Method for separating positive electrode material of waste lithium battery from aluminum foil by using micro-nano bubbles

The micro-nano bubble separation method solves the problem of separating cathode materials from aluminum foil in waste lithium batteries, achieving low-energy consumption, pollution-free, and efficient separation. It is applicable to a variety of cathode materials, has a high separation rate, and the separation liquid can be reused.

CN116111225BActive Publication Date: 2026-11-24STATE GRID HENAN ELECTRIC POWER ELECTRIC POWER SCI RES INST +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310249888.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-15
Publication Date
2026-11-24
Estimated Expiration
2043-03-15

AI Technical Summary

Technical Problem

Existing technologies are insufficient for efficiently and cleanly separating the cathode material of waste lithium batteries from aluminum foil, and traditional methods suffer from high energy consumption and severe pollution.

Method used

The micro-nano bubble separation method is adopted. By introducing micro-nano bubbles under heating conditions, the binder between the positive electrode material and the aluminum foil is melted. Then, the micro-nano bubbles enter the gap for separation, thus achieving physical separation of the material and the aluminum foil.

Benefits of technology

It achieves low-energy consumption and pollution-free separation, with a high separation rate, is applicable to a variety of cathode materials, and the separation liquid can be reused, reducing environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116111225B_ABST
    Figure CN116111225B_ABST
Patent Text Reader

Abstract

The application discloses a method for separating positive electrode material and aluminum foil of waste lithium battery by using micro-nano bubbles, and comprises the following steps: (1) cutting the waste lithium battery positive electrode sheet into 1-20mm long strips; (2) placing the cut positive electrode sheet in step (1) in a preheated separation liquid for heating; (3) after the adhesive between the positive electrode material and the aluminum foil is melted, micro-nano bubbles are introduced into the separation liquid to promote the separation of the aluminum foil layer and the positive electrode material layer, and then the separated aluminum foil layer and positive electrode material layer are screened and dried to obtain the separated positive electrode material and aluminum foil. The separation method does not need to classify the types of waste battery positive electrode sheets, and can be processed in large quantities in a mixed manner. By controlling the system temperature, the introduction time and particle size of the nano bubbles, the physical separation of the aluminum foil and the positive electrode material can be realized, and the method has the advantages of simple process, low cost, less reagent, no waste gas and waste liquid, no easy environmental pollution, high separation rate and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of recycling and reuse technology of waste lithium-ion battery cathode materials, specifically involving a method for separating waste lithium battery cathode materials and aluminum foil using micro-nano bubbles. Background Technology

[0002] In recent years, the lithium-ion battery industry has developed rapidly. Due to its advantages such as high voltage, high energy density, and good cycle performance, lithium-ion batteries have been widely used in mobile smart terminals, small electrical devices, grid energy storage devices, and electric vehicles. With the increasing demand for battery quality and quantity from downstream industries, especially the power battery industry, lithium-ion batteries have become one of the current research hotspots, and their production has been increasing year by year. However, widespread application has also led to a large amount of waste lithium-ion batteries. It is estimated that more than 11 million tons of retired lithium-ion batteries will be generated globally between 2017 and 2030.

[0003] Lithium-ion batteries utilize a large amount of metallic materials, such as lithium, nickel, cobalt, manganese, copper, iron, and aluminum. Therefore, discarded lithium-ion batteries contain a wealth of valuable metals. The positive electrode material is a crucial component of lithium-ion batteries and contains a significant portion of the metal resources' value. Furthermore, lithium-ion batteries also contain fluorinated inorganic electrolytes and organic binders; improper recycling methods can cause serious environmental pollution. Therefore, the recycling of lithium-ion batteries is of great economic and environmental importance. How to efficiently, cleanly, and cheaply recycle used lithium-ion batteries has become one of the most significant energy, resource, and environmental challenges facing human society.

[0004] Generally, the recycling technology route for spent lithium-ion batteries includes discharge treatment, dismantling treatment, separation of active materials containing aluminum foil, dissolution treatment, and resynthesis of new materials. Among these steps, separating the active materials containing aluminum foil is one of the key steps to achieve efficient recycling of lithium-ion batteries. The adhesion between graphite particles and copper foil in spent lithium-ion batteries is low, so graphite can be easily recycled through mechanical processing. In contrast, the more valuable cathode material and aluminum foil are tightly bonded together by polyvinylidene fluoride (PVDF), making them difficult to separate and recycle using traditional methods.

[0005] Currently, common methods for separating aluminum foil and cathode materials include: (1) heating the cathode sheet at high temperature to separate the cathode material from the aluminum foil; in this method, toxic gases such as dioxins generated during the heating process will cause serious environmental pollution problems. (2) rapidly cooling the cathode sheet with liquid nitrogen and then crushing it, and recovering aluminum through electrostatic separation after crushing; this method consumes a lot of energy during the separation process. (3) soaking the cathode sheet in organic solvents such as N,N-dimethylformamide (DMF) and N-methylpyrrolidone (NMP), heating and stirring; this method will generate a large amount of organic wastewater during the separation process, and the equipment investment is relatively large. Summary of the Invention

[0006] To address the shortcomings of existing technologies, the present invention aims to provide a method for separating waste lithium battery cathode materials from aluminum foil using micro-nano bubbles. This separation method has advantages such as simple process, low cost, few reagents required, no waste gas or waste liquid generated, minimal environmental pollution, and high separation rate.

[0007] To achieve the above objectives, the present invention adopts the following technical solution:

[0008] A method for separating waste lithium battery cathode material and aluminum foil using micro / nano bubbles includes the following steps:

[0009] (1) Crush the waste lithium battery positive electrode sheet into long strips of 1-20mm;

[0010] (2) Place the shredded positive electrode sheet from step (1) into the preheated separation solution and heat it;

[0011] (3) After the adhesive between the positive electrode material and the aluminum foil melts, micro-nano bubbles are introduced into the separation liquid to promote the separation of the aluminum foil layer and the positive electrode material layer. Then, the separated aluminum foil layer and the positive electrode material layer are screened and dried to obtain the separated positive electrode material and aluminum foil.

[0012] Furthermore, in step (1), the lithium battery positive electrode is any one or more of the following: lithium iron phosphate battery positive electrode, nickel cobalt manganese lithium battery positive electrode, and lithium cobalt oxide battery positive electrode.

[0013] Furthermore, the separation liquid in step (2) is a high-boiling-point liquid with a boiling point temperature above 170°C, including benzyl alcohol, tetrabromoethane, dimethyl ester, ethyl benzoate, sulfolane, diphenyl ether, and glycerol.

[0014] Furthermore, in step (2), the heating temperature of the positive electrode in the separation liquid is 170-220℃, and the heating time is 30-180min.

[0015] Furthermore, in step (3), the micro-nano bubbles are bubbles that are insoluble in organic liquids, including air bubbles, carbon dioxide bubbles, nitrogen bubbles, argon bubbles, oxygen bubbles, and ozone bubbles.

[0016] Furthermore, in step (3), the particle size of the micro-nano bubbles is 10nm-100um.

[0017] Furthermore, the introduction time of micro-nano bubbles in step (3) is 120-360 min.

[0018] Compared with the prior art, the positive and beneficial effects of this invention are as follows:

[0019] (1) The present invention uses a micro-nano bubble separation method to separate the positive electrode material of waste lithium battery from aluminum foil. It does not require the classification of waste lithium batteries with different types of positive electrode materials. The separation method of the present invention can be used directly to complete the separation of the positive electrode material and aluminum foil in the waste lithium battery. Since the temperature only needs to reach the melting point of the bonding layer between the positive electrode material and aluminum foil in the separation process, it is not necessary to vaporize the bonding layer, which greatly reduces the separation temperature and thus reduces the energy consumption in the separation process.

[0020] (2) This invention achieves the separation of aluminum foil and positive electrode material by reasonably controlling the particle size and introduction time of micro-nano bubbles. When the bubble particle size is less than 10 nm, a longer introduction time is required to fill and expand the gap, resulting in excessive energy consumption. When the bubble particle size is greater than 100 μm, the large bubbles cannot enter the gap, resulting in poor separation effect. When the aeration time is less than 120 min, the amount of bubbles entering is insufficient, resulting in insufficient gap size and poor separation effect. When the aeration time is greater than 360 min, the positive electrode material and aluminum foil have already been separated, and the excessively long aeration time is unnecessary and will only increase energy consumption. Moreover, the method of separating waste lithium battery positive electrode material and aluminum foil using micro-nano bubbles is a physical separation method. This method does not produce chemical reactions, generates no waste gas or wastewater, is environmentally friendly, the separation liquid can be reused, saves costs, and does not affect the chemical properties of the lithium battery positive electrode material, creating favorable conditions for subsequent wet leaching and reuse of the positive electrode material.

[0021] (3) The present invention has the advantages of simple process, low cost, few reagents required, no waste gas or waste liquid generated, and low environmental pollution and high separation rate. Attached Figure Description

[0022] Figure 1 This is a flowchart of the method for separating waste lithium battery cathode material and aluminum foil using micro-nano bubbles according to the present invention;

[0023] Figure 2This is a flowchart of the equipment used in the method for separating waste lithium battery cathode material and aluminum foil using micro-nano bubbles according to the present invention.

[0024] Figure 3 This is an XRD comparison image of the pure cathode material (top) and the cathode material stripped by this invention (bottom);

[0025] Figure 4 The images show a comparison of SEM images of waste cathode material (left image) and cathode material stripped from the present invention (right image);

[0026] Figure 5 This is a TG-DSC graph used to detect the melting point of the PVDF binder between the cathode material and the aluminum foil. Detailed Implementation

[0027] The following specific embodiments are intended to further illustrate the content of the present invention, rather than to limit the scope of protection of the claims.

[0028] Example 1

[0029] Waste lithium nickel cobalt manganese oxide cathode sheets were crushed into long strips of 1-5 mm and placed in benzyl alcohol heated to 180°C for 60 minutes. When the cathode material is placed in the heated benzyl alcohol, heat is transferred from the surface to the interior until the interior of the cathode material also reaches 180°C. The PVDF (polyvinylidene fluoride) bonding layer between the cathode material and the aluminum foil begins to melt, changing from a solid to a liquid state. Then, micro-nano bubbles (air bubbles) are introduced, with a particle size mainly distributed in the 10-100 nm range, for 180 minutes. During this time, the cathode material continuously enters the bonding layer with the bubbles, thus separating from the aluminum foil. In this embodiment, the separation rate of the lithium nickel cobalt manganese oxide cathode material from the aluminum foil is 92.84%. The cathode material obtained in this embodiment is a ternary lithium nickel cobalt manganese oxide cathode material. Figure 3 The upper curve is the XRD pattern of pure lithium nickel cobalt manganese oxide ternary cathode material, and the lower curve is the lithium nickel cobalt manganese oxide ternary cathode material obtained by the method of this patent. Figure 3 It can be seen that the XRD patterns of the cathode material lithium nickel cobalt manganese oxide obtained by the separation method in this embodiment are almost indistinguishable from those of pure lithium nickel cobalt manganese oxide. This indicates that the separation method in this invention does not affect the crystal form of the cathode material lithium nickel cobalt manganese oxide. Lithium nickel cobalt manganese oxide still has a good crystal form, which is beneficial to the subsequent regeneration and utilization of cathode materials. Figure 4 The images are SEM images of lithium nickel cobalt manganese oxide ternary cathode sheets. The left image is the SEM image of the waste lithium nickel cobalt manganese oxide ternary cathode sheet, and the right image is the SEM image of the cathode material obtained by the separation method in this embodiment. It can be seen that since this method is a physical peeling, when the temperature decreases, PVDF (polyvinylidene fluoride) re-solidifies and adheres to the cathode material particles, but it has no effect on the crystal form of the cathode material particles.

[0030] Example 2

[0031] Waste lithium iron phosphate cathode sheets were crushed into 6-10 mm long strips and placed in tetrabromoethane heated to 200°C for 30 minutes. When the cathode material is placed in the heated tetrabromoethane, heat is transferred from the surface to the interior until the interior of the cathode material also reaches 200°C. The PVDF (polyvinylidene fluoride) bonding layer between the cathode material and the aluminum foil begins to melt, changing from a solid to a liquid state. Then, micro-nano bubbles (nitrogen bubbles) are introduced, with the bubble size mainly distributed in the 10-20 nm range, for 240 minutes. During this time, the cathode material continuously enters the bonding layer with the bubbles, thus separating from the aluminum foil. In this embodiment, the separation rate of the cathode material lithium nickel cobalt manganese oxide from the aluminum foil is 96.33%. The high-purity lithium iron phosphate and high-purity aluminum foil obtained in this embodiment can be directly recycled into batteries through subsequent purification and lithium source replenishment. The high-purity aluminum foil can be directly used for cathode sheet fabrication by flattening.

[0032] Example 3

[0033] Waste lithium cobalt oxide cathode sheets were crushed into 10-15 mm long strips and placed in dimethyl ester heated to 190°C for 120 min. When the cathode material is placed in the heated dimethyl ester, heat is transferred from the surface to the interior until the interior of the cathode material also reaches 190°C. The PVDF (polyvinylidene fluoride) bonding layer between the cathode material and the aluminum foil begins to melt, changing from a solid to a liquid state. Then, micro-nano bubbles, which are nitrogen bubbles, are introduced, with the bubble particle size mainly distributed between 10 nm and 50 μm, for 300 min. At this time, the cathode material continues to enter the bonding layer with the bubbles and thus separates from the aluminum foil. In this embodiment, the separation rate of the cathode material lithium cobalt oxide from the aluminum foil is 91.73%.

[0034] Example 4

[0035] Waste lithium nickel cobalt manganese oxide cathode sheets were crushed into 13-16 mm long strips and placed in glycerol heated to 200°C for 100 min. When the cathode material is placed in heated glycerol, heat is transferred from the surface to the interior until the interior of the cathode material also reaches 200°C. The PVDF (polyvinylidene fluoride) bonding layer between the cathode material and the aluminum foil begins to melt, changing from a solid to a liquid state. Then, micro-nano bubbles, which are nitrogen bubbles, are introduced, with the bubble particle size mainly distributed between 20 nm and 60 μm, for 120 min. At this time, the cathode material continues to enter the bonding layer with the bubbles and thus separates from the aluminum foil. In this embodiment, the separation rate of the lithium nickel cobalt manganese oxide cathode material from the aluminum foil is 91.26%.

[0036] Example 5

[0037] Waste lithium iron phosphate cathode sheets were crushed into 5-10 mm long strips and placed in ethyl benzoate heated to 190°C for 120 minutes. When the cathode material is placed in the heated ethyl benzoate, heat is transferred from the surface to the interior until the interior of the cathode material also reaches 190°C. The PVDF (polyvinylidene fluoride) bonding layer between the cathode material and the aluminum foil begins to melt, changing from a solid to a liquid state. Then, nanobubbles, which are nitrogen bubbles, are introduced, with the bubble particle size mainly distributed in the range of 10-100 μm, for 130 minutes. At this time, the cathode material continues to enter the bonding layer with the bubbles, thus separating from the aluminum foil. In this embodiment, the separation rate of the lithium iron phosphate cathode material from the aluminum foil is 90.82%.

[0038] Comparative Example 1

[0039] Except for the different particle size of the introduced bubbles, the rest is the same as in Example 4. The particle size of the introduced micro-nano bubbles in this comparative example is 101-200 μm. The separation rate of the positive electrode material lithium nickel cobalt manganese oxide and the aluminum foil obtained in this comparative example is 60.85%.

[0040] Comparative Example 2

[0041] Except for the time of bubble introduction, the rest is the same as in Example 5. In this comparative example, the time of bubble introduction is 30 min. The separation rate of the positive electrode material lithium iron phosphate and aluminum foil obtained in this comparative example is 22.41%.

[0042] Comparative Example 3

[0043] Except for the different particle size of the introduced bubbles, the rest is the same as in Example 2. In this comparative example, the particle size of the introduced micro-nano bubbles is 1-6 nm. The separation rate of the positive electrode material lithium iron phosphate and aluminum foil obtained in this comparative example is 70.36%.

[0044] Comparative Example 4

[0045] Except for the time of bubble introduction, the rest is the same as in Example 2. The time of bubble introduction in this comparative example is 450 min. The separation rate of lithium iron phosphate cathode material and aluminum foil obtained in this comparative example is 50.78%.

[0046] The principle of this invention, which uses micro / nano bubbles to separate waste lithium battery cathode materials from aluminum foil, is as follows:

[0047] This invention utilizes the characteristic that the adhesive layer between the positive electrode material and the aluminum foil transforms from a solid to a liquid state after reaching its melting point. The temperature of the separation liquid is raised to near the melting point of the adhesive layer. After the adhesive layer melts and transforms from a solid to a liquid, the adhesive force weakens, and micro-gaps begin to appear between the aluminum foil and the adhesive. At this point, micro-nano bubbles are introduced. These micro-nano-sized bubbles enter the micro-gaps. The energy generated by the bursting of some bubbles continues to widen the gaps, while some unburst bubbles accumulate in the gaps. As the number of bubbles increases, the gaps are widened further, ultimately completing the separation of the positive electrode material from the aluminum foil. The flowcharts of the specific separation method and the equipment used in the separation process are shown below. Figure 1 and Figure 2 As shown. In the above method for separating the positive electrode material and the aluminum foil, the temperature of the separation liquid is not lower than the melting temperature of the binder in the positive electrode sheet. The binder will only begin to melt and change from solid to liquid above the melting temperature. If the temperature of the separation liquid is lower than the melting temperature of the binder layer, the binder layer will be solid, and there will be no gap between the positive electrode material and the aluminum foil, making it impossible to separate the positive electrode material from the aluminum foil using micro-nano bubbles. The TG-DSC diagram of the melting point of the PVDF binder in this invention is shown below. Figure 5 As shown, by Figure 5 As can be seen, an endothermic peak appeared at 162.3℃, indicating that PVDF began to melt and change from solid to liquid. Gaps began to appear between the positive electrode material and the aluminum foil. As can be seen from the figure, the heating temperature of the medium should be higher than this temperature to ensure that PVDF melts. Based on this temperature, it can be determined that the boiling point of the required medium should be higher than 162.3℃.

[0048] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from its spirit or essential characteristics. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, all variations falling within the meaning and scope of equivalents of the claims are intended to be included within the present invention. No reference numerals in the claims should be construed as limiting the scope of the claims.

Claims

1. A method for separating waste lithium battery cathode material and aluminum foil using micro / nano bubbles, characterized in that, Includes the following steps: (1) Crush the waste lithium battery positive electrode sheet into long strips of 1-20mm; (2) Place the shredded positive electrode sheet from step (1) into the preheated separation solution and heat it; (3) After the adhesive between the positive electrode material and the aluminum foil melts, micro-nano bubbles are introduced into the separation liquid to promote the separation of the aluminum foil layer and the positive electrode material layer. Then the separated aluminum foil layer and the positive electrode material layer are sieved and dried to obtain the separated positive electrode material and aluminum foil. In step (3), the micro-nano bubbles are bubbles that are insoluble in organic liquids; In step (3), the particle size of the micro-nano bubbles is 10nm-100um.

2. The method for separating waste lithium battery cathode material and aluminum foil using micro / nano bubbles according to claim 1, characterized in that, In step (1), the lithium battery positive electrode is any one or more of the following: lithium iron phosphate battery positive electrode, nickel cobalt manganese lithium battery positive electrode, and lithium cobalt oxide battery positive electrode.

3. The method for separating waste lithium battery cathode material and aluminum foil using micro-nano bubbles according to claim 1, characterized in that, The separation liquid in step (2) is a high-boiling-point liquid with a boiling point temperature above 170°C, including benzyl alcohol, tetrabromoethane, dimethyl ester, ethyl benzoate, sulfolane, diphenyl ether, and glycerol.

4. The method for separating waste lithium battery cathode material and aluminum foil using micro / nano bubbles according to claim 1, characterized in that, In step (2), the heating temperature of the positive electrode in the separation liquid is 170-220℃, and the heating time is 30-180min.

5. The method for separating waste lithium battery cathode material and aluminum foil using micro-nano bubbles according to claim 1, characterized in that, The micro-nano bubbles in step (3) include air bubbles, carbon dioxide bubbles, nitrogen bubbles, argon bubbles, oxygen bubbles, and ozone bubbles.

6. The method for separating waste lithium battery cathode material and aluminum foil using micro-nano bubbles according to claim 1, characterized in that, The introduction time of micro-nano bubbles in step (3) is 120-360 min.

Citation Information

Patent Citations

  • Method for separating positive electrode active material and current collector of waste lithium battery

    CN114430081A

  • Solvothermal pretreatment method and application of waste lithium battery positive electrode material

    CN114512738A