Surface functionalized affinity membranes

By fixing spacer arms on a membrane support and coupling ligands to a surface-functionalized affinity membrane, the problems of high pressure drop and low binding capacity in existing protein A affinity chromatography techniques are solved, achieving efficient IgG purification and cost reduction.

CN116133739BActive Publication Date: 2026-11-20NANOPAREIL LLC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202180026983.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-04-01
Filing Date
2021-04-01
Publication Date
2026-11-20
Estimated Expiration
2041-04-01

AI Technical Summary

Technical Problem

Existing protein A affinity chromatography techniques for IgG production suffer from problems such as high pressure drop, high buffer consumption, low capacity, low productivity, and high cost, and the binding capacity of macroporous membranes is limited.

Method used

By employing surface-functionalized affinity membranes, multiple spacer arms are fixed on a membrane support and coupled with ligands, and high specific surface area and customized coupling chemicals, ligand density and spacer arm length are used to enhance binding capacity.

Benefits of technology

This method achieves efficient IgG purification, reduces pressure drop at high flow rates, improves binding capacity and productivity, and lowers costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116133739B_ABST
    Figure CN116133739B_ABST
Patent Text Reader

Abstract

The present disclosure provides surface functionalized affinity membranes. The surface functionalized affinity membranes are capable of providing increased binding capacity through improved coupling chemistries, ligand density, spacer arm types, and spacer arm lengths. Also provided are methods of making the surface functionalized affinity membranes and methods of using the surface functionalized affinity membranes to isolate targets of interest comprising nucleic acid molecules and proteins from a sample.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Authorization Reference

[0002] This invention was made with government support under license number IIP-1329377 granted by the National Science Foundation. The government holds certain rights to this invention.

[0003] Cross-reference to related applications

[0004] This application claims priority to U.S. Provisional Application No. 63 / 003,629, filed April 1, 2020, which is incorporated herein by reference in its entirety. Technical Field

[0005] This disclosure generally relates to the field of chromatography. More specifically, this disclosure relates to the modification of membrane surfaces for the customized arrangement and immobilization of affinity ligands. Background Technology

[0006] The immense potential of monoclonal antibodies as therapeutic agents and diagnostic tools has led to extensive research efforts in the biotechnology industry to produce high-purity antibodies. Large-scale production of immunoglobulin G (IgG) requires both high-volume upstream processing units and highly efficient downstream processing units to produce extremely pure products. Recent improvements in upstream cell culture titers for antibody production over the past decade have placed enormous pressure on downstream processing, which can account for up to 80% of the actual production cost of IgG. Protein A affinity chromatography is commonly used as the first step in purifying immunoglobulins. The high affinity interaction between the Fc region of IgG and protein A forms the basis for the affinity purification of many subclasses of IgG. Due to this reversible interaction, cell culture medium (CCF) passing through a protein A column results in the binding of IgG and the flow of unwanted impurities (e.g., viruses, host cell proteins, DNA, etc.) through the chromatographic medium. However, conventional resin-based protein A chromatography is limited by factors such as high pressure drop, high buffer consumption, low capacity, low productivity (especially at high flow rates), and high cost. Therefore, much research has focused on developing protein A-based membrane adsorbers as an alternative to resin-based purification steps in IgG production. Several macroporous membranes have been reported. Although these membranes exhibit faster adsorption kinetics and higher permeability compared to packed-bed resins, they suffer from low binding capacity due to the limited surface area available for adsorption.

[0007] Therefore, there is a need for alternative compositions and methods for purifying immunoglobulins and other biomolecules that offer favorable adsorption kinetics, high surface area, high porosity, high binding capacity, and ease of functionalization. Summary of the Invention

[0008] In a preferred embodiment, the surface-functionalized affinity membrane includes: a membrane support; a plurality of spacer arms fixed to the membrane support, each spacer arm including a terminal end; and a ligand coupled to the terminal end. The membrane support may include a cast membrane, an electrospun membrane, or a combination thereof. In a preferred embodiment, the membrane support further includes one or more inert functional groups fixed to the surface of the membrane support.

[0009] In a preferred embodiment, the method for preparing a surface-functionalized affinity membrane includes: providing a nanofiber membrane support; fixing spacer arms to the membrane support, wherein each spacer arm includes an end; and coupling a ligand to the end of the spacer arm via a reactive functional group. The membrane support may include a cast membrane, an electrospun membrane, or a combination thereof. In a preferred embodiment, the membrane support further includes one or more inert functional groups fixed to the surface of the membrane support.

[0010] In a preferred embodiment, the method for separating the target of interest from a sample includes contacting the sample containing the target of interest with the surface-functionalized affinity membrane to adsorb the target of interest. The membrane support may include a cast membrane, an electrospun membrane, or a combination thereof. In a preferred embodiment, the membrane support further includes one or more inert functional groups fixed to the surface of the membrane support.

[0011] While several embodiments have been disclosed, other embodiments of the invention will become apparent to those skilled in the art from the following detailed description illustrating and describing illustrative embodiments of the invention. Therefore, the drawings and detailed description should be considered illustrative in nature and not restrictive. Attached Figure Description

[0012] The following drawings form part of this specification and are included to further illustrate certain embodiments or various aspects of the invention. In some cases, embodiments of the invention are best understood by referring to the accompanying drawings in combination with the detailed description presented herein. The description and drawings may highlight a particular example or aspect of the invention. However, those skilled in the art will understand that portions of an example or aspect may be used in combination with other examples or aspects of the invention.

[0013] Figure 1 This displays various functional groups capable of coupling amine-containing molecules. These include epoxides or ethylene oxides, NHS esters, aldehydes, and sulfonyl chlorides (from left to right).

[0014] Figure 2A This demonstrates the difference between activation density and ligand density used to immobilize protein A onto an epoxide-activated surface.

[0015] Figure 2BThe surface exhibits a condition where the minimum ligand density is exceeded due to spatial interactions and size limitations, thus preventing an increase in IgG binding capacity.

[0016] Figure 2C The paper demonstrates a surface optimized to maximize ligand efficiency by varying the activation density and customizing the surface functionalization to include inert functional groups and an exemplary affinity ligand (protein A).

[0017] Figure 2D A surface with multiple spacers of different molecular lengths is shown to maximize IgG binding.

[0018] Figure 3 This demonstrates the introduction of a hydrocarbon spacer molecule for subsequent activation with a carboxylic acid group. X = F, Cl, Br, or I. n = 0 to infinity.

[0019] Figure 4 This exhibit showcases various biepoxide spacers / linking molecules immobilized onto a cellulose matrix. This includes butylene glycol diglycidyl ether, poly(ethylene glycol) diglycidyl ether (average Mn = 500), and poly(ethylene glycol) diglycidyl ether (average Mn = 500). n =2000 (from left to right).

[0020] Figure 5 This exhibits possible optimized surfaces with different epoxides, and therefore different ligands, densities, and spacer molecular lengths to maximize potential IgG binding.

[0021] Figure 6 This study demonstrates the effect of different spacer molecular lengths on the binding utility of protein A and IgG on the epoxide surface.

[0022] Figure 7 This study demonstrates the effect of different spacer molecule lengths on the IgG binding capacity per ml of membrane.

[0023] Figure 8 This study demonstrates the effect of different spacer molecular lengths on protein uptake from 50 mg of protein A in 1 ml.

[0024] Figure 9 This study demonstrates the effect of different spacer molecular lengths on the binding utility of NHS surface protein A to IgG.

[0025] Figure 10 This study demonstrates the effect of different spacer molecule lengths on the IgG binding capacity per ml of membrane. Detailed Implementation

[0026] This disclosure relates to surface-functionalized affinity membranes having multiple ligands attached to the membrane surface via spacer arms. Affinity membranes offer numerous advantages over existing separation techniques, including packed-bed resins, macroporous membranes, and surface-functionalized membranes. For example, affinity membranes exhibit higher binding capacity due to their high specific surface area, increased ligand density, and increased ligand efficiency. According to this disclosure, these advantages can be achieved by customizing the coupling chemicals, ligand density, spacer arm type, and spacer arm length. The embodiments described herein are applicable to any affinity membrane that is variable and understood by those skilled in the art.

[0027] To facilitate a better understanding of the invention, certain terms are first defined. Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which embodiments of the invention pertain. Many methods and materials similar to, modified, or equivalent to those described herein can be used to practice embodiments of the invention without extensive experimentation; preferred materials and methods are described herein. In describing and claiming embodiments of the invention, the following terms will be used in accordance with the definitions set forth below.

[0028] The numerical ranges listed in this specification include the numbers that define the ranges and include every integer within the defined range. Throughout this disclosure, all aspects of the invention are presented in range format. It should be understood that the use of range format is for convenience and brevity only and should not be construed as a rigid limitation on the scope of the invention. Therefore, the description of ranges should be considered as having explicitly disclosed all possible subranges, fractions, and individual numerical values ​​within the range. For example, a description of a range, such as from 1 to 6, should be considered as having explicitly disclosed subranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., and individual numbers within the range, such as 1, 2, 3, 4, 5, and 6, and decimals and fractions, such as 1.2, 3.8, 1, etc. 1 / 2 and 4 3 / 4. This applies regardless of the breadth of the scope.

[0029] It should be understood that all terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting in any way or scope. For example, unless the content expressly indicates otherwise, the singular forms "a / an" and "the" as used in this specification and the appended claims may include multiple indicators. Furthermore, all units, prefixes, and symbols may be represented in their SI-recognized forms.

[0030] As used herein, the term "about" refers, for example, to a numerical quantity that may occur relative to any quantifiable variable (including, but not limited to, mass, volume, time, temperature, length, molecular weight, density, absorption, and binding capacity) using typical measuring techniques and equipment. Furthermore, in the case of solid and liquid handling procedures used in the real world, certain unintentional errors and variations exist, which may be due to differences in the manufacture, source, or purity of the ingredients used to manufacture the composition or carry out the method, etc. The term "about" also covers these variations. Whether or not modified by the term "about," the claims contain equivalents of this quantity.

[0031] As used herein, the terms “membrane,” “felt,” and “pad” are interchangeable and refer to a nonwoven or randomly overlapped collection of fibers, optionally formed by applying additional steps to form a final composition, including, but not limited to, annealing, fusion, heating, pressing, coating, and crosslinking. The fibers forming the membrane can have any suitable diameter. In a preferred embodiment, the membrane comprises nanofibers, microfibers, or a combination of nanofibers and microfibers. The membrane can be cylindrical or substantially planar.

[0032] The term "membrane support" refers to a membrane, including cast membranes, electrospun membranes, or a combination of cast and electrospun membranes. A membrane support may include multiple membranes that can be stacked together.

[0033] As used in this article, the term "nanofiber membrane" refers to an assembly of nanofibers, which may also include microfibers added for strength, enhanced flux, and other properties.

[0034] As used in this article, the term "microfiber" refers to fibers with a diameter greater than 1.0 micrometer and typically between 1.0 micrometer and 1.0 millimeter.

[0035] As used in this article, the term "nanofiber" refers to fibers with a diameter of less than 1.0 micrometer and typically between 10 nanometers and 1.0 micrometer, such as between 200 nm and 600 nm.

[0036] As used herein, the term "hybrid nanofiber membrane" refers to a nonwoven or randomly stacked collection of fibers composed of at least two types of polymers, said polymers being a combination of single-component fibers or composite fibers with at least one other single-component fiber or at least one other composite fiber.

[0037] As used in this article, “composite nanofibers” refers to nanofibers produced from at least two different polymers.

[0038] As used in this article, the term "electrospinning" refers to applying electricity to the spinning solution to form nanofibers.

[0039] As used in this article, the term "spinning solution" refers to a polymer solution used in electrospinning processes.

[0040] As used in this article, the term “capacity” refers to the amount of product bound per unit of adsorbent.

[0041] The term "affinity chromatography" is used in this document to refer to a specific chromatographic mode in which ligands interact with a target via a locked-bond mechanism through bioaffinity. Examples of useful interactions in affinity chromatography include, for example, enzyme-substrate interactions, biotin-avidin interactions, antibody-antigen interactions, etc.

[0042] The terms “protein,” “polypeptide,” or “peptide” are used interchangeably and refer to any natural or recombinant molecule comprising amino acids linked together by peptide bonds between adjacent amino acid residues. A “peptide bond,” “peptide link,” or “amide bond” is a covalent bond formed between two amino acids when the carboxyl group of one amino acid reacts with the amino group of another amino acid. The terms “amino acid,” “amino acid residue,” and “residue” are used interchangeably herein.

[0043] As used herein, the term "nucleic acid" refers to single-stranded and / or double-stranded polynucleotides, such as deoxyribonucleic acid (DNA) and ribonucleic acid (RNA), as well as analogs or derivatives of RNA or DNA. The term "nucleic acid" also includes analogs of nucleic acids, such as peptide nucleic acids (PNA), phosphate-thioester DNA, and other such analogs and derivatives or combinations thereof.

[0044] "Vector" refers to a composition of substances comprising isolated nucleic acids and capable of delivering the isolated nucleic acids into cells. Examples of vectors include, but are not limited to, linear polynucleotides, polynucleotides associated with ionic or amphiphilic compounds, plasmids, and viruses. Therefore, the term "vector" includes autonomously replicating plasmids or viruses. The term is also interpreted as including non-plasmid and non-viral compounds that facilitate the transfer of nucleic acids into cells, such as polylysine compounds, liposomes, etc. Examples of viral vectors include, but are not limited to, adenovirus vectors, adeno-associated virus vectors, retroviral vectors, etc.

[0045] As used herein, “virus-like particle” or “VLP” refers to at least one viral particle that does not contain any nucleic acid. Therefore, VLPs can be used for vaccination or to induce an immunogenic response in an individual. However, because they lack nucleic acid, VLPs cannot replicate in host cells and are therefore non-replicating.

[0046] As used herein, the terms “lipid nanoparticles” or “LNP” are general terms used to describe lipid-based particles in the submicron range. LNPs may have structural features of liposomes and / or alternative non-bilayer types of structures. LNPs constitute an alternative to other particulate systems (e.g., emulsions, liposomes, micelles, microparticles, and / or polymeric nanoparticles) for delivering active ingredients (e.g., oligonucleotides and small molecule drugs).

[0047] As used herein, the term "exosome" refers to small secretory vesicles (typically about 30 to 150 nm) that may be contained in or already present in their membranes, nucleic acids, proteins or other biomolecules and can serve as carriers of this cargo at different locations in the body or biological system.

[0048] As used interchangeably in this document, the terms “purification,” “separating,” or “isolating” refer to increasing the purity of a molecule of interest or a target molecule from a composition or sample comprising molecules and one or more impurities.

[0049] As used interchangeably in this article, the terms "spacer molecule," "spacer arm," or "connector" refer to the element that moves the ligand away from the membrane support.

[0050] As used in this article, the term "ligand" refers to a molecule or compound that can interact with a target compound (e.g., an antibody).

[0051] As used herein, the term "sample" refers to any liquid or solid material intended for use in the methods described herein. For example, a sample may be a solution containing eukaryotic or prokaryotic cells or cellular material, or viruses or viral material, or bacteria or bacterial material, or microorganisms or pathogens. A sample may be substantially water or a buffer solution or composed of any artificially introduced chemicals, and may or may not contain nucleic acids or proteins.

[0052] As used herein, a “biological sample” means any sample obtained from a living or viral source or other macromolecular and biomolecular source, and containing any cell type or tissue from which nucleic acids or proteins or other macromolecules can be obtained. A biological sample can be a sample obtained directly from a biological source or a processed sample. For example, amplified and isolated nucleic acids constitute a biological sample. A biological sample can contain biological solid material, biological fluid, or biological tissue. Examples of biological solid material include tumors, cell spheroids, or biopsies. Examples of biological fluid include cell cultures, cell homogenates, cell suspensions in culture media, urine, blood, plasma, serum, sweat, saliva, semen, feces, sputum, cerebrospinal fluid, mouthwash, tears, mucus, sperm, amniotic fluid, etc. Biological tissue is typically an aggregate of a specific type of cells and their intercellular material, forming one of the structural materials of humans, animals, plants, bacteria, fungi, or viruses, including connective tissue, epithelial tissue, muscle, and nerve tissue. Examples of biological tissue also include organs, tumors, lymph nodes, arteries, and individual cells. The definition of biological samples also includes soil, water and other environmental samples, including industrial waste and natural water bodies (lakes, streams, rivers, oceans) that may contain viruses, bacteria, fungi, algae, protozoa and their components.

[0053] Membrane support

[0054] The affinity membrane compositions disclosed herein comprise a membrane support. The membrane support may be a cast membrane, an electrospun membrane, or a combination thereof. The membrane support comprises fibers. The fibers forming the membrane support may have any desired diameter. In a preferred embodiment, the membrane support comprises nanofibers, microfibers, or mixtures thereof. The membrane support may be made of various types of polymeric materials. In a preferred embodiment, the membrane support comprises cellulose, cellulose derivatives, non-cellulose polymers, composite nanofibers, or mixtures thereof.

[0055] In a preferred embodiment, the membrane comprises cellulose. Cellulose is a preferred substrate material for affinity membrane compositions because its extremely low nonspecific binding characteristics allow for specific interaction with target biomolecules via intended immobilized ligands, without direct interaction with the substrate material. The hydroxyl groups (-OH) in cellulose can be readily converted to other desired functionalities for coupling reactions using various surface grafting methods.

[0056] The membrane support can be prepared or obtained in a preparatory form. The membrane support can be a hybrid membrane containing cellulose and non-cellulose-based polymers. Suitable hybrid membranes and methods for their preparation are described in U.S. Patent Publication No. 2015 / 0360158, which is incorporated herein by reference in its entirety. If the membrane support is a hybrid membrane, then the hybrid membrane preferably comprises at least 30 wt.%, at least 40 wt.%, at least 50 wt.%, at least 60 wt.%, or at least 70 wt.% of cellulose-based fibers. In another embodiment, the membrane support may consist of or be substantially composed of cellulose-based fibers. The membrane support may include surface functionalization and may be further surface functionalized according to the methods described herein.

[0057] In a preferred embodiment, the majority of the hybrid membrane by mass may be derived from a cellulose-based polymer, and the incorporation of additional types of fibers within the membrane can provide the functionality required for membrane applications. Therefore, the presence of additional fibers within the membrane is desirable because it provides increased mechanical strength, allows for the incorporation of multiple functionalities into the membrane, and provides stability to the manufacturing process.

[0058] Many non-cellulose polymers have been successfully used to form membrane supports by casting or electrospinning. Non-cellulose polymers suitable for forming membrane supports include, but are not limited to, (1) thermoplastic homopolymers, such as vinyl polymers, acrylic polymers, polyamides, polyesters, polyethers, and polycarbonates; (2) thermoplastic copolymers, such as vinyl-co-vinyl polymers, acrylic-co-acrylic copolymers, and vinyl-co-acrylic polymers; (3) elastomeric polymers, such as triblock copolymer elastomers, polyurethane elastomers, and ethylene-propylene-diene elastomers; (4) high-performance polymers, such as polyimides and aromatic polyamides; (5) liquid crystal polymers, such as poly(p-phenylene terephthalamide) and polyarylamides; (6) textile polymers, such as polyethylene terephthalate and polyacrylonitrile; (7) conductive polymers, such as polyaniline; and (8) biocompatible polymers (i.e., “biopolymers”), such as polycaprolactone, polylactide, chitosan, and polyglycolic acid. As described, the fibers forming the membrane support may include one or more of these polymers, or may be copolymers of two or more of the polymer types mentioned above, and may be composite fibers including cellulose and / or cellulose derivatives and one of the aforementioned polymers.

[0059] An exemplary electrospinning process can typically be described as follows:

[0060] Step 1:The spinning solution (e.g., a polymer solution) is placed in a container with a spinneret (1), and a DC high voltage (2), typically in the range of 5 to 40 kV, is applied to the solution via electrodes (e.g., copper wires) (3). An electrically grounded current collector (4) is placed at a distance from the spinneret (referred to as the gap distance) (5). The gap distance can range from a few centimeters to one meter. When the electrostatic field reaches a critical value and the electricity overcomes the surface tension and viscoelastic force, the jet / filament is ejected and travels a straight distance (referred to as the jet length).

[0061] Step 2: The jet then begins to bend, forming helical loops. This phenomenon is known as "bending (or churning) instability." Typically, bending instability causes the jet length to elongate by more than 10,000 times within an extremely short time period (50 ms or less). Therefore, the elongation rate during bending instability is extremely high (up to 1,000,000 s). -1 This extremely fast elongation rate can effectively stretch macromolecular chains and make them closely aligned along the nanofiber axis.

[0062] Step 3: The jet solidifies either by evaporating the solvent or by cooling the melt below the solid-liquid transition temperature. The longer the solidification time, the more the jet can elongate. Solidification time is related to many factors, such as solvent vapor pressure, solvent diffusivity, the volume charge density carried by the jet, and the strength of the applied electrostatic field.

[0063] Optional electrospinning post-treatment

[0064] After the collected nanofibers have been cured, there are certain additional steps that can be performed to “customize” the nanofibers for a specific purpose. Exemplary additional steps are discussed below:

[0065] a. Heating and pressing

[0066] In a preferred embodiment, the membrane prepared from electrospun fibers can be heated and pressed together to anneal and / or fuse the fibers together.

[0067] b. Remove polymer

[0068] In some cases, composite nanofibers containing one or more polymers, particularly those comprising distinguishably removable polymers, can have one of the distinguishably removable polymers removed using higher heat and / or solvents. The removal of the distinguishably removable polymer provides additional surface area and improved porosity to the remaining polymeric fibers. This is because, after the removal of the distinguishably removable polymer, the remaining polymer has "pores" of controlled size left at the locations where the removed polymer occupied space. This additional "pore space" provides a larger surface area on the resulting membrane support, which can, for example, increase the adsorption-binding capacity of the separation, improve the selectivity of size-based separation, and improve the flux from the additional porosity.

[0069] c. Cellulose regeneration

[0070] In embodiments employing derived cellulose, after preparing “as electrospun” nanofibers, the derived cellulose can be converted into cellulose through a regeneration process. The regenerated cellulose will possess the same properties as the previously described pure natural cellulose. The regeneration process is accomplished by contacting the nanofibers containing derived cellulose with, for example, a strong alkali (e.g., sodium hydroxide) or other solvent. After the regeneration reaction to convert into cellulose, the nanofibers can be washed to remove any excess solvent used during the process.

[0071] More detailed electrospinning techniques are further disclosed in U.S. Patent No. 9,604,168, which is incorporated herein by reference in its entirety.

[0072] Surface functionalization

[0073] After preparing or obtaining the membrane support, the surface of the membrane support is functionalized. More specifically, the fiber surface is functionalized. The fiber surface can be functionalized regardless of its diameter. In a preferred embodiment, the functionalized fiber surface includes nanofibers, microfibers, or mixtures thereof.

[0074] Preferably, functionalization includes the addition of an affinity ligand, which includes, but is not limited to, viral conjugates, antibodies, enzyme substrates, and small molecule biomimetic substances. The added affinity ligand may also include monoclonal antibodies, polyclonal antibodies, antibody fragments, nucleic acids, oligonucleotides, proteins, oligopeptides, polysaccharides, oligosaccharides, sugars, peptides, antigens, aptamers, affinity molecules, small organic compounds, drugs, and other ligands. Examples of suitable affinity ligands are available in published literature and are well known. Preferably, the ligand can bind to immunoglobulins. Non-limiting examples of such ligands include protein A, protein G, and protein L.

[0075] For use in bioseparation, surface-functionalized membranes are ideally bioinert, meaning they should resist nonspecific binding to insoluble solids such as cells and cell debris, as well as unwanted interactions with proteins, sugars, nucleic acids, viruses, and other soluble components present in many bioproduction systems.

[0076] In a preferred embodiment, the surface-functionalized membrane for bioseparation exhibits one or more of the following technical features: (1) small-diameter fibers allowing for a maximum specific area; (2) good control and narrow pore size distribution among the fibers allowing for uniform flow distribution during adsorption applications; (3) fibers with excellent mechanical and chemical stability to withstand potentially high operating pressures and harsh cleaning conditions; and (4) fibers with well-defined and spatially consistent size and chemical composition. In a more preferred embodiment, the membrane support comprises cross-linked fibers. In the most preferred embodiment, the membrane support comprises cross-linked cellulose nanofibers; for example, cross-linked nanofibers as described in U.S. Patent No. 10,919,986, which is incorporated herein by reference in its entirety.

[0077] For adsorption processes where macromolecular products (e.g., proteins, nucleic acids, and viruses) are the primary targets, the large specific surface area associated with the surface-functionalized membranes described herein provides multiple potential binding sites for adsorption bioseparation. Membrane supports can be modified by adding surface functionalizations to contain multiple binding sites, and adsorption can occur on the surface of the fibers, making the binding sites immediately available without requiring internal diffusion of the target molecules. Each of the binding sites includes an affinity ligand attached via surface functionalization. In this respect, the affinity ligand is immobilized on the membrane support. When using conventional porous resin beads, internal diffusion can often limit the ability of many adsorption processes of bioproducts due to the relatively large size of the target molecules. Furthermore, because membrane supports can be made from many different polymer- and cellulose-based fibers, adsorption ligands can be tailored to meet specific separation needs.

[0078] The surface-functionalized affinity membranes described herein offer improvements over conventional resin bead separation techniques. Two of these improvements are (1) flow through the micropores and macropores of the membrane support (as opposed to tightly packed resin beads), and (2) adsorption occurring on the surface of the fibers, where internal diffusion is not required. These factors reduce the problem of high pressure drop at high flow rates and eliminate the slow intraparticle diffusion required for adsorption within resin beads. We have found that the binding capacity of biomolecules to surface-functionalized affinity membranes is quantitatively similar to that of resin beads, but can be operated at processing flow rates more than 10 times faster than packed beds. These factors allow for much faster processing times and potentially higher binding levels for the purification of valuable bioproducts. This is highly desirable, especially for large biomolecules (molecular weights greater than 100 kDa and / or hydrodynamic diameters of 20 to 300 nm), which are difficult to purify using packed beds due to the limited mass transfer within the small pores of resin beads.

[0079] Coupling chemicals

[0080] Various types of chemicals can be used to permanently bind desired ligands to the surface of membrane supports. The choice of reactive chemicals must be carefully considered to ensure the absence of interfering side reactions under chromatographic conditions. For example, if the purified molecules are eluted under high salt concentration variations, salt-resistant ligands and coupling chemicals should be selected to maintain the reusability of the culture medium. Since almost all protein or peptide molecules can be immobilized via amine coupling, reactive functional groups that can be coupled to amine-containing molecules are preferred. Examples of common functional groups used in amine coupling processes are shown in […]. Figure 1 middle.

[0081] Amine reactive functional groups include, but are not limited to, isothiocyanates, isocyanates, acyl azides, NHS esters, sulfonyl-NHS esters, acyl chlorides (e.g., sulfonyl chlorides), aldehydes and glyoxal, epoxides and ethylene oxides, carbonates, carbamates, aryl halides, alkyl halides, imine esters, carbodiimides, acid anhydrides, fluorophenyl esters, triazines, and combinations thereof. These functional groups can be attached directly to the surface of the membrane support by attaching to the surface of the fibers constituting the membrane, or they can be part of the spacer molecules.

[0082] As an example, epoxides or ethylene oxide groups react with primary amine nucleophiles during ring-opening, producing secondary amines containing β-hydroxyl groups on the epoxide, thus anchoring it to the membrane. This process is readily carried out at moderately alkaline pH values, typically in the range of 8 to 10. Under the assumption that the immobilized protein or ligand is stable under these conditions, higher pH values ​​can be used to accelerate the coupling process and improve coupling efficiency. The main side reaction occurring with the epoxide group is the hydrolysis of the epoxide ring, which is more readily observed at lower pH values, resulting in the formation of adjacent hydroxyl groups. In media such as agarose and cellulose, for example, hydroxyl groups on the membrane surface can be activated with epichlorohydrin under slightly higher temperatures and strongly alkaline conditions to generate functional epoxide groups.

[0083] In another example, carboxylic acids can be converted into activated esters for coupling with nucleophilic primary amines to produce secondary amides. Most commonly, this activation is used to produce N-hydroxysuccinimide (NHS) esters via carbodiimide and NHS or disuccinimide carbonate (DSC). This ester is then used to immobilize biomolecules (e.g., enzymes) on a support for purification and reaction by exchanging the NHS of the activated carboxylic acid-NHS ester with any free nucleophilic amine to form an amide bond. This method is useful because it readily occurs at physiological pH 8.6 or lower, due to the much slower hydrolysis of NHS and therefore higher coupling yields below this pH. NHS coupling is also buffer-dependent. The activated esters produced prior to coupling can be used immediately or stored under cool, anhydrous conditions, making them highly useful for activation. Additional chemicals for activating functional groups are described in U.S. Patent No. 8,114,611, which is incorporated herein by reference in its entirety.

[0084] The surface of the membrane support can be functionalized with reactive functional groups to immobilize affinity ligands, and functionalized with inert functional groups to improve the efficiency of ligand immobilization and reduce the possibility of steric hindrance at the binding site. For demonstration purposes, Figure 2C Non-limiting examples illustrating this situation are presented. In this regard, the surface of the membrane support is bifunctionalized with inert functional groups and binding sites, the binding sites being reactive functional groups that react to attach an exemplary affinity ligand protein A. The inert functional groups can be selected based on the affinity ligand chosen for a particular application; specifically, the inert groups can be selected based on their non-reactivity with the functionality required to attach a particular affinity ligand. For example, an epoxide ring reacts with an amine functional group and is therefore a reactive group in some embodiments; however, in embodiments where the reactive group does not react with the epoxide, the epoxide can be used as an inert group.

[0085] As described herein, combinations of amine functional groups can be used to permanently immobilize biomolecular ligands onto the surface of nanofibers in membrane compositions. Additionally, these amine functional groups can be combined with ion-exchange functional groups. In one example, some of the hydroxyl groups on the membrane surface can be activated with 3-chloro-2-hydroxypropyltrimethylammonium chloride (CHPTAC), resulting in the introduction of quaternary ammonium cations for anion exchange separation. The use of CHPTAC is particularly advantageous because it results in a net change of zero with respect to the hydroxyl groups on the surface. Any remaining hydroxyl groups can then be activated with bis(ethylene oxide), such as 1,4-butanediol diglycidyl ether, resulting in the introduction of epoxide groups for covalent ligand immobilization. The end result is a bifunctionalized membrane support with both active coupling functionality (ligand affinity) and inert coupling functionality, which prevent steric hindrance at binding sites and reduce or eliminate inefficient use of immobilized ligands. This bifunctional membrane support may include quaternary ammonium ions, which serve as strong attracting centers to bring biomolecular ligands very close to the epoxide group, thus enabling them to be covalently immobilized.

[0086] In another example, some of the hydroxyl groups on the membrane surface can be activated with sodium 3-chloro-2-hydroxypropanesulfonate (CHPSAS), resulting in the introduction of sulfonic acid groups for cation exchange separation. Similarly, as previously described, the result is a net change of zero in the number of hydroxyl groups on the surface. Any remaining hydroxyl groups can then be activated with bis(ethylene oxide), such as 1,4-butanediol diglycidyl ether, resulting in the introduction of epoxide groups for covalent ligand immobilization. The end result is a bifunctionalized material with sulfonic acid groups that use strong attracting centers to bring biomolecular ligands very close to the epoxide groups, thus enabling covalent immobilization. Therefore, any ligand that can be affected by anionic or cation attracting centers may potentially benefit from immobilization with a bifunctionalized surface. This bifunctionalization can be extended to any amine functional group, cationic or anionic group, and combinations thereof. The advantage of this is that the ligand density and the spacing between ligands can be more specifically controlled and customized.

[0087] Activator density

[0088] The activation density can be determined depending on the type of chemical substance applied to the nanofiber membrane. Activation density refers to the amount of activator covalently bonded to each gram of membrane material. For example, in the case of activating the membrane with epoxide groups, the activation density can be expressed as the number of moles of epoxide groups per gram of membrane material. Determining the activation density is an important parameter because it provides an indication of the maximum achievable binding capacity of the material. After applying the chemical substance and thus activating the material, the theoretical binding capacity will never exceed the activation density. Due to steric hindrance and molecular interactions, efficiency losses always occur between activation and coupling, and between coupling and static / dynamic binding. Figure 2AThe simplified example shown illustrates this loss of site density during the ligand coupling step. Due to these complex molecular interactions, it may be necessary to decrease or increase the activation density to achieve a higher overall binding capacity in nanofiber membranes.

[0089] Coupling ligand density

[0090] Another parameter to consider is the amount of ligands immobilized on the surface of the culture medium, or more precisely, the density. For example... Figure 2B The example shown presents a simplified illustration of the effect of ligand concentration on IgG binding, assuming only one IgG molecule binds to each protein A (ProtA) molecule. It should be understood that, in contrast, theoretically there are four potential IgG binding sites per fixed protein A molecule. However, the effective number of binding sites may be less than four, due to steric and repulsive interactions preventing IgG from approaching and thus binding affinityably due to overcrowded surfaces. Nevertheless, Figure 2B This example demonstrates that although five protein A molecules are present, and therefore five potential binding sites, only three IgG molecules are able to bind to the surface. This results in a loss of protein A utilization on the culture medium surface, and consequently, higher costs due to the relatively high price of protein A. Therefore, the efficiency of protein A utilization can be optimized by varying the ligand density on the culture medium surface while maintaining IgG binding capacity.

[0091] The benefit of this disclosure is that it provides a mechanism for improving efficiency by customizing surface functionalization to avoid steric hindrance and repulsive interactions. Two mechanisms exist for achieving this. First, the membrane support can be surface-functionalized with bifunctionality as previously described, i.e., by attaching active binding functionalization (which binds and immobilizes affinity ligands) and inert functionality to avoid steric hindrance and unwanted ligand binding. Second, the surface can be customized to include spacer arms of a defined length to avoid steric hindrance. Both mechanisms can be used together on the same membrane support. Advantageously, any one or both of these mechanisms can be used to increase ligand binding efficiency by customizing surface functionalization to reduce the probability of steric hindrance and avoid binding of ligands that are not used due to steric hindrance.

[0092] The ligand can be present at densities from about 10 mg / g to about 1000 mg / g. Examples provide densities from about 10 mg / g to about 100 mg / g, from about 10 mg / g to about 200 mg / g, from about 10 mg / g to about 250 mg / g, from about 10 mg / g to about 300 mg / g, from about 10 mg / g to about 400 mg / g, from about 10 mg / g to about 500 mg / g, from about 10 mg / g to about 600 mg / g, from about 10 mg / g to about 700 mg / g, from about 10 mg / g to about 750 mg / g, from about 10 mg / g to about 800 mg / g, from about 10 mg / g to about 900 mg / g, from about 50 mg / g to about 100 mg / g, from about 50 mg / g to about 200 mg / g, and from about 50 mg / g to about 250 mg / g. mg / g, approximately 50 mg / g to approximately 300 mg / g, approximately 50 mg / g to approximately 400 mg / g, approximately 50 mg / g to approximately 500 mg / g, approximately 50 mg / g to approximately 600 mg / g, approximately 50 mg / g to approximately 700 mg / g, approximately 50 mg / g to approximately 750 mg / g, approximately 50 mg / g to approximately 800 mg / g, approximately 50 mg / g to approximately 900 mg / g, approximately 50 mg / g to approximately 1000 mg / g, approximately 100 mg / g to approximately 200 mg / g, approximately 100 mg / g to approximately 250 mg / g, approximately 100 mg / g to approximately 300 mg / g, approximately 100 mg / g to approximately 400 mg / g, approximately 100 mg / g to Approximately 500 mg / g, approximately 100 mg / g to approximately 600 mg / g, approximately 100 mg / g to approximately 700 mg / g, approximately 100 mg / g to approximately 750 mg / g, approximately 100 mg / g to approximately 800 mg / g, approximately 100 mg / g to approximately 900 mg / g, approximately 100 mg / g to approximately 1000 mg / g, approximately 200 mg / g to approximately 250 mg / g, approximately 200 mg / g to approximately 300 mg / g, approximately 200 mg / g to approximately 400 mg / g, approximately 200 mg / g to approximately 500 mg / g, approximately 200 mg / g to approximately 600 mg / g, approximately 200 mg / g to approximately 700 mg / g, approximately 200 mg / g to approximately 750 mg / g g / g, approximately 200 mg / g to approximately 800 mg / g, approximately 200 mg / g to approximately 900 mg / g, approximately 200 mg / g to approximately 1000 mg / g, approximately 250 mg / g to approximately 300 mg / g, approximately 250 mg / g to approximately 400 mg / g, approximately 250 mg / g to approximately 500 mg / g, approximately 250 mg / g to approximately 600 mg / g, approximately 250 mg / g to approximately 700 mg / g, approximately 250 mg / g to approximately 750 mg / g, approximately 250 mg / g to approximately 800 mg / g, approximately 250 mg / g to approximately 900 mg / g, approximately 250 mg / g to approximately 1000 mg / g, approximately 300 mg / g to approximately 400 mg / g,Approximately 300 mg / g to approximately 500 mg / g, approximately 300 mg / g to approximately 600 mg / g, approximately 300 mg / g to approximately 700 mg / g, approximately 300 mg / g to approximately 750 mg / g, approximately 300 mg / g to approximately 800 mg / g, approximately 300 mg / g to approximately 900 mg / g, approximately 300 mg / g to approximately 1000 mg / g, approximately 400 mg / g to approximately 500 mg / g, approximately 400 mg / g to approximately 600 mg / g g, approximately 400 mg / g to approximately 700 mg / g, approximately 400 mg / g to approximately 750 mg / g, approximately 400 mg / g to approximately 800 mg / g, approximately 400 mg / g to approximately 900 mg / g, approximately 400 mg / g to approximately 1000 mg / g, approximately 500 mg / g to approximately 600 mg / g, approximately 500 mg / g to approximately 700 mg / g, approximately 500 mg / g to approximately 750 mg / g, approximately 500 mg / g to approximately 800 mg / g, approximately 500mg / g to approximately 900mg / g, approximately 500mg / g to approximately 1000mg / g, approximately 600mg / g to approximately 700mg / g, approximately 600mg / g to approximately 750mg / g, approximately 600mg / g to approximately 800mg / g, approximately 600mg / g to approximately 900mg / g, approximately 600mg / g to approximately 1000mg / g, approximately 700mg / g to approximately 750mg / g, approximately 700mg / g to approximately 800mg / g Ligands present at densities of 0 mg / g, approximately 700 mg / g to approximately 900 mg / g, approximately 700 mg / g to approximately 1000 mg / g, approximately 750 mg / g to approximately 800 mg / g, approximately 750 mg / g to approximately 900 mg / g, approximately 750 mg / g to approximately 1000 mg / g, approximately 800 mg / g to approximately 900 mg / g, approximately 800 mg / g to approximately 1000 mg / g, or approximately 900 mg / g to approximately 1000 mg / g. Examples provide ligands that can be present at densities of about 10 mg / g, about 50 mg / g, about 100 mg / g, about 200 mg / g, about 250 mg / g, about 300 mg / g, about 400 mg / g, about 500 mg / g, about 600 mg / g, about 700 mg / g, about 750 mg / g, about 800 mg / g, about 900 mg / g, or about 1000 mg / g.

[0093] Spacer molecule (spacer arm)

[0094] One option for enhancing ligand immobilization is to introduce spacer molecules between the nanofiber membrane and the affinity ligands. By introducing multiple spacer molecules onto the surface of the membrane support, steric hindrance between the matrix and the immobilized ligands, as well as the adsorbate, can be reduced or even eliminated. For example, both protein A and IgG are very large biomolecules and therefore can have significant amounts of steric hindrance, limiting their access to the matrix during both protein A immobilization and IgG dynamic binding. Additionally, high ligand density can limit adsorption density, as steric hindrance blocks potential active sites on ligand molecules that are very close to each other. Introducing long spacer molecules can also indirectly reduce ligand density. Reduced steric hindrance from both the ligands and the matrix allows for easier access to IgG molecules during dynamic binding, resulting in increased adsorption capacity.

[0095] The chemical composition of the spacer arm can significantly influence affinity chromatography, depending on the support, immobilized ligand, and binding target. This influence can be multifaceted, attributing not only to hydrophobic and hydrophilic interactions but also to specific associative bonds from other side chains. Figure 3 Examples of incorporating hydrocarbon spacer molecules for subsequent activation with carboxylic acids are shown. The incorporation of hydrophilic spacer molecules prevents nonspecific hydrophobic side-chain bonding between the support, spacer, ligand, and target, which promotes positive or negative bonding effects on the membrane. The hydrophilic effect can be achieved by incorporating electronegative atoms into the spacer arms, as seen in the PEG example. Figure 4 To maximize the affinity binding effect relative to hydrophobic or hydrophilic binding, the buffer ion concentration should be evaluated to maximize the affinity binding between protein A and IgG.

[0096] Each spacer arm has a terminal portion containing either a reactive or inert functional group. The reactive functional group can react to bind an affinity ligand. In this regard, the affinity ligand may be located at the terminal portion. The spacer arm is typically a straight chain of carbon, oxygen, and nitrogen atoms. The spacer arm may comprise a branched chain, an unbranched chain, or a cyclic chain. The composition may comprise hydrophilic spacer arms, hydrophobic spacer arms, or a combination of hydrophilic and hydrophobic spacer arms. Preferably, the spacer arms have lengths between 1 and 100 atoms, between 1 and 90 atoms, between 1 and 80 atoms, between 1 and 70 atoms, between 1 and 60 atoms, and between 1 and 50 atoms. The embodiments provide spacer arms having lengths between 1 and 5 atoms, between 1 and 10 atoms, between 1 and 15 atoms, between 1 and 20 atoms, between 1 and 25 atoms, between 5 and 10 atoms, between 5 and 15 atoms, between 5 and 20 atoms, between 5 and 25 atoms, between 5 and 30 atoms, between 10 and 15 atoms, between 10 and 20 atoms, between 10 and 25 atoms, between 10 and 30 atoms, between 15 and 20 atoms, between 15 and 25 atoms, between 15 and 30 atoms, between 20 and 25 atoms, between 20 and 30 atoms, or between 25 and 30 atoms. The embodiments provide spacer arms with lengths of 1 atom, 2 atoms, 3 atoms, 4 atoms, 5 atoms, 6 atoms, 7 atoms, 8 atoms, 9 atoms, 10 atoms, 11 atoms, 12 atoms, 13 atoms, 14 atoms, 15 atoms, 16 atoms, 17 atoms, 18 atoms, 19 atoms, 20 atoms, 21 atoms, 22 atoms, 23 atoms, 24 atoms, 25 atoms, 26 atoms, 27 atoms, 28 atoms, 29 atoms, or 30 atoms.

[0097] Customize all parameters for specific ligand applications

[0098] Coupling chemicals, ligand density, spacer molecule type, and spacer molecule length can all be simultaneously combined and optimized to maximize ligand utilization efficiency and the dynamic binding capacity of the target of interest during affinity chromatography. Each of these parameters independently affects process performance, and when combined, they lead to greater overall utilization and performance of the adsorption medium.

[0099] Surfaces with multiple spacer lengths can exhibit greater dynamic binding capacity for targets of interest than surfaces with only one type of spacer length, because spaced ligands may result in greater availability of active sites for ligand binding. Examples of this concept are found in… Figure 5 Protein A is used as an exemplary ligand in the example shown.

[0100] Figure 5This study presents a possible surface combination with varying ligand densities and multiple spacer molecule lengths, as well as some hydroxyl groups that are activated in the absence of spacer molecules. It should be noted that this is merely one of many possible combinations that can arise when attempting to maximize the dynamic binding efficiency of IgG and protein A. For example, multiple different chemicals, such as NHS esters and epoxide groups, can be used in parallel when activating the membrane. Alternatively, only one type of activating chemical may be present, but with multiple different linker lengths and types. An example of this would involve activating the hydroxyl groups on the cellulose matrix with both hydrophobic and hydrophilic biepoxide spacer molecules (each with different spacer arm lengths). For each of these cases, an optimal ligand density can also be determined to further optimize performance.

[0101] Membrane-based methods

[0102] Surface-functionalized affinity membranes can be used to separate a target of interest from a sample by contacting the composition, including the target of interest, with the sample to adsorb the target of interest. The method may further include contacting the composition with an eluent to release and recover the target of interest. The target of interest may comprise any molecule that specifically binds to a selected ligand. The target molecule may be a protein or nucleic acid molecule, including a carrier, viral vector, or virus. In some embodiments, the target molecule is an immunoglobulin, such as immunoglobulin G (IgG). The target of interest may also comprise any nanoparticles that specifically bind to a selected ligand. Target nanoparticles may comprise encapsulated nanoparticles, lipid nanoparticles, virus-like particles, and / or extracellular bodies.

[0103] Nucleic acids can be in the form of deoxyribonucleic acid (DNA), ribonucleic acid (RNA), or peptide nucleic acid (PNA), as well as analogs, derivatives, or any combination thereof. Such derivatives may contain, for example, nucleotide analogs or "backbone" bonds other than phosphodiester bonds, such as phosphotriester bonds, aminophosphate bonds, thiophosphate bonds, or thioester bonds. Naturally occurring RNA molecules include, but are not limited to, transfer RNA (tRNA), ribosomal RNA (rRNA), messenger RNA (mRNA), or genomic RNA, such as RNA from influenza or hepatitis C viruses. Other forms of RNA include, but are not limited to, small interfering RNA (siRNA) and microRNA (miRNA). Nucleic acid molecules can be single-stranded (ss; and they can be sense or antisense), double-stranded (ds), or a combination of both, and can be linear or circular, wherein the latter can be open or closed circular.

[0104] Nucleic acid molecules can serve as vectors. The vector can be a viral vector, preferably a lentiviral vector, adenovirus vector, adeno-associated virus (AAV) vector, vesicular stomatitis virus (VSV) vector, herpes simplex virus (HSV) vector, vaccinia virus vector, poxvirus vector, influenza virus vector, respiratory syncytial virus vector, parainfluenza virus vector, foamy virus vector, or retroviral vector.

[0105] In aspects of the invention, compared to previously described methods, the composition can provide enhanced binding capacity of the target molecule, such as static and dynamic capacity. The composition may have a static binding capacity between about 10 mg / g and about 200 mg / g by weight, preferably between about 60 mg / g and about 100 mg / g.

[0106] Example

[0107] Preferred embodiments of this disclosure are further illustrated in the following non-limiting examples. It should be understood that these examples, while indicating certain preferred embodiments, are given only by way of illustration. Based on the foregoing discussion and these examples, those skilled in the art can determine the essential features of the invention, and various changes and modifications can be made to the embodiments of the invention to adapt it to different uses and conditions without departing from its spirit and scope. Therefore, various modifications to the embodiments of the invention, in addition to those shown and described herein, will be apparent to those skilled in the art based on the foregoing description. Such modifications are also intended to fall within the scope of the appended claims.

[0108] Ligand-functionalized membranes were produced according to the methods described herein, and various factors were evaluated. These factors included protein A coupling, dynamic binding, and static binding. Coupling was evaluated by BCA or Bradford assays, in which the initial concentration was compared to the remaining concentration to determine the amount of ligand bound.

[0109] To evaluate performance, GE Akta Pure 150 was used. The equilibration buffer used was 0.1 M sodium phosphate pH 7.0, 0.1 M sodium phosphate pH 7.0 for binding 1 mg / ml human IgG, and 0.1 M glycine pH 2.5 for elution. To calculate IgG binding, the elution peak was integrated and the total amount bound was calculated. Static capacity was measured by shaking the sample in a known solution of 1 mg / ml human IgG in 0.1 M sodium phosphate pH 7.0 for 24 hours, using the Bradford IgG Residual Control, a known standard.

[0110] Example 1: Functionality of Epoxides

[0111] Epoxide coupling without spacer molecules, epichlorohydrin, and protein A

[0112] Epoxide activation of hybrid cellulose nanofiber membranes was performed using epichlorohydrin as follows: 15 mL of 1M NaOH was preheated to 60 °C in a hot water bath. 0.0255 g of the hybrid cellulose nanofiber membrane material was immersed in the pre-prepared solution and placed on an air-heated rotary shaker at 60 °C. After immersion for 15 minutes, 1.5 mL of epichlorohydrin (Epi.) was added, and the reaction was carried out at 60 °C with vigorous shaking (>100 rpm) for 4 hours. The membrane material was then washed with reverse osmosis (RO) H₂O for a sufficient amount of time (>30 min). The maximum potential epoxide groups were estimated based on the amount of activator used.

[0113] Epoxide-activated cellulose nanofiber membrane material was coupled to protein A using the following method: A coupling buffer consisting of 1 M ammonium sulfonate and 0.1 M sodium carbonate, pH 8.75, was prepared and adjusted using HCl. The membrane material was added to 900 μL of the coupling buffer and 100 μL of 50 mg / mL protein A (Repligen). The membrane was shaken at room temperature (>100 rpm) for 24 hours. After coupling, unreacted epoxide groups were blocked using a 1 M ethanolamine solution adjusted to pH 9 with HCl. The final amount of protein A in solution was determined using a Pierce BCA protein assay kit (Thermo Fischer Scientific) with protein A as a standard curve. The maximum amount of protein A coupled to the membrane material was considered as the difference between the initial and final protein concentrations added.

[0114] Contains spacer molecules, poly(ethylene glycol) diglycidyl ether (average M n =500) and epoxide coupling of protein A

[0115] Epoxide activation of hybrid cellulose nanofiber membranes using epichlorohydrin was performed as follows: 15 mL of 1M NaOH was prepared. 0.0264 g of the hybrid cellulose nanofiber membrane material was immersed in the previous solution and placed on a rotary shaker at room temperature. After immersion for 15 minutes, 187.5 μL of poly(ethylene glycol) diglycidyl ether (PEG-500) with an average molecular weight of 500 was added, and the reaction was carried out with vigorous shaking (>100 rpm) at room temperature for 4 hours. The membrane material was then washed with RO H2O for a sufficient amount of time (>30 min). The maximum potential epoxide groups were estimated based on the amount of activator used.

[0116] Epoxide-activated cellulose nanofiber membrane material was coupled to protein A according to the following method: A coupling buffer consisting of 1 M ammonium sulfonate and 0.1 M sodium carbonate, pH 8.75, was prepared and adjusted with HCl. The membrane material was added to 900 μL of the coupling buffer and 100 μL of 50 mg / mL protein A (Repligen). The membrane was shaken at room temperature (>100 rpm) for 24 hours. After coupling, unreacted epoxide groups were blocked using a 1 M ethanolamine solution adjusted to pH 9 with HCl. The final amount of protein A in the solution was determined using a Pierce BCA protein assay kit (Thermo Fischer Scientific) with protein A as a standard curve. The maximum amount of protein A coupled to the membrane material was considered as the difference between the initial and final protein concentrations. Table 1 summarizes the epoxide-protein A coupling results.

[0117] Contains spacer molecules, poly(ethylene glycol) diglycidyl ether (average M n =2000) and epoxide coupling of protein A

[0118] Epoxide activation of hybrid cellulose nanofiber membranes was performed using epichlorohydrin as follows: 0.1681 g of poly(ethylene glycol) diglycidyl ether (PEG-2000) with an average molecular weight of 2000 was completely dissolved in 15 mL of 1 M NaOH. 0.0268 g of the hybrid cellulose nanofiber membrane material was immersed in the previous solution and placed on a rotary shaker, where it was vigorously shaken (>100 rpm) at room temperature for 4 hours. The membrane material was then washed with RO H₂O for a sufficient amount of time (>30 min). The maximum potential epoxide groups were estimated based on the amount of activator used.

[0119] Epoxide-activated cellulose nanofiber membrane material was coupled to protein A according to the following method: A coupling buffer consisting of 1 M ammonium sulfonate and 0.1 M sodium carbonate, pH 8.75, was prepared and adjusted with HCl. The membrane material was added to 900 μL of the coupling buffer and 100 μL of 50 mg / mL protein A (Repligen). The membrane was shaken at room temperature (>100 rpm) for 24 hours. After coupling, unreacted epoxide groups were blocked using a 1 M ethanolamine solution adjusted to pH 9 with HCl. The final amount of protein A in the solution was determined using a Pierce BCA protein assay kit (Thermo Fischer Scientific) with protein A as a standard curve. The maximum amount of protein A coupled to the membrane material was considered as the difference between the initial and final protein concentrations. Table 1 summarizes the epoxide-protein A coupling results.

[0120] Table 1

[0121]

[0122]

[0123] The static binding capacity of IgG to protein A-conjugated cellulose nanofiber membranes was determined using the following method: A solution of 1 mg / mL IgG in 0.1 M NaHPO4 was prepared at pH 7. The protein A-conjugated cellulose nanofibers were placed in 2 mL of the previously mentioned solution and incubated overnight on a rotary shaker (>100 rpm). Using IgG as a standard curve, the IgG concentration in the solution was determined using a Bradford protein assay (Sigma-Aldrich). The maximum amount of IgG bound to the membrane material was considered the difference between the initial and final IgG concentrations. Dynamic binding properties were determined using the method previously mentioned above. The results of static and dynamic binding of IgG to epoxide-activated protein A-conjugated cellulose nanofiber membranes are summarized in Table 2 below.

[0124] Table 2

[0125]

[0126] The results shown in Table 1 illustrate the effects of functional group density and spacer arm length on the amount of protein A that can be immobilized onto the matrix. The first row indicates epoxide groups without active binding sites, the third row uses PEG-500 as a spacer arm, and the fourth row uses PEG-2000 as a longer spacer arm. Experimentally, the maximum potential molar number of epoxide groups added to the surface decreases with increasing spacer length, thus altering both parameters simultaneously. Although the potential molar number of epoxides coupled to protein A is small, the amount of protein A coupled to the membrane increases with increasing spacer arm length.

[0127] Figure 6 This study demonstrates the effect of different spacer molecule lengths on the efficiency of protein A immobilization. For both static and dynamic conditions, the results show that increasing the spacer molecule length leads to greater utilization of protein A.

[0128] Table 2 and Figure 7This study demonstrates the effect of increasing the length of the spacer molecule on the static and dynamic binding capacity of IgG. Results show that introducing the spacer molecule increased dynamic binding from 2.60 mg / mL to 3.74 mg / mL, and increasing the length of the spacer molecule increased dynamic binding from 3.74 mg / mL to 4.29 mg / mL. These results are supported by the fact that the elution peak height and integrated area increased accordingly with increasing spacer molecule length. Similarly, for static binding, introducing the spacer molecule increased binding from 6.46 mg / mL to 14.43 mg / mL, and increasing the length of the spacer molecule increased binding from 14.43 mg / mL to 15.81 mg / mL.

[0129] Example 2: NHS Functionality

[0130] To investigate the conjugation of nanofiber membranes, cellulose nanofibers were reacted with haloalkanoic acids of various lengths in a caustic alkaline solution. In this case, the haloalkanoic acids comprised monochloroacetic acid (MCA), bromohexanoic acid (BrHex), bromoundecanoic acid (uBr), and combinations of one-third of each of those reacting onto the nanofiber surface. The membrane was pre-soaked in 0.4 L / g membrane at 60 °C in 1.2 M NaOH for 15 min, followed by the addition of a 0.7 mol / L haloalkanoic acid solution and vigorous shaking to dissolve. The reaction was then reheated at 60 °C with shaking for 4 h, the reactants were washed, and stored in RO water. This resulted in the grafting of various haloalkanoic acids onto cellulose nanofibers of different lengths via ether bonds. The capacity and flow conditions of the resulting membranes were characterized based on the lysozyme cation exchange (CEX) capacity at pH 7 in 20 mM sodium phosphate. Furthermore, these were coupled with protein A to determine the effect of different spacer arm lengths on IgG retention capacity.

[0131] The CEX membrane was then activated using disuccinimide carbonate (DSC), triethylamine (TEA), and acetonitrile. First, the membrane was washed with 0.3M HCl, repeatedly rinsed with RO water, and then dehydrated using acetone / water mixtures of 25:75, 50:50, and 75:25, followed by two 15-minute washes with pure water to ensure complete dehydration. Next, the membrane was added to a mixture of 167 ml anhydrous acetonitrile and 83.5 ml TEA per gram of membrane (dry basis) and activated with 54 g DSC / L acetonitrile under shaking. This activation was performed for 12 hours. The membrane was then washed clean and stored in isopropanol (IPA) at 4°C. To check the activation, a coin-sized amount was removed from the IPA, rinsed with ice-cold 1 mM HCl, and shaken in 20 mM Tris buffer at pH 9. UV 280 nm was used to estimate the amount of NHS bound per gram of membrane material.

[0132] For coupling, 0.1M sodium bicarbonate and 0.5M NaCl buffer were mixed into Repligen rSPA protein A to produce a pH 7.8 solution of 50 mg / ml protein A. The activated membrane of a small test coin was washed with ice-cold 1mM HCl to remove IPA, and then placed in 33.3 ml of protein A solution / g membrane, using approximately 0.01 g of membrane per sample, with 3 samples per type of membrane. The membrane was incubated at 4°C with shaking for 12 hours. Afterward, the membrane was removed from the solution and washed with water. This was followed by shaking with 20 mM Tris 1.0M NaCl pH 9 for 4 hours to check for adsorbed protein A.

[0133] Table 3 summarizes the NHS-protein A coupling results. The results indicate that the amount of protein A attached via NHS chemicals decreases with increasing linker length, despite increased membrane activation (MCA for the shortest spacer arm length and Ubr for the longest spacer arm length). Note that the amount of protein A attached in the composite samples is slightly increased due to the presence of a certain proportion of short-additive agents. Figure 8 This effect is further illustrated below. It is expected to have an adverse impact on the final IgG binding performance.

[0134] Table 3

[0135]

[0136] The longer linker length in the hydrophobic spacer arm can also be shown to affect the effectiveness of protein A binding to IgG. Figure 9 This demonstrates how a longer linker length increases the binding efficiency of protein A to IgG. As the linker length changes from 2 carbon atoms to 11 carbon atoms, the efficiency of protein A binding to IgG (mg / mg) increases from 3.4% to 8.3% for dynamic binding and from 6.3% to 16.4% for static binding. This can be attributed to any number of factors, including hydrophobic chemicals in the spacer arms, reduced density of binding sites, or reduced steric hindrance to protein A-IgG binding due to the increased linker length moving the binding further away from the support matrix.

[0137] Table 4 summarizes the static and dynamic IgG binding on the NHS-protein A coupled membrane. Table 4 and Figure 10 The study demonstrates the effect of increasing linker length on binding capacity. It should be noted that the lowest protein A load with the longest linker exhibits the highest capacity, with 78 mg / g static and 40 mg / g dynamic capacity. This is likely attributable to both the ligand density effect and the linker length.

[0138] Table 4

[0139]

[0140] The foregoing examples demonstrate that affinity ligands can be immobilized on the surface of a membrane support through surface functionalization. Furthermore, it has been shown that the length of the spacer arms can be customized to avoid steric hindrance, and that bifunctionalization can be utilized on the surface of the membrane support to improve binding efficiency. By customizing surface functionalization, optimal conditions can be achieved for specific affinity ligands and their targets of interest to maximize effective ligand density, ligand binding efficiency, and avoid steric hindrance. Although protein A is typically used as the affinity ligand in the foregoing examples, the present invention is by no means limited to the use of protein A; in fact, the use of protein A is only for consistency and illustrative purposes between examples. The teachings provided in this disclosure can be applied to a variety of affinity ligands to separate a variety of targets of interest.

[0141] Having been described thus, it will be apparent that the invention can be varied in many ways. Such variations will not be considered as departing from the spirit and scope of the invention, and all such modifications are intended to be included within the scope of the following claims. The foregoing description provides a description of the manufacture and use of the disclosed compositions and methods. Since many embodiments can be made without departing from the spirit and scope of the invention, the invention is attributed to the claims.

Claims

1. An affinity membrane comprising: Membrane support; The membrane support is a cast membrane support, an electrospun membrane support, or a combination thereof; Multiple linear spacer arms are fixed to the membrane support; each linear spacer arm includes an end; and A ligand coupled to the terminal, wherein the ligand is bound to the membrane support via the straight-chain spacer arm; The ligands are present on the membrane support at a density of 10 mg / g to 1000 mg / g; The straight-chain spacer arm has a length between 5 and 30 atoms.

2. The membrane according to claim 1, wherein the membrane support comprises nanofibers, microfibers, or a combination thereof.

3. The membrane according to claim 1 or 2, wherein the membrane support is an electrospun membrane support.

4. The membrane according to claim 1 or 2, wherein the membrane support further comprises one or more inert functional groups fixed to the surface of the membrane support.

5. The membrane according to claim 1 or 2, wherein the plurality of straight-chain spacer arms comprises straight-chain spacer arms of different lengths.

6. The membrane according to claim 1 or 2, wherein the ligand is coupled to the end of the linear spacer arm via a reacted amine functional group.

7. The membrane according to claim 2, wherein the membrane support comprises nanofibers and the nanofibers comprise cellulose.

8. The membrane of claim 2, wherein the membrane support comprises nanofibers and the nanofibers comprise a non-cellulose polymer.

9. The membrane according to claim 1 or 2, wherein the linear spacer arms are hydrophilic.

10. The membrane according to claim 1 or 2, wherein the linear spacer arms are hydrophobic.

11. The membrane according to claim 1 or 2, wherein the affinity membrane composition further comprises a cation exchange group or an anion exchange group.

12. The membrane according to claim 1 or 2, wherein the ligand is a peptide.

13. The membrane according to claim 12, wherein the peptide is protein A, protein G, or protein L.

14. The membrane according to claim 1 or 2, wherein the ligand is capable of binding protein or nucleic acid molecules.

15. The membrane according to claim 1 or 2, wherein the ligand is capable of binding DNA molecules, RNA molecules, vectors, viruses, or immunoglobulins.

16. The membrane of claim 15, wherein the ligand is capable of binding a viral vector.

17. A method for preparing a surface-functionalized affinity film, the method comprising: Provide membrane support; The membrane support is a cast membrane support, an electrospun membrane support, or a combination thereof; A plurality of linear spacer arms are fixed to the membrane support, wherein each linear spacer arm includes an end; and The ligand is coupled to the end of the linear spacer arm via a reactive functional group; The ligands are present on the membrane support at a density of 10 mg / g to 1000 mg / g; The straight-chain spacer arm has a length between 5 and 30 atoms.

18. The method of claim 17, wherein the membrane support comprises nanofibers, microfibers, or a combination thereof.

19. The method according to claim 17 or 18, wherein the membrane support is an electrospun membrane support.

20. The method according to claim 17 or 18, wherein the membrane support further comprises one or more inert functional groups fixed to the surface of the membrane support.

21. The method of claim 17 or 18, wherein the plurality of straight-chain spacer arms comprises straight-chain spacer arms of different lengths.

22. The method of claim 17 or 18, wherein the ligand is coupled to the end of the linear spacer arm via an amine reactive functional group.

23. The method of claim 22, wherein the amine reactive functional group is an epoxide, an N-hydroxysuccinimide ester, or a combination thereof.

24. The method according to claim 23, wherein the amine reactive functional group is ethylene oxide.

25. The method of claim 18, wherein the membrane support comprises nanofibers and the nanofibers comprise cellulose.

26. The method of claim 18, wherein the membrane support comprises nanofibers and the nanofibers comprise a non-cellulose polymer.

27. The method of claim 17 or 18, wherein the linear spacer arm is hydrophobic.

28. The method according to claim 17 or 18, wherein the linear spacer arm is hydrophilic.

29. The method according to claim 17 or 18, wherein the ligand is a peptide.

30. The method of claim 29, wherein the peptide is protein A, protein G, or protein L.

31. The method according to claim 17 or 18, wherein the ligand is capable of binding protein or nucleic acid molecules.

32. The method of claim 17 or 18, wherein the ligand is capable of binding immunoglobulins.

33. A method for separating a target of interest from a sample, comprising: The sample, including the target of interest, is brought into contact with an affinity membrane according to any one of claims 1 to 16 to adsorb the target of interest.

34. The method of claim 33, further comprising: The affinity membrane is brought into contact with the eluent to release the target of interest; and the target of interest is recovered.

35. The method according to claim 33 or 34, wherein the target of interest is a protein or nucleic acid molecule.

36. The method of claim 35, wherein the target of interest is a DNA molecule, RNA molecule, vector, virus, or immunoglobulin.

37. The method of claim 36, wherein the target of interest is a viral vector.

38. The method of claim 36, wherein the immunoglobulin is immunoglobulin G.

39. The method of claim 33 or 34, wherein the target of interest is a nanoparticle, a virus-like particle, or an extracellular organism.

40. The method of claim 39, wherein the target of interest is encapsulated nanoparticles or lipid nanoparticles.

41. The method according to claim 33 or 34, wherein the sample is a biological sample.

42. The method according to claim 41, wherein the sample is a cell culture medium.

Citation Information

Patent Citations

  • Porous polymeric cellulose prepared via cellulose crosslinking

    US10919986B2

  • Hybrid felts of electrospun nanofibers

    US20150360158A1

  • Affinity chromatography matrices and methods of making and using the same

    US8114611B2

  • Hybrid felts of electrospun nanofibers

    US9604168B2

  • Receptor linked regenerated cellulose membrane and methods for producing and using the same

    US20170276671A1