However, as the overall size of such magnetic machines shrinks to the sub-millimeter scale, their design and functionality become severely limited by available manufacturing methods, which are only suitable for a limited selection of materials, geometries, and magnetization profiles.

[0003] While recent research has advanced small magnetic soft machinery from two-dimensional (2D) molding and laser cutting methods to extrusion-based and ultraviolet (UV) lithography-based 3D printing methods, the integration of various arbitrary material compositions with arbitrary 3D magnetic programming and geometries has yet to be achieved. Furthermore, existing methods are subject to several fundamental constraints that limit their further improvement. Specifically, extrusion-based methods cannot fabricate finer magnetic fibers to weave complex structures due to stringent requirements on storage modulus, performance degradation caused by added magnetic particles, and extrusion swelling of the soft elastomer. Additionally, the strong localized interactions of magnetic particles within uncured liquid photoresist limit the arbitrary magnetization of adjacent voxels via lithography-based methods. Summary of the Invention

[0004] In view of these challenges, an object of the present invention is to provide a method for manufacturing magnetically deformable machinery, which can be produced in a manner that is as easy and repeatable as possible, even at sub-millimeter scales where the aforementioned disadvantages are overcome. Another object of the present invention is to provide usable magnetic machinery that can be remotely deformed at a target site and can be moved through various environments before reaching the target site.

[0005] This objective is achieved by the method and magnetically deformable machinery according to the subject matter of the respective independent claims.

[0006] This method for manufacturing magnetic deformable machinery comprising isomeric voxels (i.e., voxels with different properties, characteristics, and compositions) includes the following sequential steps: - Define the deformation characteristics of magnetic machinery; - The blueprint for the magnetic machinery is created by referencing the deformation characteristics of the magnetic machinery. - Provide a plurality of voxels, at least one of the plurality of voxels, preferably some voxels, is magnetic and wherein at least one of the plurality of voxels has a Young's modulus of less than 500 MPa; - Using adhesives, multiple voxels are bonded together to assemble a magnetic mechanism according to a blueprint; and - To cure the adhesive.

[0007] Therefore, the present invention provides a bottom-up assembly method in which individual voxels are progressively bonded together to form deformable magnetic machinery. Compared to prior art methods using a top-down approach, unprecedented accuracy in forming magnetic machinery can be achieved. Furthermore, the current method is very simple to implement because the individual building blocks (i.e., voxels) can be adapted to the specific function of the magnetic machinery and then simply connected to their directly adjacent voxels according to a blueprint.

[0008] For example, certain voxels can be configured to allow the magnetic mechanism to be transported between a first position and a second position by means of the magnetic properties of the magnetic mechanism through the application of a first magnetic field, while other voxels can be configured to alter the appearance of the magnetic mechanism, i.e., to allow the magnetic mechanism to deform, for example by expanding or restricting its size, or to allow a component of the magnetic mechanism to move relative to another part of the magnetic mechanism, for example by applying a second magnetic field different from the first magnetic field.

[0009] Depending on the type of magnetic machinery, deformation of the magnetic machinery is required to enable movement of the magnetic machinery and / or to alter the appearance of the magnetic machinery for a specific application. This invention also enables the production of deployable magnetic machinery by being able to manufacture deformable magnetic machinery that can thus perform specific functions.

[0010] For example, if a packaged magnetic mechanism is selected to transport a payload from a first position to a second position for unloading, then the size of the magnetic mechanism must be selected according to the payload, the stiffness properties of the magnetic mechanism must be selected to reliably transport the payload, the magnetic properties of the magnetic mechanism must be selected to move the magnetic mechanism from the first position to the second position, and the deformation characteristics must be selected to load the payload at the first position and release the payload from the magnetic mechanism at the second position. That is, in addition to the way the magnetic mechanism can be deformed to move the magnetic mechanism from the first position to the second position, a second magnetic field can be applied to deform the magnetic mechanism.

[0011] To determine the dimensions, the intended use environment is examined; for example, if the capsule is intended to deliver a payload in a person's stomach, an average capsule size of, for example, 5 to 20 mm is chosen. The stiffness properties are then determined, for example, by the amount of payload that must be delivered. These are the steps that can be implemented to define the deformation characteristics of the magnetic machinery and then to create a blueprint for the magnetic machinery.

[0012] At this point, it should be noted that the blueprint is an instruction manual that references the deformation characteristics of a magnetic machine to assemble different building blocks (i.e., voxels) relative to each other and uses an adhesive to bond them together to form the desired magnetic machine.

[0013] Current bottom-up manufacturing approaches allow for the high-resolution production of composite 3D micro-wireless magnetic softmachines with arbitrary multi-material compositions, arbitrary 3D geometries, and arbitrary configurable 3D magnetization profiles based on heterogeneous assembly in 3D microfabrication strategies. This approach facilitates the realization of diverse properties on prototype machines, such as configurable shape gradients, negative Poisson's ratios, composite stiffness distributions, directional joint bending, and remagnetization for shape reconfiguration. These properties further liberate the design and realization of various biomedical device-related functions, such as peristaltic pumping, active cargo transport and delivery, controlled surface anchoring and release, and information encryption. This 3D heterogeneous integration approach significantly improves the level of achievable complexity for 3D magnetic softmachines, and thus enhances their future capabilities and performance in robotics, biomedical devices, and bioengineering applications. A unique advantage of this assembly approach is that such voxels can be fabricated using arbitrary geometries, materials, and magnetic settings through arbitrary / different microfabrication processes.

[0014] The steps for defining the deformation characteristics of magnetic machinery may include at least one of the steps selected from the group consisting of: - Define the applications of magnetic machinery; - Define the working environment for the corresponding applications of magnetic machinery; - Define the deformation parameters of the magnetic machinery; - Select the size of the magnetic machinery; - Choose the shape of the magnetic machinery; And combinations of the foregoing items. In this way, users of the method can adapt the manufacture of magnetic machinery to their specific working environment and produce customized magnetic machinery.

[0015] The blueprint may include: the number of corresponding voxels for forming the magnetic machinery, the arrangement of the corresponding voxels for forming the magnetic machinery, the properties of the corresponding voxels for forming the machinery (e.g., Young's modulus, magnetization profile, stiffness, mechanical strength, durability, deformation, maximum strain or stress, drug or other molecular loading capacity, remote heating properties, porosity, gas, liquid or molecular permeability, electrical or thermal conductivity, thermal expansion, liquid swelling properties, stimulus response (e.g., pH, chemical, temperature, humidity, flow rate, pressure, glucose), biocompatibility, biodegradability or solubility, visibility in a specific imaging technique (e.g., fluorescence imaging, near-infrared imaging, magnetic resonance imaging, positron emission tomography, ultrasound imaging, photoacoustic imaging, fluorescence microscopy, computed tomography), immune response properties, protein absorption properties, enzyme reaction properties, temporary or permanent adhesion to other voxels, biological tissues or other surfaces), and the arrangement of the curing agent at the voxels for forming the magnetic machinery.

[0016] Therefore, the blueprint includes instructions on which voxels are needed in which arrangement to produce magnetic machinery suitable for the corresponding working environment.

[0017] In this respect, it should be noted that the magnetization profile defines the spatial profile of the vector field of the magnetic field of a voxel, which expresses the density of permanent or induced magnetic dipole moments in the magnetic material.

[0018] The steps for creating a blueprint for a magnetic mechanism may include at least one of the steps selected from a group of the following: - Select materials with different voxels to define the stiffness properties of the magnetic machinery; - Select one or more materials for the appropriate voxel used in the magnetic machinery; - Select a uniform 3D magnetization profile or a non-uniform 3D magnetization profile of the magnetic voxel to define the moment-based deformation properties or magnetic force-based deformation properties of the magnetomechanic. - Select the appropriate voxel size; - Select the shape of the corresponding voxel; - Select the magnetic properties of the corresponding voxel; - Select the material properties of the corresponding voxels; - Simulate the behavior and / or deformation of magnetomechanics based on blueprints; - Adjust the blueprint of the magnetic machinery based on the simulation results of the behavior and / or deformation of the magnetic machinery; And combinations of the aforementioned items.

[0019] In this way, specific building blocks of magnetic machinery can be assembled to produce magnetic machinery suitable for the corresponding working environment.

[0020] Each voxel can have a 3D shape and can have a predefined shape and size, and can have predefined magnetic properties and predefined material properties, such as Young's modulus, magnetization profile, stiffness, mechanical strength, durability, deformation, maximum strain or stress, drug or other molecular loading capacity, remote heating properties, porosity, gas, liquid or molecular permeability, electrical or thermal conductivity, thermal expansion, liquid swelling properties, stimulus response (e.g., pH, chemicals, temperature, humidity, flow rate, pressure, glucose), biocompatibility, biodegradability or solubility, visibility in specific imaging techniques (e.g., fluorescence imaging, near-infrared imaging, magnetic resonance imaging, positron emission tomography, ultrasound imaging, photoacoustic imaging, fluorescence microscopy, computed tomography), immune response properties, protein absorption properties, enzyme reaction properties, and temporary or permanent adhesion to other voxels, biological tissues or other surfaces.

[0021] By using the above types of voxels, each building block can be adapted to very specific functions, such as the stability of magnetic machinery, the transport of magnetic machinery, and the deformation of magnetic machinery.

[0022] The magnetization profile of a magnetic voxel in a magnetic machine can be seen through magnetic sensing or imaging techniques (e.g., magneto-optical sensing using the Kerr and / or Faraday effects, magnetic force microscopy, magnetic X-ray microscopy). In this way, some voxels in a magnetic machine may be invisible to imaging techniques but visible to tracking techniques, and vice versa. If magnetic machines are deployed as microrobots, for example in the medical field, this could be beneficial for tracking and placement applications that can be implemented using magnetic machines.

[0023] The step of bonding multiple voxels together can be performed at one or more faces and / or one or more edges of the voxels. In this way, the working accuracy of deformable magnetic machinery can be improved because, for example, the movement of the voxels relative to each other can be affected according to how the voxels are bonded together.

[0024] The step of bonding multiple voxels together may include bonding one voxel to another in a subsequent step; and / or the step of bonding multiple voxels together may include bonding one group of voxels to another group of voxels in turn. In this way, if, for example, a very flexible and / or sensitive part of a machine is being assembled, the individual voxels can be attached to each other in a subsequent step; however, if a rigid but not particularly flexible or sensitive part of a magnetic machine is being assembled, the voxels forming this part of the machine can be bonded together in a similar batch process by bonding several voxels together at the same time.

[0025] In this respect, a similar batch process could be one in which several voxels are placed into supports and molded together at the same time, wherein the supports have a predefined shape and size that matches at least a portion of the magnetic machinery to be formed.

[0026] The corresponding voxels can be magnetized before, during, or after being bonded to their adjacent voxels. In this way, the method can be more versatile in forming machines.

[0027] The step of bonding multiple voxels together may include the following steps: providing a fixture, particularly one or more fixtures, having at least a portion of a negative shape of a magnetically deformable mechanism; placing a predefined number of voxels into the fixture; and then bonding the predefined number of voxels together in the fixture. The use of the fixture enables improved and more accurate placement of voxels and thus more accurate formation of the mechanism.

[0028] One or more of a predefined number of voxels can be placed into a fixture at a single point in time using a robot (not shown). Using a robot to place voxels can improve placement accuracy and, for example, help maintain a sterile environment in the formation of medical devices.

[0029] One or more of a predefined number of voxels can be magnetized before being placed in the fixture or after adjacent voxels that have been placed in the fixture and bonded to one or more of the voxels. Therefore, the fixture can also be used to magnetize voxels to provide them with a desired predefined magnetization orientation.

[0030] The curing step of the adhesive can be carried out at room temperature or at another specific temperature and in the environment in which the bonding step is performed. The curing step can be performed using an ultraviolet (UV) light source or a light source of another wavelength, or it can be performed in an oven or on a hot plate. This type of bonding method ensures a reliable and easy manufacturing process for magnetic machinery.

[0031] The corresponding side length of the magnetic machinery can be less than 10,000 mm, particularly less than 100 mm; and / or each voxel can have a 3D shape, wherein the corresponding side length of the 3D shape is selected in the range of 2,500 mm to 5 nm, particularly in the range of 25 mm to 1 µm; and / or each voxel can have a shape selected from the group consisting of: square voxels, rectangular voxels, circular voxels, polygonal voxels, triangular voxels, and any arbitrary 3D shape voxels, as well as combinations thereof. In this way, a wide variety of magnetic machinery can be formed in the sub-millimeter range and for a wider range of applications. It should be noted that voxels with dimensions greater than 10 mm can be formed in corresponding molds into which the corresponding material is cast.

[0032] In this respect, it should be noted that such shapes can be advantageously formed using techniques such as 3D printing and / or two-photon laser lithography or lithography and / or casting. Generally speaking, voxels can be formed using any form of manufacturing method, as long as voxels with the desired shape, size, and properties can be provided.

[0033] According to another aspect, the present invention also relates to a deformable 3D magnetic mechanism having a dimension of less than 10,000 mm, the magnetic mechanism comprising a plurality of voxels, at least one of the voxels, preferably some of the voxels, being magnetic, wherein at least one of the voxels has a dimension of less than 500. A Young's modulus of MPa is used to bond multiple voxels together with an adhesive, wherein each voxel has a predefined shape, size, predefined magnetic properties, and predefined material properties, such as Young's modulus, magnetization profile, stiffness, mechanical strength, durability, deformation, maximum strain or stress, drug or other molecular loading capacity, remote heating properties, porosity, gas, liquid or molecular permeability, electrical or thermal conductivity, thermal expansion, liquid swelling properties, response to stimuli (e.g., pH, chemicals, temperature, humidity, flow rate, pressure, glucose), biocompatibility, biodegradability or solubility, visibility in specific imaging techniques (e.g., fluorescence imaging, near-infrared imaging, magnetic resonance imaging, positron emission tomography, ultrasound imaging, photoacoustic imaging, fluorescence microscopy, computed tomography), immune response properties, protein absorption properties, enzyme reaction properties, and temporary or permanent adhesion to other voxels, biological tissues or other surfaces.

[0034] Using the methods discussed above, magnetic mechanics can thus be formed with improved accuracy in movement and deployment compared to existing technologies. This is because they can achieve significantly improved resolution compared to existing technologies that use top-down assembly rather than a bottom-up approach. Furthermore, the methods described above can be advantageously used to integrate a variety of different materials into a single device. The advantages discussed above naturally also apply to the magnetic mechanics discussed below.

[0035] By providing at least one, preferably some, of a plurality of voxels that are magnetic, the magnetic mechanism can be moved between different locations that are spatially separated, and the magnetic mechanism can be actuated such that the shape of the magnetic mechanism can be changed if a particular desired function is to be performed by the magnetic mechanism.

[0036] Each voxel can be made of a material with a different Young's modulus to define the stiffness mode of the magnetic mechanism. By defining the stiffness mode, the magnetic mechanism is deformed, so that it can be actuated to perform a desired change in shape to achieve a desired function.

[0037] In this regard, it should be noted that a voxel is a building block that can be made of magnetized material, hard / soft material, biodegradable or non-biodegradable material, which is selected to implement a bottom-up manufacturing process rather than a top-down manufacturing method and to adapt each part of the magnetic machinery to the specific movement and / or actuation function of the magnetic machinery.

[0038] The corresponding side length of the magnetic machinery can have a dimension of less than 100 mm, particularly less than 5 mm; and / or each voxel can have a 3D shape, wherein the dimension of the corresponding side length of the 3D shape is selected in the range of 500 mm to 5 nm, particularly in the range of 10 mm to 1 µm; and / or each voxel can have a shape selected from the group consisting of: square voxels, rectangular voxels, circular voxels, polygonal voxels, triangular voxels, and any arbitrary 3D shape voxels.

[0039] Magnetic machinery can be a cargo delivery device (e.g., drugs, stem cells, genes, imaging agents, T cells, macrophages) that can transport the cargo and release it at the target site by deforming or opening the device; or magnetic machinery can be one of the following: anchoring devices, supports, soft peristaltic pumps or other types of liquid pumps, soft cubic frames, information encryption devices, deformable metamaterials, shape-adaptive or shape-configurable robots, grippers, foldable devices, blocking devices, swimming robots, organ models, synthetic hearts or other organs, and retractable toroidal flowers. Such magnetic machinery can be used in a wide variety of environments for a wide range of applications.

[0040] The materials of at least some of the nonmagnetic voxels in the magnetic machinery can be selected from the group of nonmagnetic materials consisting of: elastomers, thermoplastic elastomers, rubber, rigid plastics, thermoplastic plastics, such as polydimethylsiloxane, aliphatic aromatic copolyesters or modified polyesters, or modified copolyesters, polyurethane elastomers, silicone rubber, natural rubber, latex, styrene-vinyl butene-styrene, butyl rubber, fluorosilicone rubber, polyester, nylon, thermoplastic polyurethane; biodegradable synthetic materials, such as polyglycolic acid, poly(caprolactone), poly(p-dioxanone), poly(poly(dioxanone)). (Ethylene glycol) diacrylate, poly(N-isopropylacrylamide); biomaterials, such as gelatin, chitosan, alginate, agarose, hyaluronic acid derivatives, elastin, chitosan, fibroin glue, cellulose, fibronectin, collagen, silk; hydrogels; ionogels; liquid crystal polymers, elastomers or gels; shape memory polymers; photoresist polymers, such as SU-8; biological proteins, such as cuttlefish cephalopod protein; textile materials; nonmagnetic metals; silicone; silica; glass; wood; carbon fiber; and derivatives and combinations thereof. Thus, magnetic machinery can be adapted for its specific applications.

[0041] At least some of the materials in the magnetic voxels can be selected from the group consisting of: magnetic materials existing in the form of a large number of particles, disks, wires, fibers, or asymmetric particles, such as chromium dioxide (CrO2), samarium cobalt (SmCo), neodymium iron boron (NdFeB), cobalt (Co), ferrites, permalloy (NiFe), carbon steel, tungsten steel, magnetic steel, iron, stainless steel, nickel (Ni), iron platinum (FePt), iron oxide, barium ferrite, and magnets; combinations or composites of the foregoing; and / or voxels coated with a magnetic film or magnetic layer made of the above magnetic materials or combinations thereof. Furthermore, magnetic composite materials can be embedded within, or cover or deposited on, the aforementioned non-magnetic voxel materials to form voxels. Additionally, various combinations of magnetic voxels can be used to form magnetic machinery.

[0042] The adhesive material can be selected from the group consisting of: uncured silicone rubber, PDMS, polyurethane, modified copolyester, silicone rubber and other uncured polymers of the foregoing, temperature-curing polymers, UV or other wavelength light-curing polymers, chemically cured polymers, waxes, tapes, super glues, surgical adhesives, various biopolymers (e.g., gelatin, deoxyribonucleic acid (DNA) and base adhesives), and combinations thereof. Such adhesives allow for the formation of more accurate and higher-resolution magnetic mechanics suitable for carrying out their respective applications.

[0043] For example, for a uniform magnetic voxel, the magnetic voxel can have any arbitrary 3D magnetization profile, and each voxel can have an average surface magnetic field strength selected in the range of 0 to 1 T, preferably in the range of 0 to 50 mT, wherein each voxel has a predefined orientation of the magnetic field strength, such as parallel to the face of the corresponding voxel, perpendicular to the face of the corresponding voxel, or tilted about one or more faces of the corresponding voxel. For a non-uniform magnetic voxel, each voxel can have a non-uniform magnetization distribution throughout the voxel and a varying magnetic orientation throughout the voxel.

[0044] High-resolution magnetic mechanics can be formed by selecting appropriate shapes, sizes, and material compositions of corresponding voxels, as well as binders. In this way, magnetic mechanics capable of moving rapidly and efficiently between various spatially separated locations are obtained, and the magnetic mechanics can change its shape and / or size at a desired target location to perform its desired function.

[0045] According to one aspect, the invention also relates to the use of magnetic mechanics for at least one of the following: a cargo delivery device (e.g., a drug, stem cell, gene, imaging agent, T cell, macrophage) capable of transporting the cargo and releasing it at a target site by deforming or opening the device; an anchoring device; a support; a soft peristaltic pump or other type of liquid pump; a soft cubic frame; an information encryption device; a deformable metamaterial; a shape-adaptive or shape-configurable robot; a gripper; a foldable device; a blocking device; a swimming robot; an organ model; a synthetic heart or other organ; and a retractable ring flower. Attached Figure Description

[0046] The invention will be described in detail with reference to the accompanying drawings. It is shown that: Figures 1a to 1e The schematic diagram illustrates the steps of a 3D fabrication process based on heterogeneous integration for small magnetic soft machines, wherein... Figure 1e It shows the use of Figure 1c Representative steps of the fixture-assisted assembly process for one of the 3D rings shown; Figures 2a to 2d The proposed manufacturing method demonstrates a resolution characterization and capability for creating arbitrary 3D magnetization profiles. Figure 2a It is a checkerboard assembly consisting of four cubic magnetic voxels with sides of 35 µm. SEM images show the high-fidelity shape of the voxels, and the checkerboard exhibits magnetic field characteristics measured near its surface. v The heterogeneous magnetization profile was verified by the normal component. Figure 2b Three cubic voxels with sides of 100 µm were magnetized to have different 3D orientations. v Their corresponding v By measuring their corresponding v To verify, Figure 2c These are the measured and theoretical magnetization values ​​of cubic magnetic voxels with 100 µm sides and different MMP concentrations and various magnetizing magnetic field strengths. The bars and columns represent the mean and standard deviation (SD) values ​​of the measurements of three samples in the same group, respectively. "Measurements that cannot be distinguished from background noise are marked." Figure 2d The hollow cube has letters and symbols set in the magnetized outlines of its six faces, and the invisible letters and symbols are revealed by imaging each face using a magnetic field imaging (magneto-optical imaging) instrument (MagView S with a Type B sensor, Matesy Ltd.). Figures 3a to 3d Various miniature magnetic soft machines exhibiting diverse properties are shown; Figures 4a to 4c Various miniature magnetic soft machines with potential biomedical functions are shown; Figures 5a to 5e The mold casting and magnetization steps of the proposed manufacturing method are illustrated, along with its versatility. Figure 5a Two-photon polymerization (TPP), i.e., 3D printing and mold casting, is used to create voxel molds and ultimately create voxels. Scanning electron microscope (SEM) images of NdFeB and cobalt magnetic microparticles (MMPs) are provided. Figure 5b This is an SEM image of an example voxel made from PDMS embedded with NdFeB (left) and cobalt MMP (right). Figure 5c These are SEM images and schematic diagrams of some example voxels with various shapes, fabricated using the proposed strategy. SEM images were obtained using a LEO Gemini 1530 VP at an accelerating voltage of 3 kV. All SEM images were adjusted using GIMP for better visibility. Figure 5d This involves fixing multiple voxels to their respective 3D angles within a fixture and batch magnetizing them inside a VSM to set each voxel with the desired 3D magnetization. v . Figure 5e It is an example of a 100 µm side-length cubic voxel made of PDMS with MNP (cobalt iron oxide, 30 nm particle size, Merck KGaA) embedded in a 10:1 mass ratio and magnetized in a magnetic field of 1.8 T; Figures 6a to 6c The magnetic mechanism shown is in the form of a retractable ring under increasing applied force. Deformation below; Figure 7a and Figure 7bThe finite element analysis (FEA) simulation (a) and experimental demonstration (b) of the soft cube frame are shown. Figures 8a to 8c The design, simulation verification, and manufacturing process of the flower-shaped machine are shown. Figure 8a It involves the design of the overall magnetization profile of the machine and the geometry design of its voxels. Figure 8b It is the simulated shape-gradient behavior of this machine. Figure 8c These are sketches and experimental photographs of the design of the auxiliary fixtures and the manufacturing of the machinery; Figures 9a to 9b The side and top profiles of the magnetic machinery designed as a peristaltic pump are shown, along with the design and results of a modified version of the pump. Figure 10 The measured criticality that allows the loaded liquid fluid to be expelled from the soft microcapsule is shown. Amplitude and Spatial gradient ( )value; Figure 11a and Figure 11b The deformation of the magnetic machinery in the form of an anchoring device in the tube is shown, (a) the normalized area and the applied... The relationship between amplitudes, and (b) indicating how the anchoring device can be applied repeatedly in small amplitudes. To restore it to its initial configuration; Figure 12a and Figure 12b The design, simulation verification, and manufacturing process of the starfish-shaped machine are shown. Figure 12a It involves the design of the overall magnetization profile of the machine and the geometry design of its voxels. Figure 12b These are sketches and experimental photographs of the design of the auxiliary fixture and the manufacture of the starfish-shaped mechanism; Figure 13a and Figure 13b The design, simulation verification, and manufacturing process of the capsule-shaped machine are shown. Figure 13a It refers to the overall magnetization profile and voxel geometry design of the machine. Figure 13b These are sketches and experimental photographs of the design of the auxiliary fixtures and the manufacturing of the machinery; Figure 14a and Figure 14b The diagram illustrates the design and manufacturing process of a peristaltic pump. Figure 14a This involves designing the overall magnetization profile of the pump and its voxels, and verifying the deformation through simulation. Figure 14b These are sketches and experimental photographs illustrating the design and manufacturing process of the auxiliary fixture; Figures 15a to 15c The magnetic characterization of the MMP used in this work is shown. Figure 15aImaging of magnetic fields generated by 100 μm voxels with different mass ratios of MMP (NdFeB, MQP-15-7, Magnequench) magnetized along different directions (MagView S with Type B sensor, Matesy Ltd.). Figure 15b The results show the magnetic characterization of pure MMP (NdFeB, MQP-15-7, Magnequench) samples measured using VSM at maximum field strengths of 0.6 T (l1), 1.2 T (l2), and 1.8 T (l3), respectively. Figure 15c The results are magnetic characterizations of samples of two MMPs (i.e., NdFeB and cobalt (Sigma-Aldrich)) from three base polymers measured using VSM at a maximum field strength of 1.8 T. Figure 16a and Figure 16b A schematic diagram of the face and edge bonding method is shown. Figure 16a The illustration shows three configurations for applying adhesive to the faces of a voxel using tweezers and for removing excess adhesive. Figure 16b It is a process of using an auxiliary clamp to perform edge bonding, where the pocket is on the side of the auxiliary clamp and everything is at the bottom of the auxiliary clamp; Figure 17 illustrates the loading of live stem cells into a microcage heterogeneously integrated onto the top surface of an anchored soft mechanical structure. Figure 17a The process involves assembling cell microcages into anchoring soft machinery, with tenons at the bottom of the cages inserted into mortises at the voxels of the anchoring machinery, and applying uncured polymer for bonding. Figure 17b The cells are seeded into cell cages. Figure 17c The entire device is placed in a culture vessel for 24 hours to allow for cell attachment. Detailed Implementation

[0047] Figures 1a to 1d The steps performed in manufacturing the magnetic deformable machine 10 are shown. The magnetic machine 10 includes a plurality of isomorphous voxels 12, 12', 12''.

[0048] For example in Figure 1d The deformable 3D magnetic machinery 10 shown has a size of less than 10,000 mm, i.e., about 4 mm. Some of the multiple voxels 12, 12', 12'' are bonded together with adhesive 14, wherein each voxel 12, 12', 12'' has a predefined shape, size, predefined magnetic properties, and predefined material properties, such as Young's modulus, magnetization profile, stiffness, mechanical strength, durability, etc.

[0049] The corresponding side length of the magnetic mechanical device 10 can be less than 100 mm, especially less than 5 mm, and... Figure 1d In the current example, the side length is 4 mm. Each voxel 12, 12', 12'' has a 3D shape, wherein the dimensions of the corresponding side length of the 3D shape are selected in the range of 2500 mm to 5 nm, particularly in the range of 25 mm to 1 µm. In the current example, the side length along the edge 20 of the voxel reaches 25 μm.

[0050] As in Figure 1a The specification indicates that voxel 12 has a rectangular 3D shape and voxel 12' includes a mixture of triangular and rectangular 3D shapes. Generally, voxels 12, 12', 12'' can be rectangular 3D voxels 12, 12', 12'', circular 3D voxels 12, 12', 12'' (e.g., spherical voxels), polygonal 3D voxels 12, 12', 12'', triangular voxels 12, 12', 12'', arbitrarily shaped 3D voxels 12, 12', 12'', and combinations thereof.

[0051] The magnetic mechanism 10 can be a cargo delivery device (e.g., drugs, stem cells, genes, imaging agents, T cells, macrophages) that can transport the cargo and release it at a target site by deforming or opening the magnetic mechanism 10. Alternatively, the magnetic mechanism 10 can be one of the following: an anchoring device, a support, a soft peristaltic pump or other type of liquid pump, a soft cubic frame, an information encryption device, a deformable metamaterial, a shape-adaptive or shape-configurable robot, a gripper, a foldable device, a blocking device, a swimming robot, an organ model, a synthetic heart or other organ, and a retractable ring flower.

[0052] At least some of the nonmagnetic voxels 12, 12', and 12'' of the magnetic machinery 10 may be selected from the group consisting of: elastomers, thermoplastic elastomers, rubber, rigid plastics, thermoplastic plastics, such as polydimethylsiloxane, aliphatic aromatic copolyesters or modified polyesters, or modified copolyesters, polyurethane elastomers, silicone rubber, natural rubber, latex, styrene ethylene butylene styrene, butyl rubber, fluorosilicone rubber, polyester, nylon, thermoplastic polyurethane; biodegradable synthetic materials, such as poly(glycolic acid), poly(caprolactone), poly(p-dioxanone), poly(ethylene glycol) diacrylate, ... N- Isopropylacrylamide); biomaterials, such as gelatin, chitosan, alginate, agarose, hyaluronic acid derivatives, chitosan, fibrin glue, elastin, cellulose, fibronectin, collagen, silk; hydrogels; ionogels; liquid crystal polymers, elastomers or gels; shape memory polymers; photoresist polymers, such as SU-8; biological proteins, such as cuttlefish circodont protein; fabric materials; nonmagnetic metals; silicone; silica; glass; wood; carbon fiber; and derivatives and combinations thereof.

[0053] The materials of at least some of the magnetic voxels 12, 12', and 12'' may be selected from the group consisting of: magnetic materials existing in the form of a large number of particles, disks, wires, fibers, or asymmetric particles, such as chromium dioxide (CrO2), samarium cobalt (SmCo), neodymium iron boron (NdFeB), cobalt (Co), ferrites, permalloy (NiFe), carbon steel, tungsten steel, magnetic steel, iron, stainless steel, nickel (Ni), iron platinum (FePt), iron oxide, barium ferrite, and magnets; combinations or composites of the foregoing; and / or voxels 12, 12', and 12'' coated with a magnetic film or layer made of the above magnetic materials or combinations thereof, wherein the aforementioned magnetic voxel materials are uniformly or non-uniformly embedded within or covering or deposited on the aforementioned non-magnetic voxel materials; and / or combinations of the foregoing.

[0054] The material of adhesive 14 is selected from the group consisting of: uncured silicone rubber, PDMS, polyurethane, modified copolyester, silicone rubber and other uncured polymers of the foregoing, temperature-curing polymers, UV or other wavelength light-curing polymers, chemically cured polymers, waxes, tapes, super glues, surgical adhesives, various biopolymers (e.g., gelatin, deoxyribonucleic acid (DNA) and base adhesives), and combinations thereof.

[0055] The magnetic voxel 12 can have any arbitrary 3D magnetization profile, such as for uniform magnetic voxels 12, 12', 12'', wherein each voxel can have an average surface magnetic field strength selected in the range of 0 to 1 T, preferably in the range of 0 to 50 mT, wherein each voxel 12 has a predefined orientation of the magnetic field strength, for example parallel to the face 18 of the respective voxel 12, 12', 12'', or perpendicular to the face 18 of the respective voxel 12, 12', 12'', or inclined relative to one or more faces 18 of the respective voxel 12, 12', 12''.

[0056] For non-uniform magnetic voxels 12, 12', 12'', each voxel 12, 12', 12'' can have a non-uniform magnetization distribution throughout voxels 12, 12', 12'' and a varying magnetic orientation throughout voxels 12, 12', 12''.

[0057] When implementing the method, the deformation characteristics of the magnetic machinery 10 to be manufactured must be defined. This means, for example, defining the application of the magnetic machinery 10 and the working environment of the corresponding application. This may also include selecting the size and possible shape of the magnetic machinery 10.

[0058] For example, if the magnetic mechanism 10 is to be used as a cargo delivery device 10, for instance, to deliver cargo 16 in the form of a drug via the esophagus to a patient's stomach, then the magnetic mechanism 10 can be designed to have the shape of a capsule 10 that can open at a second position (i.e., the target site) to deliver the drug at the second position. Deformation can be caused, for example, by expanding the magnetic mechanism 10, such that the cargo 16 can exit the magnetic mechanism 10 by compressing the magnetic mechanism 10 to expel the cargo 16 or by opening a portion of the magnetic mechanism 10 by opening flaps, etc.

[0059] Therefore, in order to load and unload cargo 16 (i.e., deliver drugs), the magnetic mechanism 10 can be deformed by applying a magnetic field due to its deformability. It should be noted that, at this point, the magnetic field used to deform the magnetic mechanism 10 is different from the magnetic field applied to move the magnetic mechanism 10 from one position to another.

[0060] To move the magnetic mechanism 10 from a first position to a second position, magnetic force is used to move the magnetic mechanism 10. Furthermore, different magnetic fields can then be used to actuate the deformation of the magnetic mechanism 10, thereby causing changes in its shape and / or size. For this purpose, it may also be necessary to define the deformation parameters of the magnetic mechanism 10.

[0061] After defining the application and deformation characteristics of the magnetic machinery 10, a blueprint for the magnetic machinery 10 is created with reference to the deformation characteristics of the magnetic machinery 10. The blueprint typically includes the number of the respective plurality of voxels 12, 12', 12'' used to form the magnetic machinery 10, the arrangement of the respective voxels 12, 12', 12'' used to form the magnetic machinery 10, the properties of the respective voxels 12, 12', 12'' used to form the magnetic machinery 10, and the arrangement of the curing agent at the plurality of voxels 12, 12', 12'' used to form the magnetic machinery 10.

[0062] It should be noted that, at this point, the steps for creating the blueprint for the magnetic mechanism 10 include at least one of the steps selected from the group of members consisting of: - Select materials with different voxels 12, 12', 12'' to define the stiffness properties of the magnetomechanical 10; - Select one or more materials for the corresponding voxels 12, 12', 12'' used in the magnetic machinery 10; - Select uniform or non-uniform 3D magnetization profiles of magnetic voxels 12, 12', 12'' to define the deformation properties of the magnetomechanics 10 based on magnetic torque or magnetic force; - Select the appropriate voxel size: 12, 12', 12''; - Select the shape of the corresponding voxel 12, 12', 12''; - Select the magnetic properties of the corresponding voxels 12, 12', 12''; - Select the material properties of the corresponding voxels 12, 12', and 12''; - Simulate the behavior and / or deformation of the magnetic machinery 10 based on blueprints; - Adjust the blueprint of the magnetic machinery 10 based on the simulation results of the behavior and / or deformation of the magnetic machinery 10; And combinations of the aforementioned items.

[0063] Once the blueprint has been created, voxels 12, 12', and 12'' are provided. One, preferably some, of voxels 12, 12', and 12'' are magnetic, and one or more of the voxels 12, 12', and 12'' have a Young's modulus of less than 500 MPa. In some cases, one or more of the voxels 12, 12', and 12'' have a Young's modulus of less than 5 MPa. In very special cases, one or more of the voxels 12, 12', and 12'' have a Young's modulus of less than 100 kPa.

[0064] According to the blueprint, voxels 12, 12', 12'' are bonded together with adhesive 14 to assemble the magnetic mechanism 10. The bonding of multiple voxels 12, 12', 12'' to each other can be performed at one or more faces 18 of each voxel 12, 12', 12''. Alternatively or additionally, the bonding of multiple voxels 12, 12', 12'' to each other can be performed at one or more edges 20 of the voxels 12, 12', 12''.

[0065] In this respect, the step of bonding multiple voxels 12, 12', 12'' to each other includes bonding one voxel 12, 12', 12'' to another voxel 12, 12', 12'' in a subsequent step. Alternatively or additionally, the step of bonding multiple voxels 12, 12', 12'' to each other includes bonding one group of voxels 12, 12', 12'' to another group of voxels in turn. After bonding the voxels 12, 12', 12'', the adhesive is cured.

[0066] In this respect, it should be noted that at least some of the voxels 12, 12', 12'' of the magnetomechanical 10 may be invisible to imaging techniques but visible to tracking techniques, and vice versa.

[0067] The step of curing the adhesive 14 can be carried out at room temperature or another specific temperature and in the environment in which the bonding step is performed, wherein the step of curing the adhesive 14 can be carried out by a light source of ultraviolet (UV) or another wavelength, or the step of curing the adhesive 14 can be carried out in an oven or on a hot plate.

[0068] Figures 1a to 1d The 3D fabrication of a small magnetic soft mechanical 10 based on heterogeneous integration is shown. Figure 1a It shows different materials, shapes and magnetization profiles. Voxels 12 and 12' (different in both amplitude and orientation) are used as building blocks for the soft magnetic machinery 10 (also referred to as the magnetic machinery 10). The various voxels 12 and 12' are integrated together by an adhesive 14, which is then cured to ensure good bonding between the various voxels 12 and 12'.

[0069] Figure 1b The adhesive 14 is applied in two different ways to join adjacent voxels: face bonding and edge bonding, which respond differently to an external magnetic field. Regarding surface bonding, adhesive 14 is applied to the surfaces 18 of the respective voxels 12, 12' to bond them together. In contrast, regarding edge bonding, adhesive 14 is applied to the edges 20 of the respective voxels 12, 12', that is, at the locations where two or more surfaces 18 of each voxel are adjacent to each other.

[0070] Figure 1c An example soft magnetic mechanism 10 design with two interconnected circular rings is shown. The magnetic mechanism 10 is fabricated by assembling a number of isomeric voxels 12, 12' at specified 3D locations and orientations. The illustrations show the locations where two bonding options are used. At this point, it should be noted that in order to... Figure 1c As is more readily apparent in most of the following diagrams (see, for example, Figure 3), the adhesive 14 in the surface bonding connection is omitted in all schematic diagrams.

[0071] Figure 1d Experimental results for the fabricated soft magnetic mechanism 10 are shown. The experimental results indicate that the 3D device with metamaterial properties exhibits a negative Poisson's ratio, thus consistent with the designed shape gradient behavior. Figure 1d The lower image of the two images shows how a magnetic machine can move through a magnetic field when a magnetic field is applied. Figure 1d The two images are deformed by shrinking compared to the expanded state shown in the top image.

[0072] To illustrate the capabilities of the proposed fabrication method, a design example of a soft magnetic mechanism 10 is presented. The magnetic mechanism 10 consists of two interconnected circular rings with 3D metamaterial properties (Figure 1). The circular rings have a diameter of approximately 1 mm and are composed of voxels 12, 12', and 12'', which are made of three elastomers with different Young's moduli (i.e., stiffness): Dragonskin, Ecoflex-10 silicone rubber, and polydimethylsiloxane (PDMS). These voxels 12, 12', and 12'', representing a variety of magnetic and non-magnetic soft materials with various shapes and stiffnesses, are mass-produced using soft photolithography (see Figure 5). The magnetic voxels 12, 12', and 12'', made of soft elastomers (e.g., silicone rubber) embedded with hard magnetic microparticles (MMPs; e.g., NdFeB microparticles), are pre-magnetized to set their respective local magnetic moments. These voxels 12, 12', 12'' are precisely assembled together using adhesive 14 (i.e., a liquid non-crosslinked soft elastomer), which is applied to bond adjacent voxels 12, 12', 12'' on the face 18 or edge 20 of adjacent voxels (see [link to adhesive]). Figure 1b This results in different shape gradient behaviors.

[0073] The soft mechanical 10's designed 3D shape and magnetized profile can... Figure 1c As can be seen from this. When an external uniform magnetic field is applied... ( When mT), each ring and the entire soft mechanical 10, which contracts in its radial direction, behave as a negative Poisson's ratio metamaterial. Figure 1d The following will explain one of the rings in different... The deformation characterization is shown below (see also Figure 6). Figure 1 illustrates the unique advantages of the proposed assembly-based strategy: it enables free heterogeneous integration of different materials at high resolution compared to previous methods, and achieves uncoupled, arbitrary, and 3D geometries and magnetization profiles, which were previously unattainable.

[0074] To demonstrate the resolution of the proposed manufacturing method (i.e., the minimum size of voxels 12, 12', 12''), a chessboard was assembled from four 35 μm side-length cubic voxels 12, 12', 12''. Figure 2a This is less than half the resolution produced by current 3D printing methods using magnetic soft machinery 10. This resolution can be further improved in the future to sub-10 μm and even sub-μm scales by using nanoscale magnetic particles embedded within soft synthetic voxels or voxels based on biomaterials, DNA-type settable bio-adhesives, and optical tweezers-type precision micro / nano manipulation systems. At this high manufacturing resolution, each voxel 12, 12', 12'' can also possess a local magnetic moment. . It can point in any 3D direction ( Figure 2b Besides assuming uniform (constant) magnetization, It can also be set to be variable in space. Additionally, It can have any value from zero to a maximum value limited by the magnetic properties of MMPs. This maximum magnitude can be determined by the MMP concentration in a given voxel and the field used to magnetize the voxel. Tuning by amplitude ( Figure 2c ).

[0075] To demonstrate the proposed manufacturing strategy's ability to set up high-fidelity 3D magnetized profiles with abrupt changes, a hollow cubic machine 10 was fabricated from 218 cubic voxels with 100 μm side lengths. Figure 2d The abrupt out-of-plane change in magnetization profile is difficult to achieve using extrusion-based or UV lithography-based 3D printing methods, as the pre-magnetized MMPs used in these methods tend to remain within the 2D geometric plane and are unwilling to change orientation abruptly. Furthermore, such a fully sealed hollow structure cannot be fabricated using previously reported UV lithography-based methods because the printed top surface requires support material and uncured photoresist cannot be expelled from the waterproof surface. Each face of the fabricated hollow cube has an coded letter or symbol in its corresponding magnetization profile, i.e., “MPI-IS”. Under inspection by a magnetic field imaging instrument (e.g., a magneto-optical sensor), the established magnetization profile shows clear changes between adjacent voxels 12, 12', 12'' and delivers legible information, thus validating the ability to encode accurate magnetization profiles at the voxel level. Since magnetization profiles established on hard MMPs are invisible to the naked eye and difficult to erase, setting invisible, complex patterns in magnetic soft machinery has potential applications in information storage and encryption.

[0076] Figure 1e It shows the use of Figure 1c The following are representative steps of the jig-assisted assembly process for one of the 3D rings shown. First, the magnetic voxel 12 is inserted into the slit jig 100 and covered with a cover 102. Adhesive 14 is applied through the holes 103 of the cover 102, and then excess adhesive 14 is removed using a scraper 106 to form an edge bond.

[0077] Next, magnetic and non-magnetic voxels 12 and 12' are inserted into a 2D fixture 108 manufactured by two-photon polymerization (TPP) or die casting. The 2D fixture 108 has... Figure 1c The shape of one of the rings shown defines the basic shape of this ring in the machine 10. Magnetic and non-magnetic voxels 12, 12' are assembled in the fixture 108 by face bonding to form a ring. Alternatively, only half of the ring in the fixture 108 can be filled with magnetic and non-magnetic voxels 12, 12' to form a semi-ring.

[0078] Finally, the ring and two half-rings are inserted into the 3D fixture 110 (manufactured via TPP-based 3D printing) to define... Figure 1c The shape of the complete machine is shown. The three parts of the machine 10 are assembled in a fixture, and then an adhesive is applied to the corresponding surfaces 18 to form the 3D soft machine 10 by surface bonding.

[0079] Figures 2a to 2d The resolution and versatility of the proposed 3D manufacturing strategy are demonstrated. Figure 2a A chessboard assembly consisting of four cubic magnetic voxels 12 with sides of 35 µm is shown. Scanning electron microscopy (SEM, LEO Gemini 1530 VP) images reveal the high-fidelity shape of the voxels 12. The chessboard exhibits characteristics obtained by measuring its near-surface magnetic field. The heterogeneous magnetization profile was verified by the normal component. SEM images were obtained at an accelerating voltage of 3 kV. Artificial pigments were manually added in the GNU Image Manipulation Program (GIMP) to define partial boundaries using the lasso tool.

[0080] Figure 2b It shows magnetization with different 3D orientations Three cubic voxels, each with a side length of 100 μm, are 12. Their corresponding... By measuring them Let's verify.

[0081] Figure 2c The magnetic field components of a cubic magnetic voxel 12 with a side length of 100 μm and different MMP concentrations and various magnetization field intensities are shown. The measured values ​​are shown. Four samples with MMP weight ratios of 0.0%, 33.3%, 50.0%, and 66.7%, respectively, are presented.

[0082] Figure 2d A cubic softmechanism is shown, featuring letters and symbols set into the magnetized contours of its six faces 18, as an example of potential information encryption applications. (Measured) The clear edges indicate abrupt changes in magnetization profile between adjacent voxels 12, 12', and 12''. Information invisible to the naked eye is revealed by imaging each face using a magnetic field imaging (magneto-optical sensor) instrument (MagView S, Matesy).

[0083] Figures 3a to 3d A miniature magnetic soft machine 10 exhibiting different and diverse properties is shown. Figure 3a A hollow cubic device 10a exhibiting negative Poisson's ratio 3D metamaterial properties is shown: it exists in In the case of shrinking in all three dimensions. Figure 3b A flower-shaped soft mechanical device 10b with a composite stiffness distribution is shown. The petals of this flower-shaped soft mechanical device bloom sequentially under increasingly stronger magnetic field strengths. Figure 3c A starfish-shaped machine 10c with directional joint bending is shown, fabricated using two layers of magnetic voxels. The flat body of this starfish-shaped machine expands vertically and contracts horizontally under a uniform magnetic field.

[0084] Figure 3d A capsule-shaped mechanism 10d is shown, in which two cylindrical voxels / parts are embedded with MMPs of different coercivity to achieve reconfigurable magnetization. The capsule-shaped mechanism remains closed due to the attractive magnetic interaction between its two parts. After a pulsed remagnetizing field, the part with the low-coercivity MMP reverses its magnetic moment direction, changing the magnetic interaction from attraction to repulsion, which opens the capsule. This device 10d demonstrates configurable remagnetization capability by using voxels with different magnetic materials.

[0085] Such capsules can be used to deliver liquid medication 16 to target locations in the human body, such as in the stomach or gastrointestinal tract, using minimally invasive techniques. Therefore, when defining the deformation characteristics of the magnetic mechanism 10 and when creating a blueprint for the magnetic mechanism 10 with reference to these deformation characteristics, it has been found that the magnetic mechanism 10 may possess the following characteristics: 1. It has a hollow shape to hold drugs.

[0086] 2. It is soft enough to squeeze out the contents and interact safely with human tissue.

[0087] 3. It is controlled by an external magnetic field for movement and drug release control.

[0088] 4. Biocompatibility.

[0089] To achieve the aforementioned characteristics, the blueprint for the magnetic mechanism 10 is designed as a hollow spherical capsule composed of nine soft rings. The overall dimensions of the magnetic mechanism can be determined for different applications. The magnetization of each ring of the magnetic mechanism 10 is designed such that the capsule can pass through the applied overall magnetic field. When the intensity exceeds a critical value, the chamber is squeezed to release drug 16, and the capsule maintains its intensity while the rotating magnetic field is in operation. When smaller, it rolls on an uneven surface. The diameter of the orifice is specifically designed to retain the drug during rolling. Each ring is formed from a single voxel, with each capsule formed from multiple cyclic voxels and two or more plate-shaped voxels. In the current example, two plate-shaped voxels and seven cyclic voxels are used to form the capsule. The material used for the corresponding voxels can be an elastomer, thermoplastic elastomer, rubber, rigid plastic, thermoplastic plastic, such as polydimethylsiloxane, aliphatic aromatic copolyester or modified polyester, or modified copolyester, polyurethane elastomer, silicone rubber, natural rubber, latex, styrene-ethylene-butene-styrene, butyl rubber, fluorosilicone rubber, polyester, nylon, thermoplastic polyurethane; biodegradable synthetic materials, such as poly(glycolic acid), poly(caprolactone), poly(p-dioxanone), poly(ethylene glycol) diacrylate, ... N - Isopropylacrylamide); biomaterials, such as gelatin, chitosan, alginate, agarose, hyaluronic acid derivatives, chitosan, fibrin glue, elastin, cellulose, fibronectin, collagen, silk; hydrogels; ionogels; liquid crystal polymers, elastomers or gels; shape memory polymers; photoresist polymers, such as SU-8; biological proteins, such as cuttlefish circodont protein; fabric materials; and derivatives and combinations thereof.

[0090] The unprecedented versatility of the proposed manufacturing method enables the realization of numerous key design features of soft machinery that were previously difficult to manufacture. To demonstrate this key feature capability, a cubic bare-edge framework with a negative Poisson's ratio in 3D is first created by assembling sixty-eight 100 μm side-length cubic voxels 12, 12', and 12'' constructed using Ecoflex 0050, ensuring large deformation under achievable magnetic fields. Figure 3a This shape (i.e., a hollow cube with bare edges) is difficult to manufacture using existing methods without supporting material. At 370 mT Below, the cube shrinks horizontally by 11% (along...) x shaft and y (axis) and vertically contracted by 6% (along the axis) z (axis), thus exhibiting 3D metamaterial properties. The deformation of this structure can be further tuned using voxels 12, 12', and 12'' with different moduli.

[0091] Secondly, the composite stiffness distribution can further broaden the design space of the soft machinery 10. The assembly method allows for the free selection of building materials with a wide range of moduli. As an example, a flower-shaped machinery 10 with a sequential petal blooming response was formed. Figure 3bThe mechanism (~1 mm in diameter) is made of 126 cubic magnetic voxels with sides of 100 μm and a central hexagonal non-magnetic voxel. Although the magnetization profile of each petal is the same (Fig. 8), its voxels 12, 12', and 12'' are made of two polymer materials: Ecoflex 0050 silicone rubber (relatively soft) and PDMS (relatively hard). These two types of voxels 12, 12', and 12'' with carefully selected stiffness values ​​are used to fine-tune the stiffness distribution of the magnetic mechanism 10. Thus, three petals of the magnetic mechanism 10 are fully opened at 40 mT and the other three are opened at 90 mT. Figure 3b This was further confirmed through simulation analysis.

[0092] Next, edge bonding technology breaks the bending symmetry, thereby endowing the material with the ability to implement directional bending at the joint. To illustrate, a starfish-shaped origami-like magnetic mechanical 10c ( Figure 3c The machine is made of twenty-four triangular, flat, magnetic voxels 12, 12', and 12''. The joints are bent towards the side with the adhesive 14, marked in pink in the illustration. All voxels 12, 12', and 12'' are magnetic, and the mass ratio of polymer to MMP is 1:3. In this case, the magnetic mechanical 10c extends vertically from its initial flat shape while simultaneously contracting horizontally.

[0093] Ultimately, the possibility of using multiple materials enabled reconfigurable magnetization profiles. A prototype of a capsule-shaped soft machine, consisting of two cylindrical voxels / parts joined together by edge bonding, was fabricated using two different MMP materials (NdFeB and Cobalt) with different coercivity values. Figure 3d The machine remains closed in its inactive state due to localized magnetic attraction between its two parts. To change the magnetization direction of one of its parts, a pulsed remagnetizing field (peak amplitude 295 mT, the pulse decaying to half its peak value within 1.33 ms) is applied. This field is strong enough and fast enough to reverse the magnetic direction of the cobalt part, which has lower coercivity, without affecting the NdFeB part, which has higher coercivity. Thus, localized magnetic interaction... In the original Bit The process switches from attraction to repulsion, thereby opening the capsule and maintaining this activated state stably, even when no such attraction is present. The same applies at other times. This device can be used to deliver internal cargo in a gentle manner (without jet stress), enabling the delivery of fragile cargo such as stem cells and genes to the target location. Additionally, the device has the potential to be used in the future as a fluid biopsy tool to collect localized biofluid samples from the body (e.g., microbial samples from the gut). This machine demonstrates the ability of this manufacturing method to integrate multiple MMP types into the same machine to achieve a reconfigurable magnetized profile for reconfigurable soft mechanical designs.

[0094] Figure 4 shows a miniature magnetic soft machine 10 with potential biomedical functions. Figure 4a A peristaltic soft pump inspired by the intestine is shown as a magnetic mechanism 10. The rotation of the tubular pump in the xy-plane is also illustrated. The material forms a wavy deformation on its body. When placed at the bottom of the reservoir, a viscous liquid (e.g., PDMS base material in this case) is mechanically pumped and transports solid polystyrene balls with a diameter of 1 mm as its creeping waves propagate downwards.

[0095] Therefore, it is desirable to develop a machine 10 that can function as a miniature peristaltic pump and pump various liquids and solids. This peristaltic pump needs the following characteristics: 1. It can pump liquids and solids.

[0096] 2. It has a miniature body and can therefore work in a small and constrained environment.

[0097] When developing the blueprint based on this, creep deformation is chosen as the method to achieve the desired pumping function. The device generally has a tubular shape and creep deformation can be generated by a deformation pattern that propagates along the length of the tube.

[0098] To achieve propagation behavior, the tube is divided into circular slices along its length. All slices in the blueprint have similar magnetization profiles. However, a phase transition is added between the magnetization profiles of adjacent slices. To use the phase transition to propagate deformation, the actuating magnetic field is chosen as a rotating magnetic field, with its axis of rotation collinear with the length of the tube. In the rotating magnetic field, each slice deforms and recovers periodically. However, as a result of the phase transition, the deformation of different slices is synchronized with the time delay between slices, thus causing the propagation phenomenon. For this design, 4 to 32 voxels can be used per slice, the material of the corresponding voxels can be selected as described herein, and the side lengths of the corresponding voxels 12, 12', and 12'' can be selected in the range of 35 µm to 10 mm.

[0099] Figure 4b The micro-soft capsule is shown as a magnetic mechanical device 10. A critical magnetic field is applied. Subsequently, the internal liquid cargo can be discharged as needed through its designed top opening. The capsule rolls on the surface of the stomach phantom and releases edible dye as needed. Five such mechanisms are moved and activated together to release the internal pseudo-drug fluid.

[0100] Figure 4c A surface anchoring device as a magnetic mechanism 10 is shown. It can anchor and release inside a pipe with a fluid (water) flow rate of 20 cm / s as needed. The design of the mechanism 10 and its application are schematically illustrated. The device anchors itself in the tube and in the absence of In the case of resisting fluid flow. Once applied It releases itself through fluid flow and / or an externally applied magnetic field gradient. (Formed by an external permanent magnet) it moves to anchor at the target location inside the tube. For easier visualization, the adhesive in the surface bonding connection is omitted in all schematic diagrams.

[0101] In order to anchor the anchoring device inside the blood vessel, the micromechanical device 10 needs to have the following characteristics.

[0102] 1. It can move and anchor inside the tubular structure as needed.

[0103] 2. It can withstand high-speed blood flow.

[0104] To achieve these objectives, the blueprint for the magnetic mechanism 10 includes multiple retractable rings connected by linkages. Each ring has a diameter slightly larger than the cross-section of the target workspace, allowing it to anchor itself when no magnetic field is applied. The magnetization of each ring is specifically determined so that when an external magnetic field is applied... When this occurs, the ring can contract significantly, thus releasing itself from the anchoring position. Another advantage of this design is that the ring does not impede flow and therefore experiences minimal fluid resistance. The number of voxels used to form each ring can range from 24 to 120, and the average side length of each voxel can range from 35 µm to 10 mm. The material used for the corresponding voxels can be any of the materials mentioned in this document.

[0105] By endowing them with the ability to achieve the four key characteristics mentioned above, three novel wireless micro-magnetic soft machines 10 exhibiting potential medical functions are presented. These examples confirm that the proposed fabrication strategy can significantly expand the feasible design space of the magnetic soft machines 10 to meet the needs of a variety of potential real-world biomedical and other applications. In the first demonstration, an intestinal-inspired tubular soft peristaltic pump was developed. The machine's thirty-seven vertically stacked annular horizontal slices (slice thickness: 100 µm, outer diameter: 1.2 mm, inner diameter: 1.0 mm) have a specific magnetization profile that can respond to... x- y Rotation in a plane And with a specific phase difference (e.g., stacked voxels 12, 12', 12'' between adjacent slices) exist xy The magnetic mechanical 10 periodically contracts and expands (rotating 10° in the plane) to form a traveling wave along the tubular soft pump (see Figure 5). Due to the phase transition set in the magnetization profile of adjacent slices, the magnetic mechanical 10 forms an axial traveling wave-like deformation on its body (see Figure 5). Figure 4a This traveling wave can pump fluids forward or backward and transport solid objects, depending on the direction of the wave. Figure 4a (See Figure 5). The magnetic mechanism 10 is mounted vertically and horizontally, and it is controlled to pump in opposite directions to isolate environmental factors such as gravity. The results confirm that the observed pumping behavior is indeed caused by the traveling wave-like deformation of the body of the magnetic mechanism 10. Such pumping on a small scale can have various "lab-on-a-chip" device applications (e.g., clinical assays) and can be used to form ureteral models with peristalsis for surgical training. Furthermore, it has potential future medical applications by forming small tubular (e.g., intestinal or ureter) wireless implants inside the human body that can actively pump internal biological fluids.

[0106] The second demonstration showed hollow spherical microcapsules (maximum size: 600 µm) that wirelessly rolled on an uneven surface (i.e., a stomach phantom) to a target location. Once activated at the desired location, the capsules expelled their enclosed liquid cargo (here, an edible dye, which could be replaced in the future by a drug, gene, or imaging agent) and eventually moved away from the working environment. Figure 4b In cancer treatment and other disease treatments, such wireless microcapsules, capable of carrying and locally administering drugs as needed, hold promise for future targeted drug delivery applications. At that time, the capsule itself contracts and compresses. When smaller (for this particular design <100 mT), the orifice at the tip of the capsule is closed. Once Exceeding the threshold (>100 mT for this particular design), the pressure built up inside the capsule is large enough to open the orifice and expel the pseudo-liquid drug. In both cases, the net magnetic moment of the capsule... Allowing it to roll on uneven surfaces and pass through The movement passes over obstacles. In the method section, three liquids of different viscosities are loaded into capsules, and the required critical values ​​are reported. (See) Figure 10 Furthermore, five of these capsules 10 can be deployed as a team, where they move and deliver liquid cargo simultaneously. This teaming of capsules can achieve higher delivery efficiency and potentially utilize non-uniform magnetic fields or heterogeneous robotic designs for independent control.

[0107] As the final device demonstrated, a surface anchoring device is formed as a magnetic machine 10 (outer diameter: 1.68 mm, length: 1.70 mm), which can be released, moved, and anchored as needed inside a tube with internal fluid flow. Figure 4c This device could potentially be used inside blood vessels in the future to reach target sites deep within the body and perform minimally invasive interventions. The anchoring device has a diameter slightly larger than the cross-section of the target working space (in this case, the inner diameter of the tube). This design allows force to be applied to the tube wall once deployed. When no force is applied... At that time, the device 10 anchors itself inside the tube and resists the flow of liquid (e.g., water) with a velocity of 20 to 45 cm / s. Figure 4c (at 0s in the middle). After applying... In this case, the mechanical device 10 can retract to a size smaller than the inner diameter of the tube, release itself from the anchoring position, and move with the fluid flow in the tube. For better positioning of the anchoring device 10, it can also be generated by an external permanent magnet. Appropriate spatial gradient ( ), to flow together with the fluid (in Figure 4c (at 8 s) or against (in) Figure 4c The fluid flow (at 14 to 15 seconds) moves the device. Once removed... The device will then recover its expanded shape due to its stored elastic energy and anchor itself back inside the tube (in Figure 4c(See also Figure 11). The inner diameter of the glass tube used in the experiment (1.62 mm) and the flow rate (20 cm / s for dynamic anchoring tests and 45 cm / s for static anchoring tests) are within the range of clinical measurements for lumen diameter and blood flow velocity in human coronary arteries. To make it more medically functional in the future, this soft device could be loaded with a drug that could be released over an extended period of time in the target vascular region after anchoring. When the drug has been depleted, the device could be released from its anchoring position and retrieved from the body. Furthermore, this device could potentially be used as a wireless stent in the cardiovascular system.

[0108] Figure 5 shows a schematic diagram of the proposed manufacturing strategy for producing prototypes of various magnetic soft machines 10. Figure 5a The illustration shows the manufacturing process for voxels 12, 12', and 12'' using photolithography, TPP, and die casting techniques. Figure 5b SEM images and schematic diagrams of some example voxels 12, 12', 12'' with various shapes produced using the proposed strategy are shown. Figure 5c This demonstrates that after curing, magnetic voxels 12, 12', 12'' are oriented to the desired 3D angle and then magnetized inside a vibrating specimen magnetometer (VSM; Microsense EZ7) with a high (up to 1.8 T) uniform magnetic field to set the desired 3D magnetization intensity and orientation. . Figure 5d The assembly of a number of voxels 12, 12', 12'' together is shown, wherein adhesive 14 is applied by face bonding or edge bonding methods.

[0109] Figure 6 illustrates the shrinkable ring under increased application. The following deformation. Figure 6a An experimental snapshot of the contraction process is shown. Figure 6b A detailed view of the curvature of the α and β joint is shown. Figure 6c The standardized area and the applied area are shown. The relationship between amplitudes. Experiments were conducted on the water surface to eliminate friction. The normalized region was determined by the current state and the state when closed. The ratio of the enclosed regions between states at time is defined.

[0110] Figure 7 shows the finite element analysis (FEA) simulation and experimental demonstration of the soft cube frame. Figure 7a Deformation analysis of a cube frame made of different materials is shown. Figure 7b The experimental results show the mechanical grasping, transporting, and releasing of the soldering iron ball from the glycerin to the target location.

[0111] Figure 8 shows a schematic diagram of the flower-shaped soft machinery and an FEA simulation. Figure 8a A schematic diagram of the magnetization profile of the flower-shaped soft machinery is shown. Figure 8b The FEA simulation of petal structure deformation is shown. The deformation of a softer (left) petal and a harder (right) petal are simulated. The applied magnetic field is shown in both cases. It is 40 mT.

[0112] Figure 9 shows an observation of the side and top profiles of the peristaltic pump, as well as the design and results of a modified version of the soft pump. Figure 9a It shows the rotation The side and top profiles of the peristaltic pump observed in the image. Angle. Defined in Figure 4. Figure 9b A comparison of experimental results for different pumping directions in viscous fluids is shown. Figure 9b This machine is shown transporting solid polystyrene balls through the air. The ball positions can be identified in Supplementary Video 1.

[0113] Figure 10 The measured criticality that allows the loaded liquid fluid to be expelled from the soft microcapsule is shown. Amplitude and Spatial gradient ( Value. Three samples with different viscosities were used.

[0114] Figure 11 shows the deformation of the anchoring device in the pipe. Figure 11a The standardized area and the applied area are shown. The relationship between amplitudes. The normalized region consists of the current state and the state where it does not exist. The ratio of the enclosed regions between the states at different times is defined. Experiments are conducted in a glass tube. Figure 11b It is shown that the anchoring device can be repeatedly applied in small increments. To restore it to its initial configuration. The red arrow indicates... The direction.

[0115] The 3D fabrication of the magnetomechanical 10 based on precision assembly initially involved designing voxels 12, 12', and 12'' in Solidworks (Dassault Systèmes). The designs were then fabricated into male molds with raised features using two methods: two-photon polymerization (TPP) and photolithography. IPS (Nanoscribe GmbH) and SU8 (MicroChem) were used for TPP and photolithography, respectively. TPP offers the advantage of greater accuracy in dimensions away from the plane and allows for non-uniform thickness. Photolithography offers the advantages of being more time- and cost-effective. Female molds were then fabricated by casting PDMS (Sylgard 184, Dow Chemical Company) at a base-to-curing agent mass ratio of 5:1. These molds were treated with silane to facilitate voxel curing and release. Voxels of various materials and shapes were fabricated as basic building blocks by casting uncured polymers with optional MMPs into these shaped female molds. The voxels were cured in batches within the female molds. The curing temperatures and times required by the polymer handbook are as follows. This voxel manufacturing process is in Figure 5a The diagram is schematically shown. Various polymers used in this work include Ecoflex 0010 (Smooth-On), Ecoflex 0030 (Smooth-On), Ecoflex 0050 (Smooth-On), Ecoflex Gel (Smooth-On), Dragon Skin 30 (Smooth-On), and PDMS. Figure 5b Some example voxels with a variety of geometries that can be manufactured are shown.

[0116] The methods for manufacturing voxels 12, 12', and 12'', as well as fixtures 100, 108, 110, and 112, will be discussed in detail below.

[0117] Magnetic voxels 12, 12', and 12'' consist of NdFeB hard magnetic microparticles (MQP-15-7, Magnequench; average diameter 5 µm) mixed in an uncured polymer at a mass ratio corresponding to the desired MMP concentration. In this work, the mass ratio between polymer and MMP is 1:1 unless otherwise specified. After curing, voxels 12, 12', and 12'' are manually removed from the mold using tweezers. Magnetic voxels 12, 12', and 12'' are positioned in the designed 3D orientation and magnetized using a vibrating specimen magnetometer (VSM; EZ7, Microsense) to generate voxel magnetic moments with 3D pre-set strength and orientation. ( Figure 5cThe magnetizing field has a strength of 1.8 T unless otherwise specified. Finally, magnetic and non-magnetic voxels 12, 12', 12'' are assembled together, wherein an adhesive 14 is applied to connect adjacent voxels 12, 12', 12''. The position and orientation of each voxel 12, 12', 12'' are controlled during assembly, resulting in a heterogeneous 3D geometry and 3D magnetization profile of the final magnetomechanical 10. The adhesive 14 is an uncured liquid soft elastomer that cures upon contact with the voxels it is attached to.

[0118] Adhesive 14 is used when assembling voxels into their designated positions in the manufactured 3D soft machinery. Figure 5d The binder 14 is selected as an uncured liquid soft elastomer that can cure upon contact with adjacent voxels 12, 12', 12''. The function of the binder 14 is to connect adjacent voxels 12, 12', 12'' and integrate them to form a synthetic 3D magnetic machinery 10. In this work, two methods are used to apply the binder 14: The selected adhesive 14 is applied to the entire area of ​​the faces 18 of voxels 12, 12', 12''. Then, the second voxels 12, 12', 12'' are brought near and aligned with the first voxels 12, 12', 12'', so that the adhesive 14 is in the middle of the two faces 18. The two voxels 12, 12', 12'' are moved toward each other until contact is made. The adhesive 14 cures between the faces 18 of the two voxels 12, 12', 12'' and integrates them into a composite. The connection formed by this method is symmetrical, meaning that the connection has no directional preference when bent. The joined voxels 12, 12', 12'' form a continuous soft body without obvious joints. A special case of face bonding is that the two faces 18 form acute angles rather than being parallel to each other. The adhesive 14 not only connects adjacent voxels 12, 12', 12'', but also acts as voxels 12, 12', 12'' and itself complements the geometry of the final machine. This may occur when voxels 12, 12', 12'' made of the same elastomer as adhesive 14 are required at the joint location, but they are too small to be manufactured and assembled effectively.

[0119] To form an asymmetric connection, an adhesive 14 is applied to the side surfaces 20 of the contact surfaces 18 of two adjacent voxels 12, 12', 12''. Without the adhesive 14 between the contact surfaces 18 of two adjacent voxels, the two adjacent voxels 12, 12', 12'' could easily detach from each other once a suitable torque is applied. However, the adhesive 14 applied at the edges 20 where two or more surfaces meet fixes the voxels 12, 12', 12'' on one side, thereby breaking the bending symmetry by making it easier for the joint to open from the opposite side of the adhesive 14. Thus, when a torque is applied in the preferred direction, the voxels 12, 12', 12'' detach and the joint opens, while when the torque is applied in the opposite direction, the voxels 12, 12', 12'' compress each other and the joint remains closed. The open joint allows for greater deformation using relatively small torques. In contrast, closed joints force the entire soft body to bend, and thus make it more difficult to bend, resulting in smaller deformation at the same moment amplitude.

[0120] Considering the desired shape gradient behavior at specific joints in a given machine, two bonding methods are selected item by item for each joint between voxels. Most machines utilize both methods in their manufacturing process.

[0121] This means that the binder 14, similar to voxels 12, 12', 12'', contributes to the deformability of the mechanism. By placing the appropriate binder 14 at predefined locations other than specific voxels 12, 12', 12'', hinge-like features can be introduced into the magnetic mechanism 10, around which and relative to these hinge-like features, the magnetic mechanism 10 can deform. For example, in... Figure 1d The image below shows the magnetic mechanism 10 deformed compared to the image above when a magnetic field is applied. Deformation is possible because the relatively soft voxels 12, 12', 12'' allow the magnetic mechanism 10 to buckle relative to the relatively hard voxels 12, 12', 12'' by moving the magnetized (generally harder) voxels 12, 12', 12'' relative to the unmagnetized (generally softer) voxels 12, 12', 12''.

[0122] In this respect, it should be noted that the Young's modulus of voxels 12, 12', and 12'' of the relatively soft material is smaller than that of the relatively hard material. It should also be noted that the Young's modulus of the relatively soft material is typically chosen to be at least 5 kPa smaller than that of the relatively hard material.

[0123] After fabrication, the prototype magnetomechanical 10 was placed inside its designated test setup, such as inside a circular tube, and observed using an optical microscope. A handheld permanent magnet (neodymium, N42, nickel-plated, Supermagnete) was used to generate a magnetic field vector in any 3D direction within the workspace. Observed specimen deformation and motion were captured using a camera (Point Grey Research) and a high-speed camera (Phantom Cinemag II v641). Each specimen was reversibly tested multiple times, with no observable signs of performance degradation.

[0124] In this work, heterogeneous integration of voxels was performed manually using tweezers under a stereomicroscope. While offering great flexibility and versatility, manual operation limits the effectiveness and repeatability of the fabricated machinery, further hindering the efficient use of voxels with dimensions smaller than 35 μm. It is hoped that in the future, remotely operated or automated micromanipulators will replace the manual fabrication process to achieve greater accuracy, repeatability, and speed. To validate the feasibility of this research direction, a preliminary demonstration was shown of assembling four 100 µm side-length cubic magnetic voxels into a checkerboard pattern using two remotely operated micromanipulators.

[0125] A uniform magnetic field can be provided The shrinkage process of the ring was investigated in a vibrating specimen magnetometer (VSM; EZ7, Microsense) (e.g., see...). Figure 1c The ring was placed on the water surface to achieve in-plane deformation. The results shown in Figure 6 illustrate the nonlinear relationship between the external magnetic field and the deformation quantified using a normalized region. Figure 6c The standardized area is the ratio between the current closed area and the original closed area. The joint is designed to have a higher ratio The joint has low bending stiffness and initiates ring deformation. Figure 6b ). and The bending at the joint reduces the circumference of the ring, thus causing contraction in all directions.

[0126] The Ecoflex 0050 used to construct the cube frame ensures large deformation of the device, which can be achieved through... Figure 7aThe simulation results are presented here. The neo-Hookean model is used to simulate the strain-stress relationship of the materials. Three materials used in the literature are selected for comparison: Ecoflex 0050 (shear modulus: 27.6 kPa, bulk modulus: 2 GPa), Dragon Skin 0030 (shear modulus: 197.6 kPa, bulk modulus: 2 GPa), and PDMS (shear modulus: 290 kPa, bulk modulus: 1 GPa). Under a uniform magnetic field, it is assumed that each voxel 12, 12', 12'' of the frame tends to align with the field applied by a torque, which is further decoupled into forces acting on the voxel boundary surfaces. The cubic frame made solely of Ecoflex 0050 exhibits significant shrinkage under a 200 mT magnetic field. The cubic frame has a non-zero net magnetic moment. Therefore, it can roll on the surface under a rotating magnetic field. With a hollow interior space and 3D metamaterial properties, the control mechanism 10 grasps the cargo, rolls it for transport, and releases it at the target location. Figure 7b ).

[0127] Will have different material properties (see Figure 8a The effect of voxels 12, 12', and 12'' patterning on petal bending can be further analyzed through simulation. In the simulation, downward application... This will not cause bending because the magnetization direction of the petals is set vertically aligned and the torque will not act on them initially. Therefore, a small perturbation is introduced to initiate the bending process. Figure 8b Simulation results of softer and harder petals under a magnetic field of 40 mT are shown, demonstrating that the effective bending stiffness of the entire structure of the magnetomechanical 10 can be tuned by patterning voxels made of different materials.

[0128] The tubular soft peristaltic pump, designed as a magnetomechanical 10, relies on the cross-linking of its stacked rings. A continuous phase transition. This phase transition value was chosen to be 10° to balance the smoothness of the traveling wave-based shape deformation with the amount of stacking required to create an observable pumping effect. Larger phase transition angles (e.g., 20°) would further discretize the deformation, while smaller angle values ​​(e.g., 5°) would require a larger number of stacked rings to produce the traveling wave-like deformation for pumping liquids and transporting solids. In this case, each ring exhibits a different deformed profile, which is determined by the ring's... With the whole The relative angle between them determines this. When During rotation, this angle of any particular ring changes continuously, causing periodic deformation of the ring. Therefore, the traveling wave-based shape deformation of the tubular machine 10 propagates along its axial direction, the direction of propagation of which is determined by… The direction of rotation determines the peristaltic pump's rotation. The side and top profiles in the case Figure 9a As shown in the image.

[0129] To characterize how much is needed Amplitude and Spatial gradient ( To expel the fake liquid drug 16 loaded inside the microcapsule 10, experiments were conducted and... Figure 10 The experiment is illustrated in the figure. A full analysis of this critical value requires a detailed investigation of the magnetic deformation of the microcapsule, the sealing of the orifice (due to the self-adhesion of Ecoflex Gel), the properties of the loading fluid, and the fluid surrounding the capsule. Within the scope of this work, the focus is solely on altering the viscosity of the liquid inside the capsule while keeping others constant. Specifically, the same capsules were pre-filled with edible dye (assuming a viscosity similar to water, with a viscosity ≈ 8.955 at 25 °C). m 2 / s), a 1:1 ratio food dye / glycerin solution (viscosity ≈ 6.018 at 25 °C). m 2 / s) and pure glycerol (viscosity ≈ 7.201 at 25 °C). m 2 / s). Then, the capsule is placed in a fluid container, and a permanent magnet is used to approach the capsule while recording the critical temperature required to expel the liquid inside. and For example, in Figure 10 The results shown in the image require a large amount of data. and To release liquid drugs with high viscosity.

[0130] To characterize the shrinkage performance of surface anchoring devices, experiments were conducted to find... The relationship with the standardized area. The anchoring device 10 is placed in a glass tube with an inner diameter of 1.62 mm, which is related to the... Figure 4c The same is used. VSM is used to apply uniformity. Unlike the contraction process of a retractable ring floating on the water surface, the contraction of the anchoring device 10 has a critical... (Approximately 150 mT), exceeding this will significantly increase the contraction rate. Figure 11a This observation can be caused by the constraint of the inner tube wall and the adhesion between the inner tube wall and the outer surface of the anchoring device. The final saturation (approximately 220 mT) prevents device 10 from shrinking further, even at a larger scale. The same applies below. At this stage, device 10 cuts... It will not be fully restored to its original configuration afterward, and significant out-of-plane deformation of each ring is observed. Figure 11b (The first line in the text). To restore device 10 to its original configuration, it can be simply applied repeatedly in small increments from different directions. . Figure 11b The second line shows a feasible path for restoring the device.

[0131] In summary, many functional micro-magnetic soft machines 10 that are difficult to fabricate using existing manufacturing techniques have been presented. Due to the bottom-up nature of the proposed manufacturing strategy based on heterogeneous precision assembly, the constituent materials, 3D geometries, and 3D magnetization profiles of these soft machines 10 are completely separated from each other and can be designed individually and independently. In contrast, previously reported 3D printing-based methods suffer from severe limitations imposed on the design space by rheological properties, local magnetic interactions between MMPs, and layer-by-layer methods.

[0132] Compared to extrusion and UV lithography-based techniques, the proposed strategy, as an advantage, can combine multiple materials at high resolution (down to 35 µm along each dimension). The proposed device 10 expands the search space of wireless magnetic soft machinery 10 by enabling complex 3D designs, thereby enriching the full range of advanced functionalities required in real-world medical and other potential applications. The currently employed manual assembly process limits the speed, resolution, and accuracy of the largest achievable device prototyping, which can be further improved by using remotely operated or automated micromanipulation systems (see Methods section). Although two MMPs (i.e., NdFeB and Cobalt) are used in this work, other magnetic hard or soft microparticles and nanoparticles can be selected to better suit specific application requirements. For example, in future… living Biocompatible and biodegradable magnetic particles, such as iron oxide nanoparticles, can be used in medical applications.

[0133] Figure 8 illustrates the design and fabrication of the flower-shaped machine 10. This machine 10 demonstrates a stiffness distribution achieved through the versatility of the proposed fabrication method. The flower-shaped machine 10 is made of 127 magnetic voxels 12. The central hexagonal voxel 12 and 51 magnetic voxels 12 are made of PDMS (Sylgard 184, Dow Corning, base material and curing agent mixed in a 10:1 mass ratio) embedded with MMP (NdFeB, MQP-15-7, Magnequench) in a 1:1 mass ratio. The remaining 75 voxels 12 are made of Ecoflex 50 (Smooth-On, portions A and B mixed in a 1:1 mass ratio) embedded with MMP (NdFeB, MQP-15-7, Magnequench) in a 1:1 mass ratio. The measured Young's moduli of the two types of voxels 12 are 0.96 MPa and 98 kPa, respectively.

[0134] The mass-produced voxels 12 were magnetized in a jig 112 under a uniform 1.8 T magnetic field generated by a VSM (Microsense EZ7). Based on the density of the MMP (7.61 g / cm3, NdFeB, MQP-15-7, Magnequench provided by the manufacturer), the polymer density (1.07 g / mL, Ecoflex 0050, Smooth-On provided by the manufacturer; 1.03 g / mL, Sylgard 184, Dow Corning provided by the manufacturer), and the remanent magnetization of the MMP (Figure S1), the final magnetization of the voxels 12 was calculated to be 78 kA / m for PDMS-based voxels 12 and 80 kA / m for Ecoflex 50-based voxels 12. In the above design and voxel configuration, simulations showed that the mechanism 10 did not deform toward the desired shape, and that patterning voxels 12 with different material properties did not change the overall bending stiffness. Figure 8b ).

[0135] exist Figure 8c The design and corresponding functions of auxiliary fixtures 100, 108, and 112, as well as a sketch of their assembly process, are schematically shown in the diagram. Initially, voxels 12 are magnetized in fixture 112 for magnetization. Then, the individual voxels 12 are placed in the fixture and surface-bonded using uncured silicone rubber (Ecoflex 0050, Smooth-On, parts A and B mixed in a 1:1 mass ratio) as adhesive 14 to form part of the flower-shaped mechanism 10.

[0136] Magnetic voxels are magnetized using a vibrating specimen magnetometer (VSM) in a magnetic field with an intensity >1 T. For this purpose, a handheld permanent magnet (12 mm cubic magnet, neodymium, N48, nickel-plated, Webcraft Ltd.) is brought near the specimen to apply the desired magnetic field in the vertical direction. This process is performed only once for the magnetization of the voxels. If the magnetic orientation of the voxels needs to be reset, this process is repeated only.

[0137] In contrast, a permanent magnet can be used to induce a gradual change in the shape of device 10. The magnetic field generated by the magnet is in the range of 0 to 300 mT. This magnetic field does not intend to, and cannot, change the magnetization of the device. Instead, this field applies a distributed magnetic torque to device 10 and causes deformation of device 10.

[0138] Once the parts have been assembled, they can be placed in fixture 108 to form the components of the flower-shaped machine 10. After this, and similarly... Figure 1e The embodiment shown allows components to be assembled in fixture 108 and bonded together to form a flower-shaped machine 10.

[0139] Figure 12 illustrates the design of the starfish-shaped machine 10. This machine 10 demonstrates how edge bonding technology breaks bending symmetry and causes bending at the directional joint. The machine is made of 24 identical triangular flat magnetic voxels 12. PDMS (Sylgard 184, Dow Corning, base material and curing agent mixed at a mass ratio of 10:1) was used as the base polymer, and MMP (NdFeB, MQP-15-7, Magnequench) was uniformly mixed into the polymer at a mass ratio of 1:3.

[0140] Voxel 12 was mass-produced using die casting technology. The manufactured voxel 12 was magnetized in a uniform 1.8 T magnetic field generated by a VSM (Microsense EZ7). Based on the MMP density, polymer density, and remanent magnetization of the MMP, the final magnetization of voxel 12 was calculated to be 188 kA / m. Simulations show that in the above design and voxel configuration, the mechanics does not deform towards the desired shape. Figure 12a ).

[0141] exist Figure 12b The design and corresponding functions of auxiliary clamps 100 and 110, as well as a sketch of their assembly process, are schematically shown in the diagram. Clamp 112 has a triangular shape for the individual voxels 12 of the starfish-shaped mechanism 10. Clamp 100 is used to bond two of the triangular voxels 12 to each other using adhesive 14. Uncured silicone rubber (Ecoflex 0010, Smooth-On, portions A and B mixed in a 1:1 mass ratio) is used as adhesive 14 to bond the edges of the magnetic voxels 12.

[0142] Then another jig 100 can be used to bond the two of the already connected triangular voxels 12 to each other using adhesive 14. Finally, the parts of the starfish-shaped mechanism are assembled in the jig that forms the female mold of the starfish-shaped mechanism, so that the parts can be bonded to each other again using adhesive 14.

[0143] Bring a handheld permanent magnet (12 mm cube magnet, neodymium, N48, nickel plated, Webcraft Ltd.) near the sample to apply a desired magnetic field of 500 mT in the vertical direction.

[0144] Figure 13a and Figure 13bThe design and fabrication of a capsule-shaped machine 10 are shown. This machine 10 functions via a reconfigurable magnetization profile, achieved through the flexibility of the proposed method that works with different MMPs. The machine 10 has two magnetic parts, one containing NdFeB (MQP-15-7, Magnequench, coercivity = 6120 Oe) and the other containing cobalt (Sigma-Aldrich, average diameter 2 µm, coercivity = 209 Oe). The machine 10 is made of two magnetic voxels 12 and two non-magnetic voxels 12'. The two magnetic voxels 12 are geometrically identical. One voxel 12 is made of PDMS (Sylgard 184, Dow Corning, base material and curing agent mixed at a mass ratio of 10:1) mixed with NdFeB in a 1:3 mass ratio. The other voxel 12 is made of PDMS mixed with cobalt in a 1:1 mass ratio.

[0145] Both magnetic voxels 12 were magnetized in a negative-shaped magnetization fixture 112 under a uniform magnetic field of 1.8 T generated by a VSM (EZ7, Microsense). The theoretical final magnetizations of the two magnetic voxels 12 are 188 kA / m (NdFeB) and 10 kA / m (Cobalt), respectively. The theoretical values ​​were calculated based on the density of the MMP, the polymer density, and the remanent magnetization of the MMP.

[0146] exist Figure 13b The diagram schematically illustrates the design and corresponding functions of the auxiliary clamps 112 and 110, as well as a sketch of the assembly process of this machine 10.

[0147] Other embodiments of clamps 112, 110, similar to clamps 100, 108, 110, 112, have a corresponding negative shape of the voxel 12, part or component of the corresponding machine 10 currently being formed.

[0148] Two non-magnetic voxels 12' are face-bonded to magnetic voxels 12 using uncured PDMS (Sylgard 184, Dow Corning, base material and curing agent mixed in a 10:1 mass ratio) as binder 14. The two magnetic voxels are edge-bonded using uncured silicone rubber (Ecoflex 0010, Smooth-On, portions A and B mixed in a 1:1 mass ratio) as binder 14.

[0149] When different cavity sizes are desired but the overall mechanical dimensions 10 cannot be altered, the strength of magnetic attraction / repulsion can be maintained by increasing the concentration of MMPs, resulting in a stronger magnetic moment. Alternatively, the geometry of the device 10 can be modified to increase or decrease the contact area between the two main body parts, and thus tune the strength of the magnetic interaction. For example, using a square cross-section instead of the current circular cross-section in the current design would provide a 28% increase in the contact area. Alternatively, if the design is changed so that the capsule opens longitudinally instead of laterally, the contact area would increase by 94%. In general, due to the flexibility of the proposed method, there are multiple ways to increase the cavity size to increase the dosage per capsule without sacrificing the magnetic strength of the capsule.

[0150] In the reported experiments, capillary effects and the hydrophobicity of the material played a negligible role in performance. If these factors become more significant in future configurations, negative effects can be overcome if they occur during testing phases using one or more strategies supported by the versatility of the proposed method. For example, utilizing longitudinal openings instead of transverse openings would reduce the impact of capillary effects on the device and facilitate material exchange between its cavity and the environment. Similarly, the versatility of the proposed manufacturing method gives users greater freedom in designing the device and makes it easier to find customized designs suitable for specific tasks. The hydrophobicity of the silicone rubber used in this device can be altered through surface treatment techniques such as plasma treatment. If the need is to recover biofluids from the human body rather than for drug delivery, preloading the cargo area with cotton or tissue paper, in addition to plasma treatment of the silicone rubber, would also be helpful.

[0151] In the reported experiment, the proposed capsule-shaped machine was remagnetized by a vertically applied pulsed magnetic field. A custom-made electromagnetic coil system, consisting of 18 turns of copper coils with a diameter of 1 mm and a diameter of 1 mm, generated the pulsed magnetic field. Each turn had a diameter of 19 mm. A cylindrical soft iron (16 mm in diameter and 3 cm in length) was placed inside the coil system to enhance the field strength. The coil system and the iron cylinder were aligned at one end. A 4.3 mF capacitor charged to 180 V was connected to the electromagnetic coil system, thereby generating a pulsed magnetic field with a peak amplitude of 295 mT, which decayed to half its peak value within 1.33 ms.

[0152] In the reported experiments, the specimen was not fixed and moved freely during the application of the field. A pulsed magnetic field was first applied vertically. Then, a vertical magnetic field generated by a handheld permanent magnet was applied before the pulsed magnetic field to align the specimen vertically. This specific orientation ensured that the magnetic direction of the NdFeB portion was aligned with the subsequent pulsed magnetic field, thereby stabilizing the specimen during remagnetization.

[0153] The direction of the pulsed magnetic field is fixed by physical settings that are typically not easily changed in real time. Therefore, as a more cost-effective alternative, alignment prior to remagnetization has been widely used in remagnetization studies reported to date to bring the specimen to the desired orientation, rather than changing the settings to generate a pulsed field suitable for the current specimen orientation. The specimen orientation determines the magnetic orientation of the cobalt portion after remagnetization and further determines the final magnetization profile. In practice, a separate magnetic field (weaker and slower than the pulsed magnetic field) is typically used to manipulate the position and orientation of the specimen in its workspace because, in addition to a reconfigurable magnetization profile, practical applications often expect wireless controllability. Such a controllable magnetic field can be readily used to perform this alignment.

[0154] The pulsed magnetic field is strong and fast enough to reverse the magnetic orientation of the cobalt portion, even when the mechanism is not mechanically secured. When the pulse is applied, the alignment between the magnetic field and the NdFeB portion provides a stabilizing force that holds the device in place, while the cobalt portion is remagnetized. Even with a deliberately slowed pulsed magnetic field, the sample will not fly away because the NdFeB portion is more magnetic than the cobalt portion. Instead, the cobalt portion will twist to align with the applied magnetic field, which will still open the capsule.

[0155] Figure 14a The design of a peristaltic pump is shown. This mechanism exhibits a response to rotation. The pump utilizes the continuous spatiotemporal deformation formed on its main body to pump both liquids and small solid objects. The pump is made of 296 geometrically identical magnetic voxels 12 based on an elastic polymer (Ecoflex Gel, Smooth-On, with portions A and B mixed in a 1:1 mass ratio) embedded with MMP (NdFeB, MQP-15-7, Magnequench). The voxels 12 are mass-produced using a die-casting technique.

[0156] Voxels 12 were then placed inside an auxiliary fixture 112 for the magnetization step, which fixed the orientation of each voxel 12 within a VSM (EZ7, Microsense). The VSM generated a 1.8 T magnetic field to magnetize the voxels 12, resulting in a theoretical magnetization of 74 kA / m. This value was calculated by combining the polymer density (0.98 g / cm³ provided by the manufacturer Smooth-On) and the density of the MMP (7.61 g / cm³, NdFeB, MQP-15-7, Magnequench provided by the manufacturer) with the remanent magnetization of NdFeB measured after magnetization at 1.8 T (Figure S1).

[0157] exist Figure 14bThe design and assembly process of auxiliary fixtures 100, 112, and 108 are schematically illustrated. Adjacent voxels 12 are joined together using a surface bonding method, where an uncured polymer (Ecoflex Gel, Smooth-On, portions A and B mixed in a 1:1 mass ratio) is used as the adhesive 14. Initially, individual voxels with semi-circular external shapes are assembled on fixture 100 and surface-bonded together to form one half of a hollow cylinder. This process is repeated to form the other half of the hollow cylinder. Subsequently, the two half-hollow cylinders are placed in fixture 108 and bonded together using adhesive 14 to form the mechanism 10.

[0158] Rotating uniform magnetic field The proposed peristaltic pump is used to start the pump, which is formed from a custom-made Heilbeck cylinder. This cylinder is mounted on a stepper motor (MOONS) that drives the cylinder to rotate relative to its central axis, thereby... Rotation. The motor is driven by a motor driver (Brian Schmalz's EasyDriver) controlled by a microcontroller (Arduino UNO), which regulates its rotational speed and direction. This setup is powered by a power supply (EX355P-USB, Aim-TTi).

[0159] As shown in Figures 12 to 15, various fixtures 100, 108, 110 and 112 can be used to magnetize voxels 12, connect voxels 12, 12', 12'' to each other in a predefined orientation with adhesive 14 to form parts and / or components of a machine, and finally assemble the machine from multiple parts and / or components in a desired orientation.

[0160] The corresponding voxels 12, 12', 12'' can be magnetized before, during, or after being bonded to their adjacent voxels 12, 12', 12''. The step of bonding a plurality of voxels 12, 12', 12'' to each other may include the following steps: providing a clamp 100, 108, 110, 112 having at least a portion of a magnetically deformable mechanism 10, and placing a predefined number of voxels 12, 12', 12'' into the clamp 100, 108, 110, 112 and then bonding the predefined number of voxels 12, 12', 12'' in the clamp 100, 108, 110, 112.

[0161] One or more of a predefined number of voxels 12, 12', 12'' can be placed into fixtures 100, 108, 110, 112 at a single point in time using a robot (not shown). The robot can be a pick-and-place robot adapted to grip the corresponding voxels 12, 12', 12'' from a supply container and place them into one of the fixtures 100, 108, 110, 112. After the bonding step, the robot can then grip a part or component of the machine and transport it to another fixture 100, 108, 110, 112 to form machine 10 or another part or component of machine 10, etc.

[0162] One or more of a predefined number of voxels 12, 12', 12'' can be magnetized before being placed in the fixtures 100, 108, 110, 112 or after being placed in the fixtures 100, 108, 110, 112 and bonded to their adjacent voxels 12, 12', 12''.

[0163] As basic building blocks, various magnetic and non-magnetic materials and voxels 12, 12', and 12'' in shapes are fabricated by casting uncured polymers with optional magnetic microparticles (MMPs) into reusable, defined-shape female molds. Voxels 12, 12', and 12'' are then batch-cured in these molds. Prior to this step, male molds with raised features are designed in Solidworks (Dassault Systèmes) and formed using two-photon polymerization (TPP, Photonic Professional GT, Nanoscribe Ltd.). TPP is used in this study because it can produce high-fidelity three-dimensional (3D) geometry for rapid prototyping and iteration. Photoresists IP-S and IP-Q (Nanoscribe Ltd.) are used. Polydimethylsiloxane (PDMS, Sylgard 184, Dow Corning, binder, and curing agent mixed in a 5:1 mass ratio) is cast into these male molds to produce female molds with corresponding concave features. Vacuum degassing is performed in this step to remove any trapped air. These negative molds are silanized with trichloro(1H,1H,2H,2H-perfluoro)silanes (PFOCTS, Merck KGaA) to promote the crosslinking of soft polymers and the release of voxels, and are then used to manufacture voxels 12, 12', and 12''. All molds are reusable to reduce costs and increase efficiency. This voxel manufacturing process is... Figure 5a It is shown schematically in the middle.

[0164] Molds can be manufactured via TPP and general photolithography. However, since molds are reusable and many voxels 12, 12', and 12'' can be produced in a single molding process, there is no need to manufacture molds in batches; iterative mold design is more critical. Additionally, it should be noted that generating complex 3D geometries is challenging for photolithography. Therefore, this should only be considered an option when design compatibility is required. With the mold prepared, the selected base material is mixed with selected magnetic microparticles (MMPs) or magnetic nanoparticles (MNPs), such as neodymium iron boron (NdFeB, MQP-15-7, Magnequench, average diameter 5 µm), at a specific mass ratio that can be tuned to achieve different magnetic moment intensities. Figure 2c The materials discussed earlier can be used to form voxels 12, 12', and 12''. The fluid mixture is cast onto a negative mold and degassed under vacuum to remove any trapped air. Excess mixture is removed using a scraper blade. The mixture within the mold cures into voxels with the designed geometry. The curing temperature and time specified in the polymer handbook are as follows. These cured voxels 12, 12', and 12'' are then removed with tweezers or a needle for the next step.

[0165] The base materials used in this work include platinum-catalyzed silicone rubber (Ecoflex series, including 0010 to 0050 and gel), PDMS, polyurethane plastics, and gelatin. The strain-stress relationships of the materials used in these devices were characterized by tensile testing of specimens according to ASTM D412 on a general-purpose testing machine (Instron 5942, Instron, Norwood, MA). In addition to material selection, the geometry of individual voxels can be designed. Figure 16c shows some example voxels 12, 12', and 12'' with various geometries that can be fabricated. The ability to fabricate various voxel geometries can potentially save manufacturing time and costs. The reasons are a) they can create better geometric profiles for the device 10, for example, it is difficult to create a smooth surface for the peristaltic pump 10 using universal cubic voxels 12, 12', 12''; and b) when feasible, larger voxels 12, 12', 12'' with non-universal geometry can replace a set of universal voxels 12, 12', 12'' in the device to improve manufacturing efficiency, for example, using rings 12, 12', 12'' in the capsule 10 saves manufacturing time compared to using a set of universal cubic voxels.

[0166] With the aid of auxiliary fixtures, magnetic voxels 12, 12', and 12'' were positioned in the desired 3D orientation and magnetized using a vibrating specimen magnetometer (VSM; EZ7, Microsense) to set voxel magnetic moments with 3D strength and orientation. v ( Figure 5d The magnetizing field has a strength of 1.8 T unless otherwise specified. Simultaneously, it is precisely controlled via the MMP concentration in the voxel and through the graphical user interface of the VSM. m Control the intensity v The intensity. Exemplary voxels 12, 12', and 12'' with different MMP concentrations and magnetized along different directions in Figure 15a Imaging was performed. The magnetic properties of bare MMPs were also experimentally measured. Figure 15b ).

[0167] VSM is generated within the gap between two parallel circular plates positioned 1 cm apart. m . m The orientation is perpendicular to the circular plate, and its strength is controlled by the VSM's control terminal. Voxels 12, 12', and 12'' are fixed to their corresponding orientations in a clamp 112 for magnetization. The clamp 112 is then fixed to a 1 cm wide cubic acrylic plate. This cubic acrylic plate is clamped by the two circular plates of the VSM, thereby positioning voxels 12, 12', and 12'' at the geometric center of the gap. Then, the VSM generates... m To magnetize voxels 12, 12', and 12''. Instruct VSM to increase at 0.2 T / s. m The desired intensity is held for 2 s at that desired intensity (e.g., 1.8 T), and then slopes down to 0 at -0.2 T / s.

[0168] The auxiliary fixture 112 can also fix the deformation of voxels 12, 12', 12'' or a group of voxels 12, 12', 12'' in this step to set a varying magnetization profile on the body of voxels 12, 12', 12'' or a group of voxels 12, 12', 12''. Generally, voxels are magnetized before assembly to maximize manufacturing versatility. However, in some designs, a group of voxels 12, 12', 12'' can be assembled first and then magnetized for improved efficiency, such as capsule 10 in Figure 13 and anchoring device 10 in Figure 11. Both methods are illustrated using an example 3D ring (Figure 1).

[0169] Magnetic and non-magnetic voxels 12, 12', 12'' are assembled together, with adhesive 14 applied to connect adjacent voxels 12, 12', 12''. Auxiliary jigs 100, 108, 110, 112 are used during assembly to control the position and orientation of each voxel 12, 12', 12'', thereby producing the final 3D geometry and magnetization profile of the mechanical 10. This mechanical fixation helps overcome magnetic interactions between voxels 100, 108, 110, 112.

[0170] Two methods, surface bonding and edge bonding, are used to bond voxels 12, 12', and 12'' together to form the synthetic 3D soft machinery 10. An adhesive 14 is used to form the inter-voxel bond that holds each voxel 12, 12', and 12'' in its designated position. The adhesive is chosen as an uncured liquid soft elastomer that cures upon contact with adjacent voxels. Mechanical interlocking structures can be applied in rare cases where a suitable elastomer is unavailable. Various adhesives, such as super glue and optical glue, can also be used as alternatives. Future investigations will be needed to fully investigate the energy dissipation caused by the mechanical interlocking structures and the compatibility of various adhesives with voxels 12, 12', and 12''. Details of the fabrication process for all reported machines, including material design and magnetization field strength, have been discussed above.

[0171] The assembly process was performed under a stereomicroscope (ZEISS Stemi 508, Carl Zeiss Microscopy GmbH), with magnification ranging from 6.3x to 50x. The microscope's zoom and focus could be easily adjusted using two sets of knobs symmetrically located on the left and right sides of the microscope. This microscope allows users to quickly adjust the zoom and focus of the field of view, which is particularly useful when assembling 3D structures. In addition to the microscope, tweezers (5-SA Outils Rubis SA, Switzerland) or iron needles (Agani 30G needles, Terumo) were used as the primary handheld tools for performing the assembly. The latter was preferred when the tweezers tips were too large for some voxels 12, 12', 12'' (such as the smallest voxels 12, 12', 12'' reported in this study as cubic shapes with 35 µm side lengths). A 0.03 mm diameter copper wire is nested within the Seque / Pro capillary tip (Bio-Rad Laboratories) as a tool to apply adhesive 14 at the desired location to form a surface bond or edge bond. Additionally, a magnetized iron needle is occasionally used to distinguish voxels 12, 12', and 12'' during operation. v The aforementioned instruments are low-cost and readily available to most people in academia and industry.

[0172] Auxiliary fixtures 100, 108, 110, and 112 are used in the assembly process. Fixtures 100, 108, 110, and 112 provide guidance and reference for manufacturing and help fix the relative position and orientation of the working voxels 12, 12', and 12'', which controls manufacturing accuracy and enhances repeatability. These fixtures 100, 108, 110, and 112 can be reused after manufacturing.

[0173] Fixtures 100, 108, 110, and 112 are either 2D or 3D. 2D fixtures are similar to molds used in die casting steps, having concave features to accommodate corresponding parts, such as fixtures for assembling rings (Fig. 1) or layers of peristaltic pumps (Figs. 9 and 15). The dimensions of fixtures 100, 108, 110, and 112 are based on the design of parts made from multiple voxels 12, 12', and 12''. However, the dimensions of the concave features should be designed to be slightly larger than the contours of the corresponding parts to ensure that the parts can be freely inserted. Fixtures 100, 108, 110, and 112 are produced directly via two-photon polymerization (TPP) (i.e., 3D printing) or die casting techniques. In the latter case, the mold is made by casting PDMS (Sylgard 184, Dow Corning, base material and curing agent mixed in a 5:1 mass ratio) onto the structure produced by TPP to form a negative mold. 3D fixtures have out-of-plane features to create 3D parts by forming new working planes. Figure 1e These are fabricated directly via TPP using special objectives (10x and 25x, Nanoscribe Ltd.) designed for printing relatively large features (compared to conventionally sized TPPs). These jigs 100, 108, 110, and 112 are designed similarly to scaffolding used in building construction. A typical example is jigs 100, 108, 110, and 112 for assembling 3D rings (Figure 1). The reported jig designs 100, 108, 110, and 112 are by no means the only feasible jigs. Like mechanical designs in this field, jig designs are mostly heuristically created and based on experience and trial and error.

[0174] Surface bonding is used to bring two voxels 12, 12', 12'' together "face to face," with binder 14 in the middle to form a continuous structure without obvious joints. The bonding interface plays a minimal role in influencing the shape gradient behavior of the device 10, thus allowing material properties such as Young's modulus to dominate deformation. The amount of binder 14 is considered negligible because excessive binder would be extruded by pushing the two voxels 12, 12', 12'' together. Furthermore, no observable difference exists between surface-bonded and integrally cast beams.

[0175] Figure 16a The implementation process is illustrated. Three methods exist: (i) Place one voxel 12, 12', 12'' in fixtures 100, 108, 110, 112, while placing another voxel 12, 12', 12'' near but outside fixtures 100, 108, 110, 112.

[0176] (ii) Alternatively, another voxel 12, 12', 12'' may be placed in clamps 100, 108, 110, 112, with a distance between the two voxels 12, 12', 12''.

[0177] (iii) Two voxels 12, 12', 12'' can be placed in clamps 100, 108, 110, 112, with their contact ends remaining outside the clamps 100, 108, 110, 112, particularly for soft voxels 12, 12', 12''. A 0.03 mm diameter copper wire is nested in the Seque / Pro capillary tip (Bio-Rad Laboratories) as a tool to dip into the adhesive 14 and remove some at its tip. The wire is moved close to the surface of voxels 12, 12', 12'' until the liquid adhesive 14 contacts surface 18. The wire is then removed. A small amount of adhesive 14 at the voxel surface 18 automatically spreads across the entire surface area. Next, the second voxels 12, 12', 12'' are (i) placed in clamps 100, 108, 110, 112, or (ii) moved towards the first voxels 12, 12', 12'' in clamps 100, 108, 110, 112. In a third case, (iii) the portions of the two voxels 12, 12', 12'' outside clamps 100, 108, 110, 112 are pushed into clamps 100, 108, 110, 112. The two voxels 12, 12', 12'' come into close contact with each other and excess applied adhesive 14 is squeezed out. The excess adhesive 14 squeezed out of clamps 100, 108, 110, 112 is removed using tweezers or a needle. The surface bonding is symmetrical, meaning that it has no orientation preference when bent.

[0178] Edge bonding joins two adjacent voxels 12, 12', 12'' by forming a distinct joint and an asymmetrical connection. To form edge bonding, an adhesive 14 is applied to one side of the contact surface 18 of the two voxels 12, 12', 12''. Specifically, the two voxels 12, 12', 12'' can be placed in clamps 100, 108, 110, 112 with additional space on the sides or bottom. Figure 16bSimilar to mold casting technology, adhesive 14 is cast into this pocket and excess adhesive 14 is removed by tweezers or a needle. The amount of adhesive 14 in the edge bonding is controlled by the shape of the auxiliary clamps 100, 108, 110, and 112.

[0179] Without an adhesive 14 between the contact surfaces 18 of the two voxels 12, 12', 12'', the two voxels 12, 12', 12'' can easily detach from each other during deformation. Figure 1b In a typical example shown, adhesive 14 applied at the top edge fixes voxels 12, 12', 12'' at the top side, thereby breaking the bending symmetry by making the joint easier to open from the bottom side. In this design, when c When pointing upwards, voxels 12, 12', and 12'' disengage and the junction opens. This opened junction ( Figure 1b The intermediate case in "edge bonding" allows for large deformations to be achieved using relatively small torques. When c Upon inversion, voxels 12, 12', and 12'' compress against each other, and the junction remains closed. This closed junction ( Figure 1b The third case in “edge bonding” forces the entire soft body to bend, and thus makes it more difficult to bend, resulting in smaller deformation at the same torque size.

[0180] Edge bonding is specifically designed to generate large deformations and break deformation symmetry under weak magnetic actuation. It is not designed to bear significant loads along the preferred deformation direction. However, its load-bearing capacity is unaffected in the opposite direction. Conventionally, large deformations require strong actuating magnetic fields or soft materials. This asymmetric edge bonding method achieves large deformations under relatively weak actuating magnetic fields, allowing for greater freedom in designing shape-gradient devices.

[0181] After voxels 12, 12', and 12'' are assembled together, the entire device 10 is stored at a specified temperature to allow the adhesive 14 to cure. These temperatures are determined by the curing requirements provided by the corresponding manufacturer of the selected adhesive 14. Non-magnetic hot plates and an oven are used to provide an environment at the specific temperature for this step.

[0182] After fabrication, the circular mechanical device 10 was placed inside its designated test setup, such as inside a circular tube used for anchoring devices (Figure 11), and observed using an optical microscope. A handheld permanent magnet (neodymium, nickel-plated, Supermagnete) was used to generate a magnetic field in any 3D direction within the workspace. Observed specimen deformation and motion were captured using a camera (Point Grey Research) and a high-speed camera (Phantom Cinemag II v641). Each specimen was observed multiple times, and no observable signs of performance degradation were found.

[0183] Human adipose-derived mesenchymal stem cells 120 (haMSCs, ATCC) were cultured in a 75 cm² polystyrene cell culture flask in a humidified environment at 37 °C and 5% CO₂. The flask contained MSC basal medium (ATCC) supplemented with ATCC for low serum (2% fetal bovine serum, Gibco), 2% fetal bovine serum (FBS), and penicillin (25 μL). 1) and streptomycin (25 µg mL) 1) Mesenchymal stem cell growth kit. Cells were divided using 0.25% Tyrpin-EDTA (Gibco) solution before reaching 80% confluence.

[0184] To capture stem cells 120, microcages 122, 3D printed via TPP, were heterogeneously integrated into the anchoring mechanism. Figure 17a This anchoring mechanism is half of the six-ring anchoring mechanism 10. Cage 122 is made of commercially available, biocompatible IP-Visio photosensitive resin (Nanoscribe Ltd.) specifically designed for cell culture and tissue engineering. Cage 122 is designed with tenons so that it can be fitted into corresponding tenons on the anchoring mechanism 10. During assembly, a small amount of uncured silicone elastomer (Ecoflex 0010) is applied to the tenons of voxels 12, 12', and 12'' before inserting cage 122. Before seeding cells, the entire device is placed in 1x phosphate-buffered saline (PBS) solution and sterilized under UV for 1 h. After sterilization, the cells are placed in 25 µg / mL of 1x PBS. The entire device was cultured in fibronectin solution at 37 °C for 2 h to increase cell attachment to microcages 122. After fibronectin treatment, the entire device 10 was washed with PBS and cells 120 in suspension were seeded from the top (in 50 µL volumes) at a density of 1.5 x 10⁶ cells 120 per mL. The device 10 with the captured cells 120 was then transferred to a humidified environment at 37 °C and 5% CO₂.

[0185] To investigate cell viability 24 h after cell capture, live and dead cells were stained using the LIVE / DEAD® Viability / Cytotoxicity Kit with manufacturer-based fluorescence microscopy. Simply put, live green vials were thawed and mixed with dead red vials to produce a 2x working solution, which was then added to a trap containing an anchoring device 10 with an equal volume of growth medium. Device 10 and cells 120 were incubated in solution at room temperature for 30 min before imaging. Live and dead cells 120 were imaged using a vortex-plate confocal microscope (Nikon Instruments Ltd., Eclipse Ti-E).

[0186] In the future, cell attachment and retention within the microcage 122 can be further controlled by creating artificial cell niches within the cage. Modifying the inner surface of the microcage 122 with natural extracellular matrix-derived cell attachment peptides and proteins can regulate cell fate and behavior. Furthermore, tuning the mechanical properties of the cage to generalize the physical properties of the native stem cell environment can support the stability and retention of cells 120 during transport in device 10.

[0187] 2. Resolution and capability to generate arbitrary 3D magnetization profiles The proposed manufacturing method enables the production of machines 10 with 3D-to-3D shape gradient capabilities at a higher resolution compared to previous methods. To characterize the resolution of the proposed manufacturing method, a chessboard was assembled from four 35 μm side-length cubic voxels 12, 12', and 12''. Figure 2a This is less than half the resolution produced by current 3D printing methods using magnetic soft machinery. Manufacturing resolution is defined as the 3D size of the smallest voxels (12, 12', 12'') that can be precisely and repeatedly assembled. This definition is based on the fact that the proposed method can alter the magnetic properties of the material down to the final mechanical properties of the individual voxels in 3D.

[0188] At this high manufacturing resolution, each voxel can have a local magnetic moment. v This local magnetic moment can point in any 3D direction ( Figure 2b Besides assuming uniform (constant) magnetization, relatively large voxels 12, 12', 12'' on v It can also be configured to vary spatially by exhibiting some deformation during magnetization. Additionally, v It can have any value from zero to a maximum value limited by the magnetic properties of MMP. vThe exact value of | can be determined by the MMP concentration in the given voxels 12, 12', 12'' and the field used to magnetize voxels 12, 12', 12''. m The amplitude is used for tuning. Figure 2c The measured magnetization values ​​of voxels 12, 12', and 12'' of MMPs with different mass ratios (0.0%, 33.3%, 50.0%, and 66.7%) are shown, along with comparisons to the corresponding theoretical values. The results indicate that the magnetization can be improved by varying the concentration of MMPs and the magnetizing magnetic field. m Adjust the intensity | v |

Claims

1. A method for manufacturing a magnetically deformable machine (10) comprising multiple voxels (12, 12', 12'') with different properties, characteristics, and compositions, said method comprising the following sequential steps: - Define the deformation characteristics of the magnetic deformable machine (10); - The blueprint for the magnetic deformable machine (10) is made with reference to the deformation characteristics of the magnetic deformable machine (10); - Provide the plurality of individual voxels (12, 12', 12''), at least some of the plurality of individual voxels being magnetic, and at least some of the plurality of voxels (12, 12', 12'') having a Young's modulus of less than 500 MPa; - According to the blueprint made, the plurality of individual voxels (12, 12', 12'') are bonded together with adhesive (14) to assemble the magnetic deformable machine (10). as well as - Allow the adhesive (14) to cure. Its features are, The step of bonding the plurality of voxels (12, 12', 12'') to each other includes bonding one voxel (12, 12', 12'') to another voxel (12, 12', 12'') in a subsequent step to attach the individual voxels (12, 12', 12'') to each other in a subsequent step.

2. The method according to claim 1, The step of defining the deformation characteristics of the magnetically deformable machine (10) includes at least one step selected from the group consisting of: - Define the application of the magnetic deformable machine (10); - Define the working environment for the corresponding application of the magnetic deformable machine (10); - Define the deformation parameters of the magnetic deformable machine (10); - Select the dimensions of the magnetic deformable machine (10); - Select the shape of the magnetic deformable machine (10); And combinations of the aforementioned items.

3. The method according to claim 1 or claim 2, The blueprints mentioned therein include: The number of the respective plurality of voxels (12, 12', 12'') used to form the magnetic deformable machinery (10), the arrangement of the respective voxels (12, 12', 12'') used to form the magnetic deformable machinery (10), the properties of the respective voxels (12, 12', 12'') used to form the magnetic deformable machinery (10), and the arrangement of the curing agent at the plurality of voxels (12, 12', 12'') used to form the magnetic deformable machinery (10).

4. The method according to claim 1 or 2, The step of creating the blueprint for the magnetically deformable machine (10) includes at least one step selected from the group consisting of: - Select materials with different voxels (12, 12', 12'') to define the stiffness properties of the magnetic deformable machine (10); - Select one or more materials for the corresponding voxels (12, 12', 12'') used in the magnetic deformable machinery (10); - Select a uniform 3D magnetization profile or a non-uniform 3D magnetization profile of the magnetic voxels (12, 12', 12'') to define the deformation properties of the magnetic deformable machine (10) based on magnetic torque or magnetic force. - Select the size of the corresponding voxel (12, 12', 12''); - Select the shape of the corresponding voxel (12, 12', 12''); - Select the magnetic properties of the corresponding voxels (12, 12', 12''); - Select the material properties of the corresponding voxels (12, 12', 12''); - Simulate the behavior and / or deformation of the magnetic deformable machine (10) based on the blueprint; - Magnetize one or more of the corresponding voxels (12, 12', 12''); - Adjust the blueprint of the magnetic deformable machine (10) based on the simulation results of the behavior and / or deformation of the magnetic deformable machine (10); And combinations of the aforementioned items.

5. The method according to claim 1 or 2, Each voxel (12, 12', 12'') has a 3D shape and a predefined shape, size, predefined magnetic properties, and predefined material properties, and / or The corresponding voxels (12, 12', 12'') are magnetized before being bonded to the adjacent voxels (12, 12', 12''), simultaneously with being bonded to the adjacent voxels (12, 12', 12''), or after being bonded to the adjacent voxels (12, 12', 12'').

6. The method according to claim 1 or 2, The magnetization profiles of the magnetic voxels (12, 12', 12'') of the magnetic deformable machine (10) can be seen by magnetic sensing technology or magnetic imaging technology.

7. The method according to claim 1 or 2, The step of bonding the plurality of voxels (12, 12', 12'') to each other is performed at one or more faces (18) and / or one or more edges (20) of the voxels (12, 12', 12'').

8. The method according to claim 1 or 2, The step of bonding the plurality of voxels (12, 12', 12'') to each other includes bonding one group of voxels (12, 12', 12'') to another group of voxels in turn.

9. The method according to claim 1 or 2, The step of bonding the plurality of voxels (12, 12', 12'') to each other includes the following steps: A clamp (100, 108, 110, 112) having at least a portion of the magnetic deformable machinery (10) is provided, and a predefined amount of the plurality of voxels (12, 12', 12'') is placed into the clamp (100, 108, 110, 112) and then the predefined amount of the plurality of voxels (12, 12', 12'') is bonded in the clamp (100, 108, 110, 112).

10. The method according to claim 9, One or more of the predefined amount of voxels (12, 12', 12'') are placed into the fixture (100, 108, 110, 112) by means of a robot at a certain point in time.

11. The method according to claim 9, One or more of the predefined amount of the plurality of voxels (12, 12', 12'') are magnetized before being placed in the fixture, or after being placed in the fixture (100, 108, 110, 112) and bonded to adjacent voxels (12, 12', 12'') of one or more of the plurality of voxels (12, 12', 12'').

12. The method according to claim 1 or 2, The step of curing the adhesive (14) is performed at room temperature or another specific temperature and within the environment in which the bonding step is performed. The step of curing the adhesive (14) is performed by an ultraviolet (UV) light source or a light source of another wavelength, or The step of curing the adhesive (14) is carried out in an oven or on a hot plate.

13. A deformable 3D magnetic machine (10), the magnetic machine (10) having a size of less than 10,000 mm, the magnetic machine (10) comprising a plurality of voxels (12, 12', 12'') with different properties, properties and compositions, at least one of the plurality of voxels being magnetic, wherein at least one of the voxels (12, 12', 12'') has a Young's modulus of less than 500 MPa, the plurality of voxels (12, 12', 12'') being bonded together with an adhesive (14), wherein each voxel (12, 12', 12'') has a predefined shape, size, predefined magnetic properties and predefined material properties, The deformable 3D magnetic machinery can be obtained by the method according to any one of claims 1 to 12.

14. The deformable 3D magnetic machinery (10) according to claim 13. Each voxel (12, 12', 12'') can have a shape selected from a group of members consisting of: square voxels (12, 12', 12''), rectangular voxels (12, 12', 12''), circular voxels (12, 12', 12''), polygonal voxels (12, 12', 12''), triangular voxels (12, 12', 12''), and any 3D shape voxel (12, 12', 12''), as well as combinations thereof.

15. The deformable 3D magnetic machinery (10) according to claim 13 or 14. The magnetic mechanism (10) is a cargo delivery device capable of transporting cargo and releasing the cargo at a target location by deforming or opening the magnetic mechanism; or the magnetic mechanism (10) is one of the following: anchoring device, support, soft peristaltic pump or other type of liquid pump, soft cubic frame, deformable metamaterial, shape-adaptive robot or shape-configurable robot, gripper, foldable device, blocking device, swimming robot, organ model, synthetic heart or other organ, and retractable ring flower.

16. The deformable 3D magnetic machinery (10) according to claim 13 or 14. The nonmagnetic materials of at least some of the nonmagnetic voxels (12, 12', 12'') of the magnetic machinery (10) are selected from the group consisting of: elastomers, thermoplastic elastomers, rubber, rigid plastics, thermoplastic plastics, biodegradable synthetic materials, biomaterials, hydrogels; ionogels, liquid crystal polymers, elastomers or gels; shape memory polymers; photoresist polymers, biological proteins, fabric materials; nonmagnetic metals; silicone; silicon dioxide; glass; wood; carbon fiber; and derivatives and combinations thereof.

17. The deformable 3D magnetic machinery (10) according to claim 13 or 14. The magnetic material of at least some of the magnetic voxels (12, 12', 12'') is selected from the group consisting of: magnetic materials existing in the form of a large number of particles, disks, wires, fibers or asymmetric particles; combinations or composites of the foregoing; and / or voxels (12, 12', 12'') coated with a magnetic film or magnetic layer made of the above magnetic materials or combinations thereof.

18. The deformable 3D magnetic machinery (10) according to claim 17. The magnetic materials are chromium dioxide (CrO2), samarium cobalt (SmCo), neodymium iron boron (NdFeB), cobalt (Co), ferrite, permalloy (NiFe), carbon steel, tungsten steel, magnetic steel, iron, stainless steel, nickel (Ni), iron platinum (FePt), iron oxide, barium ferrite, and magnets.

19. The deformable 3D magnetic machinery (10) according to claim 13 or 14. The magnetic voxels (12) have any arbitrary 3D magnetization profile, wherein each voxel has an average surface magnetic field strength selected in the range of 0 to 1 T, wherein each voxel (12) has a predefined orientation of the magnetic field strength, parallel to or perpendicular to the face (18) of the corresponding voxel (12, 12', 12''), or inclined about one or more faces (18) of the corresponding voxel (12, 12', 12''). For the non-uniform magnetic voxels (12, 12', 12''), each voxel (12, 12', 12'') has a non-uniform magnetization distribution throughout the voxel (12, 12', 12'') and a varying magnetic orientation throughout the voxel (12, 12', 12'').

20. The deformable 3D magnetic machinery (10) according to claim 19. Each voxel has an average surface magnetic field strength selected in the range of 0 to 50 mT, and each voxel (12) has a predefined orientation of the magnetic field strength.

21. The deformable 3D magnetic machinery (10) according to claim 19. For a uniform magnetic voxel (12, 12', 12''), the magnetic voxel (12) has any arbitrary 3D magnetization profile, wherein each voxel has an average surface magnetic field strength selected in the range of 0 to 1 T, wherein each voxel (12) has a predefined orientation of the magnetic field strength, parallel to or perpendicular to the face (18) of the corresponding voxel (12, 12', 12''), or inclined about one or more faces (18) of the corresponding voxel (12, 12', 12'').

Citation Information

Patent Citations

  • Mobile device for grasping and active release of objects

    US20180354120A1