A halogen-free flame retardant and its preparation method and application

By using halogen-free flame retardants prepared by the condensation reaction of boron and phosphorus in epoxy resins, the problems of flammable epoxy resins and poor flame retardant compatibility are solved, achieving efficient flame retardancy and improving transparency, forming Composite material with excellent flame retardancy and mechanical properties.

CN116120562BActive Publication Date: 2024-10-01JIANGSU BAOYUAN GAOXIN ELECTRIC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211585978.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-09
Publication Date
2024-10-01
Estimated Expiration
2042-12-09

Smart Images

  • Figure CN116120562B_ABST
    Figure CN116120562B_ABST
Patent Text Reader

Abstract

The present invention discloses a halogen-free flame retardant and its preparation and application. The flame retardant is obtained by condensing the obtained product with a phosphorus-containing component after a dehydration reaction between a boron-containing component and pentaerythritol. After the halogen-free flame retardant is used in the flame retardant of epoxy resin, when the formed composite material is subjected to flame combustion, the composite material generates a large amount of non-toxic and flame-suppressing white smoke, which has a significant smoke suppression effect in the gas phase, and can form a dense and thick expanded carbon layer in the condensed phase, thereby achieving a better effect of blocking heat and oxygen exchange, playing a role in the gas phase and the condensed phase at the same time, and achieving excellent flame retardant effect at a lower addition amount. Compared with commercial phosphorus-based flame retardants, the advantages of the flame retardant of the present invention are reflected in better compatibility with epoxy resin matrix, the composite material has a certain transparency, takes into account various mechanical properties, and has a higher flame retardant efficiency, and obtains a flame retardant epoxy resin composite material with excellent flame retardancy, mechanical properties, and transparency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of flame-retardant epoxy resin composite materials, and more specifically, to a halogen-free flame retardant and a preparation method and application thereof. Background Art

[0002] Epoxy resin is a very important polymer material. Due to the three-dimensional network formed by thermal curing, it has excellent mechanical properties, and also has high transparency, low shrinkage and strong bonding properties. However, epoxy resin is very easy to burn when exposed to fire, and the limiting oxygen index is only 23%-26%. At the same time, it is easy to generate a lot of black smoke when ignited, which greatly limits the expansion of epoxy resin in the field of flame retardant demand. Traditional halogen flame retardants have extremely high flame retardant efficiency, but because the by-products formed after combustion have strong bioaccumulation and toxicity, the use of halogen flame retardants is gradually being banned and replaced at home and abroad. Among the many flame retardant elements, phosphorus flame retardants are considered to be one of the most efficient halogen-free flame retardants, but commercial phosphorus flame retardants, such as ammonium polyphosphate and aluminum hypophosphite, have poor compatibility with epoxy resin, which greatly affects the curing process of epoxy resin, and have poor compatibility with epoxy resin matrix, low efficiency, and the introduction of flame retardants makes epoxy resin completely opaque. Usually, it needs to be added to 10wt% to play a more stable flame retardant effect. Therefore, more and more research and inventions tend to use multiple elements to synergistically flame retard epoxy resins

[0003] Therefore, due to the large amount of smoke generated when epoxy resin burns and the difficulty in self-extinguishing, as well as the poor compatibility of commercial flame retardants, it is very necessary to synthesize a flame retardant that is compatible with the epoxy resin matrix and maintains the transparency of the composite material. Summary of the invention

[0004] Based on the above problems, the purpose of the present invention is to provide a halogen-free flame retardant and its preparation method and application. After the halogen-free flame retardant provided by the present invention is used in the flame retardancy of epoxy resin, when the formed composite material is subjected to flame combustion, the composite material generates a large amount of non-toxic and flame-suppressing white smoke, which has a significant smoke suppression effect in the gas phase, and can form a tight and thick expanded carbon layer in the condensed phase, thereby achieving a better effect of blocking heat and oxygen exchange, and plays a role in the gas phase and the condensed phase at the same time, and can achieve excellent flame retardant effect at a lower addition amount. Compared with commercial phosphorus-based flame retardants, the advantages of the flame retardant of the present invention are reflected in better compatibility with the epoxy resin matrix, the composite material has a certain transparency, takes into account various mechanical properties, and has a higher flame retardant efficiency, and obtains a flame-retardant epoxy resin composite material with excellent flame retardancy, mechanical properties, and transparency.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] In one aspect, the present invention provides a halogen-free flame retardant, wherein the flame retardant is obtained by condensing a product obtained by dehydrating a boron-containing component and pentaerythritol with a phosphorus-containing component.

[0007] Furthermore, the molar ratio of the boron-containing component to the phosphorus-containing component is 1-2:1.

[0008] Furthermore, the molar ratio of the boron-containing component to the phosphorus-containing component is 1:1.

[0009] Furthermore, the molar ratio of the boron-containing component to pentaerythritol is 2:1.

[0010] Furthermore, the boron-containing component is selected from one of boric acid, aminophenylboric acid, phosphoric acid, tannic acid or phytic acid.

[0011] Furthermore, the phosphorus-containing component is selected from one of phenyl dichlorophosphate, phenylphosphonyl dichloride, phenyl dichlorophosphine or phosphorus oxychloride.

[0012] Furthermore, the pentaerythritol was chemically pure and purchased from Shanghai Chemical Industry Co., Ltd. The boric acid was analytically pure and purchased from Beijing Chemical Plant; and the phenyl dichlorophosphate had a purity of 97% and was purchased from Aladdin Reagent.

[0013] In another aspect, the present invention provides a method for preparing the halogen-free flame retardant as described above, comprising the following steps:

[0014] Dehydrating the boron-containing component with pentaerythritol to obtain an intermediate product;

[0015] The intermediate product is subjected to a condensation reaction with a phosphorus-containing component to obtain the halogen-free flame retardant.

[0016] Furthermore, the dehydration reaction is carried out at a temperature of 100-130° C. and for a time of 3-5 hours.

[0017] Furthermore, the condensation reaction is carried out at a temperature of 20-50° C. and for a time of 12-16 hours.

[0018] Furthermore, the preparation method comprises the following steps:

[0019] S1. Mix the boron-containing component and pentaerythritol in a molar ratio of 2:1 in an appropriate amount of toluene solvent at room temperature, heat to 130° C., separate water for four hours until no water appears in the water separator, then filter out the crude solid product TDU, dissolve it in tetrahydrofuran, filter out the insoluble boron-containing component and pentaerythritol, and obtain pure white solid TDU;

[0020] S2. TDU and an acid binder are mixed in an appropriate amount of tetrahydrofuran solution at room temperature, and then the phosphorus-containing component (molar ratio of 2:1 TDU) is dissolved in a small amount of tetrahydrofuran and added dropwise to the mixed solution below within two hours. After the addition is completed, the temperature is raised to 80°C and maintained for 12 hours. After the reaction is completed and cooled to room temperature, the generated triethylamine hydrochloride crystals are filtered out, and the solution is transferred to a rotary distiller to distill off the solvent, and finally a white paste product is obtained.

[0021] In another aspect, the present invention provides a flame retardant epoxy resin composite material, comprising an epoxy resin and the halogen-free flame retardant according to any one of claims 1 to 5.

[0022] Furthermore, the raw materials of the composite material include the following components:

[0023] 70-80 parts of epoxy resin, 15-20 parts of curing agent, and 2-10 parts of the halogen-free flame retardant.

[0024] Furthermore, the mass ratio of the epoxy resin to the curing agent is 100:21.8.

[0025] Furthermore, the epoxy resin is bisphenol A epoxy resin.

[0026] Furthermore, the epoxy equivalent of the epoxy resin is 0.44 mol / 100 g.

[0027] Furthermore, the matrix bisphenol A epoxy resin (DGEBA: E-44), the curing agent 4'4-diaminodiphenylmethane (DDM), and the flame retardant are mixed in proportion, uniformly stirred, and then vacuum degassing is performed, and then transferred to a mold for thermal curing to obtain the composite material.

[0028] Furthermore, the vacuum degree of the vacuum degassing is not higher than -0.1 MPa, the degassing temperature is 100°C, and the degassing time is two hours at 100°C and two hours at 120°C.

[0029] The beneficial effects of the present invention are as follows:

[0030] The halogen-free flame retardant provided by the present invention is a halogen-free flame retardant, which has the advantage of being more environmentally friendly. In addition, due to the introduction of boron element and its specific structure, when the halogen-free flame retardant is used for flame retardancy of epoxy resin, an expanded carbon layer with strength is generated when the composite material is burned; at the same time, the flame retardant has good compatibility in the epoxy resin matrix, has little effect on the curing and degassing process, and after curing, the composite material presents a green color with a certain degree of transparency; finally, in terms of mechanical properties, the linear structure of the flame retardant can be embedded in the three-dimensional network of the epoxy resin, and the tensile and impact properties of the composite material are improved to varying degrees compared with pure epoxy resin. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] The specific implementation modes of the present invention are further described in detail below in conjunction with the accompanying drawings.

[0032] Figure 1 A schematic diagram of the synthesis process of the flame retardant POSB used in Examples 2, 3, and 4 is shown.

[0033] Figure 2 The FTIR spectrum of the flame retardant obtained in Example 2 is shown.

[0034] Figure 3 Digital photographs showing the transparency of the epoxy resin composite materials of Examples 1, 2, 3, and 4.

[0035] Figure 4 A comparison of total heat release (THR) and total smoke release (TSP) of Example 4 and Example 1 (pure epoxy resin) in a cone calorimetry test is shown. DETAILED DESCRIPTION

[0036] In order to more clearly illustrate the present invention, the present invention is further described below in conjunction with preferred embodiments and accompanying drawings. Similar components in the accompanying drawings are represented by the same reference numerals. It should be understood by those skilled in the art that the content specifically described below is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.

[0037] The pentaerythritol was chemically pure and purchased from Shanghai Chemical Industry Co., Ltd. The boric acid was analytically pure and purchased from Beijing Chemical Plant. The phenyl dichlorophosphate had a purity of 97% and was purchased from Aladdin Reagent. Unless otherwise specified, other reagents were commercially available.

[0038] Example 1

[0039] This embodiment provides a method for preparing pure epoxy resin:

[0040] The base bisphenol A epoxy resin (DGEBA: E-44) and the curing agent 4'4-diaminodiphenylmethane (DDM) are mixed in proportion, stirred evenly and then vacuum degassed, and then transferred to the mold for thermal curing. Specifically: 100g of epoxy resin is placed in a beaker, stirred and preheated at a speed of 500r under a 90℃ hot table to increase its fluidity, then 21.8g of DDM is added, stirred briefly to dissolve the DDM, and then immediately transferred to a 100℃ vacuum oven for vacuum degassed, degassed for 20 minutes at a pressure of -0.1MPa, and then poured into the corresponding test mold, and cured at 100℃ and 120℃ for two hours respectively to obtain epoxy material.

[0041] Example 2

[0042] This embodiment provides a method for preparing a flame retardant epoxy resin:

[0043] S1. Boric acid and pentaerythritol were mixed in a proper amount of toluene solvent at a molar ratio of 2:1 at room temperature, and the temperature was raised to 130°C. Water was separated for four hours until no water appeared in the water separator. The crude solid product TDU was then filtered out and dissolved in tetrahydrofuran. The insoluble boric acid and pentaerythritol were removed by filtration to obtain pure white solid TDU.

[0044] S2. Mix TDU and triethylamine in an appropriate amount of tetrahydrofuran solution at room temperature, then dissolve phenyl dichlorophosphate (molar ratio 2:1 TDU) in a small amount of tetrahydrofuran and dropwise add it to the mixed solution below within two hours. After the addition is complete, heat to 80°C and maintain for 12 hours. After the reaction is completed and cooled to room temperature, filter out the generated triethylamine hydrochloride crystals, transfer the solution to a rotary distiller to distill and remove the solvent, and finally obtain a white paste product POSB.

[0045] S3. Mix the matrix bisphenol A epoxy resin (DGEBA: E-44), curing agent 4'4-diaminodiphenylmethane (DDM), and flame retardant POSB in proportion, stir evenly and perform vacuum degassing, and then transfer to the mold for thermal curing. Specifically: place 100g of epoxy resin in a beaker, stir and preheat at a speed of 500r under a 90℃ hot table to increase its fluidity, then dissolve 2.48g of flame retardant POSB in 10mL of methanol and mix with the epoxy resin. After the methanol is completely evaporated, add 21.8g of DDM, stir briefly to dissolve the DDM, and then immediately transfer to a 100℃ vacuum oven for vacuum degassing, degas for 20 minutes at a pressure of -0.1MPa, and then pour into the corresponding test mold, and cure at 100℃ and 120℃ for two hours respectively to obtain a flame-retardant epoxy composite material.

[0046] Example 3

[0047] This embodiment provides a method for preparing a flame retardant epoxy resin:

[0048] S1. Boric acid and pentaerythritol were mixed in a proper amount of toluene solvent at a molar ratio of 2:1 at room temperature, and the temperature was raised to 130°C. Water was separated for four hours until no water appeared in the water separator. The crude solid product TDU was then filtered out and dissolved in tetrahydrofuran. The insoluble boric acid and pentaerythritol were removed by filtration to obtain pure white solid TDU.

[0049] S2. Mix TDU and triethylamine in an appropriate amount of tetrahydrofuran solution at room temperature, then dissolve phenyl dichlorophosphate (molar ratio 2:1 TDU) in a small amount of tetrahydrofuran and dropwise add it to the mixed solution below within two hours. After the addition is complete, heat to 80°C and maintain for 12 hours. After the reaction is completed and cooled to room temperature, filter out the generated triethylamine hydrochloride crystals, transfer the solution to a rotary distiller to distill and remove the solvent, and finally obtain a white paste product POSB.

[0050] S3. Mix the matrix bisphenol A epoxy resin (DGEBA: E-44), curing agent 4'4-diaminodiphenylmethane (DDM), and flame retardant POSB in proportion, stir evenly and perform vacuum degassing, and then transfer to the mold for thermal curing. Specifically: Place 100g of epoxy resin in a beaker, stir and preheat at a speed of 500r under a 90℃ hot table to increase its fluidity, then dissolve 3.76g of flame retardant POSB in 10mL of methanol and mix with the epoxy resin. After the methanol is completely evaporated, add 21.8g of DDM, stir briefly to dissolve the DDM, and then immediately transfer to a 100℃ vacuum oven for vacuum degassing, degas for 20 minutes at a pressure of -0.1MPa, and then pour into the corresponding test mold, and cure at 100℃ and 120℃ for two hours respectively to obtain a flame-retardant epoxy composite material.

[0051] Example 4

[0052] This embodiment provides a method for preparing a flame retardant epoxy resin:

[0053] S1. Boric acid and pentaerythritol were mixed in a proper amount of toluene solvent at a molar ratio of 2:1 at room temperature, and the temperature was raised to 130°C. Water was separated for four hours until no water appeared in the water separator. The crude solid product TDU was then filtered out and dissolved in tetrahydrofuran. The insoluble boric acid and pentaerythritol were removed by filtration to obtain pure white solid TDU.

[0054] S2. Mix TDU and triethylamine in an appropriate amount of tetrahydrofuran solution at room temperature, then dissolve phenyl dichlorophosphate (molar ratio 2:1 TDU) in a small amount of tetrahydrofuran and dropwise add it to the mixed solution below within two hours. After the addition is complete, heat to 80°C and maintain for 12 hours. After the reaction is completed and cooled to room temperature, filter out the generated triethylamine hydrochloride crystals, transfer the solution to a rotary distiller to distill and remove the solvent, and finally obtain a white paste product POSB.

[0055] S3. Mix the matrix bisphenol A epoxy resin (DGEBA: E-44), curing agent 4'4-diaminodiphenylmethane (DDM), and flame retardant POSB in proportion, stir evenly and perform vacuum degassing, and then transfer to the mold for thermal curing. Specifically: place 100g of epoxy resin in a beaker, stir and preheat at a speed of 500r under a 90℃ hot table to increase its fluidity, then dissolve 6.4g of flame retardant POSB in 10mL methanol and mix with the epoxy resin. After the methanol is completely evaporated, add 21.8gDDM, stir briefly to dissolve the DDM, and then immediately transfer to a 100℃ vacuum oven for vacuum degassing, degas for 20 minutes at a pressure of -0.1MPa, and then pour into the corresponding test mold, and cure at 100℃ and 120℃ for two hours respectively to obtain a flame-retardant epoxy composite material.

[0056] Comparative Example 1

[0057] This comparative example provides a method for preparing an epoxy resin composite material:

[0058] S1. Boric acid and pentaerythritol were mixed in a proper amount of toluene solvent at a molar ratio of 2:1 at room temperature, and the temperature was raised to 130°C. Water was separated for four hours until no water appeared in the water separator. The crude solid product TDU was then filtered out and dissolved in tetrahydrofuran. The insoluble boric acid and pentaerythritol were removed by filtration to obtain pure white solid TDU.

[0059] S2. Mix the base bisphenol A epoxy resin (DGEBA: E-44), curing agent 4'4-diaminodiphenylmethane (DDM), and flame retardant intermediate TDU in proportion, stir evenly and perform vacuum degassing, and then transfer to the mold for thermal curing. Specifically: place 100g of epoxy resin in a beaker, stir and preheat at a speed of 500r under a 90℃ hot table to increase its fluidity, then dissolve 6.4g of flame retardant synthetic intermediate TDU in 10mL methanol and mix with epoxy resin. After the methanol is completely evaporated, add 21.8gDDM, stir briefly to dissolve DDM, and then immediately transfer to a 100℃ vacuum oven for vacuum degassing, degas for 20 minutes at a pressure of -0.1MPa, and then pour into the corresponding test mold, and cure at 100℃ and 120℃ for two hours respectively to obtain an epoxy composite material.

[0060] Comparative Example 2

[0061] S1. Boric acid and pentaerythritol were mixed in a proper amount of toluene solvent at a molar ratio of 2:1 at room temperature, and the temperature was raised to 130°C. Water was separated for four hours until no water appeared in the water separator. The crude solid product TDU was then filtered out and dissolved in tetrahydrofuran. The insoluble boric acid and pentaerythritol were removed by filtration to obtain pure white solid TDU.

[0062] S2. Mix the matrix bisphenol A epoxy resin (DGEBA: E-44), curing agent 4'4-diaminodiphenylmethane (DDM), flame retardant intermediate TDU, and reaction raw material phenyl dichlorophosphate in proportion, stir evenly and perform vacuum degassing operation, and then transfer to the mold for thermal curing. Specifically: Place 100g of epoxy resin in a beaker, stir and preheat at a speed of 500r under a 90℃ hot table to increase its fluidity, then dissolve 3.2g of flame retardant synthetic intermediate TDU and 3.2g of phenyl dichlorophosphate in 10mL methanol and mix with epoxy resin. After the methanol is completely evaporated, add 21.8gDDM, stir briefly to dissolve DDM, and then immediately transfer to a 100℃ vacuum oven for vacuum degassing, degas for 20 minutes at a pressure of -0.1MPa, and then pour into the corresponding test mold, and cure at 100℃ and 120℃ for two hours respectively to obtain an epoxy composite material.

[0063] Comparative Example 3

[0064] This comparative example provides a method for preparing a novel epoxy resin composite material:

[0065] Place 100g of epoxy resin in a beaker, stir and preheat at 500r on a hot plate at 90℃ to increase its fluidity, then mix 6.4g of ammonium polyphosphate with the epoxy resin. After methanol is completely evaporated, add 21.8g of DDM, stir briefly to dissolve DDM, and then immediately transfer to a 100℃ vacuum oven for vacuum degassing. Degassing for 20 minutes at a pressure of -0.1MPa, then pour into the corresponding test mold, and cure at 100℃ and 120℃ for two hours respectively to obtain an epoxy composite material.

[0066] Comparative Example 4

[0067] This comparative example provides a method for preparing a novel epoxy resin composite material:

[0068] 100g of epoxy resin was placed in a beaker, and stirred at 500r on a hot plate at 90℃ to preheat it to increase its fluidity. Then 6.4g of aluminum hypophosphite was mixed with the epoxy resin. After methanol was completely evaporated, 21.8g of DDM was added, and DDM was dissolved by stirring for a short time. Then, it was immediately transferred to a 100℃ vacuum oven for vacuum degassing. At a pressure of -0.1MPa, it was degassed for 20 minutes, and then poured into the corresponding test mold, and cured at 100℃ and 120℃ for two hours respectively to obtain a new epoxy composite material.

[0069] Comparative Example 5

[0070] This comparative example provides a method for preparing a novel epoxy resin composite material:

[0071] Place 100g of epoxy resin in a beaker, stir and preheat at 500r on a hot plate at 90℃ to increase its fluidity, then mix 6.4g of piperazine pyrophosphate with the epoxy resin. After methanol is completely evaporated, add 21.8g of DDM, stir briefly to dissolve DDM, and then immediately transfer to a 100℃ vacuum oven for vacuum degassing. Degassing for 20 minutes at a pressure of -0.1MPa, then pour into the corresponding test mold, and cure at 100℃ and 120℃ for two hours respectively to obtain an epoxy composite material.

[0072] Comparative Example 6

[0073] This comparative example provides a method for preparing a novel epoxy resin composite material:

[0074] Place 100g of epoxy resin in a beaker, stir and preheat at 500r on a hot plate at 90℃ to increase its fluidity, then mix 6.4g of montmorillonite with the epoxy resin. After methanol is completely evaporated, add 21.8g of DDM, stir briefly to dissolve DDM, and then immediately transfer to a 100℃ vacuum oven for vacuum degassing. Degassing for 20 minutes at a pressure of -0.1MPa, then pour into the corresponding test mold, and cure at 100℃ and 120℃ for two hours respectively to obtain an epoxy composite material.

[0075] The conventional mechanical properties and combustion performance tests of epoxy resin composite materials were carried out according to the following standards. The results are shown in Table 1.

[0076] Izod beam impact strength: tested in accordance with GB / T1043.1-2018 standard, the impact energy is 2J;

[0077] Tensile strength: tested in accordance with GB / T1040.1-2018 standard, the test speed is 5mm / min;

[0078] Combustion performance: LOI standard test is carried out according to GB / T 2406-2015 standard, and UL-94 standard test is carried out according to GB / T 2408-2008 standard.

[0079] Figure 1 Schematic diagram of the synthesis process of the flame retardant POSB used in Examples 2, 3, and 4.

[0080] Figure 2 The FTIR spectrum of the flame retardant obtained in Example 2 is shown. As shown in the figure, for the TDU curve, 3220 cm -1 corresponds to the stretching vibration of hydroxyl groups, while 1424 cm -1 and 1196cm -1The two peaks at 1593cm come from the BO and B-OH structures in the boric acid structure, indicating the successful synthesis of TDU. -1 The stretching vibration center of the aromatic ring is 1209cm -1 and 770cm -1 It can be attributed to P=O and PO-Ph in phenyl dichlorophosphate, thus proving that POSB was successfully prepared.

[0081] Figure 3 These are digital photos of the transparency of the epoxy resin composite materials of Examples 1, 2, 3, and 4. It can be observed that as the content of the flame retardant increases, the color of the composite material gradually turns green, but the pattern below can always be observed through the sample strip.

[0082] Figure 4 The total heat release (THR) and total smoke release (TSP) of Example 4 and Example 1 (pure epoxy resin) in the cone calorimetry test are compared. Example 1 contains 100g of epoxy resin and 21.8g of curing agent DDM; Example 4 contains 100g of epoxy resin, 21.8g of curing agent DDM, and 6.4g of flame retardant POSB. Figure 3 It can be seen that compared with the pure sample, Example 4 exhibits quite good flame retardant behavior, THR and TSP decreased by 22.8% and 25% respectively, the total heat release and smoke release of the composite material were significantly reduced, and the flame retardant properties of the epoxy resin composite material were improved.

[0083] Table 1

[0084]

[0085] Conclusion: From the performance comparison in Table 1, it can be seen that Examples 2, 3, and 4 can all reach the V-0 grade in the vertical combustion test, and as the content of the flame retardant POSB continues to increase, the LOI value also continues to increase, up to 33.8%; the total heat release and total smoke release also gradually decrease, reflecting a very excellent flame retardant and smoke suppression effect. However, the flame retardant effect of Comparative Examples 1, 2, 3, and 4 compared with Example 4 is not satisfactory. The addition of the flame retardant intermediate TDU can only reach the V-1 grade, and the introduction of ammonium polyphosphate and aluminum hypophosphite cannot pass the vertical combustion grade at the current addition amount, and the improvement of the LOI value is also very limited. In addition, when commercial phosphorus-containing flame retardants are used in epoxy resins, the results of the cone test are not good, and there is almost no effect on suppressing smoke release. The inhibitory effect on heat release is not obvious because it is not compatible with the decomposition temperature of the matrix. In terms of mechanical properties, Examples 2, 3, and 4 have a significant enhancement effect on the mechanical properties due to their own linear structure and the embedding effect with the three-dimensional network in the matrix. However, the flame retardant intermediate TDU in Comparative Example 1 increases the free volume during the curing reaction due to the effect of small molecules, resulting in excessive cavities in the matrix, thereby affecting the mechanical properties. The commercial flame retardants ammonium polyphosphate and aluminum hypophosphite are completely incompatible with the epoxy resin matrix, causing significant stress concentration after curing, thereby causing the mechanical properties to be destroyed.

[0086] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.

Claims

1. A halogen-free flame retardant, characterized in that: The flame retardant is obtained by a condensation reaction between a boron-containing component and pentaerythritol and the resulting product and a phosphorus-containing component; The preparation method of the halogen-free flame retardant comprises the following steps: Dehydrating the boron-containing component with pentaerythritol to obtain an intermediate product; Carrying out a condensation reaction between the intermediate product and the phosphorus-containing component to obtain the halogen-free flame retardant; Wherein, the boron-containing component is boric acid, and the phosphorus-containing component is phenyl dichlorophosphate; The molar ratio of the boron-containing component to pentaerythritol is 2:1; The molar ratio of the boron-containing component to the phosphorus-containing component is 1-2:1; The dehydration reaction temperature is 100-130°C and the time is 3-5 hours; The condensation reaction temperature is 20-50° C. and the reaction time is 12-16 hours.

2. A flame retardant epoxy resin composite material, characterized in that: The invention comprises epoxy resin and the halogen-free flame retardant as claimed in claim 1.

3. The flame retardant epoxy resin composite material according to claim 2, characterized in that: The raw materials of the composite material include the following components: 70-80 parts of epoxy resin, 15-20 parts of curing agent, and 2-10 parts of the halogen-free flame retardant.