A fluorine-modified polyvinyl alcohol film and its preparation method and application

CN116178775BActive Publication Date: 2024-10-11HEBEI YIKE PACKAGING TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310226632.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-10
Publication Date
2024-10-11
Estimated Expiration
2043-03-10

Smart Images

  • Figure BDA0004118656400000091
    Figure BDA0004118656400000091
  • Figure BDA0004118656400000101
    Figure BDA0004118656400000101
  • Figure BDA0004118656400000102
    Figure BDA0004118656400000102
Patent Text Reader

Abstract

The present invention provides a fluorine-modified polyvinyl alcohol film and a preparation method and application thereof, belonging to the technical field of packaging materials. The fluorine-modified polyvinyl alcohol film provided by the present invention forms an aqueous silica sol layer and a fluorine-containing surface treatment layer by spraying an aqueous silica sol solution and a fluorine-containing surface treatment composition solution on the polyvinyl alcohol layer in sequence. The fluorine-containing surface treatment layer can block the penetration of moisture into the polyvinyl alcohol layer, avoid changes in the aggregated structure of the polyvinyl alcohol layer, and effectively maintain the barrier properties and mechanical properties of the film; and the aqueous silica sol layer can form a cross-linked microstructure with the polyvinyl alcohol layer and the fluorine-containing surface treatment layer, further improving the tensile strength of the film in a water vapor environment. The fluorine-modified polyvinyl alcohol film of the present invention can achieve a tensile strength retention rate of more than 95% in a water vapor environment, has good waterproof, oil-proof and anti-fouling effects, and has a low preparation cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of packaging materials, and in particular to a fluorine-modified polyvinyl alcohol film and a preparation method and application thereof. Background Art

[0002] Polyvinyl alcohol (PVA) is a water-soluble polymer made from vinyl acetate by polymerization and alcoholysis. It is not only simple to prepare and low-cost, but also has excellent hydrophilicity, gas barrier properties, acid and alkali resistance, organic solvent resistance, outstanding biosafety and good film-forming ability. Therefore, it is widely used as a membrane material in food packaging, pervaporation, sewage treatment and other fields. PVA has a linear polymer structure and a large number of hydroxyl groups on the side chain. Although PVA film has excellent hydrophilic and anti-pollution properties, it is easy to swell or even dissolve in water, and the mechanical strength of the film is poor, which cannot meet the use requirements of PVA film in practical applications.

[0003] At present, the water resistance and mechanical properties of PVA film can be improved by modifying PVA. Patent CN106883442A discloses a method for preparing a fluoride-modified polyvinyl alcohol film, which sprays a fluoride-containing surface treatment composition solution with a concentration of 1wt% on the surface of a polyvinyl alcohol film substrate to obtain a fluoride-modified polyvinyl alcohol film. This patent improves the tensile strength of the film after treatment in a water vapor environment, but its tensile strength retention rate is still difficult to reach more than 93%; at the same time, to achieve the improvement effect of this patent, it is necessary to use a fluoride-containing surface treatment composition solution with a concentration of 1wt% to treat the surface of the polyvinyl alcohol film substrate, and the preparation cost is relatively high. Therefore, there is an urgent need for a polyvinyl alcohol film whose tensile strength retention rate in a water vapor environment can still reach more than 93% and has a low preparation cost. Summary of the invention

[0004] In view of this, the purpose of the present invention is to provide a fluorine-modified polyvinyl alcohol film and its preparation method and application. The fluorine-modified polyvinyl alcohol film provided by the present invention can retain more than 95% of its tensile strength in a water vapor environment, has good waterproof, oil-proof and anti-fouling effects, and has low preparation cost.

[0005] In order to achieve the above object, the present invention provides the following technical solutions:

[0006] A fluorine-modified polyvinyl alcohol film, the film comprising, from bottom to top, a polyvinyl alcohol layer, an aqueous silica sol layer and a fluorine-containing surface treatment layer;

[0007] Wherein, the aqueous silica sol layer is obtained by spraying an aqueous silica sol solution on the polyvinyl alcohol layer; the fluorine-containing surface treatment layer is obtained by spraying a fluorine-containing surface treatment composition solution on the aqueous silica sol layer;

[0008] The particle size of the aqueous silica sol in the aqueous silica sol solution is ≥40nm;

[0009] The fluorine-containing surface treatment composition comprises a first reactive compound and a second reactive compound; the first reactive compound contains a perfluoropolyether group, and the second reactive compound contains a perfluoroalkyl group; the concentration of the fluorine-containing surface treatment composition is 0.2 wt % to 0.8 wt %.

[0010] Preferably, the polyvinyl alcohol layer is obtained by casting a polyvinyl alcohol solution; the spraying amount of the aqueous silica sol layer is 200g to 800g of aqueous silica sol solution per square meter of polyvinyl alcohol layer; the spraying amount of the fluorine-containing surface treatment layer is 100g to 500g of fluorine-containing surface treatment composition solution per square meter of aqueous silica sol layer.

[0011] Preferably, the particle size of the aqueous silica sol in the aqueous silica sol solution is 60 nm to 120 nm; and the concentration of the aqueous silica sol solution is 3 wt % to 10 wt %.

[0012] Preferably, the pH value of the aqueous silica sol solution is 6-8.

[0013] Preferably, the concentration of the polyvinyl alcohol solution is 7 wt %.

[0014] Preferably, the content of the first reactive compound in the fluorine-containing surface treatment layer is ≥10 wt %; the first reactive compound is as shown in Formula I:

[0015] B-PFPE-A-(Si(OR)3) a Formula I;

[0016] Wherein, PFPE in formula I is a perfluoropolyether group, A is an a+1-valent organic group, R is an alkyl group, a is an integer of 1 to 10, and B is F or A-(Si(OR 1 )3) a The group represented;

[0017] The first reactive compound may be one or more of the compounds shown in formula I.

[0018] Preferably, the content of the second reactive compound in the fluorine-containing surface treatment layer is ≥10wt%; the second reactive compound is as shown in Formula II or Formula III:

[0019] R f -B-Si-(OR 2 )3 Formula II;

[0020] M(CH2CR1(-DR f )) m(CH2CR2(-E-Si(OR 3 )3)) n (CH2CR3(-I)) p N-type III;

[0021] Among them, R f is a monovalent perfluoroalkyl group, B is a divalent organic group, R 2 and R 3 is an alkyl group, M and N are monovalent organic groups, R1, R2 and R3 are H or CH3, D and E are divalent organic groups, I is a monovalent organic group, m and n are positive integers, and p is 0 or a positive integer.

[0022] Preferably, the fluorine-containing surface treatment composition may further include one or both of the first compound and the second compound;

[0023] The first compound contains both an isocyanate group or a blocked isocyanate group and -Si-(OR 4 )3 group;

[0024] The second compound does not contain a fluorine-containing group and an isocyanate group or a blocked isocyanate group, and contains -Si-(OR 5 )3 groups of siloxane compounds;

[0025] Among them, R 4 , R 5 It is an alkyl group.

[0026] The present invention also provides a method for preparing the fluorine-modified polyvinyl alcohol film in the above technical solution, comprising the following steps:

[0027] S1, casting the polyvinyl alcohol solution into a film, and naturally air-drying it at room temperature to obtain a polyvinyl alcohol layer;

[0028] S2, spraying the aqueous silica sol solution on the polyvinyl alcohol layer in S1, and naturally air-drying to obtain an aqueous silica sol layer;

[0029] S3, spraying a fluorine-containing surface treatment composition solution onto the aqueous silica sol layer in S2, and naturally air-drying the solvent to obtain a fluorine-containing surface treatment layer;

[0030] S4. Curing at room temperature for 20h to 30h to obtain fluorine-modified polyvinyl alcohol film.

[0031] The present invention also provides an application of the fluorine-modified polyvinyl alcohol film in the above technical solution in packaging materials.

[0032] Beneficial technical effects: The present invention provides a fluorine-modified polyvinyl alcohol film and its preparation method and application. By spraying an aqueous silica sol solution and a fluorine-containing surface treatment composition solution on the polyvinyl alcohol layer in sequence, an aqueous silica sol layer and a fluorine-containing surface treatment layer are formed. The fluorine-containing surface treatment layer can block the penetration of water into the polyvinyl alcohol layer, avoid changes in the aggregated structure of the polyvinyl alcohol layer, and effectively maintain the barrier properties and mechanical properties of the film; and the aqueous silica sol layer can form a cross-linked microstructure with the polyvinyl alcohol layer and the fluorine-containing surface treatment layer, further improving the tensile strength of the film in a water vapor environment. The fluorine-modified polyvinyl alcohol film of the present invention can maintain a tensile strength retention rate of more than 95% in a water vapor environment, has good waterproof, oil-proof and antifouling effects, and has a low preparation cost. DETAILED DESCRIPTION

[0033] The present invention provides a fluorine-modified polyvinyl alcohol film, which comprises, from bottom to top, a polyvinyl alcohol layer, an aqueous silica sol layer and a fluorine-containing surface treatment layer;

[0034] Wherein, the aqueous silica sol layer is obtained by spraying an aqueous silica sol solution on the polyvinyl alcohol layer; the fluorine-containing surface treatment layer is obtained by spraying a fluorine-containing surface treatment composition solution on the aqueous silica sol layer;

[0035] The particle size of the aqueous silica sol in the aqueous silica sol solution is ≥40nm;

[0036] The fluorine-containing surface treatment composition comprises a first reactive compound and a second reactive compound; the first reactive compound contains a perfluoropolyether group, and the second reactive compound contains a perfluoroalkyl group; the concentration of the fluorine-containing surface treatment composition is 0.2 wt % to 0.8 wt %.

[0037] In the present invention, the polyvinyl alcohol layer is preferably obtained by casting a polyvinyl alcohol solution, the polyvinyl alcohol solution is preferably a polyvinyl alcohol aqueous solution, and the concentration of the polyvinyl alcohol solution is preferably 7 wt %; the degree of polymerization of the polyvinyl alcohol is preferably a medium degree of polymerization.

[0038] In the present invention, the spraying amount of the aqueous silica sol layer is preferably 200g to 800g of aqueous silica sol solution per square meter of polyvinyl alcohol layer; the spraying amount of the fluorine-containing surface treatment layer is preferably 100g to 500g of fluorine-containing surface treatment composition solution per square meter of aqueous silica sol layer.

[0039] In the present invention, the particle size of the aqueous silica sol in the aqueous silica sol solution is more preferably 60nm to 120nm, and most preferably 80nm to 120nm; the concentration of the aqueous silica sol solution is preferably 3wt% to 10wt%, and more preferably 5wt%. Too low particle size of the aqueous silica sol will affect the mechanical properties of the final polyvinyl alcohol film, and by controlling the concentration of the aqueous silica sol solution, it can be ensured that the aqueous silica sol layer can be evenly covered on the polyvinyl alcohol layer.

[0040] In the present invention, the pH value of the aqueous silica sol solution is preferably 6-8.

[0041] In the present invention, the content of the first reactive compound in the fluorine-containing surface treatment layer is preferably ≥10 wt %; the first reactive compound is preferably as shown in Formula I:

[0042] B-PFPE-A-(Si(OR)3) a Formula I;

[0043] Wherein, PFPE in formula I is a perfluoropolyether group, A is an a+1-valent organic group, R is an alkyl group, a is an integer of 1 to 10, and B is F or A-(Si(OR 1 )3) a The group represented;

[0044] The first reactive compound is more preferably as shown in Formula I-1:

[0045] B-PFPE-CON(CH2CH2CH2Si(OR 1 )3)2 Formula Ⅰ-1;

[0046] Wherein, PFPE in Formula I-1 is a perfluoropolyether group, R 1 is a C1-4 alkyl group, B is F or CON(CH2CH2CH2Si(OR 1 )3)2;

[0047] The first reactive compound is most preferably as shown in Formula I-2:

[0048] B-PFPE-CON(CH2CH2CH2Si(OCH3)3)2 formula I-2;

[0049] Wherein, PFPE in formula Ⅰ-2 is a perfluoropolyether group, and B is F or CON(CH2CH2CH2Si(OCH3)3)2;

[0050] In the present invention, in the reactive compound containing perfluoropolyether groups, the compound in which B is a group represented by CON(CH2CH2CH2Si(OCH3)3)2 accounts for at least 50% by weight of the reactive compound containing perfluoropolyether groups.

[0051] In the present invention, the perfluoropolyether group is preferably F(CF(CF3)CF2O) a CF(CF3)-, F(CF(CF3)CF2O) a CF2CF2-, CF3O(CF2CF2O) a CF2-, CF3O(CF2O) b (CF2CF2O) a CF2-, -CF(CF3)O(CF(CF3)CF2O) a CF(CF3)-,-CF2CF2O(CF(CF3)CF2O) a CF2CF2-, -CF2O(CF2CF2O) a CF2-, -CF2O(CF2O) b (CF2CF2O) a CF2-, etc., wherein a and b are integers from 1 to 100; the a+1 valent organic group is preferably: -CONH(CH2) k -、-CH2O(CH2) k -、-CH2OCONH(CH2) k -、-CONHCH2CH2OCONH(CH2) k -、-CH2OCOCH2CH2N(CH3)(CH2) k -, -CH2OCH2CH2CH2Si(CH3)2OSi(CH3)2CH2CH2-, -CON((CH2) k -)2, etc., wherein k is an integer from 2 to 10; the alkyl group is preferably: CH3, CH2CH3, CH(CH3)2, C(CH3)3, etc.

[0052] In the present invention, the first reactive compound may preferably be one or more of the compounds represented by formula I.

[0053] In the present invention, the content of the second reactive compound in the fluorine-containing surface treatment layer is preferably ≥10 wt %; the second reactive compound is preferably as shown in Formula II or Formula III:

[0054] R f -B-Si-(OR 2 )3 Formula II;

[0055] M(CH2CR1(-DR f )) m (CH2CR2(-E-Si(OR 3 )3)) n(CH2CR3(-I)) p N-type III;

[0056] Among them, R f is a monovalent perfluoroalkyl group, B is a divalent organic group, R 2 and R 3 is an alkyl group, M and N are monovalent organic groups, R1, R2 and R3 are H or CH3, D and E are divalent organic groups, I is a monovalent organic group, m and n are positive integers, and p is 0 or a positive integer. The perfluoroalkyl group is preferably CF3 (CF2) c 、(CF3)2CF(CF2) c , CF3, etc., wherein c is an integer of 0 to 20; the divalent organic group is preferably: -CH2CH2-, -CH2OCH2CH2CH2-, -CH2CH2OCH2CH2CH2-, -CH2CH2OCONHCH2CH2CH2-, etc.; the alkyl group is preferably: CH3, CH2CH3, CH(CH3)2, C(CH3)3, etc. The first reactive compound and the second reactive compound of the present invention usually contain hydrolyzable cross-linked siloxane groups, which can react with the hydroxyl groups in polyvinyl alcohol and aqueous silica sol to form chemical bonds, and cooperate with each other to give the fluorine-modified polyvinyl alcohol film better performance.

[0057] In the present invention, the fluorine-containing surface treatment composition may also preferably include one or both of a first compound and a second compound; the first compound is a compound containing both an isocyanate group or a blocked isocyanate group and -Si-(OR 4 )3 group compounds, such as: OCNCH2CH2CH2Si(OCH)3, OCN-T-NHCONHCH2CH2CH2Si(OCH)3, OCN-T-NHCONHCH2CH2CH2Si(OCH2CH)3, Y-CONH-T-NHCONHCH2CH2CH2Si(OCH)3, (OCN)2-Q-NHCONHCH2CH2CH2Si(OCH)3, (Y-OCONH)2-Q-NHCONHCH2CH2CH2Si(OC H)3, etc., wherein T is a residue after removing the diisocyanate group from hexamethyl diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate, etc., Q is a trimer of hexamethyl diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate, etc., or a residue after removing the triisocyanate group from triphenylmethane triisocyanate, and Y is a residue after removing the activated glassy hydrogen from 2-methylimidazole, methyl ethyl ketone oxime, etc.; the second compound is a compound that does not contain a fluorine-containing group and an isocyanate group or a blocked isocyanate group and contains -Si-(OR 5 )3 groups of siloxane compounds; wherein R4 , R 5 It is an alkyl group, such as ethyl orthosilicate (Si(OCH2CH3)4), methyltrimethoxysilane (CH3Si(OCH3)3), ethyltrimethoxysilane (CH3CH2Si(OCH3)3), cyclohexyltrimethoxysilane, isobutyltriethoxysilane, n-hexyltriethoxysilane, n-butyltrimethoxysilane, n-octyltrimethoxysilane, n-octyltriethoxysilane, dodecyltrimethoxysilane, hexadecyltrimethoxysilane, 3-glycidyloxypropyltriethoxysilane, phenyltrimethoxysilane, etc.

[0058] In the present invention, the solvent of the fluorine-containing surface treatment composition solution is preferably a fluorine-containing solvent, a chlorine-containing solvent or a conventional hydrocarbon solvent free of halogen, wherein the fluorine-containing solvent is preferably perfluorocyclic ether, 7200 (nonafluorobutyl ethyl ether), 7100 (nonafluorobutyl methyl ether), 347 (CF3CH2OCF2CF2H), 494 (CH3CH2CH2OCF2CF2H), etc.; the chlorine-containing solvent is preferably dichloromethane, vinylidene chloride, trichloroethane, tetrachloroethane, etc.; the conventional hydrocarbon solvent free of halogen is preferably butyl acetate, ethyl acetate, heptane, hexane, cyclohexane, petroleum ether, D40, methyl isoamyl ketone, diethylene glycol dimethyl ether, etc. Preferred fluorocarbon solvents are 7200 and 7100.

[0059] The present invention also provides a method for preparing the fluorine-modified polyvinyl alcohol film in the above technical solution, comprising the following steps:

[0060] S1, casting the polyvinyl alcohol solution into a film, and naturally air-drying it at room temperature to obtain a polyvinyl alcohol layer;

[0061] S2, spraying the aqueous silica sol solution on the polyvinyl alcohol layer in S1, and naturally air-drying to obtain an aqueous silica sol layer;

[0062] S3, spraying a fluorine-containing surface treatment composition solution onto the aqueous silica sol layer in S2, and naturally air-drying the solvent to obtain a fluorine-containing surface treatment layer;

[0063] S4. Curing at room temperature for 20h to 30h to obtain fluorine-modified polyvinyl alcohol film.

[0064] In the present invention, the parameters and effects of the raw materials and each layer are the same as those described above and will not be described in detail herein.

[0065] The present invention also provides an application of the fluorine-modified polyvinyl alcohol film in the above technical solution in packaging materials.

[0066] There is no particular limitation on the type of application in the present invention, and any type of application acceptable to the fluorine-modified polyvinyl alcohol film in this field may be used.

[0067] In order to better understand the present invention, the content of the present invention is further explained in conjunction with the following examples, but the content of the present invention is not limited to the following examples. The materials, reagents, etc. used in the examples and test examples of the present invention, unless otherwise specified, can be obtained from commercial channels; the methods used in the examples and test examples of the present invention, unless otherwise specified, are conventional methods.

[0068] Examples 1 to 11 and Comparative Examples 1 to 3

[0069] 1.1 Materials

[0070] (1) First reactive compound:

[0071] a1: The first reactive compound PFPE-CONH(CH2CH2CH2Si(OCH3)3)2 shown in formula I is prepared by reacting perfluoropolyether monocarboxylate (PFPE-COOCH3 purchased from Solvay) with NH2(CH2CH2CH2Si(OCH3)3)2 (purchased from Nanjing Nengde).

[0072] a2: The first reactive compound ((H3CO)3SiCH2CH2CH2)2NHCO-PFPE-CONH(CH2CH2CH2Si(OCH3)3)2 shown in formula I is prepared by reacting perfluoropolyether dicarboxylate (H3COCO-PFPE-COOCH3 purchased from Solvay) with NH2(CH2CH2CH2Si(OCH3)3)2.

[0073] (2) Second reactive compound:

[0074] b: CF3(CF2)5CH2CH2Si(OCH3)3 (purchased from Juhua Group);

[0075] c: CH2=C(CH3)COOCH2CH2(CF2)5CF5 (purchased from Fujian Sannong New Materials Co., Ltd.), CH2=CHCOOCH2(CH2) 10 CH3 (purchased from Hubei Jusheng Technology Co., Ltd.) and CH2=CHCH2Si(OCH3)3 (purchased from Nanjing Nengde) were copolymerized in a mass ratio of 6:2:2 by free radical solution copolymerization to obtain a reactive compound containing a perfluoroalkyl group as shown in Formula III.

[0076] (3) The first compound:

[0077] d: OCN-T-NHCONHCH2CH2CH2Si(OCH)3 (T is the isophorone diisocyanate residue after removing two isocyanate groups) prepared by isocyanate reaction of an aminosiloxane compound (NH2CH2CH2CH2Si(OCH)3 purchased from Nanjing Xiangqian Chemical Co., Ltd.) and an equimolar amount of isophorone diisocyanate (purchased from Dow Chemical, USA).

[0078] e: OCNCH2CH2CH2Si(OCH)3 (purchased from Nanjing Nengde).

[0079] (4) The second compound:

[0080] f: (Y-OCONH)2-Q-NHCONHCH2 CH2CH2Si(OCH)3 (Q is the residue after removing the triisocyanate group from the hexamethyl diisocyanate trimer, and Y is the residue after removing the active glassy hydrogen by methyl ethyl ketone oxime) obtained by reacting hexamethylene diisocyanate trimer (purchased from BASF) with an equimolar amount of NH2CH2CH2CH2Si(OCH)3 and then capping it with methyl ethyl ketone oxime (purchased from Zhejiang Sheng'an Chemical Co., Ltd.).

[0081] g: Si(OC2H5)4 (purchased from Changzhou Wujin Hengye Chemical Co., Ltd.);

[0082] h: CH3Si(OCH3)3 (purchased from Nanjing Xiangqian Chemical Co., Ltd.).

[0083] (5) Aqueous silica sol:

[0084] k1: aqueous silica sol, particle size 80 nm, pH 7.4, concentration 30 wt% (purchased from Zhangjiagang Churen New Materials Technology Co., Ltd.);

[0085] k2: aqueous silica sol, particle size 120 nm, pH 6.5, concentration 30 wt% (purchased from Zhangjiagang Churen New Materials Technology Co., Ltd.);

[0086] k3: aqueous silica sol, particle size 10 nm to 25 nm, pH 7.2, concentration 30 wt% (purchased from Zhangjiagang Churen New Materials Technology Co., Ltd.);

[0087] k4: aqueous silica sol, particle size 80 nm, pH 9.5, concentration 30 wt% (purchased from Zhangjiagang Churen New Materials Technology Co., Ltd.)

[0088] (6) Polyvinyl alcohol:

[0089] The degree of polymerization of polyvinyl alcohol (purchased from Shanghai Kaidu Industrial Development Co., Ltd.) is medium.

[0090] 1.2 Preparation method

[0091] (1) preparing polyvinyl alcohol into an aqueous solution with a concentration of 7 wt %;

[0092] (2) According to the silica sol selected from Table 1, the concentration of the silica sol in Examples 1 to 4 was diluted to 5 wt %, the concentration of the silica sol in Examples 5 to 6 was diluted to 10 wt %, the concentration of the silica sol in Examples 7 to 8 and 11 was diluted to 5 wt %, the concentration of the silica sol in Examples 9 to 10 was diluted to 3 wt %, and the concentration of the silica sol in Comparative Examples 1 to 7 was diluted to 5 wt %.

[0093] (3) According to the ratio (mass ratio) in Table 1, the fluorine-containing surface treatment compositions of Examples 1 to 4 and 11 were prepared into solutions with a concentration of 0.5 wt %, and the solvent was fluorocarbon solvent 7200; the fluorine-containing surface treatment compositions of Examples 5 to 6 were prepared into solutions with a concentration of 0.2 wt %, and the solvent was fluorocarbon solvent 7200; the fluorine-containing surface treatment compositions of Examples 7 to 8 were prepared into solutions with a concentration of 0.8 wt %, and the solvent was fluorocarbon solvent 7200; the fluorine-containing surface treatment compositions of Examples 9 to 10 were prepared into solutions with a concentration of 0.6 wt %, and the solvent was fluorocarbon solvent 7100; the fluorine-containing surface treatment compositions of Comparative Examples 1 to 3 were prepared into solutions with a concentration of 0.5 wt %, and the solvent was fluorocarbon solvent 7200; the fluorine-containing surface treatment compositions of Comparative Examples 4 to 7 were prepared into solutions with a concentration of 0.5 wt %, and the solvent was fluorocarbon solvent 7200.

[0094] Table 1 Ratio (mass ratio) of each raw material in Examples 1 to 11 and Comparative Examples 1 to 7

[0095]

[0096]

[0097] (3) According to the settings of each embodiment and comparative example, the polyvinyl alcohol solution is cast into a film, and naturally air-dried at room temperature to obtain a polyvinyl alcohol layer; the aqueous silica sol solution is sprayed on the dried polyvinyl alcohol layer, and naturally air-dried to obtain an aqueous silica sol layer; the fluorine-containing surface treatment composition solution is sprayed on the aqueous silica sol layer, and the solvent is naturally air-dried to obtain a fluorine-containing surface treatment layer, which is cured at room temperature to obtain a fluorine-modified polyvinyl alcohol film;

[0098] Among them, the spraying amounts of aqueous silica sol solutions and fluorine-containing surface treatment compositions of Examples 1 to 11 and Comparative Examples 1 to 7 are shown in Table 2; Examples 1 to 4 and 11 are cured at room temperature for 24 hours; Examples 5 to 7 are cured at room temperature for 20 hours, Examples 8 to 10 are cured at room temperature for 30 hours, Comparative Examples 1 to 4 are cured at room temperature for 24 hours, and Examples 5 to 7 are cured at room temperature for 24 hours to obtain fluorine-modified polyvinyl alcohol films.

[0099] Table 2 Spraying amount of aqueous silica sol solution and fluorine-containing surface treatment composition of Examples 1 to 11 and Comparative Examples 1 to 7

[0100]

[0101]

[0102] 1.3 Performance Testing

[0103] (1) Waterproof test

[0104] The fluorine-modified polyvinyl alcohol films obtained in Examples 1 to 11 and Comparative Examples 1 to 7 were respectively tested for water resistance. The water resistance evaluation standard was implemented according to GB / T 4745-1997 "Test for Determination of Surface Moisture Resistance of Textile Fabrics by Water Splashing". The water resistance evaluation standard is shown in Table 3.

[0105] Table 3 Waterproof evaluation standard

[0106] Waterproof grade state 5 No wet surface 4 Slightly moist surface 3 Partially wet surface 2 Surface Wetting 1 All surfaces are wet

[0107] (2) Oil resistance test

[0108] The fluorine-modified polyvinyl alcohol films obtained in Examples 1 to 11 and Comparative Examples 1 to 7 were respectively tested for oil repellency. The oil repellency evaluation standard was implemented in accordance with GB / T 19977-2005 "Test for Oil Repellency and Hydrocarbon Resistance of Textiles". The oil repellency evaluation standard is shown in Table 4.

[0109] Table 4 Oil resistance evaluation standard

[0110]

[0111]

[0112] (3) Evaluation of antifouling performance

[0113] The fluorine-modified polyvinyl alcohol films obtained in Examples 1 to 11 and Comparative Examples 1 to 7 were respectively evaluated for antifouling performance. Oil pen test: a line was drawn on the modified surface with an oil pen, and then the changes in the ink trace were carefully observed and evaluated according to the following standards:

[0114] E: Ink shrinks quickly

[0115] F: Ink shrinkage

[0116] NG: The ink hardly shrinks.

[0117] (4) Tensile strength

[0118] The fluorine-modified polyvinyl alcohol films obtained in Examples 1 to 11 and Comparative Examples 1 to 7 were respectively tested for tensile strength using a tensile testing machine. The width of the test samples was 5 cm. The test samples for tensile strength needed to be double-sided treated. The treatment in a water vapor environment means placing the double-sided treated test samples in an environment with a humidity of 80% for 24 hours. At the same time, the obtained tensile strength was converted into the tensile strength when the film thickness was 50 μm.

[0119] 1.4 Results

[0120] The performance test results of the fluorine-modified polyvinyl alcohol films obtained in Examples 1 to 11 and Comparative Examples 1 to 7 are shown in Table 5.

[0121] Table 5 Performance test results of fluorine-modified polyvinyl alcohol films obtained in Examples 1 to 11 and Comparative Examples 1 to 7

[0122]

[0123]

[0124] As can be seen from Table 5, the waterproof performance grade of the fluorine-modified polyvinyl alcohol film obtained in Examples 1 to 11 can reach 5, the oil-proof performance grade is 7 to 8, and the antifouling performance grade is E, which are all better than the waterproof performance, oil-proof performance and antifouling performance of Comparative Examples 1 to 7. At the same time, the tensile strength of the fluorine-modified polyvinyl alcohol film obtained in Examples 1 to 11 can reach 58.0 MPa to 62.3 MPa, the tensile strength after treatment in a water vapor environment is 55.2 MPa to 59.9 MPa, and the tensile strength retention rate can reach 95.2% to 97.2%, which is significantly higher than the tensile strength of the fluorine-modified polyvinyl alcohol film obtained in Comparative Examples 1 to 7, the tensile strength after treatment in a water vapor environment, and the tensile strength retention rate.

[0125] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A fluorine-modified polyvinyl alcohol film, It is characterized in that The film comprises, from bottom to top, a polyvinyl alcohol layer, an aqueous silica sol layer and a fluorine-containing surface treatment layer; Wherein, the aqueous silica sol layer is obtained by spraying an aqueous silica sol solution on the polyvinyl alcohol layer; the fluorine-containing surface treatment layer is obtained by spraying a fluorine-containing surface treatment composition solution on the aqueous silica sol layer; The particle size of the aqueous silica sol in the aqueous silica sol solution is ≥40 nm; The fluorine-containing surface treatment composition comprises a first reactive compound and a second reactive compound; the first reactive compound contains a perfluoropolyether group, and the second reactive compound contains a perfluoroalkyl group; the concentration of the fluorine-containing surface treatment composition is 0.2wt% to 0.8wt%; The particle size of the aqueous silica sol in the aqueous silica sol solution is 60nm to 120nm; the concentration of the aqueous silica sol solution is 3wt% to 10wt%; The pH value of the aqueous silica sol solution is 6 to 8; The content of the first reactive compound in the fluorine-containing surface treatment layer is ≥10 wt %; the first reactive compound is as shown in Formula I: B-PFPE-A-(Si(OR 1 ) 3 ) a Formula I; Wherein, PFPE in formula I is a perfluoropolyether group, A is an a+1-valent organic group, R is an alkyl group, a is an integer of 1 to 10, and B is F or A-(Si(OR 1 ) 3 ) a The group represented; The first reactive compound may be one or more of the compounds shown in Formula I, and at least one of the compounds in Formula I wherein B is A-(Si(OR 1 ) 3 ) a compound represented by a group; The content of the second reactive compound in the fluorine-containing surface treatment layer is ≥10wt%; the second reactive compound is as shown in Formula II or Formula III: R f -B-Si-(OR 2 ) 3 Formula II; M(CH 2 CR 1 (-D-R f )) m (CH 2 CR 2 (-E-Si(OR 3 ) 3 )) n (CH 2 CR 3 (-I)) p Formula III; Among them, R f is a monovalent perfluoroalkyl group, B is a divalent organic group, R 2 and R 3 is an alkyl group, M and N are monovalent organic groups, R 1 , R 2 and R 3 H or CH 3 , D and E are divalent organic groups, I is a monovalent organic group, m and n are positive integers, and p is 0 or a positive integer.

2. The fluorine-modified polyvinyl alcohol film according to claim 1, It is characterized in that The polyvinyl alcohol layer is obtained by casting a polyvinyl alcohol solution; the spraying amount of the aqueous silica sol layer is 200g to 800g of aqueous silica sol solution per square meter of polyvinyl alcohol layer; the spraying amount of the fluorine-containing surface treatment layer is 100g to 500g of fluorine-containing surface treatment composition solution per square meter of aqueous silica sol layer.

3. The fluorine-modified polyvinyl alcohol film according to claim 2, It is characterized in that The concentration of the polyvinyl alcohol solution is 7 wt %.

4. The fluorine-modified polyvinyl alcohol film according to claim 1, It is characterized in that The fluorine-containing surface treatment composition may also include one or both of the first compound and the second compound; The first compound contains both an isocyanate group or a blocked isocyanate group and -Si-(OR 4 ) 3 Compounds of groups; The second compound does not contain a fluorine-containing group and an isocyanate group or a blocked isocyanate group, and contains -Si-(OR 5 ) 3 Siloxane compounds containing groups; Among them, R 4 , R 5 It is an alkyl group.

5. A method for preparing the fluorine-modified polyvinyl alcohol film according to any one of claims 1 to 4, It is characterized in that The following steps are involved: S1, casting the polyvinyl alcohol solution into a film, and naturally air-drying it at room temperature to obtain a polyvinyl alcohol layer; S2, spraying the aqueous silica sol solution on the polyvinyl alcohol layer in S1, and naturally air-drying to obtain an aqueous silica sol layer; S3, spraying a fluorine-containing surface treatment composition solution onto the aqueous silica sol layer in S2, and naturally air-drying the solvent to obtain a fluorine-containing surface treatment layer; S4. Curing at room temperature for 20h to 30h to obtain fluorine-modified polyvinyl alcohol film.

6. Use of the fluorine-modified polyvinyl alcohol film according to any one of claims 1 to 4 in packaging materials.