Balancing weight for an electric compressor motor and method of manufacturing the same

By using powder metallurgy to manufacture balancing weights with main balancing materials such as brass, pure copper, or iron and specific gravity adjusting materials such as tungsten, the problems of high specific gravity and miniaturization have been solved, achieving high-density and economical manufacturing.

CN116210140BActive Publication Date: 2026-11-20宋永国
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202180056266.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-08-10
Filing Date
2021-08-10
Publication Date
2026-11-20
Estimated Expiration
2041-08-10

AI Technical Summary

Technical Problem

Existing counterweight materials are harmful to the human body, difficult to achieve high specific gravity and miniaturization, and suffer from high processing costs and low precision during manufacturing.

Method used

Using brass, pure copper, or iron as the main counterweight material, and combining tungsten, molybdenum, or tungsten carbide as the specific gravity adjustment material, the balance counterweight is manufactured by powder metallurgy, including the steps of mixing powders, pressing and molding, and sintering, and the specific gravity is adjusted to achieve the target density.

Benefits of technology

It achieves high specific gravity balance, supports miniaturized design, expands the range of applicable equipment, reduces processing steps, and improves economy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116210140B_ABST
    Figure CN116210140B_ABST
Patent Text Reader

Abstract

In the embodiment of the present application, the balance weight for the motor of the electric compressor can contain a main weight substance and a specific gravity adjusting substance. The balance weight for the motor of the compressor of the present application can change the content of the specific gravity adjusting substance to achieve the required specific gravity, can increase the specific gravity to adjust the size, thus being beneficial to miniaturization, can realize the improvement of the motor design, and can expand the range of applicable equipment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a counterweight for an electric compressor motor and its manufacturing method. Background Technology

[0002] A balance weight is a component used to achieve weight balance in mechanical devices, especially dynamic devices such as motors or wheels. It is widely used in electric vehicles, washing machines, elevators, and air conditioners.

[0003] Generally, refrigeration equipment such as air conditioners or refrigerators contain a compressor that reduces the refrigerant to a liquid state. Based on the characteristics of the compressor, a motor with high torque and high-speed rotation is used. At this time, in order to prevent vibration caused by weight deviation during rotor rotation, a counterweight is required to balance the system.

[0004] In the past, lead (Pb) was used as a material for balancing weights. However, although lead is easy to process, it is not used much recently because it is harmful to the human body, and there is a risk of corrosion during long-term use.

[0005] In addition, in Korean Patent Publication No. 10-2005-0017849, although brass was used as a material for balancing counterweight, the specific gravity could not be increased to a level higher than that of brass, thus limiting miniaturization.

[0006] On the other hand, the traditional method for manufacturing counterweights primarily used die-casting. However, die-casting involves melting the raw metal and injecting it under high pressure into a metal frame. While it offers the advantage of achieving true density, it requires additional machining steps when precise dimensions are needed, resulting in higher processing costs. Furthermore, recent advancements in processing technology have enabled the manufacturing of counterweights by machining round steel bars, including forging and machining processes. However, this method suffers from significant material loss and high manufacturing costs.

[0007] In addition, cutting is sometimes used, but this has the disadvantage of requiring a lot of processing costs.

[0008] In order to manufacture counterweights that meet both the size requirements of modern equipment and economic needs, it is necessary to develop technologies with high specific gravity and adjustable specific gravity as needed, compared to previous counterweights.

[0009] Existing technical documents

[0010] Patent Document 1: Republic of Korea Patent Publication No. 10-2005-0017849 Summary of the Invention

[0011] Technical problems to be solved

[0012] The technical problem to be solved by the present invention is to provide a counterweight for an electric compressor motor that can achieve a desired specific gravity and a method for manufacturing the same.

[0013] The technical problems to be solved by the present invention are not limited to those mentioned above. Those skilled in the art can clearly understand other technical problems not mentioned from the following description.

[0014] means for solving problems

[0015] To address the aforementioned technical challenges, one embodiment of the present invention provides a counterweight for an electric compressor motor.

[0016] In embodiments of the present invention, the counterweight for the electric compressor motor may include a main counterweight material and a specific gravity adjusting material.

[0017] In embodiments of the present invention, the main counterweight material may include brass, pure copper, or iron.

[0018] In embodiments of the present invention, the specific gravity adjusting material may include tungsten (W), molybdenum (Mo), or tungsten carbide (WC).

[0019] In an embodiment of the present invention, the main counterweight material is brass, the specific gravity adjusting material is tungsten, and the electric compressor motor counterweight contains more than 10 wt% of the tungsten in total weight, so the specific gravity can be more than 8.5.

[0020] To address the aforementioned technical challenges, another embodiment of the present invention provides a method for manufacturing a counterweight for an electric compressor motor.

[0021] In an embodiment of the present invention, a method for manufacturing a counterweight for an electric compressor motor includes: selecting a main counterweight material and a specific gravity adjusting material to achieve a target specific gravity; mixing the specific gravity adjusting material powder and the main counterweight material powder to form a mixed powder; pressing the mixed powder and then sintering it to form a sintered body; and pressing the sintered body again.

[0022] In embodiments of the present invention, the main counterweight material may include brass, pure copper, or iron.

[0023] In an embodiment of the present invention, when the target specific gravity is set to be higher than the specific gravity of the main counterweight, the specific gravity adjusting substance may include tungsten (W), molybdenum (Mo), or tungsten carbide (WC).

[0024] In embodiments of the present invention, the average particle size of the main counterweight powder can be from 10 μm to 140 μm.

[0025] In embodiments of the present invention, the average particle size of the above-mentioned specific gravity adjusting material powder can be from 10 μm to 100 μm.

[0026] In an embodiment of the present invention, when the average particle size of the above-mentioned specific gravity adjusting material powder is less than 10 μm, between the steps of selecting the main counterweight material and the specific gravity adjusting material and the steps of forming the mixed powder, a step of granulating the powder of the above-mentioned specific gravity adjusting material is further included.

[0027] Invention Effects

[0028] The counterweight for the electric compressor motor according to an embodiment of the present invention enables the desired specific gravity to be achieved by changing the content of the specific gravity adjusting substance, thereby increasing the specific gravity to adjust the size, which is beneficial for miniaturization, improving motor design, and expanding the range of applicable equipment.

[0029] In addition, the use of powder metallurgy reduces processing steps and is economical.

[0030] The effects of the present invention are not limited to those described above, but should be understood to include all effects that can be inferred from the inventive structure described in the specification or claims of the present invention. Attached Figure Description

[0031] Figure 1 This is a perspective view, top view, front view, and cross-sectional view along line A'-A" of an electric compressor motor based on an embodiment of the present invention.

[0032] Figure 2 This is a diagram of a counterweight for an electric compressor motor based on an embodiment of the present invention.

[0033] Figure 3 This is a sequence diagram of a method for manufacturing a counterweight for an electric compressor motor based on an embodiment of the present invention. Detailed Implementation

[0034] The present invention will now be described with reference to the accompanying drawings. However, the present invention can be implemented in various different ways and is therefore not limited to the embodiments described herein. Furthermore, for the purpose of clearly illustrating the present invention, parts unrelated to the description have been omitted from the drawings, and similar reference numerals have been used for similar parts throughout the specification.

[0035] Throughout the specification, when a part is described as being "connected (joined, contacted, joined)" to other parts, this includes not only "direct connection" but also "indirect connection" with other components in between. Furthermore, when a part is described as "containing" a certain constituent element, unless otherwise specified, this implies that other constituent elements may also be included, rather than excluding them.

[0036] The terminology used in this specification is for illustrative purposes only and is not intended to limit the invention. Unless the context clearly indicates otherwise, a single expression encompasses multiple expressions. In this specification, terms such as "comprising" or "having" are used to describe the presence of features, numbers, steps, actions, constituent elements, components, or combinations thereof described in the specification, without precluding the presence or additional possibilities of one or more other features or numbers, steps, actions, constituent elements, components, or combinations thereof.

[0037] A counterweight for an electric compressor motor based on an embodiment of the present invention will be described.

[0038] Figure 1 These are perspective views, top views, front views, and cross-sectional views along line A'-A" of an electric compressor motor based on an embodiment of the present invention.

[0039] Figure 2 This is a diagram of a counterweight for an electric compressor motor based on an embodiment of the present invention.

[0040] Reference Figure 1 and Figure 2 According to an embodiment of the present invention, the counterweight 10 for an electric compressor motor includes a main counterweight material and a specific gravity adjusting material.

[0041] The main counterweight material mentioned above may include brass, pure copper (Cu), or iron (Fe).

[0042] The zinc to copper ratio of the aforementioned brass can be, for example, 2:8, but is not limited to this.

[0043] The aforementioned specific gravity adjusting substance is a substance with a greater specific gravity than the aforementioned main counterweight substance, and may include, for example, tungsten (W), molybdenum (Mo), or tungsten carbide (WC).

[0044] By adjusting the content of the specific gravity adjusting substance and including it in the above-mentioned main counterweight substance, the target specific gravity can be obtained.

[0045] For example, the main counterweight is brass with a zinc (Zn) to copper (Cu) content ratio of 2:8, and the specific gravity adjusting substance is tungsten (W). The balance weight of the present invention, which contains more than 10 wt% of the tungsten in total weight, can have a specific gravity of 8.5 or more.

[0046] For example, if the main counterweight is pure copper (Cu) and the specific gravity adjusting material is tungsten (W), the balance counterweight of the present invention, which contains 6.5 wt% or more of the tungsten in total weight, can have a specific gravity of 8.5 or more.

[0047] For example, if the main counterweight is iron (Fe) and the specific gravity adjusting substance is tungsten (W), the balance counterweight of the present invention, which contains 8.5 wt% or more of the tungsten in total weight, can have a specific gravity of 7.8 or more.

[0048] A method for manufacturing a counterweight for an electric compressor motor based on another embodiment of the present invention will be described.

[0049] Figure 3 This is a sequence diagram of a method for manufacturing a counterweight for an electric compressor motor based on an embodiment of the present invention.

[0050] Reference Figure 3 A method for manufacturing a counterweight for an electric compressor motor according to an embodiment of the present invention includes: a step of selecting a main counterweight material and a specific gravity adjusting material to achieve a target specific gravity (S100); a step of mixing the specific gravity adjusting material powder and the main counterweight material powder to form a mixed powder (S200); a step of pressing the mixed powder and then sintering it to form a sintered body (S300); and a step of pressing the sintered body again (S400).

[0051] In the first step, the main counterweight and the specific gravity adjusting substance are selected to achieve the target specific gravity (S100).

[0052] The main counterweight material mentioned above may include brass, pure copper (Cu), or iron (Fe).

[0053] The zinc to copper content ratio of the above-mentioned brass can preferably be 2:8, but is not limited to this.

[0054] The aforementioned specific gravity adjusting substance is a substance with a greater specific gravity than the aforementioned main counterweight substance, and may include, for example, tungsten (W), molybdenum (Mo), or tungsten carbide (WC).

[0055] When the target specific gravity is set to be higher than that of the main counterweight, it is possible to select a main counterweight and a specific gravity adjusting substance that are suitable for the target specific gravity and determine their contents.

[0056] For example, when the target specific gravity is 8.5 or higher, and when the main counterweight is brass and the specific gravity adjusting material is tungsten, the tungsten content can be 10 wt% or higher.

[0057] For example, when the target specific gravity is 8.5 or higher, and when the main counterweight is pure copper (Cu) and the specific gravity adjusting substance is tungsten (W), the tungsten content can be 6.5 wt% or higher.

[0058] For example, when the target specific gravity is 7.8 or higher, and when the main counterweight is iron (Fe) and the specific gravity adjusting substance is tungsten (W), the tungsten content can be 8.5 wt% or higher.

[0059] In the second step, the above-mentioned specific gravity adjusting substance powder and the above-mentioned main counterweight substance powder are mixed to form a mixed powder (S200).

[0060] The average particle size of the main counterweight powder can be from 10 μm to 140 μm.

[0061] When the average particle size of the main counterweight powder is less than 10 μm or more than 140 μm, serious weight deviations may occur during molding due to changes in the amount of powder filling.

[0062] In addition, the average particle size of the above-mentioned specific gravity adjusting material powder can be from 10 μm to 100 μm.

[0063] When the average particle size of the above-mentioned specific gravity adjusting material powder is less than 10 μm or more than 100 μm, weight deviation may occur during molding due to changes in the amount of powder filling.

[0064] When the average particle size of the aforementioned specific gravity adjusting material powder is less than 10 μm, in order to prevent segregation, the average particle size can be made to 10 μm to 100 μm through a granulation process. The granulation process will be described again later.

[0065] The average particle size difference between the main counterweight powder and the specific gravity adjusting powder is preferably less than 10 μm.

[0066] When the average particle size difference exceeds 10 μm, segregation may occur.

[0067] The segregation mentioned above is a phenomenon that occurs when two powders with large differences in specific gravity or particle size are mixed, resulting in localized non-uniformity in the mixture. This segregation can be mitigated by reducing the difference in specific gravity or particle size between the mixed powders.

[0068] The above mixing can be performed using a mixer, for example, by adding 0.5 to 1.0 wt% of the lubricant required for the molding process, using a double cone mixer or a V-type mixer.

[0069] The above mixture can, for example, run for 10 minutes to 1 hour.

[0070] In the third step, after the above-mentioned mixed powder is pressurized and molded, it is sintered to form a sintered body (S300).

[0071] Regarding the aforementioned pressure molding, a pressure of 4 to 12 tons / cm is preferred. 2 The pressure is 5 to 12 EA / min, but it is not limited to this.

[0072] Regarding the above sintering, it is preferred to perform the sintering at a temperature of 300°C to 1450°C for 10 minutes to 2 hours, but it is not limited to this.

[0073] For example, when the main counterweight material is brass and the specific gravity adjusting material is tungsten, a brass-tungsten sintered body can be manufactured by sintering at 600 to 1000°C for 20 to 40 minutes in an atmosphere containing N2 and H2.

[0074] In the fourth step, the sintered body can be pressurized again (S400).

[0075] To balance the miniaturization of the counterweight, higher density is more advantageous, but the sintered body described above may contain pores. Therefore, to maximize density, pressure can be applied as a post-processing step to minimize pores.

[0076] The aforementioned repressurization process allows the sintered body to be placed into a mold and pressure to be applied, thereby improving the dimensional accuracy and density of the sintered body.

[0077] During the aforementioned repressurization, the preferred pressure is 4 to 12 tons / cm². 2 However, it is not limited to this.

[0078] While powder metallurgy is less expensive than die casting, it struggles to achieve true density, resulting in lower density. Therefore, to mitigate this, appropriate addition of high-specific-gravity adjusting substances can be used to adjust the specific gravity to the desired level, or even to a higher level.

[0079] For example, when using brass forgings, machined products, die-cast products, etc., its specific gravity is 8.67 g / cm³. 3 When manufactured using powder metallurgy, 90 wt% brass is mixed with 10 wt% tungsten as a specific gravity adjuster. After forming, sintering, and repressurization processes, a yield of 8.67 g / cm³ can be obtained.3 The above specific gravity. Furthermore, by adding more specific gravity adjusting substances as needed, the size of the counterweight can be reduced, thus facilitating miniaturization.

[0080] In addition, powder metallurgy has high production efficiency, good material utilization, and high dimensional accuracy, and can produce near-final shapes, thus greatly reducing the need for machining.

[0081] Furthermore, when the average particle size of the above-mentioned specific gravity adjusting substance powder is less than 10 μm, between the step of selecting the above-mentioned main counterweight substance and specific gravity adjusting substance (S100) and the step of forming the above-mentioned mixed powder (S200), a step of granulating the above-mentioned specific gravity adjusting substance powder may also be included.

[0082] When the average particle size of the aforementioned gravity-adjusting material powder is less than 10 μm, uneven particle distribution and segregation may occur during the mixing process, and particle segregation and weight deviation between products may also occur during molding. Therefore, in order to increase the average particle size to more than 10 μm, the aforementioned granulation process is required.

[0083] The granulation process described above can be performed by mixing the specific gravity adjusting material powder with a slurry material containing liquid and binder, and then spraying and drying it under hot air conditions.

[0084] Ethanol or water can be used for the liquids mentioned above, but are not limited to these.

[0085] Regarding the aforementioned adhesive, polyvinyl butyral (PVB) or PVA (polyvinyl alcohol) can be used, but are not limited to these. The aforementioned adhesive performs the function of imparting bonding strength during granulation.

[0086] Through the above granulation process, the average particle size of the specific gravity regulating material powder becomes 10 μm or more, thus preventing segregation.

[0087] Manufacturing Example 1

[0088] After setting the target specific gravity to 8.5 or higher, brass, composed of 80 wt% Cu and 20 wt% Zn, was selected as the main weighting material, and tungsten (W) was selected as the specific gravity adjusting material. Next, brass powder with a particle size of 10–140 μm was prepared, and tungsten powder with a particle size of 2–10 μm was granulated to prepare tungsten particle powder with a particle size of 10–100 μm. Then, the brass powder and tungsten particle powder were prepared at a weight ratio of 90:10, and 0.7 wt% zinc stearate powder was added as a lubricant. The mixture was then mixed in a double cone mixer for approximately 10–40 minutes. Finally, the mixture was pressed in an automatic powder forming press at a speed of 4–10 ton / cm³. 3 The above-mentioned mixed powder was pressurized and shaped, and the shaped body was sintered in a reducing atmosphere (H2+N2 gas) at a temperature of 600-900°C. Then, it was pressurized again to produce a brass-tungsten sintered body.

[0089] Manufacturing Example 2

[0090] Compared to Manufacturing Example 1 above, except that the brass powder and the tungsten particle powder were prepared in a weight percentage ratio of 85:15, the brass-tungsten sintered body of Manufacturing Example 2 was manufactured in the same way.

[0091] Manufacturing Example 3

[0092] After setting the target specific gravity to 8.6 or higher, pure copper was selected as the main counterweight, and tungsten (W) was selected as the specific gravity adjuster. Next, pure copper powder with a particle size of 10–140 μm was prepared, and tungsten powder with a particle size of 2–10 μm was granulated to prepare tungsten granular powder with a particle size of 10–100 μm. Then, the pure copper powder and tungsten granular powder were prepared at a weight ratio of 93.5:6.5, with 0.7 wt% zinc stearate powder added as a lubricant, and mixed in a double cone mixer for approximately 10–40 minutes. Finally, the mixture was pressed in an automatic powder forming press at a speed of 4–10 ton / cm³. 3 The above-mentioned mixed powder was pressurized and shaped, and the shaped body was sintered in a reducing atmosphere (H2+N2 gas) at a temperature of 900-1080°C. Then, it was pressurized again to produce a pure copper-tungsten sintered body.

[0093] Manufacturing Example 4

[0094] Compared to Manufacturing Example 3 above, except that pure copper powder and the above-mentioned tungsten particle powder were prepared in a weight percentage ratio of 85:15, the pure copper-tungsten sintered body of Manufacturing Example 4 was manufactured in the same way.

[0095] Manufacturing Example 5

[0096] After setting the target specific gravity to 7.8 or higher, iron was selected as the main counterweight and tungsten as the specific gravity adjuster. Next, iron powder with a particle size of 10–140 μm was prepared, and tungsten powder with a particle size of 2–10 μm was granulated to prepare tungsten granular powder with a particle size of 10–100 μm. Then, the iron powder and tungsten granular powder were prepared at a weight ratio of 91.5:8.5, with 0.7 wt% zinc stearate powder added as a lubricant, and mixed in a double cone mixer for approximately 10–40 minutes. Finally, the mixture was pressed in an automatic powder forming press at a speed of 4–10 ton / cm³. 3 The above-mentioned mixed powder was pressurized and shaped, and the shaped body was sintered in a reducing atmosphere (H2+N2 gas) at a temperature of 1100-1400°C. Then, it was pressurized again to produce an iron-tungsten sintered body.

[0097] Manufacturing Example 6

[0098] Compared to Manufacturing Example 5 above, except that iron powder and tungsten particle powder were prepared in a weight ratio of 85:15, the pure copper-tungsten sintered body of Manufacturing Example 6 was manufactured in the same way.

[0099] Comparative Example 1

[0100] Purchased forgings, processed products or die-cast products made of brass with a zinc to copper ratio of 2:8.

[0101] Comparative Example 2

[0102] Purchased forgings, processed products, and die-cast products made of 100% copper (Cu).

[0103] Comparative Example 3

[0104] Purchased forgings, machined products, and die-cast products made of 100% iron (Fe).

[0105] Experimental Example

[0106] Table 1

[0107]

[0108]

[0109] Table 1 above shows the measured densities of the manufacturing examples and comparative examples. Referring to Table 1 above, the manufacturing examples manufactured by mixing with specific gravity adjusting substances and then sintering have a higher density than the comparative examples manufactured without mixing with specific gravity adjusting substances.

[0110] The electric compressor motor using a counterweight based on embodiments of the present invention can achieve the desired specific gravity by changing the content of the specific gravity-adjusting substance, thereby increasing the specific gravity to adjust the size, which is beneficial for miniaturization, improving motor design, and expanding the range of applicable equipment.

[0111] In addition, the use of powder metallurgy reduces processing steps and is economical.

[0112] It should be understood that the above description of the present invention is illustrative, and those skilled in the art can easily modify it into other specific embodiments without changing the technical concept or essential features of the invention. Therefore, it should be understood that the embodiments described above are illustrative and not limiting in all respects. For example, the constituent elements described in a single form can also be implemented separately, and similarly, the constituent elements described in a separate form can also be implemented in combination.

[0113] The scope of this invention is defined by the claims and should be interpreted as including all modifications or variations derived from the meaning, scope, and equivalent concepts of the claims.

[0114] Explanation of reference numerals in the attached figures

[0115] 10: Balance weight

Claims

1. A counterweight for an electric compressor motor, characterized in that, It comprises a main counterweight material and a specific gravity adjusting material, wherein the main counterweight material is brass and the specific gravity adjusting material is tungsten. The average particle size of the aforementioned main counterweight powder is 10 μm to 140 μm. The average particle size of the above-mentioned specific gravity adjusting material powder is 10 μm to 100 μm. The average particle size difference between the powder of the main counterweight substance and the powder of the specific gravity adjusting substance is less than 10 μm.

2. The counterweight for the electric compressor motor according to claim 1, characterized in that, The tungsten comprises more than 10 wt% of the total weight. The counterweight for the electric compressor motor has a specific gravity of 8.5 or higher.

3. A method for manufacturing a counterweight for an electric compressor motor, characterized in that, Include: The step of selecting a main counterweight material and a specific gravity adjusting material to achieve a target specific gravity, and making the average particle size difference between the powder of the main counterweight material and the powder of the specific gravity adjusting material less than 10 μm. The step of mixing the specific gravity adjusting substance powder and the main counterweight substance powder to form a mixed powder; The steps of pressing and molding the mixed powder and then sintering it to form a sintered body; and The step of applying pressure to the sintered body again; In the step of forming the mixed powder, The average particle size of the main counterweight powder is 10 μm to 140 μm; In the step of forming the mixed powder, The average particle size of the specific gravity adjusting material powder is 10 μm to 100 μm; The main counterweight is brass, and the specific gravity adjusting material is tungsten.

4. The method for manufacturing a counterweight for an electric compressor motor according to claim 3, characterized in that, Between the steps of selecting the main counterweight and the specific gravity adjusting substance and the step of forming the mixed powder... It also includes the step of granulating the powder of the specific gravity adjusting substance.

Citation Information

Patent Citations

  • Balance weight of motor

    KR1020050017849A

  • Sintered material, iron-based sintered sliding material and process for producing the same, sliding member and process for producing the same, and connecting apparatus

    CN101107376A

  • Balancing block of nonmagnetic compressor motor

    CN102517520A

  • Preparation method for alloy powder for producing balance block of compressor

    CN103658669A

  • Balance weight of rotater for a motor

    KR1020060031294A