A water-dispersible composite hydrophilic modified curing agent and preparation method thereof

Through the addition reaction and quaternization reaction of propylene-based polyethylene glycol, a composite modifier with a dual hydrophilic structure is obtained, which solves the challenges of water-based curing agents in water dispersion and NCO content, and achieves efficient water-based curing agents. Improved dispersion and film properties.

CN116120517BActive Publication Date: 2024-10-18WANHUA CHEMICAL (NINGBO) CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202111341641.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-12
Publication Date
2024-10-18
Estimated Expiration
2041-11-12

Smart Images

  • Figure CN116120517B_ABST
    Figure CN116120517B_ABST
Patent Text Reader

Abstract

The present invention discloses a water-dispersible composite hydrophilic modified curing agent and a preparation method thereof. The structure of the curing agent is shown as follows: The preparation of the curing agent comprises the following steps: a) adding propylene polyethylene glycol, peroxide and solvent into a reactor, introducing hydrogen bromide gas for reaction, introducing nitrogen, then adding tertiary amine for reaction, cooling the product ether for precipitation and washing, and vacuum drying to obtain a composite hydrophilic modifier; b) under nitrogen protection, adding polyisocyanate into the reactor, stirring and heating, adding the composite hydrophilic modifier into the reactor for reaction, cooling and discharging to obtain a water-dispersible composite hydrophilic modified curing agent. The present invention uses only one modifier to achieve non-ionic and ionic composite hydrophilic modification, and the obtained curing agent has good water dispersibility, high NCO content, good water resistance and hardness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polymers, and in particular relates to a water-dispersible composite hydrophilic modified curing agent and a preparation method thereof. Background Art

[0002] At present, solvent-based polyurethane coatings have been fully developed and applied, with excellent performance, but the volatile organic compound (VOC) content of solvent-based polyurethane coatings is high, causing serious environmental pollution during the construction process. With the strengthening of social environmental awareness and relevant laws and regulations, the market demand for low-VOC or VOC-free coating systems. Therefore, environmentally friendly water-based coatings are increasingly valued, and water-based polyurethane systems are gradually developing, which is one of the important directions for the development of coatings in the future. Among them, two-component water-based polyurethane coatings use water-based polyurethane dispersions or water-based emulsions with water-based curing agents as film-forming substances, and water as a dispersion medium. Two-component water-based polyurethane coatings are cured to form films through the reaction of NCO and OH, and the chemical principle is similar to that of solvent-based polyurethane coatings. Compared with other types of water-based coatings, two-component water-based polyurethane coatings have good appearance and good physical and mechanical properties after curing and forming films. At the same time, they have certain water resistance and chemical resistance, and their performance is closest to solvent-based polyurethane coatings. Among them, the water-based curing agent that provides NCO groups is one of the key factors that determine the performance of the coating. At present, the research and development of water-based curing agents is one of the hot directions of water-based coatings.

[0003] Isocyanate curing agents in oily polyurethane coatings are generally hydrophobic, and the NCO group can react with water. Traditional oily curing agents are difficult to disperse in water and need to be hydrophilic modified. The modification methods of water-based curing agents are usually non-ionic modification, ionic modification, and composite modification. Among them, non-ionic modification is mostly modified by monohydroxy polyether. Among them, US5200489 discloses a water-based curing agent modified with monofunctional polyethylene glycol with a molecular weight of 200 to 1000, but the modification ratio is greater than 10% to obtain a certain water dispersibility, the hand stirring is general, and the NCO% content is low. Further increasing the modification ratio to increase hydrophilicity will not only continue to reduce NCO%, but also cause the paint film hardness to decrease. Ionic modification often uses sulfonate modification, and the hydrophilicity is significantly improved, but it is limited by pH value. At the same time, the modification reagent is expensive and costly, and the main production technology is monopolized by foreign companies, which limits the further promotion of water-based two-component polyurethane coatings. Composite modification takes into account the advantages of both non-ionic modification and ionic modification, but the current composite modification technology is mostly achieved through two modifications, requiring two modifiers, and there are few actual cases. For example, CN105949436A uses polyether polyol and hydroxycarboxylic acid as two modifiers to obtain a water-based curing agent, and requires a multi-step process of modification-trimerization-thin film evaporation-post-modification, and the NCO% value of the obtained product is slightly low.

[0004] In addition, CN110760055A discloses a polyisocyanate composition having a quaternary ammonium salt structure obtained by using a hydroxyl-containing quaternary ammonium salt catalyst system. The composition has excellent moisture stability, but the ionic structure is introduced in the form of a catalyst, the modification ratio is low, the product is weakly hydrophilic, and has no water dispersibility.

[0005] At present, the slow development of water-based curing agents is still an important factor restricting the promotion of water-based coatings. As the country pays more and more attention to green health and environmental protection, there is an urgent need for new water-based curing agent technology. Summary of the invention

[0006] The present invention aims to provide a water-dispersible composite hydrophilic modified curing agent and a preparation method thereof. The nonionic and ionic composite hydrophilic modification is achieved by a modifier, and the obtained curing agent has good water dispersibility and high NCO content.

[0007] The present invention is achieved through the following technical solutions:

[0008] A water-dispersible composite hydrophilic modified curing agent, the structural formula is as follows:

[0009]

[0010] in Representative isocyanurate ring structure: Or the adduct structure of trimethylolpropane: Wherein R1 is selected from one or several combinations of hexylene, 2,4-toluene, 2,6-toluene, 1-methylene-1,3,3-trimethylcyclohexyl; R2 is selected from one or several combinations of C1-C4 fatty alkyl, such as methyl, ethyl, propyl, butyl; wherein n represents the number of repeating units of ethyleneoxy, which is selected from 9 to 54.

[0011] A method for preparing a water-dispersible composite hydrophilic modified curing agent comprises the following steps:

[0012] a) adding propylene polyethylene glycol, peroxide and solvent into a reactor, introducing hydrogen bromide gas at 30-55° C. under stirring, and then continuing the reaction for 30-150 min, then introducing nitrogen for 30-60 min, and then adding tertiary amine and continuing the reaction for 4-12 h, cooling and precipitating the product ether, washing 2-5 times, and vacuum drying to obtain a composite hydrophilic modifier;

[0013] b) Under nitrogen protection, polyisocyanate is added into the reactor, stirred and heated to 60-100° C., a composite hydrophilic modifier is added into the reactor, the reaction is continued for 2-6 hours, and the material is cooled and discharged to obtain a water-dispersible composite hydrophilic modified curing agent.

[0014] Preferably, the molecular weight of the propylene polyethylene glycol of the present invention is 450-2400, preferably 450-1000.

[0015] Preferably, the peroxide described in the present invention is one or more of dibenzoyl peroxide, tert-butyl peroxyacetate, acetylbenzoyl peroxide, and ethyl ketone peroxide.

[0016] Preferably, the solvent of the present invention is one or more of acetone, ethanol, pyridine, hexacyclopentane, dichloromethane, and chloroform, preferably acetone.

[0017] Preferably, the mass ratio of propylene polyethylene glycol:peroxide:solvent in the present invention is 100:0.5-1.5:100-700.

[0018] Preferably, the tertiary amine of the present invention is one or more of trimethylamine, triethylamine, dimethylbutylamine, tri-n-propylamine, diisopropylbutylamine, tri-sec-butylamine, and triisobutylamine, preferably one or more of trimethylamine, triethylamine, and dimethylbutylamine.

[0019] Preferably, the mass ratio of the tertiary amine to the propylene polyethylene glycol of the present invention is 8 to 35:100.

[0020] Preferably, the polyisocyanate of the present invention comprises one or more of HDI trimer, IPDI trimer, TDI trimer, TDI / HDI mixed trimer, HDI-TMP adduct, IPDI-TMP adduct, TDI-TMP adduct, preferably HDI trimer.

[0021] Preferably, the mass ratio of the composite hydrophilic modifier to the polyisocyanate of the present invention is 3 to 10:100, preferably 5 to 8:100.

[0022] The present invention obtains a composite hydrophilic modifier with two hydrophilic structures of vinyloxy and quaternary ammonium salt ion through addition reaction and quaternization reaction of propylene polyethylene glycol, and the modifier has strong hydrophilicity and has the characteristics of ionic modifier and nonionic modifier concurrently. Two hydrophilic structures can be introduced into polyisocyanate simultaneously by the modifier, on the one hand, because the ionic modified structure has strong hydrophilicity, a water-dispersible curing agent can be obtained using a small amount of modifier, and the NCO group consumption is low, which ensures that the product has enough functionality. On the other hand, the nonionic modified structure can improve the water stability of the product. Finally, a modifier introduces two modified structures simultaneously, simplifies the process, does not need to use two modifiers, and further reduces the consumption of the NCO group.

[0023] Compared with the prior art, the preparation method of the present invention has the following advantages: only one modifier is used to achieve non-ionic and ionic composite hydrophilic modification, the obtained curing agent has good water dispersibility and high NCO content, and the paint film cured by the curing agent has good water resistance and hardness. DETAILED DESCRIPTION

[0024] The preparation method of the water-dispersible composite hydrophilic modified curing agent of the present invention is further described below in conjunction with specific implementation examples. It should be understood that the embodiments given in the present invention are only used to illustrate the present invention and are not used to limit the scope of the present invention.

[0025] Embodiment 1:

[0026] a) Dehydrate allyl polyethylene glycol, acetone and triethylamine in advance. Add 100g of allyl polyethylene glycol (APEG 500), 1.5g of benzoyl peroxide and 500g of acetone into the reactor, and introduce hydrogen bromide gas at 40°C for 120min under stirring. Pass nitrogen for 60min, then add 20g of triethylamine and continue the reaction for 12h. After cooling, the product ether is precipitated and washed 3 times, and vacuum dried to obtain composite hydrophilic modifier I: HO-(CH2CH2O) n CH2CH2CH2N + (CH2CH3)3Br — , n≈10.

[0027] b) Under nitrogen protection, 950 g of WANNATE HT-100 was added to the reactor, stirred and heated to 90°C, 50 g of composite hydrophilic modifier I was added to the reactor, the reaction was continued for 240 min, and the material was cooled and discharged.

[0028] The product of Example 1 was subjected to HNMR nuclear magnetic analysis. The results showed that in addition to the peak positions of HDI trimer (δ3.83, 3.23, 1.60, 1.37), there were carbamate-linked methylene (NHCOO-CH2-, δ4.22), vinyloxy (-CH2CH2O-, δ3.61), quaternary ammonium salt N + Connecting methylene (N + CH2-, δ3.32) and the adjacent methyl group (N + Characteristic peaks of groups such as CH2CH3, δ1.29).

[0029] Embodiment 2:

[0030] a) Dehydrate allyl polyethylene glycol, acetone and triethylamine in advance. Add 100g allyl polyethylene glycol (APEG 700), 1.5g dibenzoyl peroxide and 600g acetone into the reactor, introduce hydrogen bromide gas at 40°C and continue the reaction for 120min. Pass nitrogen for 60min, then add 14.4g triethylamine and continue the reaction for 12h. After cooling, the product ether is precipitated and washed 3 times, and vacuum dried to obtain composite hydrophilic modifier II: HO-(CH2CH2O) n CH2CH2CH2N + (CH2CH3)3Br — , n=14~15.

[0031] b) Under nitrogen protection, 940 g of WANNATE HT-600 polyisocyanate was added to the reactor, stirred and heated to 80° C., 60 g of composite hydrophilic modifier II was added to the reactor, the reaction was continued for 240 min, and the material was cooled and discharged.

[0032] Embodiment 3:

[0033] a) Dehydrate allyl polyethylene glycol, acetone and trimethylamine in advance. Add 100g allyl polyethylene glycol (APEG 1000), 1g tert-butyl peroxyacetate and 700g acetone into the reactor, introduce hydrogen bromide gas at 40°C and continue the reaction for 150min. Pass nitrogen for 60min, then add 5.9g trimethylamine and continue the reaction for 12h. After cooling, the product ether is precipitated and washed 3 times, and vacuum dried to obtain composite hydrophilic modifier III: HO-(CH2CH2O) n CH2CH2CH2N + (CH3)3Br — , n=21~22.

[0034] b) Under nitrogen protection, 930 g of WANNATE HT-600 polyisocyanate was added to the reactor, stirred and heated to 90° C., 70 g of composite hydrophilic modifier III was added to the reactor, the reaction was continued for 240 min, and the material was cooled and discharged.

[0035] Comparative Example 1:

[0036] The preparation method disclosed in US5200489 was adopted, monomethyl ether polyethylene glycol (MPEG 550) was dehydrated in advance, 880g WANNATE HT-100 polyisocyanate was added to the reactor under nitrogen protection, stirred and heated to 100°C, 120g MPEG 550 was added to the reactor, the reaction was continued for 360min, and the material was cooled and discharged.

[0037] Comparative Example 2:

[0038] Using the preparation method of CN110760055A, 1000g of HDI was heated at 70°C, 0.5g of a 20% by mass n-butanol solution of formate of 2-hydroxy-N,N,N-trimethyl-1-propylamine was added, the NCO content in the reaction solution reached 39% by mass, and 0.16g of di-n-butyl phosphate was added to terminate the reaction. Using a thin film evaporator, the polyisocyanate composition was purified twice at 130°C and 0.2Torr. The polyisocyanate composition was heat treated at 80°C for 120min.

[0039] Comparative Example 3:

[0040] a) Dehydrate allyl polyethylene glycol, acetone and triethylamine in advance. Add 100g allyl polyethylene glycol (APEG 350), 1.5g benzoyl peroxide and 500g acetone into the reactor, introduce hydrogen bromide gas at 40°C and continue the reaction for 120min. Pass nitrogen for 60min, then add 29g triethylamine and continue the reaction for 12h. After cooling, the product ether is precipitated and washed 3 times, and vacuum dried to obtain modifier IV;

[0041] b) Under nitrogen protection, 950 g of WANNATE HT-100 was added to the reactor, stirred and heated to 90°C, 50 g of modifier IV was added to the reactor, the reaction was continued for 240 min, and the material was cooled and discharged.

[0042] The basic indicators and water dispersibility test results of the above 6 groups of curing agents are shown in Table 1 below.

[0043] Table 1 Basic indicators and water dispersibility test results of Examples 1 to 3 and Comparative Examples 1 to 2

[0044]

[0045]

[0046] Centrifugal stability test method: The examples and comparative examples were manually stirred in water for 3 minutes, then dispersed at 1200 rpm for 15 minutes, and then centrifuged at 2500 rpm for 10 minutes to observe the stratification.

[0047] As can be seen from Table 1, the water-dispersible composite hydrophilic modified curing agents of Examples 1 to 3 have high NCO content and good water dispersibility. This is because Examples 1 to 3 all have dual hydrophilicity of nonionic hydrophilic groups and quaternary ammonium salt groups, and only a small amount of modification is required.

[0048] Comparative Example 1 uses only monomethyl ether polyethylene glycol as a hydrophilic modifier, and has limited hydrophilicity. Even if the modification ratio is large, the hydrophilicity is still insufficient. Although Comparative Example 2 has a high NCO content, it has almost no hydrophilicity and is difficult to disperse in water. Comparative Example 3 has a slightly lower NCO content. Although it has good dispersibility in hand-stirred water, it has a slightly poor stability due to the small number of ethyleneoxy groups and short chain segments.

[0049] The above-mentioned Example 1, Example 2, Example 3, Comparative Example 1, Comparative Example 2, and Comparative Example 3 were respectively used as curing agents to prepare paints according to the formula in Table 2 for performance testing.

[0050] Table 2 Test formula

[0051]

[0052] Table 3 Film forming performance test results of Examples 1 to 3 and Comparative Examples 1 to 3

[0053]

[0054] *: Comparative Example 2 cannot form a uniform film, so the performance test results cannot be detected

[0055] Pencil hardness test standard: GB / T 6739-2006; Pendulum hardness test standard: GB / T 1730-2007; Flexibility test standard: GB / T 6742-2007; Adhesion test standard: GB / T 9286-1998; Water resistance test standard: GB / T5029-1985.

[0056] As shown in Table 3, Examples 1 to 3 have low modification ratios, high NCO contents, and high crosslinking densities, and therefore exhibit good hardness and water resistance. However, Comparative Example 1 has a large modification ratio, and the plasticity of the polyether segment affects the hardness of the paint film. Comparative Example 2 has almost no hydrophilicity, is difficult to disperse in water, and is difficult to form a uniform film. Comparative Example 3 has slightly poor water resistance.

Claims

1. A water-dispersible composite hydrophilic modified curing agent, the structural formula of which is as follows: in Representative isocyanurate ring structure: Or the adduct structure of trimethylolpropane: Wherein R1 is selected from one or several combinations of hexylene, 2,4-toluene, 2,6-toluene, 1-methylene-1,3,3-trimethylcyclohexyl; R2 is selected from one or several combinations of C1-C4 fatty alkyl; wherein n represents the number of repeating units of ethyleneoxy, which is selected from 9 to 54.

2. The water-dispersible composite hydrophilic modified curing agent according to claim 1, characterized in that: R2 is selected from methyl, ethyl, propyl, butyl.

3. A method for preparing the water-dispersible composite hydrophilic modified curing agent according to claim 1, comprising the following steps: a) adding propylene polyethylene glycol, peroxide and solvent into a reactor, introducing hydrogen bromide gas at 30-55° C. under stirring, and then continuing the reaction for 30-150 min, then introducing nitrogen for 30-60 min, and then adding tertiary amine and continuing the reaction for 4-12 h, cooling and precipitating the product ether, washing 2-5 times, and vacuum drying to obtain a composite hydrophilic modifier; b) Under nitrogen protection, polyisocyanate is added into the reactor, stirred and heated to 60-100° C., a composite hydrophilic modifier is added into the reactor, the reaction is continued for 2-6 hours, and the material is cooled and discharged to obtain a water-dispersible composite hydrophilic modified curing agent.

4. The method according to claim 3, characterized in that The peroxide is one or more of dibenzoyl peroxide, tert-butyl peroxyacetate, acetylbenzoyl peroxide, and ethyl ketone peroxide.

5. The method according to claim 3, characterized in that: The mass ratio of the propylene polyethylene glycol: the peroxide: the solvent is 100: 0.5-1.5: 100-700.

6. The method according to claim 3, characterized in that The tertiary amine is one or more of trimethylamine, triethylamine, dimethylbutylamine, tri-n-propylamine, diisopropylbutylamine, tri-sec-butylamine and triisobutylamine.

7. The method according to claim 3, characterized in that The mass ratio of the tertiary amine to the propylene polyethylene glycol is 8 to 35:

100.

8. The method according to claim 3, characterized in that The polyisocyanate includes one or more of HDI trimer, IPDI trimer, TDI trimer, TDI / HDI mixed trimer, HDI-TMP adduct, IPDI-TMP adduct, and TDI-TMP adduct.

9. The method according to claim 3, characterized in that: The mass ratio of the composite hydrophilic modifier to the polyisocyanate is 3 to 10:

100.

10. The method according to claim 3, characterized in that: The mass ratio of the composite hydrophilic modifier to the polyisocyanate is 5 to 8:100.

Citation Information

Patent Citations

  • Polyisocyanate composition and preparation method thereof

    CN110760055A

  • Water dispersible polyisocyanates

    US5200489A

  • Water-dispersible HDI-TDI mixed tripolymer curing agent and preparation method thereof

    CN105949436A

  • Use of hydrophilically modified polyisocyanates in field of textiles

    CN1153542A