Compositions and polymer films

By using a composition containing compound (I) to prepare a polymer membrane on a porous support, the problems of high resistance and easy foaming of bipolar membranes during fusion are solved, and a polymer membrane with low resistance, high ion exchange capacity and excellent pH stability is achieved, which is suitable for bipolar electrodialysis.

CN116234630BActive Publication Date: 2026-11-24FUJIFILM MANUFACTURING EUROPE BV +1
View PDF 30 Cites 0 Cited by

Patent Information

Application Number
CN202180065891.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-09-30
Filing Date
2021-09-27
Publication Date
2026-11-24
Estimated Expiration
2041-09-27

AI Technical Summary

Technical Problem

Existing bipolar membranes generate high resistance and are prone to bubbling during fusion, making them unattractive for commercial electrodialysis operations.

Method used

A polymer membrane is prepared on a porous support by using a composition comprising a compound of formula (I), a polymeric group, a solvent, and an optional free radical initiator, through photocuring or thermal curing methods, forming a cation exchange layer and an anion exchange layer, thereby optimizing the mechanical strength and electrical properties of the membrane.

Benefits of technology

The prepared polymer membrane has low resistance, high ion exchange capacity and excellent pH stability, and can provide high voltage at low current density, reducing energy costs and improving productivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116234630B_ABST
    Figure CN116234630B_ABST
Patent Text Reader

Abstract

This invention relates to a polymer film obtained by polymerizing a composition comprising: (a) a compound of formula (I), wherein: R is C 1‑4 Alkyl, NH2 or C 6‑12 Aryl; and M + The present invention relates to: (a) a cation; (b) a monomer containing at least two polymerizable groups; and (c) a solvent. The present invention also relates to compositions and methods for preparing polymer films.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This invention relates to compositions suitable for preparing polymer membranes, polymer membranes, cation exchange membranes, bipolar membranes, and their preparation and use.

[0002] Ion exchange membranes are used in electrodialysis, reverse electrodialysis, electrolysis, diffusion dialysis, and many other processes. Typically, ion transport across the membrane occurs under the influence of driving forces, such as ion concentration gradients or potential gradients.

[0003] Ion exchange membranes are typically classified into cation exchange membranes and anion exchange membranes based on their primary charge. Cation exchange membranes contain negatively charged groups that allow cations to pass through but repel anions, while anion exchange membranes contain positively charged groups that allow anions to pass through but repel cations. Bipolar membranes have both a cation layer and an anion layer.

[0004] Some ion exchange membranes and bipolar membranes contain porous supports that provide mechanical strength. Because of the presence of ionicly charged polymers that separate ions with opposite charges and porous supports that provide mechanical strength, these membranes are often referred to as "composite membranes".

[0005] Cation exchange membranes can be used to treat aqueous solutions and other polar liquids, and can also be used to generate electricity.

[0006] Bipolar membranes can be used to produce acids and bases from salt solutions, such as for the recovery of hydrofluoric acid and nitric acid, for the separation and treatment of organic acids such as lactic acid and citric acid, and for the production of amino acids.

[0007] Electrical energy can be generated using reverse electrodialysis (RED), in which standard ion exchange membranes or bipolar membranes can be used. Cation exchange membranes can also be used to produce hydrogen, for example, in fuel cells and batteries.

[0008] Bipolar membranes can be prepared by many different methods. In U.S. Patent Nos. 4,024,043 and 4,057,481 (both by Dege et al.), a single-membrane bipolar membrane is prepared from a pre-swollen membrane containing a relatively large amount of insoluble crosslinked aromatic polymer, on which highly dissociable cation exchange groups are chemically bonded to the aromatic nucleus to the desired depth of the membrane from only one side; subsequently, highly dissociable anion exchange groups are chemically bonded to the unreacted aromatic nucleus on the other side of the membrane.

[0009] In Japanese Patent Publications Nos. 78-158638 and 79-7196 (both Tokuyama Soda Co. Ltd.), a bipolar membrane is prepared by the following process: partially covering the membrane with a cover film, sulfonating the surface of the membrane that is not in contact with the cover film to introduce cation exchange groups, peeling off the cover film and introducing anion exchange groups on the peeled surface.

[0010] Bipolar membranes are also prepared by combining anion exchange membranes or membranes with cation exchange membranes or membranes. Two unipolar membranes with opposite selectivity can be fused together by heating and pressurization to form a bipolar membrane. For example, see Kollsman’s U.S. Patent No. 3,372,101, in which separate cation and anion membranes are combined in a hydraulic press at 150°C and a pressure of 400 Ib / sq. inch to form a bilayer bipolar membrane structure.

[0011] However, bipolar films formed in this way suffer from the drawback of high resistance resulting from their fusion. Furthermore, these films are prone to bubbling or forming water bubbles, and they can only operate for short periods at relatively low current densities.

[0012] The aforementioned drawbacks make known bipolar membranes unattractive for commercial electrodialysis operations.

[0013] According to a first aspect of the present invention, a composition is provided comprising:

[0014] (a) Compound of formula (I);

[0015]

[0016] in:

[0017] R is C 1-4 Alkyl, NH2 or C 6-12 Aryl; and

[0018] M + It is a cation;

[0019] (b) A monomer containing at least two polymerizable groups;

[0020] (c) Solvent; and

[0021] Optional (d) radical initiator.

[0022] Preferably, the composition of the first aspect of the present invention comprises:

[0023] (a) 5 to 60% by weight of component (a);

[0024] (b) 10 to 70% by weight of component (b);

[0025] (c) 10 to 50% by weight of component (c); and

[0026] (d) 0 to 10% by weight of the component (d).

[0027] In a preferred embodiment, M + It is H + Li + Na+ K + or NL4 + Each L is independently H or C 1-3 Alkyl group. Particularly preferred, M + It is Li + This is because it results in better solubility in aqueous liquids compared to many other cations.

[0028] Compounds of formula (I) can be obtained by methods similar to those described in the examples, or by commercial or known methods.

[0029] Examples of compounds of formula (I) that can be used as component (a) include compounds of formulas MM-A, MM-P and MM-M shown below.

[0030] Preferably, the composition comprises 5 to 60% by weight, more preferably 5 to 50% by weight, and most preferably 5 to 40% by weight of component (a).

[0031] Preferred polymerizable groups that may be present in component (b) include olefinically unsaturated groups, particularly (meth)acrylic acid groups and / or vinyl groups (e.g., vinyl ether groups, aromatic vinyl compounds, N-vinyl compounds and allyl groups).

[0032] Examples of suitable (meth)acrylic acid groups include acrylate (H2C=CHCO-) ​​groups, acrylamide (H2C=CHCONH-) groups, methacrylate (H2C=C(CH3)CO-) groups, and methacrylamide (H2C=C(CH3)CONH-) groups. Acrylic acid groups are preferred over methacrylic acid groups because they are more reactive.

[0033] Preferred olefinic unsaturated groups are free of ester groups, as this improves the stability and pH tolerance of the resulting composition. Olefinic unsaturated groups free of ester groups include vinyl groups.

[0034] As a preferred example of a polymerizable group, a group with the following formula may be mentioned:

[0035]

[0036] Optionally, component (b) further comprises anionic groups.

[0037] Preferably, in some embodiments, the composition comprises 10 to 70% by weight, more preferably 20 to 70% by weight, and most preferably 30 to 60% by weight of component (b).

[0038] Examples of monomers comprising at least two polymerizable groups that can be used as component (b) and further comprise anionic groups include compounds of formula (MA), (C), (ACL-A), (ACL-B), (ACL-C), and / or formula (II):

[0039]

[0040] In equation (MA):

[0041] Each R A1 Independently representing a hydrogen atom or an alkyl group;

[0042] Each Z 1 Independently represented as -O- or -NRa-, where Ra represents a hydrogen atom or an alkyl group; and

[0043] Each M + Independently as defined above.

[0044] In equation (MA), each M + The preferred solutions are defined independently as above. In one implementation, each M + It can be an organic or inorganic cation independently, preferably H. + Or alkali metal ions.

[0045] Examples of component (b) of formula (MA) include the following and their salts:

[0046]

[0047] Synthetic methods can be found, for example, in US2015 / 0353696 and US2016 / 0369017.

[0048]

[0049] In equation (C):

[0050] Each L 1 Independently representing alkylene or aralkylene;

[0051] n can be 2 or 3, with 2 being the preferred choice;

[0052] Each m is independently 1 or 2;

[0053] L 2 Indicates an n-valent linker group;

[0054] Each R 1 Independently representing a hydrogen atom or an alkyl group;

[0055] Each R 2 Independently represent -SO3- M + or -SO3 - R 3 ;

[0056] Each M + Independently as defined above; and

[0057] R 3 This indicates an alkyl group or an aryl group.

[0058] In one embodiment of formula (C), M + It is H + Inorganic or organic ions. Examples of component (b) of formula (C) include the following and their alternative salts:

[0059]

[0060] The synthesis method can be found in EP3187516.

[0061]

[0062] In equations (ACL-A), (ACL-B), and (ACL-C):

[0063] R and R' each independently represent a hydrogen atom or an alkyl group;

[0064] LL represents a single bond or a divalent linker;

[0065] LL 1 LL 1 ′、LL 2 and LL 2 Each ' independently represents a single bond or a divalent bonded atom or group;

[0066] A and A' each independently represent a sulfonyl group in the form of a methyl group, a free acid, or a salt; and

[0067] m represents 1 or 2.

[0068] Examples of component (b) of formula (ACL-A), (ACL-B), or (ACL-C) include the following and their alternative salts:

[0069] The synthesis method can be found in US2016 / 0362526.

[0070]

[0071] in:

[0072] R' is vinyl (C2H3), epoxy (C2H3O), or C 1-3alkylene mercapto (C 1-3 Alkylene (SH):

[0073] n is 1 or 2;

[0074] The value of m is 1, 2, or 3;

[0075] M ’+ It is H + Li + Na + K + Or NL4 + Each L is independently H or C 1-3 alkyl;

[0076] in:

[0077] (a) When both m and n are 1, X is a vinylphenyl or formula (III):

[0078]

[0079] In equation (III):

[0080] R” represents vinyl (C2H3), epoxy (C2H3O), or C 1-3 alkylene mercapto (C 1-3 Alkylene (SH); and

[0081] M” + It is H + Li + Na + K + or NL4 + Each L is independently H or C 1-3 alkyl;

[0082] (b) When neither m nor n is 1, then X is C 1-6 Alkylene, C 6-18 Aromatic or NR”' (3-m) Each R”' is independently H or C1-C4 alkyl;

[0083] (c) When the value of m is 1 and the value of n shown in equation (II) is 2, then X is equation (III) (as defined above) or C. 1-6 Alkyl, C 6-18 Aryl or N(R”')2, where each R”' is independently H or C. 1-4 alkyl.

[0084] Examples of component (b) of formula (II) include the following and their alternative salts:

[0085]

[0086] Synthesis methods can be found, for example, in JP2018043936.

[0087] Other examples of component (b) include compounds M-23 to M-34 and their salts, as shown below:

[0088]

[0089] Preferably, component (b) is selected from compounds of formula (ACL-B), (ACL-C) and their salts and / or formula (II), as this enables the polymer membrane to have good pH stability. Preferably, the composition contains at least 10% by weight of component (b) selected from compounds of formula (ACL-B), (ACL-C) and their salts and / or formula (II), more preferably at least 20% by weight.

[0090] Preferably, component (c) is an inert solvent. In other words, preferably, component (c) does not react with any other component of the curable composition. In one embodiment, the solvent preferably comprises water and optionally an organic solvent, particularly wherein some or all of the organic solvent is water-miscible. Water can be used to dissolve component (a) and possibly also component (b), and the organic solvent can be used to dissolve any other organic components present in the composition.

[0091] Component (c) can be used to reduce the viscosity and / or surface tension of the composition. In some embodiments, the composition contains 10 to 50% by weight, more preferably 10 to 40% by weight, particularly 16 to 40% by weight, for example 23 to 38% by weight of component (c).

[0092] Examples of inert solvents that can be used as component (c) include water, alcohol solvents, ether solvents, amide solvents, ketone solvents, sulfoxide solvents, sulfone solvents, nitrile solvents, and organophosphorus solvents. Examples of alcohol solvents that can be used or used in combination with water (particularly with water) include methanol, ethanol, isopropanol, n-butanol, ethylene glycol, propylene glycol, diethylene glycol, dipropylene glycol, and mixtures containing two or more of these. Additionally, preferred inert organic solvents that can be used for component (c) include dimethyl sulfoxide, dimethylimidazolinone, sulfolane, N-methylpyrrolidone, dimethylformamide, acetonitrile, acetone, 1,4-dioxane, 1,3-dioxolane, tetramethylurea, hexamethylphosphoramide, hexamethylphosphoric triamine, pyridine, propionitrile, butanone, cyclohexanone, tetrahydrofuran, tetrahydropyran, 2-methyltetrahydrofuran, ethylene glycol diacetate, cyclopentylmethyl ether, methyl ethyl ketone, ethyl acetate, γ-butyrolactone, and mixtures containing two or more of these. Preferably, dimethyl sulfoxide, N-methylpyrrolidone, dimethylformamide, dimethylimidazolinone, sulfolane, acetone, cyclopentylmethyl ether, methyl ethyl ketone, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, and mixtures containing two or more of these are preferred.

[0093] The composition preferably contains 0 to 2% by weight of component (d). When it is intended to cure the composition by heat or by using light (e.g., UV or visible light), the composition preferably contains 0.001 to 2% by weight, particularly 0.005 to 0.9% by weight of component (d).

[0094] Examples of suitable thermal initiators that can be used as component (d) include: 2,2'-azobis(2-methylpropionitrile) (AIBN), 4,4'-azobis(4-cyanopentanoic acid), 2,2'-azobis(2,4-dimethylpentanonitrile), 2,2'-azobis(2-methylbutanonitrile), 1,1'-azobis(cyclohexane-1-carboxylonitrile), 2,2'-azobis(4-methoxy-2,4-dimethylpentanonitrile), dimethyl 2,2'-azobis(2-methylpropionate), 2,2'-azobis[N-(2-propenyl)-2-methylpropionamide, 1-[(1-cyano-1-methylethyl)azo]formamide, 2,2'-azobis(N-butyl-2-methylpropionamide), 2,2'-azobis(N-cyclohexyl-2-methylpropionamide), 2,2'-azobis(2-methylpropionamide) 2,2'-Azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride, 2,2'-Azobis[2-(2-imidazolin-2-yl)propane] disulfate dihydrate, 2,2'-Azobis[N-(2-carboxyethyl)-2-methylpropane] hydrate, 2,2'-Azobis{2-[1-(2-hydroxyethyl)-2-imidazolin-2-yl]propane] hydrate Alkyl dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane], 2,2'-azobis(1-imino-1-pyrrolidin-2-ethylpropane) dihydrochloride, 2,2'-azobis{2-methyl-N-[1,1-di(hydroxymethyl)-2-hydroxyethyl]propionamide} and 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide].

[0095] Examples of suitable photoinitiators that can be included as component (d) in the composition include aromatic ketones, acylphosphine compounds, aromatic onium salts, organic peroxides, thio compounds, hexaaryl biimidazole compounds, ketooxime esters, borate compounds, azadinium compounds, metallocene compounds, active ester compounds, compounds having carbon-halogen bonds, and alkylamine compounds. Preferred examples of aromatic ketones, acylphosphine oxide compounds, and thio compounds include compounds having a benzophenone backbone or a thioxanone backbone, described in “RADIATION CURING IN POLYMER SCIENCE AND TECHNOLOGY”, pp. 77-117 (1993). More preferred examples include α-thiobenzophenone compounds described in JP1972-6416B (JP-S47-6416B), JP1972-3981B (JP-S47-3981). Benzoin ether compounds described in B), α-substituted benzoin compounds described in JP1972-22326B (JP-S47-22326B), benzoin derivatives described in JP1972-23664B (JP-S47-23664B), aromatic phosphonates described in JP1982-30704A (JP-S57-30704A), dialkoxybenzophenones described in JP1985-26483B (JP-S60-26483B), benzoin ethers described in JP1985-26403B (JP-S60-26403B) and JP1987-81345A (JPS62-81345A), JP1989-34242B (JPH01-34242B), and the United States The following are listed: α-aminobenzophenone as described in patents 4,318,791A and EP0284561A1; p-bis(dimethylaminobenzoyl)benzene as described in JP1990-211452A (JP-H02-211452A); thiosubstituted aromatic ketones as described in JP1986-194062A (JPS61-194062A); acylphosphine sulfides as described in JP1990-9597B (JP-H02-9597B); acylphosphine as described in JP1990-9596B (JP-H02-9596B); thioxanthone as described in JP1988-61950B (JP-S63-61950B); and coumarin as described in JP1984-42864B (JP-S59-42864B). In addition, the photoinitiators described in JP2008-105379A and JP2009-114290A are also preferred.Alternatively, the photoinitiator described on pages 65-148 of "Ultraviolet Curing System" by Kato Kiyomi (Research Center Co., Ltd., published in 1989) can be used.

[0096] Particularly preferred photoinitiators include Norrish type II photoinitiators, which exhibit maximum absorption at wavelengths greater than 380 nm when measured at 23°C in one or more of the following solvents: water, ethanol, and toluene. Examples include xanthones, flavonoids, curcumin, porphyrins, anthraquinones, phenoxazines, camphorquinones, phenazines, acridines, phenothiazines, xanthonesones, thioxanthonesones, thioxanthones, acridine ketones, flavonoids, coumarins, fluorenones, quinoline, quinolones, naphthoquinones, quinolinones, arylmethanes, azo compounds, benzophenones, carotenoids, anthocyanins, phthalocyanines, dipyrrole methylene, squarine, stilbene, styryl, triazine, or anthocyanin-derived photoinitiators.

[0097] According to a second aspect of the invention, a method for preparing a polymer film is provided, comprising polymerizing a composition comprising a compound of formula (I), wherein the compound of formula (I) is as defined above.

[0098] In a second aspect of the invention, preferred embodiments of the compound of formula (I) are as defined herein with respect to a first aspect of the invention.

[0099] In a second aspect of the invention, the composition is preferably as defined with respect to the first aspect of the invention. Preferred embodiments of the compositions used in the method of the second aspect of the invention are as described herein with respect to the first aspect of the invention.

[0100] The composition can be cured by any suitable method to prepare the film of the second aspect of the invention, including thermal curing, photocuring, electron beam (EB) irradiation, gamma irradiation, and combinations thereof. Optionally, dual curing—defined as a combination of the two curing techniques described above—can be used. However, the composition is preferably cured by photocuring (e.g., by irradiating the composition with ultraviolet or visible light), thereby polymerizing the curable components present in the composition.

[0101] Preferably, polymerization is carried out in the presence of a porous support. For example, the compound / composition of formula (I) of the first aspect of the invention is present in and / or on a porous support. The porous support provides mechanical strength to the polymer membrane produced by polymerization, which is particularly useful when the polymer membrane is intended to be used as a cation exchange membrane (CEM) or a bipolar membrane (BPM).

[0102] Examples of porous carriers that can be used include woven and nonwoven synthetic fabrics and extruded membranes. Examples include wet-laid and dry-laid nonwoven materials, spunbond and meltblown fabrics, and nanofiber webs made from, for example, polyethylene, polypropylene, polyacrylonitrile, polyvinyl chloride, polyphenylene sulfide, polyester, polyamide, polyaryletherketone (e.g., polyetheretherketone) and their copolymers. Porous carriers can also be porous membranes, such as polysulfone, polyethersulfone, polyphenylene sulfone, polyphenylene sulfide, polyimide, polyetherimide, polyamide, polyamide-imide, polyacrylonitrile, polycarbonate, polyacrylate, cellulose acetate, polypropylene, poly(4-methyl-1-pentene), polyvinylidene fluoride, polytetrafluoroethylene, polyhexafluoropropylene, and polychlorotrifluoroethylene membranes and their derivatives.

[0103] The average thickness of the porous carrier is preferably 10 to 800 μm, more preferably 15 to 300 μm, and particularly 20 to 150 μm.

[0104] Preferably, the porous support has a porosity of 30% to 95%. The porosity of the support can be measured using a porosimeter such as Porolux from IB-FT GmbH, Germany. TM 1000 was measured.

[0105] The porous support (if present) can be treated to alter its surface energy, for example, to a value higher than 45 mN / m, preferably higher than 55 mN / m. Suitable treatments include corona discharge treatment, plasma glow discharge treatment, flame treatment, ultraviolet irradiation treatment, or chemical treatment, for example, to improve the wettability of the porous support and its adhesion to polymer films.

[0106] Commercially available porous carriers are available from many sources, such as Freudenberg Filtration Technologies (Novatexx materials), Lydall Performance Materials, Celgard LLC, APorous Inc., SWM (Conwed Plastics, DelStar Technologies), Teijin, Hirose, Mitsubishi Paper Mills Ltd and Sefar AG.

[0107] Preferably, the carrier is a polymer carrier. More preferably, the carrier is a woven or nonwoven synthetic fabric or extruded film that does not contain covalently bonded ionic groups.

[0108] According to a third aspect of the present invention, a polymer film obtained by the method of the second aspect of the present invention is provided.

[0109] Preferably, the polymer membrane is a cation exchange membrane (CEM) or a bipolar membrane (BPM) comprising a cation exchange layer (CEL), which is obtained by polymerizing the composition of the first aspect of the invention and / or by the method of the second aspect of the invention. Preferably, the BPM further comprises an anion exchange layer (AEL).

[0110] Preferably, the polymer film obtained by the method of the second aspect of the present invention comprises structural groups of formula (A):

[0111]

[0112] Where M + The preferred cation is the one defined above.

[0113] In formula (A), * indicates the position where the structural group is covalently attached to other structural elements of the polymer film.

[0114] In a preferred method of the second aspect of the invention, the curable composition of the first aspect of the invention is preferably continuously applied to a moving (porous) carrier by a manufacturing unit comprising a curable composition application station, one or more irradiation sources for curing the composition, a membrane collection station, and means for moving the carrier from the curable composition application station to the irradiation sources and the membrane collection station.

[0115] The curable composition application station may be located upstream of the irradiation source, and the irradiation source may be located upstream of the membrane collection station.

[0116] Examples of suitable coating techniques for applying the curable composition of the first aspect of the invention to a porous carrier include slot coating, glide coating, air knife coating, roll coating, screen printing, and dip coating. Depending on the technique used and the desired end specifications, excess coating may need to be removed from the substrate by, for example, roll-to-roll extrusion, roll-to-blade or blade-to-roll extrusion, blade-to-blade extrusion, or by removing the coating bar. Photocuring is preferably performed at wavelengths from 400 nm to 800 nm using 40 to 1500 mJ / cm². -2 The dosage is administered. In some cases, additional drying may be required, which can be performed at temperatures ranging from 40°C to 200°C.

[0117] The method of the second aspect of the invention can be used in several ways (including multi-pass and single-pass methods) to prepare the polymer films (e.g., CEM and BPM) of the third aspect of the invention. For example, in a two-pass method, each layer of BPM (e.g., CEL and AEL) can be produced in a separate step. In a first step of manufacturing the first layer, an optional pretreated porous carrier can be impregnated with a first curable composition. To ensure a thin and pinhole-free film, extrusion is preferably performed after the coating step. The impregnated carrier can then be cured to produce a hard layer sufficient for processing in a coating machine, but still containing sufficient unreacted polymeric groups to ensure good adhesion to the second layer. In the second step, a method very similar to that of the first layer is employed: the optional pretreated porous carrier can be impregnated with a second curable composition and laminated to the first layer, then excess composition is extruded and cured.

[0118] In an alternative method for preparing BPM, a second layer can be coated onto the first layer, and then an optionally pretreated porous carrier can be laminated onto one side of the second curable composition, thereby impregnating the porous carrier with the second curable composition. The resulting laminate can be extruded and cured to produce a composite film.

[0119] In the two methods described above, preferably, the first curing composition or the second curing composition is as defined in the first aspect of the present invention.

[0120] In a more preferred single-pass method for preparing BPM, two optional pretreated porous supports are unwound, and each support is impregnated with a curable composition (e.g., simultaneously or continuously), one curable composition as defined in the first aspect of the invention to obtain a CEL, and the other curable composition containing at least one cationic curable monomer to provide an AEL. The two layers (the CEL from the composition of the first aspect of the invention and the AEL from the other curable composition) are then laminated together and extruded, and the resulting laminate is then cured to produce the final BPM.

[0121] The efficiency of BPM in the third aspect of the present invention can be improved by increasing the surface area between AEL and CEL, for example by physical treatment (roughening) or by other means.

[0122] In one embodiment, the BPM of the third aspect of the present invention may optionally include a catalyst, such as a metal salt, metal oxide, organometallic compound, monomer, polymer or copolymer or salt, preferably containing the catalyst at the interface of the CEL and AEL of the BPM.

[0123] Suitable inorganic compounds or salts that can be used as catalysts include cations selected from, for example, Groups 1a to 4a (inclusive) of the periodic table, as well as lanthanides and actinides, such as thorium, zirconium, iron, lanthanum, cobalt, cadmium, manganese, cerium, molybdenum, nickel, copper, chromium, ruthenium, rhodium, tin, titanium, and indium, as well as combinations containing two or more of the above. Suitable salts that can be used as catalysts include anions such as tetraborate, metaborate, silicate, metasilicate, tungstate, chlorate, phosphate, sulfate, chromate, hydroxyl, carbonate, molybdate, chloroplatinate, chloropaladite, orthovandate, tellurate, etc., as well as combinations containing two or more of the above.

[0124] Other examples of inorganic compounds or salts that can be used as catalysts include, but are not limited to, FeCl3, FeCl2, AlCl3, MgCl2, RuCl3, CrCl3, Fe(OH)3, Al2O3, NiO, Zr(HPO4)2, MoS2, graphene oxide, Fe-polyvinyl alcohol complexes, polyvinyl alcohol (PVA), polyethylene glycol (PEG), polyethyleneimine (PEI), polyacrylic acid (PAA), copolymers of acrylic acid and maleic anhydride (PAAMA), and hyperbranched aliphatic polyesters, as well as combinations comprising two or more of the above.

[0125] As a result of preparing CEMs from the composition of the first aspect of the invention (having a low amount of component (c), for example, 10 to 40% by weight of component (c)), the CEMs (polymer membranes) of the third aspect of the invention preferably have very high densities. Therefore, the present invention is capable of producing polymer membranes (e.g., CEMs and BPMs) with very high ion exchange capacity and thus high selectivity and low resistance (ER).

[0126] Preferably, the ER (for 0.5M NaCl) is less than 5 Ω·cm. 2 More preferably, below 2.5Ω·cm 2 .

[0127] Preferably, component (b) of the composition comprises a compound of formula (ACL-B), (ACL-C) and / or formula (II) (including the salts mentioned above), as this can enable the polymer membrane (e.g., CEM and BPM) to have excellent pH stability in the range of 0 to 14.

[0128] Furthermore, the CEM and BPM incorporating the cation exchange layer (CEL) of the present invention have low resistance. As a result, the CEM and BPM of the present invention can be used in bipolar electrodialysis to provide high voltage at low current densities. Therefore, when the BPM of the present invention is used in bipolar electrodialysis methods for producing acids and bases, they can provide low energy costs and / or high productivity.

[0129] In one embodiment, the polymer membrane of the third aspect of the present invention is preferably a bipolar membrane or a membrane that can be converted into a bipolar membrane by hydrolysis.

[0130] The anion exchange layer (AEL) of the bipolar membrane is preferably obtained by curing a composition containing a curable cationic compound (i.e., the AEL composition). Therefore, the AEL composition preferably contains a curable cationic compound.

[0131] Preferred curable cationic compounds comprise at least two olefinically unsaturated groups, such as compounds of formula (IV):

[0132]

[0133] in:

[0134] L 1 It is an alkylene or alkenylene group;

[0135] R a R b R c and R d Each is independently an alkyl group or an aryl group, or

[0136] R a and R b , and / or R c and R d They can form rings together with the atoms they are attached to;

[0137] n1 and n2 each independently represent integers from 1 to 10; and

[0138] X1 - and X2 - Each can be used to represent anion independently.

[0139] L 1 Preferably, it is ethylidene (CH2CH2), alkenylidene (CH2CH2CH2), hexylidene (CH2CH2CH2CH2CH2CH2), or vinylidene (CH=CH).

[0140] When R a R b R c and R d When any one of them is an alkyl group, C is preferred. 1-4 Alkyl groups, especially methyl groups.

[0141] When R a R b R c and R dWhen any one of them is an aryl group, C is preferred. 6-10 Aryl groups, especially phenyl groups.

[0142] When R a and R b , and / or R c and R d When the atoms to which they are attached form a ring, the ring is preferably a 5-membered or 6-membered ring.

[0143] By X1 - and X2 - The anions represented are preferably halogens, especially Cl-. - .

[0144] Therefore, the AEL composition preferably contains the following components:

[0145] (a2) A cured cationic compound containing at least two olefinic unsaturated groups;

[0146] Option (b2) is a compound containing one and only one olefinic unsaturated group;

[0147] Optional (c2) solvent; and

[0148] Optional (d2) radical initiator.

[0149] Preferably, the AEL composition comprises at least one of components (b2), (c2) and (d2), more preferably at least two, and particularly all three.

[0150] Examples of compounds of formula (IV) include the following:

[0151]

[0152] Synthetic methods can be found, for example, in EP3184558 and US2016 / 0001238.

[0153] The AEL composition preferably contains 30 to 80% by weight of component (a2), more preferably 40 to 70% by weight of component (a2).

[0154] Preferably, the AEL composition comprises:

[0155] (i) 30 to 80% by weight of the component (a2);

[0156] (ii) 0 to 40% by weight of component (b2); and

[0157] (iii) 10 to 40% by weight of the component (c2).

[0158] Component (b2) preferably contains aromatic groups.

[0159] Component (b2) preferably contains cationic groups.

[0160] Examples of compounds that can be used as component (b2) in AEL compositions include the following:

[0161]

[0162] The above compounds can be prepared as described, for example, in US2016177006.

[0163] Preferably, the molar ratio of component (a2) to component (b2) is 9:1 to 1:4.

[0164] The AEL composition comprises 0 to 60% by weight, more preferably 5 to 45% by weight, and most preferably 10 to 40% by weight of component (b2).

[0165] Component (c2) of the AEL composition preferably includes water and an optional organic solvent, particularly wherein some or all of the organic solvent is water-miscible. Water may be used to dissolve the (IV) compound and component (c2) (if present). The solvent may be used to reduce the viscosity and / or surface tension of the composition.

[0166] Examples of suitable solvents that can be used as component (c2) of an AEL composition include water, alcohol solvents, ether solvents, amide solvents, ketone solvents, sulfoxide solvents, sulfone solvents, nitrile solvents, organophosphorus solvents, and mixtures containing two or more of these. Examples of alcohol solvents that can be used as or for component (c2) (especially in combination with water) include methanol, ethanol, isopropanol, n-butanol, ethylene glycol, propylene glycol, diethylene glycol, dipropylene glycol, and mixtures containing two or more of these. Additionally, preferred inert organic solvents that can be used for component (c2) include dimethyl sulfoxide, dimethylimidazolinone, sulfolane, N-methylpyrrolidone, dimethylformamide, acetonitrile, acetone, 1,4-dioxane, 1,3-dioxolane, tetramethylurea, hexamethylphosphoramide, hexamethylphosphoric triamine, pyridine, propionitrile, butanone, cyclohexanone, tetrahydrofuran, tetrahydropyran, 2-methyltetrahydrofuran, ethylene glycol diacetate, cyclopentylmethyl ether, methyl ethyl ketone, ethyl acetate, γ-butyrolactone, and mixtures containing two or more of these. Preferably, dimethyl sulfoxide, N-methylpyrrolidone, dimethylformamide, dimethylimidazolinone, sulfolane, acetone, cyclopentylmethyl ether, methyl ethyl ketone, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, and mixtures containing two or more of these are preferred.

[0167] In some embodiments, the AEL composition comprises 10 to 40% by weight, more preferably 10 to 35% by weight, and most preferably 15 to 30% by weight of component (c2).

[0168] Examples of components (c2) to (d2) that may be included in an AEL composition for forming an AEL include those described above for compositions used as components (c) and (d) for a CEL, respectively. However, component (c2) of the AEL composition is preferably aqueous.

[0169] Component (d2) is preferably or contains a thermal initiator, a photoinitiator, or a combination thereof. Most preferably, component (d) is or contains a photoinitiator.

[0170] Examples of suitable photoinitiators that can be used as component (d2) of an AEL composition include those described above for the compositions of the first aspect of the invention.

[0171] The AEL composition preferably contains 0.001 to 2% by weight of component (d2), more preferably 0.005 to 0.9% by weight.

[0172] The AEL and CEL compositions may optionally each further comprise a polymerization inhibitor independently. The polymerization inhibitor may be used to stabilize the composition during storage and use.

[0173] As polymerization inhibitors, well-known polymerization inhibitors can be used. Examples include phenolic compounds, hydroquinone compounds, certain amine compounds, thiol compounds, and nitrocellulose free radical compounds.

[0174] Examples of phenolic compounds include hindered phenols (phenols with a tert-butyl group at the ortho position, and representative examples include 2,6-di-tert-butyl-4-methylphenol) and bisphenols. Specific examples of hydroquinone compounds include monomethyl ether hydroquinone. Specific examples of amine compounds include N-nitroso-N-phenylhydroxylamine and N,N-diethylhydroxylamine. Specific examples of nitroacyl radical compounds include 4-hydroxyTEMPO (4-hydroxy-2,2,6,6-tetramethylpiperidin-1-oxy radical).

[0175] The AEL composition and the CEL composition may optionally each independently further comprise two or more polymerization inhibitors.

[0176] When the composition used to form AEL or CEL contains a polymerization inhibitor, its content is preferably 0.01 to 5% by weight, more preferably 0.01 to 1% by weight, and even more preferably 0.01 to 0.5% by weight, relative to the total weight of the composition.

[0177] The AEL composition and the CEL composition may optionally each further comprise, independently, a surfactant, a polymer dispersant, and / or a crater inhibitor.

[0178] To adjust the film physical properties of the AEL composition and / or CEL composition, various polymer compounds may be included. Suitable polymer compounds include acrylic polymers, polyurethane resins, polyamide resins, polyester resins, epoxy resins, phenolic resins, polycarbonate resins, polyvinyl butyral resins, polyvinyl formal resins, shellac, vinyl resins, acrylic resins, rubber-based resins, waxes, and natural resins, as well as combinations of two or more of the above.

[0179] The AEL and CEL compositions may optionally, independently, further comprise surfactants, such as nonionic surfactants, cationic surfactants, or organofluorine surfactants. Specific examples of surfactants include anionic surfactants (e.g., alkylbenzene sulfonates, alkylnaphthalene sulfonates, higher fatty acid salts, sulfonates of higher fatty acid esters, sulfates of higher alcohol ethers, sulfonates of higher alcohol ethers, alkyl carboxylates and alkyl phosphates of higher alkyl sulfonamides) and nonionic surfactants (e.g., poly(ethylene oxide) alkyl ethers, poly(ethylene oxide) alkylphenyl ethers, poly(ethylene oxide) fatty acid esters, sorbitan fatty acid esters, ethylene oxide adducts of acetylenic glycols, ethylene oxide adducts of glycerols, and polyoxyethylene sorbitan fatty acid esters). Other suitable examples of surfactants include amphoteric surfactants (e.g., alkyl betaines and amide betaines), organosilicon surfactants, and fluorinated surfactants. Surfactants may suitably be selected from surfactants known in the art or derivatives thereof.

[0180] The AEL composition and the CEL composition may optionally each further comprise a polymer dispersant independently.

[0181] Specific examples of polymer dispersants include polyvinylpyrrolidone, polyvinyl alcohol, polyvinyl methyl ether, polyethylene oxide, polyethylene glycol, polypropylene glycol, and polyacrylamide. Among these, polyvinylpyrrolidone is preferred.

[0182] The AEL composition and CEL composition may optionally each independently further comprise an anti-cratering agent (sometimes called a surface conditioner), a leveling agent, or a slip agent to prevent unevenness of the CEL or AEL surface. Examples include organically modified polysiloxanes (mixtures of polyether siloxanes and polyethers), polyether-modified polysiloxane copolymers, and silicone-modified copolymers.

[0183] Examples of commercially available surfactants that can be included in compositions used to form AEL and / or CEL include Tego Glide manufactured by Evonik Industries GmbH. TM 432. Tego Glide TM 110. Tego GlideTM 130. Tego Glide TM 406. Tego Glide TM 410. Tego Glide TM 411. Tego Glide TM 415. Tego Glide TM 420. Tego Glide TM 435. Tego Glide TM 440. Tego Glide TM 450. Tego Glide TM 482. TegoGlide TM A115, Tego Glide TM B1484 and Tego Glide TM ZG400 (both are product names).

[0184] The AEL composition and the CEL composition preferably each independently contain 0 to 10% by weight, more preferably 0 to 5% by weight, and especially 1 to 2% by weight of an anti-cracking agent (relative to the total weight of the relevant composition).

[0185] In a preferred embodiment, the bipolar membrane comprises a catalyst. The catalyst may be contained in the AEL composition and / or the CEL composition curable composition. The catalyst may also be applied to the AEL (e.g., before the CEL composition is applied thereon) as a post-treatment step using methods such as (but not limited to) impregnation, air knife coating, micro-roll coating, spraying, chemical (vapor) deposition, or physical (vapor) deposition.

[0186] Examples of suitable catalysts are described above.

[0187] When the AEL composition or CEL composition contains a catalyst, the amount of catalyst is preferably up to 5% by weight, for example, from 0.001% by weight to 1% by weight, relative to the weight of the relevant composition.

[0188] Bipolar films can be prepared by a method including the following steps:

[0189] (i) Applying the AEL composition to a carrier;

[0190] (ii) Curing the AEL composition at least partially to form an anion exchange layer (AEL);

[0191] (iii) Applying the CEL composition to the AEL; and

[0192] (iv) Curing the CEL composition to form a cation exchange layer (CEL) on the AEL.

[0193] In step (ii), preferably, the AEL composition is photocured, for example, using ultraviolet light. Therefore, preferably, component (d2) of the AEL composition is or contains a photoinitiator.

[0194] In step (ii), preferably, the AEL composition is cured to such an extent that the resulting AEL can be processed in a curable composition application station while still containing unreacted olefinic unsaturated groups of monomers that can be crosslinked to the CEL composition.

[0195] In step (iv), the CEL composition is preferably thermosetting. Therefore, preferably, component (d) of the CEL composition is or contains a thermal initiator.

[0196] The suitable temperature for curing the CEL composition is 50 to 120°C, more preferably 50 to 100°C, and particularly 60 to 85°C.

[0197] Thermosetting of CEL compositions typically takes anywhere from one minute to several hours.

[0198] Optionally, the CEL composition is sandwiched between polymer films and then cured to prevent component (c) (if present) from evaporating.

[0199] The composition is preferably applied in a continuous manner in steps (i) and (iii) via a manufacturing unit comprising a composition application station, one or more curing stations including an irradiation source (when the composition is photocurable), one or more curing stations including one or more heat sources (when the composition is thermocurable), a bipolar film collection station, and means for moving a carrier from the composition application station to the curing station and the bipolar film collection station.

[0200] The composition application station may be located upstream of the curing station, and the curing station may be located upstream of the bipolar membrane collection station.

[0201] Examples of application techniques include slot coating, glide coating, air knife coating, roll coating, screen printing, and dip coating. Depending on the technique used and the required end specifications, excess composition may need to be removed from the substrate by, for example, roll-to-roll extrusion, roll-to-blade or blade-to-roll extrusion, blade-to-blade extrusion, or by removing the coating bar.

[0202] UV or visible light curing is preferably performed at wavelengths from 100 nm to 800 nm, typically using 40 to 1500 mJ / cm². 2 The light dose is applied. Thermocuring is preferably carried out at a temperature of 20°C to 100°C for a time of, for example, 0.01 hours to 24 hours.

[0203] The performance of the bipolar membrane was characterized by an intensity vs. voltage curve. A six-chamber cell was used to measure this curve. The first electrode chamber contained a platinum plate as the cathode and was separated from the second chamber by a CEM (CMX from Astom). The electrode chamber was filled with 0.5 M Na₂SO₄. A reference BPM (from Fumatech) was placed between the second and third chambers. Both the second and third chambers contained 0.5 M NaCl solution. The BPM to be analyzed was placed between the third and fourth chambers. The same reference BPM (from Fumatech) was placed between the fourth and fifth chambers, and a CEM (CMX from Astom) was placed between the fifth and sixth chambers. The fourth and fifth chambers were also filled with 0.5 M NaCl solution. The sixth chamber, containing a platinum plate as the anode, was the electrode chamber and contained 0.5 M Na₂SO₄.

[0204] By using the aforementioned battery cell, the solution is subjected to an application of 600 A / m at a temperature of 25°C. 2 The current density is pumped through the compartment. The bipolar voltage is measured by using Harber luggin capillaries placed on each side of the BPM to be analyzed. Example

[0205] Table 1: Ingredients

[0206]

[0207]

[0208] The lithium content of the prepared compound of formula (I) was quantified using inductively coupled plasma atomic emission spectrometry (ICP-OES). Thermo iCAP from Thermo Fisher Scientific was used. TM ICP-OES analysis was performed using the PRO XP ICP-OES instrument. A concentric nebulizer was used in conjunction with a cyclone chamber. Approximately 50 mg of each analyte was dissolved in a 50 cm³ solution. 3 The dissolved compound was diluted 100-fold in Milli-Q water and acidified with 0.5% concentrated nitric acid containing yttrium as an internal standard. All samples were prepared and measured in duplicate. Results are expressed as g Li / kg monomer.

[0209] The structure of compound (I) was obtained using a Magritek Spincolve 60-carbon (60 MHz, 4 scans) NMR spectrometer. 1 ¹H-NMR confirmed the results. Analytical samples were prepared by dissolving 5% by weight of each compound of formula (I) in DMSO-d6.

[0210] The purity of compound (I) was determined by HPLC-MS. A Waters ACQUITY UPLC system with 2D technology was used. This UPLC is equipped with two pumps (BSM and QSM), an FTN sample manager, a column manager, and a PDA detector (192 to 400 nm). The HPLC was equipped with a Waters Xbridge C8 5 μm 2.1*150 mm column operating at 45 °C. Additionally, the instrument was equipped with a Waters Q-TOF premier mass spectrometer with ESI and ESCi ionization options. Chromatograms were collected using dual detection mode. The PDA detector collected the signal at 245 nm. The mass detector was set to negative mode to detect anionic molecules. Samples containing compound (I) were prepared as follows: 5 mg of compound (I) was dissolved in 50 mL of Milli-Q water. The resulting solution was diluted 10-fold with Milli-Q water, and 10 μL was injected into the HPLC-MS instrument for analysis.

[0211] Table 2 shows a typical method for eluting samples of compound (I) shown in Table 3. Table 3 provides an overview of retention times and molecular weights recorded for material identification.

[0212] Table 2: HPLC methods

[0213]

[0214] Table 3: Identification of materials and impurities in the examples

[0215] compound Precision quality (Da) Observed quality (Da) Retention time (minutes)* LiSS 190 183 12.2 MM-M 267 260 12.5 MM-A 268 261 11.5 MM-P 329 322 17.9 MM-TF 321 314 17.5

[0216] *The retention period is indicative.

[0217] The solubility of compounds of formula (I) was determined visually or by ultraviolet spectroscopy. For each compound of formula (I), three solutions were prepared: a 30 wt% solution, a 60 wt% solution, and a 70 wt% solution, containing a compound of formula (I) and the crosslinking agent Li-BVBSI in a molar ratio of 1:1. All three solutions contained 500 ppm 4OH-TEMPO to prevent premature polymerization. The solutions were stored overnight in a 40°C water bath and centrifuged before examination. The solubility was determined using quartz cuvettes with a 1 mm path length from Agilent Technologies' Cary TM The ultraviolet spectrum was recorded in a UV-Vis spectrophotometer.

[0218]

[0219] Table 4: Solubility of several Formula (I) compounds and comparative compounds in water

[0220]

[0221] In experiments conducted separately from those shown in Table 4, for comparison, the highest solubility obtained by mixing lithium styrene sulfonate (LiSS) and DVBS-Na was found to be 55% by weight. Furthermore, when the compound of formula (I) shown in Table 2 (where M is Li) was combined with DVBS-Na, a solubility of at least 60% by weight was obtained in all cases. When the compound of formula (I) shown in Table 4 (where M is Li) was combined with a crosslinking agent from the disulfonamide family (e.g., formula (II)), the highest solubility obtained reached a solid content exceeding 70% by weight.

[0222] The ER (Ω·cm) of the polymer membrane prepared in the examples 2 The method described by Dlugolecki et al. in J. of Membrane Science, 319 (2008), pp. 217-218, was used with the following modifications:

[0223] • The auxiliary membranes are CMX and AMX from Tokuyama Soda in Japan;

[0224] • The capillary and Ag / AgCl reference electrode (Metrohm 6.0750.100 type) contain 3M KCl;

[0225] • The calibration liquid and the liquids in compartments 2, 3, 4 and 5 are 0.5M NaCl solutions at 25°C;

[0226] • The effective membrane area is 9.62 cm². 2 ;

[0227] • The distance between capillaries is 5.0 mm;

[0228] • The measured temperature is 25℃;

[0229] • All compartments are driven by a Cole Parmer Masterflex console (77521-47) with an Easy-Load Type II 77200-62 gear pump;

[0230] • The flow rate per stream was controlled at 475 ml / min using a Porter Instrument flow meter (150AV-B250-4RVS model) and a Cole Parmer flow meter (G-30217-90 model); and

[0231] • Before measurement, equilibrate the sample in a 0.5M NaCl solution at room temperature for at least 1 hour.

[0232] Preferably, the ER (for 0.5M NaCl) is less than 5 Ω·cm. 2 More preferably, below 2.5Ω·cm 2 .

[0233] Measurement of permeation selectivity (PS)

[0234] The permeation selectivity PS (%) was measured as follows, which is the selectivity for ions with opposite charges to those of the cationic membrane prepared in the examples. The membrane to be analyzed was placed in a two-compartment system. One compartment was filled with 0.05 M NaOH solution, and the other compartment was filled with 0.5 M NaOH solution.

[0235] set up:

[0236] • The capillary and Ag / AgCl reference electrode (Metrohm 6.0750.100 type) contain 3M KCl;

[0237] • The effective membrane area is 9.62 cm². 2 ;

[0238] The distance between the capillaries is approximately 15 mm;

[0239] • The measured temperature was 21.0 ± 0.2℃;

[0240] The two compartments are driven by a Cole Parmer Masterflex console (77521-47) with an easy-load Type II 77200-62 gear pump;

[0241] • The flow constant was controlled at 500 ml / min using a Porter Instrument flow meter (150AV-B250-4RVS type) and a Cole Parmer flow meter (G-30217-90 type);

[0242] • Before measurement, equilibrate the sample in 0.5M NaOH solution for 1 hour. Read the voltage from a standard VOM (multimeter) after 20 minutes.

[0243] Preferably, the PS content of NaOH is at least 50%.

[0244] pH stability

[0245] Stability under acidic and / or alkaline conditions is preferred because it broadens the range of applications for which CEM can be used. Stability is typically tested by immersing the sample in 4M HCl or NaOH at 80°C for 7 days. After this treatment, the selectivity should be at least 80% of the original selectivity to be considered stable.

[0246] Preparation of compound (I) and comparative compounds

[0247] MM-Tf, MM-A, MM-P and MM-M (as described above) have the structures shown below.

[0248]

[0249] Compounds MM-Tf, MM-A, MM-P, and MM-M were synthesized according to the following general scheme and procedure:

[0250]

[0251] General Procedure

[0252] Prior to synthesis, the corresponding sulfonamide was dried overnight in a vacuum oven at 30 °C. LiH (0.300 mol, 3 mol equivalents) as solid was immediately added to a solution of the dried sulfonamide (0.100 mol, 1 mol equivalent) and 4OH-TEMPO (30 mg, 500 ppm) in THF (100 mL). The reaction mixture was stirred at room temperature for 30 minutes. Then, a solution of vinylbenzylsulfonyl chloride (0.100 mol, 1 mol equivalent) in THF (50 mL) was added, and the reaction mixture was heated to 60 °C (water bath temperature) for 16 hours. The resulting solution was filtered through diatomaceous earth, and the resulting foam was dissolved in 500 mL of ethyl acetate. Diatomaceous earth was added, and the resulting slurry was stirred for 5 minutes. The diatomaceous earth was then filtered off, and the mixture was washed with 100 mL of ethyl acetate. The solvent was then evaporated under vacuum, and the resulting white foam was pulverized overnight with 500 mL of diethyl ether. The resulting compound of formula (i) was collected by filtration and separated into a white hygroscopic powder. Table 5 below provides data on yield and purity.

[0253] Table 5: Compounds of Formula (I) and Comparative Compounds

[0254] R Yield purity Residual solvent Residual LiSS Li content methyl 80% >94% <1% <4% 26-30g / kg Phenyl 79% >96% <1% <2% 23-28g / kg Trifluoromethyl 70% 81% 17% amino 63% >92% <1% <6% 26-40g / kg

[0255] Composition Examples (Ex) 1 to 10, Comparative Examples CEx1 to CEx4, and Polymer Films

[0256] Table 6 below describes the compositions of Examples 1 to 10 and Comparative Examples CEx1 to CEx4 of the first aspect of the present invention. Each composition was polymerized to form a polymer film with a thickness of 100 μm by coating the composition onto a porous polypropylene / polyethylene support for reinforcement using a 100 μm Meyer rod. The resistivity ER of the resulting polymer film was measured using 0.5 N NaCl, and the permeability selectivity PS was as described above; the results are shown in the last column of Table 6.

[0257] Table 6: Experimental Results

[0258]

[0259] *All formulations shown in Table 6 include 1% by weight of LAP as a photoinitiator.

[0260] The Na-AMPS amounts in the table are based on 100% solids; water present in the solution obtained from the supplier is added to the solvent amount.

[0261] Table 7: pH stability results

[0262]

[0263] Infrared analysis

[0264] ATR-FTIR spectra of polymer films were recorded using a PerkinElmer Frontier FT-IR spectrometer with a universal ATR sampling accessory equipped with a diamond top plate. The spectral recording range was 4000–580 cm⁻¹. -1 Spectral resolution of 4 cm -1 The spectrum is the average of 10 recorded spectra. For optimal peak resolution, the polymer film sample was pushed onto the ATR diamond using a tapered tip (force gauge 75). The results of Example 7 and Comparative Example CEx2 are shown in Table 8 below:

[0265] Table 8: Infrared Analysis Results

[0266] Example <![CDATA[Peaks below 60% T% were found between 900-4000 cm -1 (cm -1 )]]> Ex 7 1262,1151,1132,1076,1048,1011 CEx 2 1183,1126,1035,1010

[0267] From Table 8, the strong IR peaks at 1262, 1151, 1076, and 1048 can be used to distinguish between bis(sulfonyl)imide functional groups and sulfonate functional groups in polymer film samples.

[0268] Extraction Analysis

[0269] To analyze the degree of polymerization of the polymer membrane and to indicate the presence of the material to be protected within the polymer membrane, purified water (in 50 mL of purified water at a concentration of 10 cm⁻¹) was used. 2 The polymer membrane sample was extracted, and the extract was then analyzed using the HPLC-MS method described above.

[0270] Table 9: Extraction Results

[0271] Example Material a Extract material a (mg / ml) Material b Extract material b (mg / ml) Ex 7 MM-M 13 Li-BVBSI 8 Ex 9 MM-P 12 Li-BVBSI 9 Ex 1 MM-M 14 XL-2 11 Ex 10 MM-A 18 Li-BVBSI 15

[0272] Preparation of AEL

[0273] An AEL composition was prepared comprising 58 wt% 1,4-diazabicyclo[2.2.2]octane, 1,4-bis[(4-vinylphenyl)methyl]-,chloride, 19 wt% water, 6 wt% IPA, and 1 wt% Omnirad. TM TPO-L and 1% Omnirad TM 1173. The AEL composition was coated onto a nonwoven polyethylene fabric and cured by UV.

[0274] Prepare a CEL and apply it to an AEL to generate a BPM.

[0275] CEL compositions were prepared according to Table 7 (Example 9 and Comparative Example CEx4). The CEL composition was coated onto the AEL prepared as described above, then a second nonwoven polyethylene fabric was placed on the CEL composition layer, excess CEL composition was wiped off, and the CEL composition was cured using UV light.

[0276] The electrochemical performance and bipolar characteristics of this bipolar membrane are compared with a reference membrane using a so-called current-voltage characteristic (IU curve), where the current density is measured as a function of the applied voltage. Typically, a given current density (i.e., 600 mA / cm²) is generated. 2 The lower the required voltage (U), especially for membranes with one or two ion exchange layers and generally bipolar membranes, the lower the ion resistance. In the case of cation exchange layers, low ion resistance results in a more energy-efficient membrane.

[0277] Table 10: CEL's ER and BPM at 600mA / cm 2 The voltage U

[0278]

Claims

1. A polymer film obtained by polymerizing a composition comprising: (a) Compound of formula (I): Equation (I) in: R is C 1-4 Alkyl, NH2, or phenyl; and M + It is a cation; (b) A monomer containing at least two polymerizable groups; and (c) Solvent.

2. The polymer film according to claim 1, wherein, The composition comprises: (a) 5 to 60% by weight of component (a); (b) 10 to 70% by weight of component (b); (c) 10 to 50% by weight of component (c).

3. The polymer film according to claim 1, wherein, R is methyl, phenyl, or NH2.

4. The polymer film according to claim 1, wherein, The polymerizable groups are each independently selected from (meth)acrylic acid groups and vinyl groups.

5. The polymer film according to claim 1, wherein, Component (b) further comprises anionic groups.

6. The polymer film according to claim 5, wherein, The anionic group includes sulfonate or disulfonamide anion.

7. The polymer film according to claim 1, wherein, Component (a) does not contain fluorine atoms.

8. The polymer film of claim 1, further comprising (d) a free radical initiator.

9. A cation exchange membrane obtained by polymerizing the composition defined in claim 1.

10. A bipolar membrane comprising the polymer membrane of claim 1.

11. A method for preparing a polymer film, comprising polymerizing a composition, said composition comprising: (a) Compound of formula (I): Equation (I) in: R is C 1-4 Alkyl, NH2, or phenyl; and M + It is a cation; (b) A monomer containing at least two polymerizable groups; and (c) Solvent.

12. The method of claim 11, wherein, The composition further comprises (d) an initiator.

13. The method of claim 11, wherein, The composition comprises: (a) 5 to 60% by weight of component (a); (b) 10 to 70% by weight of component (b); (c) 10 to 50% by weight of component (c); and (d) 0 to 10% by weight of the initiator as component (d).

14. The polymer membrane of claim 1 or the bipolar membrane of claim 10, further comprising a porous carrier.

15. A composition comprising: (a) Compound of formula (I): Equation (I) in: R is C 1-4 Alkyl, NH2, or phenyl; and M + It is a cation; (b) A monomer containing at least two polymerizable groups; and (c) Solvent.

16. The composition of claim 15, further comprising (d) an initiator.

17. The composition of claim 16, comprising: (a) 5 to 60% by weight of component (a); (b) 10 to 70% by weight of component (b); (c) 10 to 50% by weight of component (c); and (d) 0 to 10% by weight of the component (d).

18. The cation exchange membrane of claim 9 is used for treating polar liquids, for generating hydrogen, or for generating electricity.

19. The bipolar membrane of claim 10 is used for the production of acids and bases, for the separation and treatment of organic acids, or for the generation of electricity.

20. The bipolar membrane of claim 10, further comprising an anion exchange layer (AEL), said anion exchange layer (AEL) being obtained by curing a composition comprising a compound of formula (IV): Formula (IV) in: L 1 It is an alkylene or alkenylene group; R a R b R c and R d Each is independently an alkyl group or an aryl group, or R a and R b , and / or R c and R d They form rings together with the atoms they are connected to; n1 and n2 each independently represent integers from 1 to 10; and X1 - and X2 - Each can be used to represent anion independently.

Citation Information

Patent Citations

  • Alpha-aminoacetophenones as photo initiators

    EP0284561A2

  • Composition for forming polymeric membrane, process for producing same, polymeric membrane, separation membrane module, and ion exchange device

    EP3184558A1

  • JP1972003981B1

  • JP1972006416B1

  • JP1972022326B1