Debondable urethane adhesive based on heat-expandable microspheres

By using a debondable polyurethane adhesive based on thermally expandable microspheres, the problem of incomplete debonding of adhesives during wafer dicing in existing technologies has been solved, achieving efficient and clean bonding and debonding effects, suitable for wafer dicing and mechanical property testing.

CN116234850BActive Publication Date: 2026-11-24BASF SE
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202180066747.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-09-30
Filing Date
2021-09-07
Publication Date
2026-11-24
Estimated Expiration
2041-09-07

AI Technical Summary

Technical Problem

Existing adhesives are difficult to effectively debond under different conditions during wafer dicing, especially in hot water where debonding is incomplete and may cause wafer damage or residue, failing to meet the requirements for efficient and clean bonding and debonding.

Method used

A detackable polyurethane adhesive based on thermally expandable microspheres is used. Through the combined reaction of diisocyanate, polyol, catalyst and thermally expandable microspheres, the isocyanate index is set in the range of 28 to 65, and the detack temperature and time of the adhesive are adjusted.

Benefits of technology

It achieves efficient and clean debonding of the bonded surface in hot water, reduces residue, adapts to different cutting conditions, and improves the efficiency and quality of wafer dicing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116234850B_ABST
    Figure CN116234850B_ABST
Patent Text Reader

Abstract

This invention relates to a debonded polyurethane adhesive based on thermally expandable microspheres, which can be obtained or is obtainable by reacting (A) at least one diisocyanate or polyisocyanate, (B) at least one polyol, (C) a catalyst, (D) thermally expandable microspheres, and (E) other additives, wherein the isocyanate index of the reaction is set in the range of 28 to 65. The invention also relates to the use of said debonded polyurethane adhesive for debonding metal and dicing pads during wafer dicing. Furthermore, the invention relates to the use of said debonded polyurethane adhesive in the preparation of samples for mechanical property testing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a debonded polyurethane adhesive based on thermally expandable microspheres, which can be obtained or is obtainable by reacting (A) at least one diisocyanate or polyisocyanate, (B) at least one polyol, (C) a catalyst, (D) thermally expandable microspheres, and (E) other additives, wherein the isocyanate index of the reaction is set in the range of 28 to 65. The invention also relates to the use of said debonded polyurethane adhesive for debonding metal and dicing pads during wafer dicing. Furthermore, the invention relates to the use of said debonded polyurethane adhesive in the preparation of samples for mechanical property testing. Background Technology

[0002] Detachable adhesives are a type of adhesive that provides necessary bonding between various surfaces when needed, but may fail under specific external conditions (such as heat, light, UV radiation, etc.). Detachable adhesives that can effectively detach from bonded surfaces have a wide range of applications, such as consumer electronics and home repair. To facilitate the detachment of the adhesive from the bonded surface, expandable microspheres are incorporated into the adhesive formulation. When the material is heated above the "initial temperature" of the microspheres, this adhesive undergoes significant thermal expansion, resulting in rapid and clean detachment from the bonded surface.

[0003] Expandable microspheres are a type of particle with a core-shell structure, where the shell is composed of a cross-linked polymer and the core is composed of a physical foaming agent (e.g., a low-boiling-point alkane). By adjusting the wall thickness, T... g By considering the composition of the microspheres' walls and the foaming agent (i.e., a low-boiling-point compound), microspheres can be designed to have a wide range of expansion initiation temperatures and expansion rates. This material has recently been explored as a special foaming agent for PU foam systems, but its application in PU adhesives remains a relatively unexplored area.

[0004] Multi-wire diamond sawing is a key process for manufacturing monocrystalline and polycrystalline silicon wafers for use in the photovoltaic industry and microelectronic chips. This technology has seen significant market growth in recent years and continues to evolve rapidly, becoming the mainstream dicing technology in the wafer industry. This manufacturing process requires two types of debonding adhesives: 1) between the silicon ingot and the disposable dicing pad, and 2) between the disposable dicing pad and the metal plate on the dicing equipment. Both adhesives need to debond under different conditions to allow for clean separation of the wafer slices and recycling of the metal plate. The adhesive technique described in this paper exhibits significant debonding in hot water (near boiling point) while remaining stable at 70°C, a highly challenging task.

[0005] CN104031597B discloses a PU-acrylate anaerobic adhesive that can be debonded in hot water. This adhesive is reportedly capable of automatic debonding at 60 to 75°C. It is presumed that this debonding is due to the adhesive's glass transition, causing it to soften in hot water. This temperature is relatively low and does not allow for the differentiation of the distinct two-step debonding process required for wafer dicing. Furthermore, no expandable microspheres are added to the adhesive.

[0006] US9714317B2 discloses an epoxy adhesive as a temporary adhesive to provide bonding to silicon ingots, which can be debonded in water at 55 to 80°C. The epoxy resin solution exhibits significantly higher rigidity and a higher Shore D hardness. This solution has a potential weakness: a higher wafer damage rate due to the higher product hardness and brittleness, which can lead to edge damage of the wafer. The epoxy resin solution described herein contains a water-soluble polymer, which presents a potential failure risk during diamond wire cutting because the adhesive is continuously exposed to water spray, weakening due to hydrosolubilization. Another disadvantage is the high thiol odor of the adhesive. This has implications for operator safety. Also, expandable microspheres are not added to its adhesive.

[0007] CN1192070C discloses a composition comprising an adhesive (e.g., PU) having thermally expandable microspheres dispersed therein as pressure actuators. The microcapsules are thermally activated, releasing at least one volatile agent encapsulated within the microcapsule shell. However, this patent does not include any embodiments, and therefore no experimental data is available to support the claimed effects. Throughout the patent, no detailed information is provided regarding the preparation of the PU adhesive. Furthermore, because the composition is used as a glass adhesive, the thermally expandable microcapsules expand in atmospheric air rather than in hot water, allowing for an initial temperature as high as 150°C.

[0008] There is still a need in the art for adhesives for debonding bonded surfaces, which can provide the necessary adhesion under various conditions and can be effectively and cleanly debonded when heated in a specific medium (e.g., hot water). In particular, the adhesive can debond rapidly with almost no residue on the surface. Furthermore, the debonding temperature can be easily adjusted as needed. Summary of the Invention

[0009] One object of the present invention is to provide a debonded polyurethane adhesive for debonding adhesive surfaces without the aforementioned problems. This object is achieved by a debonded polyurethane adhesive based on thermally expanded microspheres, which is obtained or can be obtained through the reaction of the following components:

[0010] (A) at least one diisocyanate or polyisocyanate;

[0011] (B) At least one polyol;

[0012] (C) Catalyst;

[0013] (D) Thermally expandable microspheres; and

[0014] (E) Other additives.

[0015] The isocyanate index for this reaction is set in the range of 28 to 65.

[0016] In one embodiment, the isocyanate index of the reaction is set in the range of 30 to 60, preferably 30 to 50, and more preferably 35 to 50.

[0017] In another embodiment, the polyol (B) is selected from polyether alcohols and / or polyester alcohols having 2 to 8 hydrogen atoms that are reactive to isocyanates.

[0018] In another embodiment, the polyurethane adhesive has a debonding time of less than 10 minutes in hot water at 75°C or higher.

[0019] The present invention also provides a method for preparing a detangleable polyurethane adhesive based on thermally expandable microspheres, which includes the step of mixing the above components, wherein the isocyanate index of the reaction is set in the range of 28 to 65.

[0020] The present invention also relates to the use of a thermally expandable microsphere-based debonded polyurethane adhesive for debonding metal and cutting pads during wafer dicing, and the use of a thermally expandable microsphere-based debonded polyurethane adhesive in the preparation of mechanical property test samples.

[0021] Compared to conventional adhesives, the debonded polyurethane adhesive of this invention can achieve more efficient and cleaner debonding of bonded surfaces in hot water, with little or no residue or odor issues. Furthermore, the debonding time and temperature can be well controlled by adjusting the composition and mixing ratio of the adhesive. Attached Figure Description

[0022] Figure 1 shows a typical wafer dicing process. The diagram shows that polyurethane adhesive is used to debond the metal plate and the cutting pad in step 4.

[0023] Figure 2 It is a description of specific thermally expandable microspheres, including SEM images of 2(a) microspheres, planar images of 2(b) microspheres, and internal structures of 2(c) microspheres. Detailed Implementation

[0024] Unless otherwise defined, all technical and scientific terms used herein have the meanings commonly understood by one of ordinary skill in the art to which this invention pertains. Unless otherwise stated, as used herein, the following terms have the meanings assigned to them as follows.

[0025] As used in this article, the articles "a" and "an" refer to one or more (i.e., at least one) grammatical objects of an article or component. For example, "an element" refers to one or more elements.

[0026] As used herein, the term “approximately” should be understood to mean a range of numbers that a person skilled in the art would consider equivalent to the value in achieving the same function or result.

[0027] As used herein, the term "additive" refers to an additive contained in a formulation system to enhance its physical or chemical properties and provide desired results. Such additives include, but are not limited to, dyes, pigments, toughening agents, impact modifiers, rheology modifiers, plasticizers, thixotropic agents, natural or synthetic rubber, fillers, reinforcing agents, thickeners, inhibitors, fluorescent or other markers, thermal degradation inhibitors, thermal resistance imparting agents, surfactants, wetting agents, defoamers, dispersants, flow or slip agents, bactericides, and stabilizers.

[0028] Unless otherwise stated, all percentages (%) are "weight percentages".

[0029] The basic definitions or descriptions described above in the general terms or preferred scope apply to the final product, and correspondingly to the starting materials and intermediates. These basic definitions can be combined with each other as needed, i.e., combinations between general definitions and / or their respective preferred scopes and / or embodiments.

[0030] All embodiments and preferred embodiments disclosed herein may be combined as needed, and such combinations are also considered to be within the scope of the invention.

[0031] Unless otherwise stated, temperature refers to room temperature and pressure refers to ambient pressure.

[0032] Unless otherwise stated, solvents refer to all organic and inorganic solvents known to those skilled in the art and do not contain any type of monomer molecules.

[0033] This invention relates to a detangleable polyurethane adhesive based on thermally expandable microspheres, which can be obtained or is obtained through the reaction of the following components:

[0034] (A) at least one diisocyanate or polyisocyanate;

[0035] (B) At least one polyol;

[0036] (C) Catalyst;

[0037] (D) Thermally expandable microspheres; and

[0038] (E) Other additives.

[0039] The isocyanate index for this reaction is set in the range of 28 to 65.

[0040] Diisocyanate or polyisocyanate (A)

[0041] The diisocyanate or polyisocyanate (A) used can be any aliphatic, alicyclic, or aromatic isocyanate known for use in the production of polyurethanes. The aliphatic diisocyanate used is a conventional aliphatic and / or alicyclic diisocyanate, such as tri-, tetra-, penta-, hexa-, hepta-, and / or octamethylene diisocyanate, 2-methylpentamethylene 1,5-diisocyanate, 2-ethyltetramethylene 1,4-diisocyanate, hexamethylene 1,6-diisocyanate (HDI), pentamethylene 1,5-diisocyanate, butene 1,4-diisocyanate, trimethylhexamethylene 1,6-diisocyanate. Esters, 1-isocyano-3,3,5-trimethyl-5-isocyanomethylcyclohexane (isophorone diisocyanate, IPDI), 1,4- and / or 1,3-bis(isocyanate methyl)cyclohexane (HXDI), cyclohexane-1,4-diisocyanate, 1-methylcyclohexane 2,4- and / or 2,6-diisocyanate, methylene dicyclohexyl 4,4'-, 2,4'- and / or 2,2'-diisocyanate (H12MDI). Suitable aromatic diisocyanates, especially 1,5-naphthalene diisocyanate (NDI), 2,4- and / or 2,6-toluene diisocyanate (TDI), 3,3'-dimethyl-4,4'-biphenyl diisocyanate (TODI), terephthalic diisocyanate (PDI), diphenylethane 4,4'-diisocyanate (EDI), diphenylmethane diisocyanate, dimethyl diphenyl 3,3'-diisocyanate, diphenylethane 1,2-diisocyanate and / or diphenylmethane diisocyanate (MDI).

[0042] The diisocyanate or polyisocyanate (A) used preferably includes isocyanates based on diphenylmethane diisocyanate, particularly polymeric MDI. The functionality of the diisocyanate and polyisocyanate (A) is preferably from 2.0 to 2.9, particularly preferably from 2.1 to 2.8. According to DIN 53019-1 to 3, the viscosity of the diisocyanate or polyisocyanate (A) at 25°C is preferably from 5 to 600 mPas, particularly preferably from 10 to 300 mPas.

[0043] Diisocyanates and polyisocyanates (A) can also be used in the form of polyisocyanate prepolymers. These polyisocyanate prepolymers can be obtained by reacting an excess of the above-mentioned polyisocyanate (component (a-1)) with a compound (component (a-2)) having at least two groups reacting with isocyanates, for example, at a temperature of 30 to 100°C, preferably at about 80°C, to obtain the prepolymer. The NCO content of the polyisocyanate prepolymer of the present invention is preferably 20 to 33% by weight, and particularly preferably 25 to 35% by weight.

[0044] In a preferred embodiment, the diisocyanate or polyisocyanate (A) is selected from 2,2'-MDI, 4,4'-MDI, MDI prepolymers or mixtures thereof.

[0045] Diisocyanate or polyisocyanate (A) may be present in the polyurethane adhesive in an amount of 25 to 70% by weight, preferably 30 to 65% by weight, more preferably 35 to 60% by weight, based on the total weight of the polyurethane adhesive.

[0046] Polyol (B)

[0047] The polyol (B) used herein can be any aliphatic, alicyclic, or aromatic polyol known for the production of polyurethanes. Polyether alcohols and / or polyester alcohols having 2 to 8 hydrogen atoms reactive to isocyanates are preferred. The hydroxyl values ​​of these compounds are typically in the range of 20 to 2000 mg KOH / g, preferably in the range of 40 to 1000 mg KOH / g. The average hydroxyl value of all compounds (B) having at least two isocyanate-reactive groups used herein is 100 to 1000 mg KOH / g, preferably 200 to 900 mg KOH / g. The molecular weight (Mw) of the polyol can be from 200 to 50000 g / mol, preferably 400 to 8000 g / mol.

[0048] Polyether alcohols are obtained by known processes, such as anionic polymerization of epoxides with at least one added starting molecule containing 2 to 8, preferably 2 to 6, particularly preferably 2 to 4 reactive hydrogen atoms, in the presence of a catalyst. The catalysts used may include alkali metal hydroxides, such as sodium hydroxide or potassium hydroxide, or alkali metal alkoxides, such as sodium methoxide, sodium ethoxide, potassium ethoxide, or potassium isopropoxide; or, in the case of cationic polymerization, Lewis acids, such as antimony pentachloride, boron trifluoride ether, or bleaching earth. Other catalysts that can be used are bimetallic cyanides, known as DMC catalysts.

[0049] The alkyl oxides used preferably comprise one or more compounds having 2 to 4 carbon atoms in the alkylene moiety, such as tetrahydrofuran, ethylene oxide, 1,2-epoxypropane, 1,2-epoxybutane or 2,3-epoxybutane, used alone or in mixtures in each case, and preferably 1,2-epoxypropane and / or ethylene oxide, especially 1,2-epoxypropane.

[0050] Examples of starting molecules that may be used are ethylene glycol, diethylene glycol, glycerol, trimethylolpropane, pentaerythritol, sugar derivatives (e.g., sucrose), hexyl alcohol derivatives (e.g., sorbitol), methylamine, ethylamine, isopropylamine, butylamine, benzylamine, aniline, toluidine, toluenediamine, naphthylamine, ethylenediamine, diethylenetriamine, 4,4'-diaminodiphenylmethane, 1,3-propanediamine, 1,6-hexanediamine, ethanolamine, diethanolamine, triethanolamine, and other dihydroxy alcohols or polyhydroxy alcohols, or diamines or polyamines.

[0051] The polyester alcohols used are mainly prepared by condensation of polyols having 2 to 12 carbon atoms (such as ethylene glycol, diethylene glycol, butanediol, trimethylolpropane, glycerol, or pentaerythritol) with polycarboxylic acids having 2 to 12 carbon atoms (such as isomers of succinic acid, glutaric acid, adipic acid, octanoic acid, azelaic acid, sebacic acid, dodecanoic acid, maleic acid, fumaric acid, phthalic acid, isophthalic acid, terephthalic acid, and naphthalenedicarboxylic acid, or their anhydrides).

[0052] Other starting materials that can be used simultaneously in the production of polyester alcohols are hydrophobic substances. Hydrophobic substances are substances insoluble in water that contain a nonpolar organic moiety and also have at least one reactive group selected from hydroxyl, carboxylic acid, carboxylic acid esters, or mixtures thereof. The equivalent amount of the hydrophobic material is preferably 130 to 1000 g / mol. Examples of such materials that can be used are fatty acids, such as stearic acid, oleic acid, palmitic acid, lauric acid, or linoleic acid, and fats and oils, such as castor oil, corn oil, sunflower oil, soybean oil, coconut oil, olive oil, or tall oil. If the polyester contains a hydrophobic substance, the percentage of the hydrophobic substance, based on the total monomer content of the polyester alcohol, is preferably 1 to 30 mol%, particularly preferably 4 to 15 mol%.

[0053] The functionality of the polyester alcohol used is preferably 1.5 to 5, and particularly preferably 1.8 to 3.5.

[0054] In a particularly preferred embodiment, the polyol (B) having groups reacting with isocyanates comprises polyether alcohols, particularly only polyether alcohols. The practical average functionality of the polyether alcohol is preferably 2 to 4, particularly preferably 2.5 to 3.5, especially 2.8 to 3.2, and its hydroxyl value is preferably 20 to 900 mg KOH / g. The content of its secondary hydroxyl groups is preferably at least 50%, preferably at least 60%, particularly preferably at least 70%, and especially at least 80%. The polyether alcohols used herein preferably comprise polyether alcohols based on glycerol as an initiator and 1,2-epoxypropylene.

[0055] The polyol (B) may be present in the polyurethane adhesive in an amount of 15 to 45% by weight, preferably 18 to 40% by weight, more preferably 25 to 35% by weight, based on the total weight of the polyurethane adhesive.

[0056] Catalyst (C)

[0057] The polyurethane catalyst (C) can comprise any conventional catalyst used in the production of polyurethane. Such catalysts are described, for example, in Chapter 3.4.1 of the "Polyurethane Handbook" by Carl Hanser Verlag, second edition, 1993. Examples of such catalysts that may be used herein are organometallic compounds, such as complexes of tin, zinc, titanium, zirconium, iron, mercury, or bismuth, preferably organotin compounds, such as stannous salts of organic carboxylic acids, such as stannous acetate, stannous octoate, stannous isooctanoate, and stannous laurate; and dialkyltin (IV) salts of carboxylic acids, such as dibutyltin diacetate, dibutyltin dilaurate, dibutyltin maleate, and dioctyltin diacetate; and phenylmercuric neodecanoate, bismuth carboxylic acids, such as bismuth neodecanoate (III), bismuth 2-ethylhexanoate, and bismuth octoate, or mixtures thereof. Other viable catalysts are basic amine catalysts. Examples of such catalysts include amidines, such as 2,3-dimethyl-3,4,5,6-tetrahydropyrimidine, and tertiary amines, such as triethylamine, triethylenediamine, tributylamine, dimethylbenzylamine, N-methyl, N-ethyl, N-cyclohexylmorpholine, N,N,N',N'-tetramethylethylenediamine, N,N,N',N'-tetramethylbutanediamine, N,N,N',N'-tetramethylhexanediamine, pentamethyldiethylenetriamine, and tetramethyldiethylenediamine. The catalyst may contain aminoethyl ether, bis(dimethylamino)propylurea, dimethylpiperazine, 1,2-dimethylimidazolium, 1-azabicyclo[3.3.0]octane, and preferably 1,4-diazabicyclo[2.2.2]octane, 1,8-diazabicyclo[5.4.0]undec-7-ene, as well as alkanolamine compounds, such as triethanolamine, triisopropanolamine, N-methyldiethanolamine and N-ethyldiethanolamine, and dimethylethanolamine. The catalyst may be used alone or in mixtures. A mixture of metal catalysts and basic amine catalysts may optionally be used as catalyst (C).

[0058] These catalysts significantly accelerate the reaction of compounds with isocyanate-reactive hydrogen atoms with diisocyanates and polyisocyanates. Preferred catalysts for the preparation of polyurethanes include, for example, amidines, such as 2,3-dimethyl-3,4,5,6-tetrahydropyrimidine, tertiary amines, such as triethylamine, tributylamine, and dimethylbenzylamine. Also preferred are organometallic compounds, especially organotin compounds, such as tin(II) salts of organic carboxylic acids, such as tin(II) acetate, tin(II) octoate, tin(II) ethylhexanoate, and tin(II) laurate.

[0059] The catalyst (C) may be present in the polyurethane binder in an amount of 0.01 to 2% by weight, preferably 0.05 to 1% by weight, more preferably 0.1 to 0.5% by weight, based on the total weight of the polyurethane binder.

[0060] Thermally expanding microspheres (D)

[0061] The thermally expandable microspheres (D) used in this invention typically have a core-shell structure, wherein the shell is formed by a cross-linked polymer, while the core is primarily composed of a foaming agent. As for the polymer, it can be prepared by (co)polymerization of any suitable monomer or comonomer. Suitable monomers that can be used to prepare the polymer include nonionic olefinically unsaturated monomers. Examples of nonionic olefinically unsaturated monomers that can be used include styrene, vinyltoluene, ethylene, butadiene, vinyl acetate, vinyl chloride, dichloroethylene, acrylonitrile, acrylamide, methacrylamide, acrylic acid, or methacrylic acid (C1 to C1). 20 )alkyl or (C3-C 20 Alkenyl esters, methacrylates, methyl methacrylate, ethyl acrylate, ethyl methacrylate, butyl acrylate, butyl methacrylate, 2-ethylhexyl acrylate, (2-ethylhexyl) methacrylate, benzyl acrylate, benzyl methacrylate, lauryl acrylate, lauryl methacrylate, oleyl acrylate, oleyl methacrylate, palmitate, palmitate methacrylate, octadecyl acrylate, octadecyl methacrylate, containing hydroxyl monomers, especially C1 to C10 hydroxyalkyl (meth)acrylates, such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, glycidyl (meth)acrylate, preferably methyl methacrylate.

[0062] Specifically, the polymer can be a copolymer prepared by copolymerizing two or more monomers listed above. Preferred monomer combinations include acrylonitrile / (methyl)methacrylate, styrene / (methyl)methacrylate, acrylamide / (methyl)methacrylate, acrylonitrile / (hydroxyethyl)methacrylate, etc. The most preferred combination is acrylonitrile / methyl methacrylate.

[0063] Crosslinking agents that can be used for polymer crosslinking are compounds having two or more olefinically unsaturated groups, such as diacrylates or dimethacrylates of at least a dibasic alcohol, such as ethylene glycol diacrylate, ethylene glycol dimethacrylate, 1,2-propanediol diacrylate, 1,2-propanediol dimethacrylate, 1,4-butanediol diacrylate, 1,4-butanediol dimethacrylate, hexanediol diacrylate, hexanediol dimethacrylate, neopentyl glycol diacrylate, neopentyl glycol dimethacrylate, 3-methylpentyl glycol diacrylate, and 3-methylpentyl glycol dimethacrylate. Another class of crosslinking agents includes diacrylates or dimethacrylates of polyethylene glycol or polypropylene glycol with a molecular weight of 200 to 9000 in each case. The polyethylene glycol and / or polypropylene glycol used to prepare the diacrylates or dimethacrylates preferably each have a molecular weight of 400 to 2000. Not only homopolymers of ethylene oxide and / or propylene oxide, but also block copolymers of ethylene oxide and propylene oxide, or random copolymers of ethylene oxide and propylene oxide comprising randomly distributed ethylene oxide and propylene oxide units, can be used. Similarly, oligomers of ethylene oxide and / or propylene oxide can also be used to prepare crosslinking agents, such as diethylene glycol diacrylate, diethylene glycol dimethacrylate, triethylene glycol diacrylate, triethylene glycol dimethacrylate, tetraethylene glycol diacrylate, and / or tetraethylene glycol dimethacrylate.

[0064] The amount of crosslinking agent used is preferably 0.1 to 30% by weight, based on the monomers to be polymerized in any stage. The crosslinking agent can be added at each stage.

[0065] The core is preferably composed of a physical blowing agent. Suitable physical blowing agents include alkanes and / or cycloalkanes having at least 4 carbon atoms, dialkyl ethers, esters, ketones, acetals, fluoroalkanes having 1 to 8 carbon atoms, and tetraalkylsilanes having 1 to 3 carbon atoms in the alkyl chain, particularly tetramethylsilane.

[0066] In a preferred embodiment of the invention, the physical blowing agent is a hydrocarbon. Particularly preferably, the physical blowing agent is selected from alkanes and / or cycloalkanes containing at least four carbon atoms. In particular, pentane is used, and isopentane and cyclopentane are preferred. Cyclopentane is preferred because rigid foam is used as insulation material in cooling equipment. The hydrocarbon compound can be mixed with water.

[0067] Examples of foaming agents usable according to the invention include propane, n-butane, isobutane and cyclobutane, n-pentane, isopentane and cyclopentane, cyclohexane, dimethyl ether, methyl ethyl ether, methyl butyl ether, methyl formate and acetone, as well as fluoroalkanes that are degradable in the troposphere and therefore ozone-free, such as trifluoromethane, difluoromethane, 1,1,1,3,3-pentafluorobutane, 1,1,1,3,3-pentafluoropropane, 1,1,1,2-tetrafluoroethane, difluoroethane and 1,1,1,2,3,3,3-heptafluoropropane, and perfluorocarbons, such as C3F8, C4F8, etc. 10 C5F 12 C6F 14 and C7F 16 The foaming agent can be used alone or in any combination of the above.

[0068] In addition, hydrofluoroolefins, such as 1,3,3,3-tetrafluoropropylene, or hydrochlorofluoroolefins, such as 1-chloro-3,3,3-trifluoropropylene, can also be used as blowing agents. Such blowing agents are described, for example, in WO 2009 / 048826.

[0069] Thermally expandable microspheres can be prepared by seed swelling of a cross-linked polymer and encapsulation with a foaming agent. The resulting microspheres have a diameter of 5 to 40 μm, preferably 10 to 20 μm, and a shell thickness of 0.5 to 10 μm. When the adhesive is immersed in hot water at a temperature below 100°C, the thermally expandable microspheres expand with the physical foaming agent upon heating the water. The diameter of the microspheres can be increased to approximately 100 μm, and the shell thickness can be reduced to 0.1 μm. The thermally expandable microspheres can have a density of 3 to 20 kg / m³. 3 The density is preferably 5 to 12 kg / m³. 3 These thermally expandable microspheres are commercially available, such as AkzoNobel Inc.'s Expancel series.

[0070] The initial temperature T of the thermally expanding microspheres start It can be 75°C or higher. In one embodiment, the initial temperature T of the thermally expanding microspheres is... start The temperature is 75 to 97°C, preferably 80 to 95°C, and more preferably 85 to 90°C. Initial temperature T start This is the temperature at which the thermally expanding microspheres begin to expand under heating. Theoretically, the polyurethane adhesive begins to debond as the thermally expanding microspheres expand; therefore, the temperature at which the adhesive begins to debond is equal to or higher than the initial temperature T of the microspheres. start .

[0071] The thermally expandable microspheres (D) may be present in the polyurethane adhesive in an amount of 2 to 20% by weight, preferably 3 to 12% by weight, more preferably 5 to 10% by weight, based on the total weight of the polyurethane adhesive.

[0072] Other additives (E)

[0073] As additives for the purposes of this invention, substances known per se may be used, such as surfactants, foam stabilizers, cell regulators, fillers, pigments, dyes, flame retardants, anti-hydrolysis agents, antistatic agents, water absorbents, and auxiliaries that have antifungal and antibacterial effects.

[0074] In a preferred embodiment, the present invention provides a detangleable polyurethane adhesive based on thermally expanded microspheres, which can be obtained or is obtainable through the reaction of the following components:

[0075] (A) 25 to 70% by weight of at least one diisocyanate or polyisocyanate;

[0076] (B) 15 to 45% by weight of at least one polyol;

[0077] (C) 0.01 to 2% by weight of catalyst;

[0078] (D) 2 to 20% by weight of thermally expandable microspheres; and

[0079] (E) Other additives, based on the total weight of the polyurethane adhesive.

[0080] The isocyanate index for this reaction is set in the range of 30 to 60.

[0081] This invention also provides a method for preparing a detangleable polyurethane adhesive based on thermally expandable microspheres, comprising the step of mixing the following components:

[0082] (A) at least one diisocyanate or polyisocyanate;

[0083] (B) At least one polyol;

[0084] (C) Catalyst;

[0085] (D) Thermally expandable microspheres; and

[0086] (E) Other additives.

[0087] The isocyanate index is set in the range of 28 to 65.

[0088] In one embodiment, the resulting polyurethane adhesive has a content of 0.8 to 1.5 g / cm³. 3 Preferably, the concentration is 1.0 to 1.2 g / cm³. 3The density. Suitable production methods for polyurethane are also disclosed, for example, in EP 0922552A1, DE 10103424 A1 or WO 2006 / 072461 A1. Depending on the material properties of the components, these are either directly mixed together or the individual components are premixed and / or pre-reacted, for example, to form a prepolymer, followed by addition polymerization. In a preferred embodiment, diisocyanate or polyisocyanate (A) is added alone as component (ii), while polyol (B), catalyst (C), thermally expandable microspheres (D), and other additives (E) are added together to form component (i). The mixing ratio of components (i) and (ii) can be from 3:1 to 1:3, preferably from 2.5:1 to 1:2, more preferably from 2:1 to 1:1.8.

[0089] By adjusting reaction parameters, such as the relative contents of the individual components, especially components (A) and (B), the isocyanate index for preparing the polyurethane adhesive is advantageously set to 28 to 65, preferably 30 to 60, more preferably 30 to 50, and most preferably 35 to 50. For conventional polyurethanes, the isocyanate index used to prepare them is typically set to about 100, for example, 95 to 104. Surprisingly, the inventors have discovered that the debonding efficiency in this invention is highly dependent on the aforementioned index of the polyurethane adhesive, and a relatively low index is a key technical point for achieving debonding of bonded surfaces in hot water with this type of adhesive.

[0090] Therefore, this invention also relates to the use of a debonded polyurethane adhesive based on thermally expandable microspheres for debonding metal and dicing pads during wafer dicing. The wafer can be any semiconductor material, such as Si, Ga, Ge, GaN, GaAs, etc. This polyurethane adhesive exhibits strong adhesion between the metal and the dicing pad (epoxy resin, rigid PU foam, etc.) under various dicing conditions (strong vibration, constant water spray, and long-term stability in acidic water at 70°C), while simultaneously exhibiting efficient debonding performance in high-temperature water (75°C or above, 80°C or above, or near boiling point). Therefore, when the bonded metal plate and dicing pad are immersed in hot water at, for example, 75°C, 80°C, 85°C, 90°C, or 97°C, the polyurethane adhesive expands with the expansion of the bonded microspheres and detaches efficiently and cleanly from the metal surface within a short time, leaving almost no residue on the metal surface. By adjusting the isocyanate index used to prepare the polyurethane adhesive, the debonding time of the adhesive can be well controlled and adjusted, thereby achieving the desired debonding performance.

[0091] Furthermore, this invention relates to the use of a removable polyurethane adhesive based on thermally expandable microspheres in the preparation of samples for mechanical property testing. Typically, when performing mechanical property (e.g., tensile strength) tests on samples, the samples are fixed in clamps, which can easily lead to sample breakage or other defects. The removable polyurethane adhesive according to the invention can be applied to metal clamps used to fix the sample to the testing equipment, and the test sample is adhered to the clamp using this removable adhesive. The removable adhesive according to the invention provides sufficient adhesion between the test sample and the test clamp. After the tensile test, the sample can be easily removed from the test clamp by placing it in a high-temperature hot water bath, the temperature of which can be adjusted by changing the composition or index of the adhesive, for example, at temperatures of 75°C, 80°C, 85°C, 90°C, or 95°C.

[0092] The debonded polyurethane adhesive based on thermally expandable microspheres offers several advantages. For example, the adhesive can be debonded efficiently with virtually no residue left on the substrate surface. This can help save processing time in wafer dicing. The debonding temperature can be well controlled and regulated by adjusting the composition and index of the polyurethane adhesive. Furthermore, since the epoxy adhesive conventionally used in the prior art can be omitted, the polyurethane adhesive of the present invention does not involve odor issues. In addition, faster debonding at the debonding temperature is achieved. The debonding time can be as low as 1 to 2 minutes, which significantly improves the efficiency of the dicing process compared to conventional debonding processes that typically last for, for example, more than an hour.

[0093] Example

[0094] The present invention will now be described with reference to embodiments and comparative embodiments, which are not intended to limit the present invention.

[0095] Use the following materials:

[0096] Isocyanate A: Elastan Iso 6572-101C-B, 4,4'-MDI prepolymer, commercially available from BASF, with an NCO value of approximately 17.6.

[0097] Polyol 1: A PO-based polyol initiated by glycerol, with a Mw of approximately 6000 and a hydroxyl value of approximately 27 mg KOH / g.

[0098] Polyol 2: An EO-based glycerol-initiated polyol with a Mw of approximately 400 and a hydroxyl value of approximately 400 mg KOH / g.

[0099] Catalyst: Dabco 33LV, a 33% triethylenediamine propylene glycol solution, commercially available from Air Products.

[0100] Thermally expandable microspheres (TEMs): spherical plastic core-shell structured particles with a particle size of 10 to 16 μm, wherein hydrocarbons (blowing agents) are encapsulated by a cross-linked acrylonitrile / methyl methacrylate copolymer network shell, and T start =80 to 95℃.

[0101] T-Slurry: Castor oil containing 50% zeolite, water absorbent.

[0102] Filler: MgSiO3

[0103] Test method:

[0104] Overlap shear test

[0105] Clean the substrate surface with ethanol and dry for 5 minutes. The stainless steel sheet is Q-Panel RS-14, obtained from Q-Lab. Mix components (i) and (ii) for 45 seconds with a spatula or in a mixer and apply to the substrate surface. The application area is 12.5mm x 25mm, with a thickness of 0.2mm. Clamp the sample with a 4kg clamp and remove any residual adhesive. After curing at room temperature for 4 hours, perform an overlap shear test at 200mm / min. Repeat the sample test 5 times.

[0106] De-adhesion test in lactic acid solution

[0107] Samples were prepared following the same procedure for the overlap shear test. After curing at room temperature for 5 hours, the samples were placed in a 10% lactic acid solution at 70°C. After soaking for 1 hour, the adhesive was observed to determine if it had failed. The sample test was repeated 3 times.

[0108] De-adhesion test in citric acid solution

[0109] Samples were prepared following the same procedure for the overlap shear test. After curing at room temperature for 5 hours, the samples were placed in a 5% lactic acid solution at 80°C. After soaking for 1 hour, the adhesive was observed to determine if it had failed. The sample test was repeated 3 times.

[0110] De-adhesion test in boiling water

[0111] Samples were prepared following the same procedure for the lap shear test. After curing at room temperature for 6 hours, the samples were placed in water at 97°C. After immersion for 1 hour, the adhesive failure time was observed and recorded. The sample test was repeated 3 times.

[0112] Viscosity

[0113] The viscosity of the adhesive was determined using a HAAKE viscometer according to procedure W00034.

[0114] gel time

[0115] Turn on the gel time meter (Brookfield DV2T) and mix components A and B with a spatula for 45 seconds. Place the mixture in the gel time meter and start recording the time until the rotator can no longer rotate. Record the stopping time as the gel time.

[0116] fixed time

[0117] Mix components A and B with a spatula for 45 seconds and prepare an overlap-shear sample. After sample preparation, continuously check the overlap-shear sample and record the time it takes for the two substrates to stop sliding as the fixed time.

[0118] Example 1:

[0119] Weigh out 24.5 parts of polyol 1, 25 parts of polyol 2, 4.9 parts of glycerol, 5 parts of T-slurry, 0.132 parts of Dabco 33LV, 20 parts of filler, and 10 parts of TEMs as component (i) in a 100 ml PP cup. Then, weigh out isocyanate A as component (ii) according to a weight mixing ratio of 100:49 (component (i) : component (ii)) and quickly add it to the cup. After sealing the cup with a cap with a pinhole (for vacuum purposes), place the cup in a high-speed mixer and mix under vacuum at 1500 rpm for 2 minutes. The mixture is then applied to the surface of a substrate and the above-mentioned properties are tested.

[0120] Examples 2 to 4:

[0121] In Examples 2 to 4, the preparation steps were the same as in Example 1, except that the amount of the components added was as shown in Table 1.

[0122] Comparative Example 1:

[0123] In Comparative Example 1, the preparation steps were the same as in Example 1, except that the amounts of the components added were as shown in Table 1. Specifically, TEMs were not added to the reaction mixture.

[0124] The performance of the adhesive samples prepared by Examples 1 to 4 and Comparative Examples 1 to 2 was tested, and the results are summarized in Table 1 below.

[0125] Table 1: Performance of adhesive samples according to Examples 1 to 4 of the Invention and Comparative Examples 1 to 2

[0126]

[0127] All prepared adhesive samples exhibited strong adhesion in the lap shear test and good stability in acid / aqueous solutions. However, the reaction mixture of Comparative Example 1 did not contain thermally expanded microspheres, resulting in a debonding time exceeding 60 minutes in 97°C hot water, which is unacceptable for debonding procedures during wafer dicing. In contrast, all adhesive samples of the present invention exhibited excellent debonding performance in less than 3 minutes in 97°C hot water. It is also noted that the debonding efficiency is highly dependent on the adhesive index. Even for inventive samples with indices falling within the range of the present invention, isocyanate indices of 40 to 50 appear to produce better results in terms of debonding time.

[0128] Examples 5 to 7

[0129] In Examples 5 to 7, the preparation steps were the same as in Example 1, except that the amounts of the components added were as shown in Table 2. By adjusting the amount of each component added and the mixing ratio of components (i) and (ii), specific isocyanate indices were achieved for the respective examples, as shown in Table 2. After mixing, the mixture was applied to the surface of a substrate and the aforementioned properties were tested.

[0130] Comparative Examples 2 to 6

[0131] In Comparative Examples 2 to 6, the preparation steps were the same as in Example 1, except that the amounts of the components added were as shown in Table 2. By adjusting the amount of each component added and the mixing ratio of components (i) and (ii), specific isocyanate indices were achieved for the respective examples, as shown in Table 2. After mixing, the mixture was applied to the surface of a substrate and the aforementioned properties were tested.

[0132] The performance of the adhesive samples prepared by Examples 5 to 7 and Comparative Examples 2 to 6 was tested, and the results are summarized in Table 2 below.

[0133] Table 2: Performance of adhesive samples according to Examples 5 to 7 of the Invention and Comparative Examples 2 to 6

[0134]

[0135] Table 2

[0136]

[0137]

[0138] As can be seen from Table 2 above, Invention Examples 5 to 7 and Comparative Examples 2 to 6 used the same components (i) (i.e., a mixture of components (B) to (E)) and (ii) (i.e., component (A)), but in different mixing ratios. By using different mixing ratios of components (i) and (ii), the various examples yielded specific polyurethane adhesives with specific indices as shown in Table 2. The performance tests shown in Table 2 indicate that when the indices of the reactants used to prepare the polyurethane adhesive fall within a suitable range, adhesive samples with the desired lap shear strength and a short detack time in hot water at 97°C can be obtained. Conversely, if the index is too low (e.g., 25), the reaction mixture forming the polymer cannot cure, and no adhesive sample can be obtained, as shown in Comparative Example 2. On the other hand, if the index is too high (e.g., 75, 90, or greater than 100), the obtained adhesive sample requires a long detack time when heated in hot water at 97°C, as shown in Comparative Examples 3 to 6. In these comparative examples, the detack time can be as long as 25 minutes or more, which, although theoretically feasible, is not commercially feasible.

[0139] Examples 8 to 10

[0140] In Examples 8 to 10, the preparation steps were the same as in Example 6, except that the amount of TEMs(D) added was as shown in Table 3. By adjusting the amount of each component added and the mixing ratio of components (i) and (ii), specific isocyanate indices were achieved for the respective examples, as shown in Table 3. After mixing, the mixture was applied to the surface of a substrate and the aforementioned properties were tested.

[0141] Comparative Example 7

[0142] In Comparative Example 7, the preparation steps were the same as in Example 6, except that the amount of TEMs(D) added was as shown in Table 3. After mixing, the mixture was applied to the substrate surface and the aforementioned properties were tested.

[0143] The performance of the adhesive samples prepared by Examples 8 to 10 and Comparative Example 7 was tested, and the results are summarized in Table 3 below and compared with the results of Example 6.

[0144] Table 3: Performance of adhesive samples according to Examples 6, 8 to 10 of the Invention and Comparative Example 7

[0145]

[0146] Examples 6 and 8 through 10 of the invention, as well as Comparative Example 7, used the same components and the same mixing ratios, the difference being that the TEMs (component D) were present in different amounts in these examples. The results shown in Table 3 indicate that as the amount of thermally expandable microspheres (D) decreases, the debonding time of the adhesive sample increases. When the amount of thermally expandable microspheres (D) is too low, the debonding time of the adhesive sample can exceed 1 hour, which is commercially unfeasible.

[0147] Example 11

[0148] In this embodiment, the use of the polyurethane adhesive according to the invention in the preparation of tensile test specimens was also tested. Specifically, 30 g of component (i) and 15 g of component (ii) were weighed and manually mixed in a sample cup. Component (i) has the same composition as described in Example 3 of Table 1. The adhesive (approximately 0.2 to 0.3 mm thick) was manually applied to the first metal clamp using a spatula. The test specimen was placed on the metal clamp with the adhesive and allowed to cure at room temperature. The adhesive was manually applied to the second metal clamp using a spatula. The second metal clamp was placed on the test specimen and secured to a universal tensile testing machine (a Zwick). After the tensile test, the metal clamp was placed in a 90°C water bath. The metal clamp could be easily separated from the specimen within approximately 1 to 2.5 minutes and was easily retrievable.

[0149] The structures, materials, compositions, and methods described herein are intended as representative embodiments of the invention, and it is to be understood that the scope of the invention is not limited to the scope of these embodiments. Those skilled in the art will recognize that the invention can be practiced by variations of the disclosed structures, materials, compositions, and methods, and such variations are considered to be within the scope of the invention. Therefore, the invention is intended to cover these modifications and variations that fall within the scope of the appended claims and their equivalents.

Claims

1. A detangleable polyurethane adhesive based on thermally expandable microspheres, obtained through the reaction of the following components: (A) at least one diisocyanate or polyisocyanate; (B) At least one polyol; (C) Catalyst; (D) Thermally expandable microspheres; and (E) Other additives. The isocyanate index for this reaction is set in the range of 28 to 65. The thermally expandable microspheres (D) are present in an amount of 5 to 10% by weight, based on the total weight of the polyurethane adhesive. The initial temperature T of the thermally expanded microspheres (D) start The temperature ranges from 75 to 97 degrees Celsius.

2. The polyurethane adhesive according to claim 1, wherein the isocyanate index of the reaction is set in the range of 30 to 60.

3. The polyurethane adhesive according to claim 1, wherein the isocyanate index of the reaction is set in the range of 30 to 50.

4. The polyurethane adhesive according to claim 1, wherein the isocyanate index of the reaction is set in the range of 35 to 50.

5. The polyurethane adhesive according to any one of claims 1 to 4, wherein the diisocyanate or polyisocyanate (A) is selected from tri-, tetra-, penta-, hexa-, hepta- and / or octa-methylene diisocyanate, 2-methylpentamethylene 1,5-diisocyanate, 2-ethyltetramethylene 1,4-diisocyanate, butene 1,4-diisocyanate, trimethylhexamethylene 1,6-diisocyanate, 1-isocyano-3,3,5-trimethyl-5-isocyanomethylcyclohexane (isophorone diisocyanate, IPDI), 1,4- and / or 1,3-bis(isocyanate methyl)cyclohexane (HXDI), cyclohexane-1,4-diisocyanate Esters, 1-methylcyclohexane 2,4- and / or 2,6-diisocyanates, methylene dicyclohexyl 4,4'-, 2,4'- and / or 2,2'-diisocyanates (H12MDI), 1,5-naphthalene diisocyanate (NDI), 2,4- and / or 2,6-toluene diisocyanate (TDI), 3,3'-dimethyl-4,4'-biphenyl diisocyanate (TODI), terephthalic diisocyanate (PDI), diphenylethane 4,4'-diisocyanate (EDI), dimethyl diphenyl 3,3'-diisocyanate, diphenylethane 1,2-diisocyanate and / or diphenylmethane diisocyanate (MDI), or prepolymers thereof.

6. The polyurethane adhesive according to any one of claims 1 to 4, wherein the diisocyanate or polyisocyanate (A) is selected from 2,2'-MDI, 4,4'-MDI, MDI prepolymer, or mixtures thereof.

7. The polyurethane adhesive according to any one of claims 1 to 4, wherein the diisocyanate or polyisocyanate (A) is present in an amount of 25 to 70% by weight, based on the total weight of the polyurethane adhesive.

8. The polyurethane adhesive according to any one of claims 1 to 4, wherein the diisocyanate or polyisocyanate (A) is present in an amount of 30 to 65% by weight, based on the total weight of the polyurethane adhesive.

9. The polyurethane adhesive according to any one of claims 1 to 4, wherein the diisocyanate or polyisocyanate (A) is present in an amount of 35 to 60% by weight, based on the total weight of the polyurethane adhesive.

10. The polyurethane adhesive according to any one of claims 1 to 4, wherein the polyol (B) is selected from polyether alcohols and / or polyester alcohols having 2 to 8 hydrogen atoms that are reactive to isocyanates.

11. The polyurethane adhesive according to any one of claims 1 to 4, wherein the polyol (B) is present in an amount of 15 to 45% by weight, based on the total weight of the polyurethane adhesive.

12. The polyurethane adhesive according to any one of claims 1 to 4, wherein the polyol (B) is present in an amount of 18 to 40% by weight, based on the total weight of the polyurethane adhesive.

13. The polyurethane adhesive according to any one of claims 1 to 4, wherein the polyol (B) is present in an amount of 25 to 35% by weight, based on the total weight of the polyurethane adhesive.

14. The polyurethane adhesive according to any one of claims 1 to 4, wherein the thermally expandable microspheres (D) have a core-shell structure, and the shell is formed of a crosslinked polymer and the core is composed of a physical foaming agent.

15. The polyurethane adhesive according to any one of claims 1 to 4, wherein the additive (E) comprises surfactants, foam stabilizers, cell conditioners, fillers, pigments, dyes, flame retardants, anti-hydrolysis agents, antistatic agents, water-absorbing agents, and auxiliaries having antifungal and antibacterial effects.

16. The polyurethane adhesive according to any one of claims 1 to 4, wherein the debonding time of the polyurethane adhesive in hot water at 75°C or higher is less than 10 minutes.

17. The polyurethane adhesive according to any one of claims 1 to 4, wherein the polyurethane adhesive is obtained by reacting the following components: (A) 25 to 70% by weight of at least one diisocyanate or polyisocyanate; (B) 15 to 45% by weight of at least one polyol; (C) 0.01 to 2% by weight of catalyst; (D) 5 to 10% by weight of thermally expanding microspheres; and (E) Other additives, based on the total weight of the polyurethane adhesive. The isocyanate index for this reaction is set in the range of 30 to 60.

18. A method for preparing a polyurethane adhesive according to any one of claims 1 to 17, comprising the step of mixing the following components: (A) at least one diisocyanate or polyisocyanate; (B) At least one polyol; (C) Catalyst; (D) Thermally expandable microspheres; and (E) Other additives. The isocyanate index is set in the range of 28 to 65.

19. The method according to claim 18, wherein component (A) is added separately as component (ii), and components (B) through (E) are added together as component (i).

20. The method according to claim 19, wherein the mixing ratio of components (i) and (ii) is in the range of 3:1 to 1:

3.

21. The method according to claim 19, wherein the mixing ratio of components (i) and (ii) is in the range of 2.5:1 to 1:

2.

22. The method according to claim 19, wherein the mixing ratio of components (i) and (ii) is in the range of 2:1 to 1:1.

8.

23. Use of the thermally expandable microsphere-based debonded polyurethane adhesive according to any one of claims 1 to 17 for debonding metal and dicing pad during wafer dicing.

24. The use according to claim 23, wherein deadhesion is carried out in hot water at a temperature of 75°C or above.

25. The use according to claim 23, wherein deadhesion is carried out in hot water at a temperature of 80°C or above.

26. The use according to claim 23, wherein deadhesion is carried out in hot water at a temperature of 90°C or above.

27. The use according to claim 23, wherein deadhesion is carried out in hot water at a temperature of 97°C or above.

28. Use of the thermally expandable microsphere-based debonded polyurethane adhesive according to any one of claims 1 to 17 in the preparation of mechanical property test samples.

Citation Information

Patent Citations

  • A kind of adhesive for hot water degumming of silicon chips and preparation method thereof

    CN104031597B

  • Adhesive composition comprising thermoexpandable microcapsules

    CN1192070C

  • Production of polyisocyanate-polyaddition products in a multi-modular plate reactor, gives thermoplastic polyurethanes or elastomeric polyurethane-ureas for producing elastomeric fibers or extrudates

    DE10103424A1

  • Process for continuous production of granules of thermoplastic polyurethanelastomers

    EP0922552A1

  • Adhesive composition for temporarily bonding use in wafer manufacturing

    US9714317B2