Positive charge filter material having excellent removal performance for charged particles and method for preparing the same
By plasma surface treatment of the porous support and coating it with a positively charged coating composition, the problem of removing organic/inorganic particles and pathogenic microorganisms from water is solved, improving the safety and filtration efficiency of the filter media.
Patent Information
- Application Number
- CN202180060496.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-07-28
- Filing Date
- 2021-06-22
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2041-06-22
AI Technical Summary
Existing technologies are ineffective at removing negatively charged organic/inorganic particles, heavy metal ions, and pathogenic microorganisms from water, and traditional positively charged filter media pose safety hazards and flow rate and pressure issues.
A porous support, comprising polypropylene, polyethylene, polyester, nylon or cellulose fibers, is modified by atmospheric pressure plasma surface treatment and coated on its surface and interior with a positively charged coating composition, comprising alcohol, acetone, water, polyfunctional amine compounds and crosslinking agents, to form a positively charged coating of 5% to 15% by weight.
It achieves excellent removal performance of negatively charged particles, reduces hazard, increases flow rate and filtration pressure, and has high productivity.
Smart Images

Figure CN116249581B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a positively charged filter material with excellent removal performance for charged particles and its preparation method, and more specifically, to a positively charged filter material with excellent selective removal performance for negatively charged organic / inorganic particles, heavy metal ions and pathogenic microorganisms in water and its preparation method. Background Technology
[0002] Water typically contains many ionic substances and chemicals, including Natural Organic Matter (NOM). However, these substances may not be removed during water treatment and could become the cause of new pollutants.
[0003] Furthermore, the existence of pathogenic microorganisms that cannot be removed by chlorine disinfection has been a subject of ongoing debate. For example, pathogenic microorganisms classified as viruses, Cryptosporidium, and Giardia are released into the environment through human and animal feces, and are present not only in sewage but also in surface and groundwater. Because of their extremely small size, including these viruses, conventional filtration methods are largely ineffective, and they can survive stably in water for months or longer by forming highly chlorine-resistant cysts.
[0004] In addition, the South Korean Ministry of Environment has published standards and regulations for heavy metals such as aluminum, iron, lead, and mercury in potable water, which are used as drinking water. These standards and regulations have been applied and are being continuously analyzed and managed to address various external environmental changes.
[0005] On the other hand, as mentioned above, in order to remove trace pollutants remaining in water, high-density flocculation, activated carbon adsorption, and membrane filtration have been proposed in water treatment processes. Furthermore, South Korea is currently conducting a large-scale national study on membrane-based water treatment technologies. In particular, although numerous studies have been conducted on membrane filtration technology recently and it has been practically applied in advanced water treatment processes, it is not yet widely used due to economic costs and technical issues.
[0006] For example, Korean Patent Publication No. 10-2004-0088046 discloses a method for preparing antiviral filter media. The method uses glass fiber as the basic filter media and prepares a positively charged filter by adding a positively charged inorganic compound during the preparation of the glass fiber. The prepared filter is then used to adsorb viruses. However, due to controversies surrounding the potential carcinogenicity and other hazards associated with the use of glass fiber, there are concerns about its applicability to water treatment processes. Furthermore, the compounds added during the preparation of glass fiber limit product diversification.
[0007] Therefore, there is a growing demand for positively charged filter media that possess excellent removal performance for negatively charged microparticles, heavy metal ions, and pathogenic microorganisms, while also exhibiting low hazard and excellent flow rate and filtration pressure. Summary of the Invention
[0008] The problem to be solved
[0009] This invention is proposed to solve the above-mentioned problems. The first problem to be solved by this invention is to provide a positively charged filter material that has excellent removal performance, low hazard, and excellent flow rate and filtration pressure for negatively charged organic / inorganic particles, heavy metal ions and pathogenic microorganisms in water.
[0010] Furthermore, the second problem to be solved by the present invention is to provide a method for preparing a positively charged filter material with excellent selective removal performance as described above, the method being a method that can improve productivity.
[0011] Solution to the problem
[0012] To address the aforementioned issues, the present invention provides a positively charged filter material comprising: a porous support containing at least one fiber selected from polypropylene (PP) fibers, polyethylene (PE) fibers, polyester fibers, nylon fibers, and cellulose fibers, and surface-modified by atmospheric pressure plasma surface treatment; and a positively charged coating formed by coating the surface and interior of the porous support with a positively charged coating composition, the positively charged coating composition containing at least one solvent selected from C2 to C5 alcohols, acetone, and water (H2O), a polyfunctional amine compound, and a crosslinking agent that undergoes an epoxy reaction with the polyfunctional amine compound, wherein the weight of the positively charged coating is 5% to 15% of the weight of the porous support.
[0013] In a preferred embodiment of the present invention, the porous support may be a composite nonwoven fabric having a layered structure in which the upper and lower layers are spunbond nonwoven fabric and the middle layer is meltblown nonwoven fabric.
[0014] In a preferred embodiment of the present invention, the average fiber diameter of the upper and lower layers can be from 10µm to 30µm, the average fiber diameter of the middle layer can be from 1µm to 30µm, and the average fiber diameter of the composite nonwoven fabric can be from 5µm to 25µm.
[0015] In a preferred embodiment of the present invention, the content of the polyfunctional amine compound may be from 1 part by weight to 10 parts by weight, based on 100 parts by weight of the positively charged coating composition.
[0016] In a preferred embodiment of the present invention, the positively charged coating composition can satisfy the following condition (Formula 1).
[0017] 1) 0.4≤C amine / C Cl ≤6
[0018] In condition 1), C amine C represents the weight content of the polyfunctional amine compound relative to the positively charged coating composition. cl This indicates the weight content of the crosslinking agent.
[0019] In a preferred embodiment of the present invention, the polyfunctional amine compound may be at least one selected from the group consisting of diphenylamine, polyethyleneimine, diethylenetriamine, dimethylene piperazine, and piperazine.
[0020] In a preferred embodiment of the present invention, the tertiary amine may account for less than 30 mol% of the polyfunctional amine compound.
[0021] In a preferred embodiment of the present invention, the crosslinking agent may be an aliphatic epoxy compound comprising at least one selected from the group consisting of polyethylene glycol diglycidyl ether, sorbitol polyglycidyl ether, diethylene glycol diglycidyl ether, and propylene glycol diglycidyl ether.
[0022] Furthermore, in order to solve the problems mentioned above, the present invention provides a method for preparing a positively charged filter material, the method comprising: step (1): subjecting a porous support comprising at least one fiber selected from polypropylene (PP) fiber, polyethylene (PE) fiber, polyester fiber, nylon fiber and cellulose fiber to atmospheric pressure plasma treatment for surface modification; step (2): contacting the surface-modified porous support with a positively charged coating composition to coat the porous support with the positively charged coating composition, wherein the positively charged coating composition comprises at least one solvent selected from C2 to C5 alcohol, acetone and water (H2O), a polyfunctional amine compound and a crosslinking agent that reacts with the polyfunctional amine compound in an epoxy reaction; and step (3): forming a positively charged coating by thermally crosslinking the porous support coated with the positively charged coating composition.
[0023] In a preferred embodiment of the present invention, step (3) can be performed under the condition that the following conditions 2), 3) or 4) are met.
[0024] 2) 60℃≤T r <90℃, 250s≤t r ≤600s
[0025] 3) 90℃≤T r <110℃, 100s≤t r ≤300s
[0026] 4) 110℃≤T r <130℃, 60s≤t r ≤l50s
[0027] In the above conditional expressions 2) to 4), T r t represents the thermal crosslinking temperature (°C). r Indicates the thermal crosslinking time (sec).
[0028] The effects of the invention
[0029] The positively charged filter media according to the present invention has excellent removal performance for negatively charged organic / inorganic particles, heavy metal ions and pathogenic microorganisms, and has low hazard and can achieve the same level of flow rate and filtration pressure as conventional filter media.
[0030] When preparing positively charged filter materials according to the preparation method of the present invention, it has the advantages of being able to uniformly form a positively charged coating and improving productivity. Attached Figure Description
[0031] Figure 1 It is a photograph of a cross-section of a positively charged filter material according to an embodiment of the present invention.
[0032] Figure 2 This is a schematic diagram illustrating the layered structure of a positively charged filter material according to an embodiment of the present invention.
[0033] Figure 3 This is a scanning electron microscope (SEM) image of a composite nonwoven fabric comprising a positively charged filter material according to an embodiment of the present invention before being coated with a positively charged coating composition.
[0034] Figure 4 This is a SEM image of a positively charged filter material according to an embodiment of the present invention.
[0035] The specific implementation method is the best way to carry out the invention.
[0036] In the following detailed description, embodiments of the invention will be given with reference to the accompanying drawings, so that those skilled in the art to which this invention pertains can readily implement it. The invention can be implemented in various different forms and is not limited to the embodiments described herein.
[0037] Generally speaking, ultrafine fiber filters, which are widely used in water treatment, have the disadvantage of low filtration efficiency due to their small filtration area and lack of electrostatic force. Membrane filters, on the other hand, have the disadvantage of high filtration efficiency but large pressure loss.
[0038] In addition, traditional positively charged filter materials pose safety concerns due to the use of substances that may be harmful to the human body, and also suffer from drawbacks such as insufficient selective removal performance of pathogenic microorganisms or low manufacturing productivity.
[0039] To address these issues, the present invention provides a positively charged filter material comprising: a porous support containing at least one fiber selected from polypropylene (PP) fibers, polyethylene (PE) fibers, polyester fibers, nylon fibers, and cellulose fibers, and surface-modified by atmospheric pressure plasma surface treatment; and a positively charged coating formed by coating the surface and interior of the porous support with a positively charged coating composition, the positively charged coating composition containing at least one solvent selected from C2 to C5 alcohols, acetone, and water (H2O), a polyfunctional amine compound, and a crosslinking agent that undergoes an epoxy reaction with the polyfunctional amine compound, the positively charged coating having a weight change rate of 5% to 15%.
[0040] The porous support of the positively charged filter material according to the present invention comprises at least one fiber selected from polypropylene fiber, polyethylene fiber, polyester fiber, nylon fiber and cellulose fiber. By using this porous support to replace glass fiber, it has the advantages of protecting the human body from harmful components and being applicable to a variety of product groups.
[0041] Furthermore, since the surface of the porous support as described above is generally hydrophobic, it is difficult to uniformly coat the positively charged coating composition which is hydrophilic. However, the present invention improves the hydrophilicity of the surface of the porous support by plasma surface treatment, thereby solving the problem described above and thus having the advantage of being able to form the positively charged coating composition more uniformly.
[0042] Furthermore, the weight of the positively charged coating contained in the positively charged filter material according to the present invention is in the range of 5% to 15% of the weight of the porous support.
[0043] When the weight ratio is less than 5%, the relatively thin parts of the coating may experience a shortened service life. When the weight ratio exceeds 15%, the drying efficiency during the preparation process will decrease, which may have an adverse effect on production efficiency and economy.
[0044] The various components will be described in detail below. First, the positively charged filter material according to the present invention will be described.
[0045] The positively charged filter material according to the present invention includes a porous support comprising at least one fiber selected from polypropylene (PP) fiber, polyethylene (PE) fiber, polyester fiber, nylon fiber and cellulose fiber, and is surface modified by atmospheric pressure plasma surface treatment.
[0046] Among the aforementioned fibers, polypropylene fibers, polyethylene fibers, polyester fibers, and nylon fibers have surfaces that are almost hydrophobic. Therefore, when coating with the hydrophilic positively charged coating composition described above, a uniform coating cannot be formed due to the chemical repulsion between the hydrophilic composition and the hydrophobic support. However, when subjected to atmospheric pressure plasma surface treatment, the surface of the porous support is modified and its hydrophilicity is enhanced, thus enabling a more uniform coating of the positively charged coating composition.
[0047] The porous support provides a framework for the filter media and filters so that they maintain a predetermined shape, and due to the numerous pores on the surface and inside, it can remove a variety of contaminants contained in the treated water.
[0048] The fibers included in the porous support may preferably comprise at least one of the group consisting of polypropylene fibers, polyethylene terephthalate (PET) fibers, and polyethylene fibers. These fibers have good spinnability and can be spun to have a uniform thickness, thus reducing deviations in pore size and thereby easily achieving a predetermined level of filtration capacity.
[0049] As described above, compared with the use of glass fiber as a support, the porous support comprising at least one fiber selected from polypropylene fiber, polyethylene fiber, polyester fiber, nylon fiber and cellulose fiber has the advantage of significantly reducing the harm to the human body, and also has the effect of significantly improving the durability of the filter material because the fiber is less brittle than glass fiber.
[0050] Furthermore, preferably, the porous support can be a nonwoven fabric prepared using the aforementioned fibers. The type of nonwoven fabric can be selected from commonly used nonwoven fabrics, for example, it can be any nonwoven fabric selected from thermal bonding nonwoven fabric, air-laid nonwoven fabric, wet-laid nonwoven fabric, needle-punching nonwoven fabric, water-spunlace nonwoven fabric, spunbond nonwoven fabric, melt-blown nonwoven fabric, stitch-bonded nonwoven fabric, and electrospun nonwoven fabric, or a composite nonwoven fabric containing two or more of these structures.
[0051] More preferably, the nonwoven fabric can be a composite nonwoven fabric with a layered structure consisting of spunbond nonwoven fabric as the upper and lower layers and meltblown nonwoven fabric as the middle layer. Compared with traditional single-layer nonwoven fabrics, the three-layer nonwoven fabric with spunbond nonwoven fabric as the upper and lower layers and meltblown nonwoven fabric as the middle layer has significantly improved tensile strength in both the machine direction (MD) and cross direction (CD). Therefore, when preparing nonwoven fabrics with the same level of physical properties, it has the advantage of improved production speed and coating speed.
[0052] Figure 2 This is a diagram illustrating the layered structure of a positively charged filter material according to a preferred embodiment of the present invention, and in particular, the layered structure of the porous support layer therein. (Refer to...) Figure 2 It is understood that the porous support layer 100 of the positively charged filter material according to the present invention can be composed of a three-layer structure of spunbond nonwoven fabric 10, meltblown nonwoven fabric 20 and spunbond nonwoven fabric 10.
[0053] The upper and lower spunbond nonwoven fabrics are respectively adhered to the upper and lower surfaces of the middle meltblown nonwoven fabric to enhance the tensile strength of the meltblown nonwoven fabric.
[0054] More preferably, the upper and lower spunbond nonwoven layers of the three-layer composite nonwoven fabric can have an average fiber diameter of 10µm to 30µm. More preferably, they can have an average fineness of 15µm to 20µm. When the average fiber diameter of the upper and lower spunbond nonwoven layers is less than 15µm, the tensile strength and tear strength of the spunbond nonwoven fabric decrease, thus causing a decrease in the overall strength of the composite nonwoven fabric, which in turn poses a risk of low productivity in the manufacturing process. Conversely, when the average fiber diameter of the spunbond nonwoven layers exceeds 30µm, there is a problem of decreased permeability pressure of the filter material.
[0055] The meltblown nonwoven fabric of the intermediate layer can have an average fiber diameter of 1µm to 30µm. More preferably, it can have an average fiber diameter of 1µm to 7µm. When the average fiber diameter of the meltblown nonwoven fabric is less than 1µm, the tensile and tear strength of the porous support layer may decrease, leading to problems such as reduced productivity in the manufacturing process, decreased durability of the positively charged filter material, and shortened service life. Conversely, compared to cases with relatively small fiber diameters, when the average fineness exceeds 30µm, the removal performance decreases due to the simultaneous increase in internal pore size.
[0056] The overall average fiber diameter of the composite nonwoven fabric can be between 5µm and 25µm. When the overall average fiber diameter is less than 5µm, the tensile and tear strength of the porous support layer may decrease, leading to reduced productivity in the manufacturing process, decreased durability of the positively charged filter material, and a shortened service life. Conversely, when the overall average fiber diameter exceeds 25µm, the processability of the nonwoven fabric may decrease, and the service life of the positively charged filter material may be shortened due to pressure differential, resulting in issues related to durability and safety.
[0057] In the positively charged filter material according to the present invention, the porous support can have an average pore size of 0.5 µm to 300 µm. More preferably, it can have an average pore size of 10 µm to 150 µm. When the average pore size of the composite nonwoven fabric is less than 0.5 µm, problems may arise regarding instantaneous flow rate reduction and shortened service life. Furthermore, when the average pore size of the composite nonwoven fabric exceeds 300 µm, even with positive charge coating, problems may exist regarding the uniformity and stability of the removal performance against microorganisms present in the treated water.
[0058] The porous support according to the present invention preferably has an average thickness of 0.2 mm to 2 mm, and more preferably an average thickness of 0.3 mm to 1 mm. Preferably, the average thickness can be an arithmetic mean obtained by averaging the thicknesses measured at 10 different locations. When the average thickness of the porous support is less than 0.2 mm, insufficient filtration thickness may lead to reduced adsorption performance at high flow rates. When the average thickness of the porous support exceeds 2 mm, the processability of the porous support decreases, and problems related to durability and safety, such as shortened service life of the positively charged filter material due to pressure differential, may occur.
[0059] When the porous support is a composite nonwoven fabric comprising an upper and lower spunbond nonwoven fabric and an intermediate meltblown nonwoven fabric, as described above, the average thickness of the meltblown nonwoven fabric intermediate layer is preferably 0.15 mm to 1.5 mm. More preferably, it can have an average thickness of 0.25 mm to 0.7 mm. When the average thickness of the meltblown nonwoven fabric intermediate layer is less than 0.15 mm, insufficient depth for filtration may result in reduced adsorption performance at high flow rates. Furthermore, when the average thickness of the meltblown nonwoven fabric intermediate layer exceeds 1.5 mm, the overall thickness of the porous support increases, reducing its processability and potentially leading to durability and safety issues such as shortened service life due to pressure differentials.
[0060] The porous support can preferably have a density of 30 g / m³. 2 Up to 150g / m 2 The average weight (basic weight), and preferably has 50 g / m³. 2 Up to 100g / m 2 The base weight.
[0061] When the basis weight of the porous support is less than 30g / m 2 At this point, the tensile strength of the nonwoven fabric decreases, which may lead to processing difficulties due to breakage problems during coating and processing. This is especially true when the basis weight of the porous support exceeds 150 g / m². 2 As the fiber density in the support increases, problems such as a rapidly shortened service life may occur due to the dense structure, which may cause pressure differentials.
[0062] When the porous support is a layered composite nonwoven fabric as described above, the basis weight of the upper and lower spunbond nonwoven fabrics is preferably 30 g / m². 2 Up to 300g / m 2 When the basis weight of the spunbond nonwoven fabric is less than 30 g / m³ 2 At this time, there may be a problem of decreased tensile strength.
[0063] Furthermore, the meltblown nonwoven fabric can have a density of 1 g / m³. 2 Up to 10g / m 2 The basis weight. When the basis weight of the meltblown nonwoven fabric is less than 1 g / m³. 2 At certain times, there may be a problem of reduced removal performance; conversely, when the basis weight exceeds 10 g / m³, there may be a problem of reduced removal performance. 2 At this time, there may be a problem of decreased tensile strength.
[0064] The following will describe the positively charged coating formed by coating the surface and interior of the porous support.
[0065] A positive charge coating is a layer formed by applying a positive charge coating composition to the surface and interior of the porous support and thermally crosslinking it. Preferably, it can be a coating applied to the surface of fibers and fiber strips contained in the surface and interior of the porous support.
[0066] By applying a positively charged coating to the aforementioned hydrophobic porous branch layer, negatively charged organic / inorganic particles, heavy metal ions, and pathogenic microorganisms contained in the treated water can be selectively removed.
[0067] The positively charged coating preferably has an average thickness of 0.01 µm to 3 µm. More preferably, it has an average thickness of 0.05 µm to 1 µm. When the average thickness of the positively charged coating is less than 0.01 µm, physical property deviations may occur due to reduced uniformity of the coating. When the average thickness of the positively charged coating is greater than 3 µm, durability and safety issues may arise because the positively charged coating composition described later may not be adequately coated and may be washed away.
[0068] The positively charged coating composition used to form the positively charged coating will be described in detail below.
[0069] The positively charged coating composition comprises at least one solvent in C2 to C5 alcohol, acetone, and water, a polyfunctional amine compound, and a crosslinking agent capable of undergoing an epoxy reaction with the polyfunctional amine compound. Preferably, the positively charged coating composition may further comprise a penetrant.
[0070] The components will be described in detail below.
[0071] In conventional positively charged filter media, at least one solvent selected from C2 to C5 alcohols, acetone, and water is used. To improve the wettability of the support, filter media with porous supports containing hydrophobic components such as polypropylene fibers use surfactants and organic solvents to enhance coating efficiency. However, this results in surfactants or organic solvents remaining inside the prepared positively charged filter media, causing problems such as unstable initial elution properties and decreased productivity due to the need for further cleaning. Furthermore, there is a problem of low tensile strength in the nonwoven fabric. In this invention, by using the aforementioned hydrophilic solvent, the use of surfactants is omitted, and productivity is significantly improved by minimizing residual solvent. Furthermore, with the problem of low tensile strength in the nonwoven fabric resolved, the durability of the filter media is improved, and its service life is extended. The solvent can preferably be water, and based on 100 parts by weight of the composition, the solvent content can be from 85 parts by weight to 98.85 parts by weight, more preferably from 94 parts by weight to 98.7 parts by weight.
[0072] Polyfunctional amine compounds are used to impart positive charge to positively charged coating compositions and positively charged filter media coated with said coating compositions. The polyfunctional amine compounds selected should not affect the physical properties of the porous support. Preferably, the polyfunctional amine compound can be at least one selected from the group consisting of diphenylamine, polyethyleneimine, diethylenetriamine, dimethylene piperazine, and piperazine. Preferably, polyethyleneimine can be used, as it has a high positive charge density, thus allowing it to be readily imparted with a positive charge through reaction with a crosslinking agent.
[0073] At this point, the polyfunctional amine compound can be selected from those with a weight-average molecular weight of 1,000 g / mol to 1,000,000 g / mol, preferably 2,000 g / mol to 700,000 g / mol. When the weight-average molecular weight of the polyfunctional amine compound is less than 1,000 g / mol, elution problems due to water pressure may occur due to durability issues. When the weight-average molecular weight of the polyfunctional amine compound exceeds 1,000,000 g / mol, the coating uniformity may decrease due to increased viscosity, and there may be problems with performance deviations and even reduced product reliability due to decreased durability.
[0074] Furthermore, 100 parts by weight of the positively charged coating composition may contain 1 to 10 parts by weight of the polyfunctional amine compound, preferably 1 to 4 parts by weight. When the 100 parts by weight of the positively charged coating composition contains less than 1 part by weight of the polyfunctional amine compound, there is a risk of deterioration in coating performance and coating uniformity due to insufficient amount of the positively charged coating composition. Furthermore, when the 100 parts by weight of the positively charged coating composition contains more than 10 parts by weight of the polyfunctional amine compound, the viscosity of the positively charged coating composition may become too high to coat the interior of the porous support. In addition, due to the reduction in the average pore size of the nonwoven fabric, problems such as reduced flow rate and shortened service life may occur.
[0075] In a preferred embodiment of the invention, the polyfunctional amine compound may include primary and secondary amines, and may also include tertiary amines; however, the molar fraction of tertiary amines may be less than 30 mol%. Compared to tertiary amine compounds, primary and secondary amines have less steric hindrance, are more readily subjected to epoxide reactions, can minimize unreacted residual amine compounds, and have the advantage of easily forming a uniform positively charged coating.
[0076] The primary, secondary, or tertiary amines may be contained together in a single molecule. In this case, by comparing the number of functional groups of the various amines, it can be determined that the molar fraction of the tertiary nitrogen is 50 mol% or more.
[0077] The crosslinking agent can not only act as a crosslinking agent and adhesive between polyfunctional amine compounds, but also, in a preferred embodiment of the present invention, the crosslinking agent can be an aliphatic epoxy compound comprising at least one selected from the group consisting of polyethylene glycol diglycidyl ether, sorbitol polyglycidyl ether, diethylene glycol diglycidyl ether, and propylene glycol diglycidyl ether.
[0078] Based on 100 parts by weight of the positively charged coating composition, it may contain 0.1 parts by weight to 2 parts by weight of the crosslinking agent, preferably 0.2 parts by weight to 1 part by weight. When the positively charged coating composition based on 100 parts by weight contains less than 0.1 parts by weight of the crosslinking agent, there is a problem of unreacted polyfunctional amine compound residues due to insufficient content of the crosslinking agent for crosslinking reaction with the polyfunctional amine compound. Furthermore, when the positively charged coating composition based on 100 parts by weight contains more than 2 parts by weight of the crosslinking agent, the surface energy may decrease, potentially leading to a reduced adsorption capacity for viruses, anionic particles, or microorganisms.
[0079] Furthermore, the content of the polyfunctional amine compound and the crosslinking agent compound can satisfy the following condition (Equation 1).
[0080] 1) 0.4≤C amine / C cl ≤6
[0081] In condition 1), C amine C represents the weight content of the polyfunctional amine compound in the positively charged coating composition. cl This indicates the weight content of the crosslinking agent.
[0082] When C amine / C cl When the value is less than 0.4 or greater than 6, the amount of unreacted residual polyfunctional amine compounds or crosslinking agents produced will become excessive, thus requiring additional cleaning processes, which will lead to a decrease in productivity.
[0083] On the other hand, since the polyfunctional amine compound and crosslinking agent are typically hydrophilic materials, it is difficult to form a coating on the surface and interior of a porous support containing hydrophobic fibers such as polyethylene fibers. Therefore, the present invention not only performs atmospheric pressure plasma treatment on the surface of the porous support to modify its surface hydrophilicity, but also uses a penetrant that can simultaneously exhibit both hydrophilicity and hydrophobicity by including both hydrophilic and hydrophobic functional groups.
[0084] The penetrant may be included in the positively charged coating composition. When the penetrant is dissolved in the solvent together with the polyfunctional amine compound and the crosslinking agent and forms a coating on the porous support, a more uniform coating can be induced by reducing the difference in chemical properties with the porous support.
[0085] The penetrant can be a known anionic, cationic, or nonionic penetrant that does not affect the physical properties of the positively charged coating and porous support of the present invention. For example, it may contain at least one selected from sodium dioctyl sulfosuccinate, potassium cocoyl glycinate, sodium dodecyl sulfate, 2-ethyl-1,3-hexanediol, 2,2,4-trimethyl-1,3-pentanediol, alkyl polyglucoside, and alkyl glucamide. However, sodium dioctyl sulfosuccinate is preferably used to maximize the wetting properties of the porous support relative to the amount added and to improve the efficiency of the cleaning process when a cleaning process is required.
[0086] At this point, a 100-part-by-weight positively charged coating composition may contain 0.05 to 1 part by weight of the penetrant, preferably 0.07 to 1 part by weight. When the 100-part-by-weight positively charged coating composition contains less than 0.05 parts by weight of the penetrant, it will be difficult to coat uniformly due to the difference in surface energy between the positively charged coating composition and the porous support, and this may result in the coating composition agglomerating on the porous support. Furthermore, when the 100-part-by-weight positively charged coating composition contains more than 1 part by weight of the penetrant, the surface energy properties of the coated porous support can be maintained at a predetermined level; however, due to the increased amount of penetrant that needs to be removed, problems such as impurities may occur, and there may be problems of decreased process efficiency and reduced productivity.
[0087] Furthermore, since the positively charged coating is formed by the above-mentioned positively charged coating composition, the positively charged filter material according to the present invention can have a surface charge of 15mV to 40mV under pH 7 conditions, preferably, it can have a surface charge of 15mV to 30mV.
[0088] As described above, the porous support has a positive surface charge, thus enabling it to adsorb and trap negatively charged organic matter or particles. When the surface charge of the porous support is less than 15mV, there may be a decrease in its adsorption capacity for organic matter such as viruses. Furthermore, when the surface charge of the porous support exceeds 40mV, although it can maintain the virus adsorption capacity at a predetermined level or higher, the production cost will increase as the reaction time and concentration used to present high surface charges increase during the preparation process, making it uneconomical.
[0089] Next, a method for preparing the positively charged filter material according to the present invention will be described.
[0090] The positively charged filter material according to the present invention is performed by the following steps: Step (1): a porous support comprising at least one fiber selected from polypropylene (PP) fiber, polyethylene (PE) fiber, polyester fiber, nylon fiber and cellulose fiber is subjected to atmospheric pressure plasma treatment to modify the surface; Step (2): the surface-modified porous support is contacted with a positively charged coating composition to coat the porous support with the positively charged coating composition, the positively charged coating composition comprising at least one solvent selected from C2 to C5 alcohol, acetone and water, a polyfunctional amine compound and a crosslinking agent that reacts with the polyfunctional amine compound in an epoxy reaction; and Step (3): a positively charged coating is formed by thermally crosslinking the porous support coated with the charged coating composition.
[0091] Preferably, a washing and drying step may be included after step (4).
[0092] First, (1) a surface modification step is performed by subjecting the surface of the porous support to atmospheric pressure plasma treatment. The composition, type, and thickness of the porous support are the same as those of the positively charged filter material described above, and are therefore omitted here.
[0093] The surface hydrophilicity and adhesion of porous supports can be improved by atmospheric pressure plasma treatment. Specifically, when performing atmospheric pressure plasma treatment, atmospheric pressure plasma can be used to treat the porous support. The plasma is preferably formed from air and has a composition of 70% to 85% nitrogen and 15% to 25% oxygen.
[0094] The plasma treatment is preferably repeated twice, and the porous support is exposed to plasma for 10 seconds during each treatment.
[0095] Atmospheric pressure plasma surface treatment can be performed by irradiation with an output power of 150W to 200W. When the plasma power is less than 150W, there is a problem that it is difficult to uniformly form a positively charged coating due to insufficient surface modification of the porous support. When it exceeds 200W, there are problems such as deformation of the porous support, reduced pore size, and low permeation pressure due to excessive energy.
[0096] (2) Next, the porous support, which has been surface-modified by plasma treatment, is brought into contact with the above-described positively charged coating composition in order to coat the porous support with the positively charged coating composition. Here, the details of the positively charged coating composition are as described above.
[0097] In step (2), as a method of contacting the positively charged coating composition with the porous support, the porous support can be immersed in a solvent containing the positively charged coating composition, or a spraying method can be used. However, when using the immersion method, the immersion time in the solvent containing the positively charged coating composition can be from 1 second to 120 seconds at room temperature, preferably from 5 seconds to 30 seconds. When the immersion time is less than 1 second, the solvent containing the positively charged coating composition does not have enough time to penetrate into the porous support, which may make it difficult to coat evenly and may lead to deterioration of the physical properties of the positively charged filter material. Furthermore, when the immersion time exceeds 120 seconds, the physical properties do not show a significant difference with the increase of coating time, which is not desirable in terms of process efficiency.
[0098] (3) Next, the porous support coated with the positively charged coating composition is subjected to a thermal crosslinking treatment to form a positively charged coating.
[0099] In step (3), to induce the thermal crosslinking reaction of the positively charged coating composition coated onto the porous support, heat treatment can be performed at a temperature of 60°C to 130°C for 60 to 600 seconds, preferably at a temperature of 80°C to 130°C for 60 to 300 seconds. Here, the relationship between the heat treatment temperature and time is preferably a longer exposure time at lower temperatures and a shorter exposure time at higher temperatures. When the heat treatment temperature is below 60°C or the time is less than 60 seconds, insufficient time for the thermal crosslinking reaction after solvent drying may result in the formation of unreacted substances. At temperatures exceeding 130°C or exceeding 600 seconds, the porous support may melt or stretch under high temperatures and prolonged periods, leading to structural deformation and potentially uneven physical properties.
[0100] Step (3) can be performed under the following conditions 2), 3) or 4).
[0101] 2) 60℃≤T r<90℃, 250s≤t r ≤600s
[0102] 3) 90℃≤T r <110℃, l00s≤t r ≤300s
[0103] 4) 110℃ <T r <130℃, 60s≤t r ≤l50s
[0104] In the above conditional expressions 2) to 4), T r t represents the thermal crosslinking temperature (°C). r This represents the thermal crosslinking time (sec). That is, it is preferable to set a longer thermal crosslinking time at low temperatures and a shorter thermal crosslinking time at high temperatures. Under these conditions, when t... r When the values are below the lower limits of each range, insufficient time for the thermal cross-linking reaction may lead to the formation of unreacted substances. r When the value exceeds the upper limit of each range, the porous support may be melted or stretched, resulting in structural deformation, which may lead to uneven physical properties.
[0105] (4) Next, a cleaning and drying step can be performed on the porous support with the positively charged coating. Step (4) may include a cleaning step and a drying step on the porous support with the positively charged coating.
[0106] The cleaning step is for removing unreacted solids or penetrants contained inside and outside the porous support. Preferably, cleaning can be performed by immersion in water or a 0.1 wt% to 10 wt% aqueous solution of C2 to C5 straight-chain or branched alcohols (preferably an isopropanol aqueous solution) for 1 to 20 minutes at a temperature of 25°C to 60°C. More preferably, cleaning can be performed by immersion in a 0.1 wt% to 10 wt% aqueous solution of isopropanol for 2 to 15 minutes at a temperature of 25°C to 45°C. Here, when the cleaning step is performed at a low temperature below 25°C, a decrease in cleaning effectiveness is expected due to the lack of mass exchange. When the temperature exceeds 60°C, durability issues may arise because the maximum temperature for practical use of the coated nonwoven fabric is exceeded. Furthermore, when the immersion time is less than 1 minute, the target cleaning effect is difficult to achieve due to insufficient immersion time, while when it exceeds 20 minutes, sufficient cleaning effect corresponding to the time cannot be obtained, making it undesirable from an economic perspective. To further improve the cleaning efficiency of the process, air aeration cleaning can be performed.
[0107] In the subsequent drying step, drying can be carried out at a temperature of 60°C to 130°C for 60 to 600 seconds, preferably at a temperature of 80°C to 110°C for 2 to 5 minutes. When the drying temperature is below 60°C or the drying time is less than 60 seconds, drying may not be sufficient. When the drying temperature exceeds 130°C or the drying time exceeds 600 seconds, the nonwoven fabric may melt or stretch, causing structural deformation, which may lead to uneven physical properties.
[0108] The invention will be described in more detail below through the following embodiments.
[0109] The following embodiments are for illustrative purposes only, and the scope of the invention is not limited to the following embodiments.
[0110] Methods of implementing the invention
[0111] <Preparation Example>
[0112] Preparation Example 1
[0113] A solvent for a positively charged coating composition was prepared by mixing 96.4 parts by weight of distilled water (as a solvent), 0.1 parts by weight of dioctyl sulfosuccinate (as a penetrant), 3 parts by weight of linear polyethyleneimine (compound A) with a weight average molecular weight of 70,000 g / mol (as a polyfunctional amine compound), and 0.5 parts by weight of polyethylene glycol diglycidyl ether (PEG DE) (as a crosslinking agent).
[0114] Polypropylene fibers with an average fiber diameter of 2µm were melt-spun to prepare fibers with an average thickness of 0.05mm and a basis weight of 7g / m³. 2 The polypropylene meltblown nonwoven fabric is composed of polypropylene fibers with an average meltblown fineness of 17µm. The average stack thickness of the upper and lower layers of the meltblown nonwoven fabric is 0.3mm, and the basis weight is 31g / m³. 2 Polypropylene spunbond nonwoven fabric was used to prepare a polypropylene composite nonwoven fabric. The total average thickness of the polypropylene composite nonwoven fabric was 0.35 mm, and the average basis weight was 38 g / m³. 2 .
[0115] The polypropylene composite nonwoven fabric was subjected to atmospheric pressure plasma surface treatment at 180W using a MyPL Auto-200 device for surface modification.
[0116] The surface-modified polypropylene composite nonwoven fabric is immersed in the solvent of the positively charged coating composition at 25°C for 5 seconds. After being removed, it is thermally crosslinked and dried at 125°C for two minutes using a hot air dryer, thereby forming a positively charged coating.
[0117] Subsequently, the composite nonwoven fabric with the positively charged coating was immersed in a 1% (w / w) isopropanol aqueous solution at 30°C for 5 minutes and then dried at 90°C for 3 minutes to prepare the positively charged filter material.
[0118] Preparation Examples 2 to 9
[0119] Positively charged filter materials were prepared in the same manner as in Preparation Example 1, except that, as shown in Table 1 below, variables such as the composition of the porous support and the positively charged coating composition differed.
[0120] Preparation Example 10
[0121] The positively charged filter material was prepared in the same manner as in Preparation Example 1, except that the thermal crosslinking time of the thermal crosslinking step was extended to 3 minutes. Other details are shown in Table 1 below.
[0122] Preparation Example 11
[0123] The positively charged filter material was prepared in the same manner as in Preparation Example 1, except that the thermal crosslinking temperature of the thermal crosslinking step was modified to 70°C. Other details are shown in Table 1 below.
[0124] Preparation Example 13
[0125] Positively charged filter materials were prepared in the same manner as in Preparation Example 1, except that the porous support had an average thickness of 0.35 mm and a basis weight of 40 g / m³. 2 The polypropylene meltblown nonwoven fabric is used instead of the three-layer composite nonwoven fabric.
[0126] Comparative Preparation Example 1
[0127] The positively charged filter material was prepared in the same manner as in Preparation Example 1, except that no crosslinking agent was added to the positively charged coating composition.
[0128] Comparative Preparation Example 2
[0129] Positively charged filter material was prepared in the same manner as in Preparation Example 1, except that a positively charged coating composition was coated onto the polypropylene composite nonwoven fabric without atmospheric pressure plasma surface treatment.
[0130] Comparative Preparation Example 3
[0131] Positively charged filter material was prepared in the same manner as in Preparation Example 1, except that the positively charged coating composition was not coated onto the polypropylene composite nonwoven fabric.
[0132] <Experimental Example 1>
[0133] 1) SEM photography
[0134] Figure 3These are SEM images (Maker: SeC, model: SNE-3000M) taken of the composite nonwoven fabric prepared in Example 1. Figure 4 This is a SEM image of the positively charged filter material prepared in Example 1.
[0135] 2) Evaluation of contact angle
[0136] The contact angles of the positively charged filter materials prepared in Preparation Examples 1 to 12 and Comparative Preparation Examples 1 to 3 were measured using a measuring instrument (Maker: KSV, Model: CAM100), and are shown in Table 1 below.
[0137] 3) Evaluation of surface charge
[0138] The surface flow potential difference of the positively charged filter materials prepared in Preparation Examples 1 to 12 and Comparative Preparation Examples 1 to 3 was measured using a measuring instrument (Maker: Anton, Model: SurPass), and the results are shown in Table 1 below.
[0139] 4) Evaluation of weight change
[0140] To evaluate the weight changes of the positively charged filter materials prepared in Preparation Examples 1 to 12 and Comparative Preparation Examples 1 to 3, an electronic balance (Maker: OHAUS, Model: PAG4102) was used to compare the weight increase of the coated positively charged filter material relative to the uncoated positively charged filter material, as shown in Table 1 below.
[0141] 5) Tensile strength evaluation
[0142] The tensile strength of the positively charged filter materials prepared in Preparation Examples 1 to 12 and Comparative Preparation Examples 1 to 3 was measured using the KS K 0520 (grab sampling method), and is shown in Table 1 below.
[0143] Table 1
[0144]
[0145]
[0146]
[0147] As can be seen from Table 1 above, compared with Preparation Example 1, the positively charged filter material of Preparation Example 1, which does not contain a crosslinking agent, has a significantly less positively charged coating, a low weight gain of less than 5%, and therefore a low surface charge.
[0148] Since no plasma surface treatment was performed on the composite nonwoven fabric, the positively charged filter material prepared according to Comparative Preparation Example 2 did not have sufficient surface hydrophilicity, and therefore did not form a good positively charged coating, and both the weight gain and surface charge were low.
[0149] In Comparative Preparation Example 3, since no positively charged coating was formed, it can be seen that the wetting angle of the water droplets is very large and the surface charge is very small.
[0150] In comparative preparation examples 4 and 5, it appears that excessive positively charged coatings were formed due to the addition of too many polyfunctional amine compounds. Therefore, the weight gain is excessively high. Since the internal average pore size of the filter media is excessively reduced, its permeation pressure is expected to decrease and its service life to shorten.
[0151] Preparation Examples 2 and 3 are positively charged filter materials prepared using compositions with excessively different ratios between polyfunctional amine compounds and crosslinking agents.
[0152] Preparation Example 4 used a polyfunctional amine compound with a tertiary amine molar fraction of 30 mol% or more (due to the branching rate of polyethyleneimine being 80% or more). Since the coating was not sufficiently formed in Preparation Example 1, it was found that the weight gain was low and the contact angle was larger.
[0153] In Preparation Example 5, the contact angle was large and the surface charge and weight gain were low due to the low content of the polyfunctional amine compound.
[0154] Preparation Example 6 used a positively charged coating composition without a penetrant. Since the porous support according to the present invention was surface modified by atmospheric pressure plasma, a positively charged filter material with physical properties substantially similar to those in Preparation Example 1 could be obtained without a penetrant. Preparation Example 7 used a positively charged coating composition with a very small content of 0.05 parts by weight. Due to the insufficient content of crosslinking agent, unreacted polyfunctional amine compounds that did not react with the porous support were generated, resulting in a low weight gain and surface charge of the positively charged filter material.
[0155] In Preparation Example 8, the crosslinking agent content was excessive, specifically 3 parts by weight, and the surface charge was very low, approximately 9 mV.
[0156] In Preparation Example 9, when preparing the positively charged filter material, polypropylene meltblown nonwoven fabric was used alone as the porous support instead of spunbond nonwoven fabric, so the tensile strength was significantly lower than that in Preparation Example 1.
[0157] In Preparation Example 10 and Preparation Example 11, there were differences in the temperature and crosslinking time during the thermal crosslinking process, indicating that the positively charged coating in Preparation Example 10 was not fully formed. At this stage, there is no significant difference in the physical properties between Preparation Example 11 and Preparation Example 1.
[0158] <Example>
[0159] Example 1
[0160] To prepare a filter cartridge including the positive charge filter prepared in Preparation Example 1 above, a 3.5m long nonwoven fabric was rolled and inserted into a polypropylene core with an outer diameter of 14mm and cut into a size of 47mm outer diameter and 116mm long, and end capping was performed. By inserting the filter cartridge thus prepared into a housing, a filter cartridge in which the inlet and permeation portions are separated was prepared.
[0161] Comparative Examples 1 to 3
[0162] The filter cartridge was prepared in the same manner as in Example 1 above, except that the positively charged filter material was changed according to Table 2 below.
[0163] Table 2
[0164]
[0165] <Experimental Example 2>
[0166] According to the Korean Ministry of Environment's Drinking Water Quality Process Testing Standard No. 2013-136, the Korea Environmental Waterway Research Institute was commissioned to conduct an analysis, and the results are shown in Table 3 below.
[0167] Table 3
[0168]
[0169] Referring to Table 3, it can be seen that, compared with the positively charged filter material of Example 1, the positively charged filter materials of Comparative Examples 1 to 3, which did not have a sufficiently formed positively charged coating, had very poor removal performance for pathogens. In Comparative Examples 4 and 5, although they had sufficient removal performance due to the formation of an excessive positively charged coating, there was a problem of reduced osmotic pressure due to the small average pore size of the support.
Claims
1. A positively charged filter material, comprising: A porous support comprising at least one fiber selected from polypropylene fiber, polyethylene fiber, polyester fiber, nylon fiber and cellulose fiber, and surface modified by atmospheric pressure plasma surface treatment; as well as A positively charged coating is formed by coating the surface and interior of the porous support with a positively charged coating composition comprising at least one solvent selected from C2 to C5 alcohols, acetone, and water, a polyfunctional amine compound, and a crosslinking agent that undergoes an epoxy reaction with the polyfunctional amine compound. The weight of the positively charged coating is 5% to 15% of the weight of the porous support. The porous support is a composite nonwoven fabric, which has an upper and lower layer of spunbond nonwoven fabric and a middle layer of fabric with a basis weight of 1 g / m³. 2 Up to 10g / m 2 The layered structure composed of meltblown nonwoven fabric The upper and lower spunbond nonwoven fabrics are surface modified by the atmospheric pressure plasma surface treatment. The average fiber diameter of the upper and lower spunbond nonwoven fabrics is 10µm to 30µm, the average fiber diameter of the middle meltblown nonwoven fabric is 1µm to 30µm, and the average fiber diameter of the composite nonwoven fabric is 5µm to 25µm. The positively charged filter material has a surface charge of 15mV to 40mV under pH 7 conditions.
2. The positively charged filter material according to claim 1, characterized in that, Based on 100 parts by weight of the positively charged coating composition, the content of the polyfunctional amine compound is from 1 part by weight to 10 parts by weight.
3. The positively charged filter material according to claim 1, characterized in that, The positively charged coating composition satisfies the following condition (Equation 1): 1)0.4≤C amine / C cl ≤6 In condition 1), C amine C represents the weight content of the polyfunctional amine compound relative to the positively charged coating composition. cl This indicates the weight content of the crosslinking agent.
4. The positively charged filter material according to claim 1, characterized in that, The polyfunctional amine compound is selected from at least one group consisting of diphenylamine, polyethyleneimine, diethylenetriamine, dimethylenepiperazine, and piperazine.
5. The positively charged filter material according to claim 1, characterized in that, The tertiary amine accounts for less than 30 mol% of the polyfunctional amine compound.
6. The positively charged filter material according to claim 1, characterized in that, The crosslinking agent is an aliphatic epoxy compound comprising at least one selected from the group consisting of polyethylene glycol diglycidyl ether, sorbitol polyglycidyl ether, diethylene glycol diglycidyl ether, and propylene glycol diglycidyl ether.
7. A method for preparing a positively charged filter material, comprising: Step (1): The porous support containing at least one fiber selected from polypropylene fiber, polyethylene fiber, polyester fiber, nylon fiber and cellulose fiber is subjected to atmospheric pressure plasma treatment for surface modification. Step (2): Contact the surface-modified porous support with the positively charged coating composition to coat the porous support with the positively charged coating composition, the positively charged coating composition comprising at least one solvent selected from C2 to C5 alcohols, acetone and water, a polyfunctional amine compound and a crosslinking agent that undergoes an epoxy reaction with the polyfunctional amine compound; as well as Step (3): A positively charged coating is formed by thermally crosslinking the porous support coated with the positively charged coating composition. The porous support is a composite nonwoven fabric, which has an upper and lower spunbond nonwoven fabric layer and a middle layer with a basis weight of 1 g / m³. 2 Up to 10g / m 2 The layered structure of meltblown nonwoven fabric, The atmospheric pressure plasma surface treatment modifies the surface of the spunbond nonwoven fabric constituting the composite nonwoven fabric. The upper and lower spunbond nonwoven fabrics have an average fiber diameter of 10µm to 30µm, the middle meltblown nonwoven fabric has an average fiber diameter of 1µm to 30µm, and the composite nonwoven fabric has an average fiber diameter of 5µm to 25µm. The positively charged filter material prepared by performing step (3) has a surface charge of 15 mV to 40 mV at pH 7.
8. The method for preparing the positively charged filter material according to claim 7, characterized in that, Step (3) is performed under the following conditions: 2), 3), or 4): 2)60℃≤T r <90℃,250s≤t r ≤600s 3)90℃≤T r <110℃,100s≤t r ≤300s 4)110℃≤T r <130℃,60s≤t r ≤l50s In the above conditional expressions 2) to 4), T r This indicates the thermal crosslinking temperature, with the unit being degrees Celsius (t). r This indicates the thermal crosslinking time, with the time unit being seconds.
Citation Information
Patent Citations
Microporous filter media, filtration apparatus containing same, and methods of making and using
KR1020040088046A
Filter material for cutting process and method of preparing the same
KR100946979B1
Antibacterial and antiviral positive electric charge-filter and method of manufacturing using the same
KR1020180109289A