Anti-corrosion high-temperature-resistant wave-absorbing composite coating and preparation method thereof
By employing a dual-layer functional hierarchical design for an anti-corrosion and high-temperature absorbing composite coating, combined with the synergistic effects of corrosion inhibitors, shielding agents, and bulk fillers, the problem of insufficient corrosion resistance and microwave absorption performance of existing coatings in high humidity and high salt spray environments has been solved. This results in a coating with high temperature resistance, corrosion resistance, and good microwave absorption performance, suitable for outdoor construction.
Patent Information
- Application Number
- CN202310043874.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-29
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-01-29
AI Technical Summary
Existing coatings are insufficient in terms of high temperature resistance and corrosion resistance, especially in high humidity, high salt spray and strong ultraviolet environments, making it difficult to meet the requirements of radar stealth and electromagnetic compatibility at the same time, and the construction conditions are demanding.
The anti-corrosion and high-temperature absorbing composite coating adopts a dual-layer functional hierarchical design. The bottom layer is an anti-corrosion layer, the middle layer is an electromagnetic wave absorbing layer, and the surface layer is a heat insulation and wave-transmitting layer. By utilizing the synergistic effect of corrosion inhibitors, shielding agents, and fillers, combined with giant dielectric materials and inorganic non-metallic materials, the coating's corrosion resistance and wave absorption performance are improved.
It significantly enhances the corrosion resistance of the coating in high salt spray and acid/alkali environments, possesses good high temperature resistance and wave absorption properties, is easy to apply, and is suitable for outdoor applications.
Smart Images

Figure CN116120810B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of functional coating technology, and in particular to a corrosion-resistant, high-temperature-resistant, microwave-absorbing composite coating and its preparation method. Background Technology
[0002] Large, open-air electromagnetic facilities primarily constructed of metal, such as substations, communication base stations, radio transmission platforms, and television (broadcast) towers, are constantly exposed to acid rain or sunlight. Therefore, their surface protective coatings must possess long-lasting high-temperature resistance and corrosion resistance. Furthermore, naval vessels, warships, and ships, also composed of metal, operate under conditions of high humidity, high salt spray, and strong ultraviolet radiation. Critical components, in particular, require radar stealth and electromagnetic compatibility. Therefore, developing corrosion-resistant, high-temperature-resistant, and radar-absorbing coatings is an effective technical approach to address these challenges.
[0003] In the prior art, patent CN114656822A discloses a method for preparing a high-temperature resistant and corrosion-resistant acrylic resin coating. This high-temperature resistant and corrosion-resistant acrylic resin coating is composed of acrylic resin, a high-temperature resistant agent, an anti-corrosion agent, a stabilizer, a solvent resistant agent, a freshener, and an aqueous solution. It has good softness, good impact resistance, and excellent high-temperature and corrosion resistance, but detailed data on specific technical effects are not disclosed. Patent CN114682459A discloses a method for preparing a high-temperature resistant low-frequency radar absorbing coating. It adopts a three-layer main structure and innovatively uses a multi-layered absorbing structure within the absorbing layer. This can effectively solve the problem of poor dispersion of the absorbing agent during thermal spraying, improve the efficiency of the absorbing agent in the coating, and effectively solve the problem of absorption of low-frequency radar waves by the thermally sprayed coating. Through the double-layer transition layer structure design, the difference in thermal expansion coefficients between the transition layer and the absorbing layer is reduced, which can improve the overall coating's adhesion and thermal shock resistance, especially increasing the coating's reliability and adaptability under drastic high and low temperature changes. However, the coating contains magnetic iron-based alloy powder, resulting in poor corrosion resistance; furthermore, the coating preparation method has high requirements for equipment and construction environment, limiting its widespread application. Patent CN111205743A discloses a high-temperature resistant electromagnetic wave absorbing coating, its preparation method, and its application. The microporous absorbing filler used is prepared by sintering low-melting-point glass material to coat the absorbing material. It achieves dual absorption functions through physical absorption and structural design, improving the material's absorption efficiency. The provided absorbing coating exhibits good absorption of microwaves in the 2-18GHz frequency range, and the preparation method is simple, low-cost, and exhibits good high-temperature resistance and absorption performance. However, the coating still contains metal powders such as iron, copper, and aluminum powder, which cannot solve the corrosion resistance problem.
[0004] Therefore, how to provide a composite coating that combines corrosion resistance and high temperature resistance with microwave absorption, especially considering the multifunctional enhancement effect of the composite coating in both the selection of the physicochemical properties of the filler powder and the synergistic design of the macroscopic multilayer structure, is an urgent problem to be solved. Summary of the Invention
[0005] This invention provides a corrosion-resistant, high-temperature-resistant, microwave-absorbing composite coating and its preparation method, the purpose of which is to solve the above-mentioned problems existing in the background art.
[0006] To achieve the above objectives, embodiments of the present invention provide a corrosion-resistant, high-temperature resistant, and microwave-absorbing composite coating and its preparation method. The coating employs a dual-layer functional hierarchical design. The bottom layer, in contact with the metal substrate, primarily serves an anti-corrosion function, utilizing the synergistic effect of multiple types of anti-corrosion fillers, including corrosion inhibitors, shielding agents, and bulk fillers, to enhance the coating's anti-corrosion performance in high-humidity and high-salt-spray environments. The middle layer is an electromagnetic wave absorption layer, filled with a high-dielectric-loss material exhibiting strong dielectric loss for incident electromagnetic waves. The surface layer provides high-temperature resistance, heat insulation, and wave transmission, employing a high-temperature resistant multi-component film-forming material and a high-temperature resistant, heat-insulating, and non-oxidizing, highly insulating filler powder, thus not affecting the composite coating's anti-corrosion performance or its ability to strongly reflect electromagnetic waves.
[0007] This invention provides a corrosion-resistant, high-temperature-resistant, and microwave-absorbing composite coating and its preparation method. The composite coating is provided with an anti-corrosion underlayer, a microwave-absorbing intermediate layer, and a heat-insulating and microwave-transparent surface layer from the inside out.
[0008] The anti-corrosion substrate includes a film-forming material 1, an anti-corrosion filler, and an additive 1, with a thickness of 0.1–0.3 mm;
[0009] The microwave absorbing intermediate layer includes a film-forming material 2, an auxiliary agent 2, and a microwave absorbing filler, with a thickness of 0.8–1.2 mm;
[0010] The heat-insulating and wave-transparent surface layer includes heat-insulating and wave-transparent filler with a thickness of 1.0 to 1.5 mm.
[0011] Furthermore, the film-forming material 1 is an epoxy-amine curing system, accounting for 30-60% of the total mass of the anti-corrosion substrate; the film-forming material 2 is made of epoxy modified silicone resin, high phenyl content silicone resin and hydroxyl-terminated butadiene-acrylonitrile rubber, accounting for 20-50% of the total mass of the microwave absorbing intermediate layer and the heat insulation and microwave transparent surface layer.
[0012] Furthermore, the corrosion-resistant filler includes corrosion-inhibiting, shielding, and bulk-filled corrosion-resistant fillers.
[0013] Furthermore, the corrosion-inhibiting filler includes zinc chromate yellow and strontium chromate yellow; the shielding corrosion-resistant filler includes mica and iron oxide; and the bulk filler corrosion-resistant filler includes spherical silica and acicular wollastonite.
[0014] Furthermore, the corrosion-inhibiting filler accounts for 15-35% of the total mass of the anti-corrosion substrate; the shielding filler accounts for 20-40% of the total mass of the anti-corrosion substrate; and the bulk filler accounts for 10-30% of the total mass of the anti-corrosion substrate.
[0015] Furthermore, the additive 1 includes a silane coupling agent, a carboxylated polyester wetting and dispersing agent, and an acrylate defoamer, accounting for 5-10% of the total mass of the anti-corrosion substrate; the additive 2 includes a controllable flocculation ester dispersing agent, an organosilicon defoamer, and an N-phenylaminomethyltriethoxysilane coupling agent, accounting for 6-15% of the total mass of the microwave absorbing intermediate layer and the heat-insulating and microwave-transparent surface layer.
[0016] Furthermore, the microwave absorbing filler is a giant dielectric material, accounting for 40-60% of the total mass of the microwave absorbing intermediate layer; the giant dielectric material is micron-sized BaTiO3 powder or CaCu3Ti4O3 doped with divalent magnesium or calcium ions. 12 At least one of powder, lithium or titanium ion-doped NiO powder.
[0017] Furthermore, the heat-insulating and wave-transparent filler is alumina fiber powder, carbon dioxide silica aerogel powder, or hollow glass micro powder.
[0018] Furthermore, the alumina fiber powder has an alumina content of over 98%, an aspect ratio of 50-150, and accounts for 20-30% of the total mass of the heat-insulating and wave-transparent surface layer; the carbon dioxide silica aerogel powder has a silica content of over 99%, a pore size of 10-50 nm, a porosity greater than 99.8%, and accounts for 5-15% of the total mass of the heat-insulating and wave-transparent surface layer; the hollow glass micropowder has a particle size of 75-150 μm and accounts for 10-20% of the total mass of the heat-insulating and wave-transparent surface layer.
[0019] Furthermore, the composite coating exhibits excellent wave absorption performance in the 2GHz-18GHz range.
[0020] Based on a general inventive concept, the present invention also provides a method for preparing the above-mentioned anti-corrosion and high-temperature absorbing composite coating, wherein the composite coating is uniformly coated onto the surface of a substrate by spraying, roller coating or brushing.
[0021] The above-described solution of the present invention has the following beneficial effects:
[0022] (1) The corrosion-resistant and high-temperature absorbing composite coating of the present invention is filled with a variety of anti-corrosion fillers, including corrosion inhibitors, shielding agents and bulk fillers, in the bottom layer. The powders filled in the middle layer and the surface layer are also inorganic non-metallic materials. The coating fully utilizes the synergistic effect of physical shielding and anti-corrosion and electrochemical corrosion inhibition to greatly improve the anti-corrosion effect of the coating in high salt spray and acid and alkali environments.
[0023] (2) The anti-corrosion and high-temperature absorbing composite coating of the present invention uses a film-forming material made of epoxy modified silicone resin, high phenyl content silicone resin and hydroxyl-terminated butadiene nitrile rubber in the intermediate and surface layers. Due to the presence of a large number of silicon-oxygen bonds, it has long-lasting high-temperature resistance. Furthermore, the alumina fiber powder, carbon dioxide silica aerogel powder and hollow glass micro powder filled in can further enhance the heat insulation and high-temperature resistance of the coating. The composite coating provided by the present invention will not crack or peel off under the high-temperature scouring of oxy-acetylene flame.
[0024] (3) The corrosion-resistant and high-temperature absorbing composite coating of the present invention has a giant dielectric material filled in the middle layer that will exhibit dielectric loss mechanisms such as dielectric polarization and electric dipole orientation polarization under electromagnetic field, thus absorbing incident electromagnetic wave energy; in addition, the high resistivity of the surface layer is conducive to the incident electromagnetic wave entering the coating and has good electromagnetic matching characteristics and wave transmission performance. Therefore, the composite coating provided by the present invention has good wave absorption performance in the range of 2GHz-18GHz.
[0025] (4) The anti-corrosion and high-temperature absorbing composite coating of the present invention can be applied by simple and convenient spraying, roller coating and brushing, with low requirements for construction conditions and can be cured at room temperature, which can meet the requirements for outdoor construction and is easier to promote and apply. Attached Figure Description
[0026] Figure 1 This is a schematic diagram of the anti-corrosion and high-temperature resistant microwave absorbing composite coating of the present invention;
[0027] Figure 2 This is a schematic diagram of the reflectivity curves of the corrosion-resistant and high-temperature absorbing composite coatings prepared in Examples 1, 2 and 3 of this invention in the 2GHz-18GHz frequency band. Detailed Implementation
[0028] To make the technical problems, technical solutions and advantages of the present invention clearer, a detailed description will be given below in conjunction with the accompanying drawings and specific embodiments.
[0029] Unless otherwise defined, all technical terms used herein have the same meaning as commonly understood by those skilled in the art. The technical terms used herein are for the purpose of describing particular embodiments only and are not intended to limit the scope of the invention.
[0030] Unless otherwise specified, all raw materials, reagents, instruments and equipment used in this invention can be purchased from the market or prepared by existing methods.
[0031] This invention addresses existing problems by providing a corrosion-resistant, high-temperature-resistant, microwave-absorbing composite coating and its preparation method. Figure 1 This is a schematic diagram of the anti-corrosion and high-temperature absorbing composite coating in the following embodiment.
[0032] Example 1
[0033] The corrosion-resistant, high-temperature-resistant, microwave-absorbing composite coating provided in this embodiment has the following bottom layer composition: 36 parts epoxy resin and polyamide curing agent (mass ratio 1:1), 1.5 parts silane coupling agent, 4 parts carboxylated polyester wetting and dispersing agent, 0.5 parts acrylate defoamer, 16 parts zinc chrome yellow and strontium chrome yellow filler (mass ratio 1:3), 20 parts mica and iron oxide (mass ratio 1:1), and 20 parts silica and wollastonite powder (mass ratio 3:1).
[0034] The intermediate layer consists of: 40 parts epoxy-modified silicone resin, high-phenyl-content silicone resin, and hydroxyl-terminated butadiene-acrylonitrile rubber (mass ratio 1:1:1), 4.5 parts N-phenylaminomethyltriethoxysilane coupling agent, 5 parts controllable flocculation ester-type dispersant, 0.5 parts silicone defoamer, and 50 parts CaCu3Ti4O 12 powder.
[0035] The surface layer consists of: 40 parts epoxy-modified silicone resin, high-phenyl-content silicone resin and hydroxyl-terminated butadiene-acrylonitrile rubber (mass ratio 1:1:1), 4.5 parts N-phenylaminomethyltriethoxysilane coupling agent, 5 parts controllable flocculation ester-type dispersant, 0.5 parts silicone defoamer, 35 parts alumina fiber powder, 5 parts carbon dioxide silica aerogel powder, and 10 parts hollow glass micro powder.
[0036] The corrosion-resistant, high-temperature-resistant, and microwave-absorbing composite coating provided in this embodiment has a bottom layer thickness of 0.2 mm and a surface layer thickness of 1.1 mm.
[0037] The reflectance curves of the composite coating in Example 1 of this invention in the 2GHz-18GHz frequency band were tested using a bow-shaped test system built on an N5230A vector network analyzer. The sample size used for testing was 180mm x 180mm (length x width). The test results are attached. Figure 2 As shown, the effective absorption bandwidth (reflectivity better than -10dB) of the composite coating obtained in Example 1 covers 10.46GHz-18.0GHz.
[0038] The high-temperature resistance of the composite coating was tested using an oxy-acetylene flame test. Oxygen flow rate: 1500 L / h, oxygen-acetylene mixing ratio: 1.4, distance between the flame nozzle and the composite coating sample: 20 mm, oxy-acetylene flame irradiation of the composite coating for 5 minutes. The composite coating provided in this embodiment did not crack or peel off.
[0039] The composite coating's resistance to neutral salt spray was tested using GB6458-86. As shown in Table 1, the composite coating provided in this embodiment did not exhibit any bubbles or rust after being tested in a salt spray chamber for 1000 hours.
[0040] The adhesion of the composite coating was tested using the pull-off method in GB / T5210. As shown in Table 1, the adhesion between the composite coating and the metal substrate provided in this embodiment is greater than 6 MPa.
[0041] Example 2:
[0042] The corrosion-resistant and high-temperature-resistant microwave-absorbing composite coating provided in this embodiment is basically the same as that in Embodiment 1, except that:
[0043] The base layer consists of: 40 parts epoxy resin and polyamide curing agent (mass ratio 1:1), 1.5 parts silane coupling agent, 4 parts carboxylated polyester wetting and dispersing agent, 0.5 parts acrylate defoamer, 18 parts zinc chrome yellow and strontium chrome yellow filler (mass ratio 1:2), 12 parts mica and iron oxide (mass ratio 1:1), and 24 parts silica and wollastonite powder (mass ratio 2:1).
[0044] The intermediate layer consists of: 45 parts epoxy-modified silicone resin, high-phenyl-content silicone resin and hydroxyl-terminated butadiene-acrylonitrile rubber (mass ratio 1:1:1), 3.5 parts N-phenylaminomethyltriethoxysilane coupling agent, 5 parts controllable flocculation ester dispersant, 0.5 parts silicone defoamer, and 46 parts CaCu3Ti4O12 powder and titanium ion-doped NiO powder (mass ratio 1:1).
[0045] The surface layer consists of: 30 parts epoxy-modified silicone resin, high-phenyl-content silicone resin and hydroxyl-terminated butadiene-acrylonitrile rubber (mass ratio 1:1:1), 4.5 parts N-phenylaminomethyltriethoxysilane coupling agent, 5 parts controllable flocculation ester-type dispersant, 0.5 parts silicone defoamer, 40 parts alumina fiber powder, 10 parts carbon dioxide silica aerogel powder, and 10 parts hollow glass micro powder.
[0046] The corrosion-resistant, high-temperature-resistant, and microwave-absorbing composite coating provided in this embodiment has a bottom layer thickness of 0.2 mm and a surface layer thickness of 1.4 mm.
[0047] Using the same testing method as in Example 1, the effective absorption bandwidth (reflectivity better than -10dB) of the composite coating obtained in Example 2 covered 9.16GHz-16.88GHz.
[0048] Using the same test method as in Example 1, the composite coating provided in this example did not crack or peel off after being scoured for 5 minutes under an oxy-acetylene flame test.
[0049] Using the same testing standards as in Example 1, as shown in Table 1, the composite coating provided in this example did not exhibit any bubbles or rust after being tested in a salt spray chamber for 1000 hours.
[0050] Using the same testing standards as in Example 1, as shown in Table 1, the adhesion between the composite coating and the metal substrate provided in this example is greater than 5 MPa.
[0051] Example 3:
[0052] The corrosion-resistant and high-temperature-resistant microwave-absorbing composite coating provided in this embodiment is basically the same as that in Embodiment 1, except that:
[0053] The base layer consists of: 50 parts epoxy resin and polyamide curing agent (mass ratio 1:1), 1.5 parts silane coupling agent, 5 parts carboxylated polyester wetting and dispersing agent, 0.5 parts acrylate defoamer, 10 parts zinc chrome yellow and strontium chrome yellow filler (mass ratio 1:1), 18 parts mica and iron oxide (mass ratio 1:2), and 15 parts silica and wollastonite powder (mass ratio 2:1).
[0054] The intermediate layer consists of: 28 parts epoxy-modified silicone resin, high phenyl content silicone resin and hydroxyl-terminated butadiene-acrylonitrile rubber (mass ratio 2:1:1), 1.5 parts N-phenylaminomethyltriethoxysilane coupling agent, 5 parts controllable flocculation ester dispersant, 0.5 parts silicone defoamer, and 65 parts CaCu3Ti4O12 powder, calcium ion-doped BaTiO3 powder and titanium ion-doped NiO powder (mass ratio 2:2:1).
[0055] The surface layer consists of: 50 parts epoxy-modified silicone resin, high-phenyl-content silicone resin and hydroxyl-terminated butadiene-acrylonitrile rubber (mass ratio 1:1:1), 4.5 parts N-phenylaminomethyltriethoxysilane coupling agent, 5 parts controllable flocculation ester-type dispersant, 0.5 parts silicone defoamer, 20 parts alumina fiber powder, 5 parts carbon dioxide silica aerogel powder, and 15 parts hollow glass micro powder.
[0056] The corrosion-resistant, high-temperature-resistant, and microwave-absorbing composite coating provided in this embodiment has a bottom layer thickness of 0.3 mm and a surface layer thickness of 1.5 mm.
[0057] Using the same testing method as in Example 1, the effective absorption bandwidth (reflectivity better than -10dB) of the composite coating obtained in Example 2 covered 7.88GHz-13.56GHz.
[0058] Using the same test method as in Example 1, the composite coating provided in this example did not crack or peel off after being scoured for 5 minutes under an oxy-acetylene flame test.
[0059] Using the same testing standards as in Example 1, as shown in Table 1, the composite coating provided in this example did not exhibit any bubbles or rust after being tested in a salt spray chamber for 1000 hours.
[0060] Using the same testing standards as in Example 1, as shown in Table 1, the adhesion between the composite coating and the metal substrate provided in this example is greater than 5 MPa.
[0061] Table 1. Temperature resistance, corrosion resistance, and microwave absorption properties of the composite coating
[0062]
[0063] The above description represents the preferred embodiments of the present invention. It should be noted that those skilled in the art can make various improvements and modifications without departing from the principles of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A corrosion-resistant and high-temperature-resistant microwave-absorbing composite coating, characterized in that, The composite coating consists of an anti-corrosion underlayer, a wave-absorbing intermediate layer, and a heat-insulating and wave-transparent surface layer, arranged sequentially from the inside out. The anti-corrosion substrate comprises a film-forming material 1, anti-corrosion fillers, and additives 1, with a thickness of 0.1~0.3 mm; the film-forming material 1 is an epoxy-amine curing system; the anti-corrosion fillers include corrosion-inhibiting, shielding, and extender-type anti-corrosion fillers; the film-forming material 1 accounts for 30~60% of the total mass of the anti-corrosion substrate; the corrosion-inhibiting anti-corrosion fillers account for 15~35% of the total mass of the anti-corrosion substrate; the shielding anti-corrosion fillers account for 20~40% of the total mass of the anti-corrosion substrate; the extender-type anti-corrosion fillers account for 10~30% of the total mass of the anti-corrosion substrate; and the additives 1 account for 5~10% of the total mass of the anti-corrosion substrate. The microwave absorbing intermediate layer comprises a film-forming material 2, an additive 2, and a microwave absorbing filler, with a thickness of 0.8~1.2 mm. The film-forming material 2 is made of epoxy-modified silicone resin, high-phenyl-content silicone resin, and hydroxyl-terminated butadiene-acrylonitrile rubber. The microwave absorbing filler is a giant dielectric material. The film-forming material 2 accounts for 20~50% of the total mass of the microwave absorbing intermediate layer; the microwave absorbing filler accounts for 40~60% of the total mass of the microwave absorbing intermediate layer; and the additive 2 accounts for 6~15% of the total mass of the microwave absorbing intermediate layer. The heat-insulating and wave-transparent surface layer comprises heat-insulating and wave-transparent filler, film-forming material 2, and additive 2, with a thickness of 1.0~1.5 mm; the heat-insulating and wave-transparent filler is alumina fiber powder, silica aerogel powder, or hollow glass micro powder; the film-forming material 2 accounts for 20~50% of the total mass of the heat-insulating and wave-transparent surface layer; the additive 2 accounts for 6~15% of the total mass of the heat-insulating and wave-transparent surface layer. The giant dielectric material is micron-sized BaTiO3 powder or CaCu3Ti4O doped with divalent magnesium or calcium ions. 12 At least one of powder, lithium or titanium ion-doped NiO powder.
2. The corrosion-resistant and high-temperature-resistant microwave-absorbing composite coating according to claim 1, characterized in that, The corrosion-inhibiting filler includes zinc chromate yellow and strontium chromate yellow; the shielding filler includes mica and iron oxide; the bulk filler includes spherical silica and acicular wollastonite.
3. The corrosion-resistant and high-temperature-resistant microwave-absorbing composite coating according to claim 1, characterized in that, The additive 1 includes a silane coupling agent, a carboxylated polyester wetting and dispersing agent, and an acrylate defoamer; the additive 2 includes a controllable flocculation ester dispersing agent, an organosilicon defoamer, and an N-phenylaminomethyltriethoxysilane coupling agent.
4. The corrosion-resistant and high-temperature-resistant microwave-absorbing composite coating according to claim 1, characterized in that, The alumina fiber powder has an alumina content of over 98%, an aspect ratio of 50-150, and accounts for 20-30% of the total mass of the heat-insulating and wave-transparent surface layer; the silica aerogel powder has a silica content of over 99%, a pore size of 10-50 nm, a porosity greater than 99.8%, and accounts for 5-15% of the total mass of the heat-insulating and wave-transparent surface layer; the hollow glass micropowder has a particle size of 75-150 μm and accounts for 10-20% of the total mass of the heat-insulating and wave-transparent surface layer.
5. The method for preparing the corrosion-resistant and high-temperature absorbing composite coating as described in any one of claims 1 to 4, characterized in that, The composite coating is applied evenly to the substrate surface sequentially by spraying, roller coating, or brushing.
Citation Information
Patent Citations
High-temperature-resistant electromagnetic wave absorbing paint, coating and preparation method and application thereof
CN111205743A
Preparation method of high-temperature-resistant low-frequency radar wave-absorbing coating
CN114682459A
Method for preparing CaCu3Ti4O12 powder
CN101880160A
Composite coating electromagnetic shielding paint and composite coating electromagnetic shielding material prepared therefrom