Surface connector of a semiconductor chip and method for manufacturing and use thereof

By performing silanization and functionalization on the surface of TiN chips, stable linkers were prepared, solving the problem of instability in nucleic acid linker synthesis on semiconductor chips. Stability was achieved in organic solvents and acid-base environments, supporting in-situ synthesis and hybridization applications of nucleic acids.

CN116250060BActive Publication Date: 2026-11-20NANJING GENSCRIPT BIOTECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202180060371.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-07-27
Filing Date
2021-07-27
Publication Date
2026-11-20
Estimated Expiration
2041-07-27

AI Technical Summary

Technical Problem

The linkers for synthesized nucleic acids using existing semiconductor chips are unstable and difficult to maintain in water, acids, alkalis, and organic solvents, which affects the industrial-scale production of subsequent applications and the development of diagnostic products.

Method used

A silanization reaction is performed on the surface of a TiN chip to form bonded molecules. These molecules are then reacted with functionalized molecules to modify hydroxyl and ester groups, thus preparing a stable linker. The silanized molecules and functionalized molecules react in a suitable solvent to form covalent bonds on the chip surface.

Benefits of technology

Stable linkage of nucleic acids on the surface of semiconductor chips has been achieved, which can remain stable in organic solvents and strong acid and alkali environments. It is suitable for in-situ synthesis and hybridization of nucleic acids and supports the development of chip diagnostic products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116250060B_ABST
    Figure CN116250060B_ABST
Patent Text Reader

Abstract

The present application relates to the field of biochip, and provides a semiconductor chip surface connector and a preparation method and application thereof, wherein the chip surface connector is prepared by taking a silanization molecule as a solute, toluene as a solvent, reacting with a chip surface to form a bonding molecule connected to the chip surface, and reacting with a functionalization molecule to modify hydroxyl and ester groups. The chip surface connector obtained by the present application can be stably combined with the chip surface, is stable under acidic and alkaline conditions, has good conductivity, power stability, and resistance to organic solvents required for nucleic acid synthesis, which is extremely beneficial to subsequent nucleic acid synthesis and other applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of biochip fabrication technology, and in particular to a surface linker for synthesizing nucleic acids on TiN chips, its preparation method, and its application. Background Technology

[0002] Stable linkers for nucleic acid synthesis on semiconductor chips are crucial. They can be used for in-situ synthesis or pre-preparation of large quantities of DNA probes, and also for firmly linking nucleic acids for subsequent applications such as in-situ hybridization. By detecting and analyzing the hybridization signal of the sample, the genetic information (gene sequence and expression information) of the sample can be obtained. This has significant applications in disease diagnosis, drug screening and new drug development, agriculture, and environmental research. Currently, nucleic acid synthesis on the market is mostly done using precious metal chips, with numerous methods, including various linkers and nucleic acid synthesis methods. However, stable linkers for nucleic acid synthesis on semiconductor chips are very rare. Because semiconductors are inexpensive, easy to fabricate, and more suitable for large-scale industrial production, developing semiconductor chip linkers and promoting the application of semiconductor chips is extremely important. Currently, most methods involve simply modifying molecules on semiconductors and then connecting polymers or grafting other materials. For example, Y. Shacham-Diamand studied the use of chemical methods to modify silanized molecules on TiN and then plating Co(W,P) materials [1]. Xuan Tuan Le modified the TiN surface using the diazonium salt method and then used it for electroplating polymers [2]. The problem with this method is that it requires electrical modification, which is not conducive to large-scale mass production. Another method is to use the direct adsorption method to adsorb small molecules onto the TiN surface for application [3]. The disadvantage of this method is that the adhesion is not strong, it is sensitive to water, and it will fall off in subsequent applications, making it difficult to further develop the required chip diagnostic products. Summary of the Invention

[0003] In view of this, the present invention provides a stable linker for synthesizing nucleic acids on semiconductor TiN chips. The main method is to perform a silanization reaction on a clean TiN surface to aminate the surface, and then modify the functionalized molecules containing hydroxyl / hydroxyl protecting groups and ester groups through a carboxyl-amino reaction, so as to realize the subsequent in-situ synthesis of nucleic acids on the chip.

[0004] On one hand, this invention provides a chip surface connector, characterized in that the connector is formed by reacting silanized molecules with the chip surface to form bonded molecules attached to the chip surface, and the bonded molecules are further modified with functionalized molecules to add hydroxyl and ester groups. Specifically, this invention provides a chip surface connector, wherein the connector is formed by reacting silanized molecules with the chip surface in a suitable solvent to form bonded molecules attached to the chip surface, and the bonded molecules are modified with functionalized molecules to add hydroxyl and ester groups. The hydroxyl groups can be free hydroxyl groups or hydroxyl groups protected by protecting groups.

[0005] In some embodiments, the silanized molecule is selected from one or more of 3-aminopropyltriethoxysilane, dodecyltrimethoxysilane, vinyltriethoxysilane, bis(γ-trimethylsilylpropyl)amine and γ-(2,3-epoxypropoxy)propyltrimethoxysilane, preferably 3-aminopropyltriethoxysilane.

[0006] In some embodiments, the silanized molecules react with the chip surface in a suitable solvent. In some embodiments, the solvent is selected from one or more of toluene, ethanol, and methanol, preferably toluene.

[0007] In some embodiments, the volume ratio of the solvent to the silanized molecules is 2:1 to 40:1, preferably 20:1 to 35:1, and more preferably 30:1. The volume ratio of the solvent to the silanized molecules can be selected from 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, 11:1, 12:1, 13:1, 14:1, 15:1, 16:1, 17:1, 18:1, 19:1, 20:1, 21:1, 22:1, 23:1, 24:1, 25:1, 26:1, 27:1, 28:1, 29:1, 30:1, 31:1, 32:1, 33:1, 34:1, 35:1, 36:1, 37:1, 38:1, 39:1, or 40:1.

[0008] In some embodiments, the temperature at which the silanized molecules react with the chip surface is 50°C to 100°C, preferably 60°C to 80°C, and more preferably 65°C. The specific reaction temperature can be selected from 50℃, 51℃, 52℃, 53℃, 54℃, 55℃, 56℃, 57℃, 58℃, 59℃, 60℃, 61℃, 62℃, 63℃, 64℃, 65℃, 66℃, 67℃, 68℃, 69℃, 70℃, 71℃, 72℃, 73℃, 74℃, 75℃, 76℃, 77℃, 78℃, 79℃, 80℃, 81℃, 82℃, 83℃, 84℃, 85℃, 86℃, 87℃, 88℃, 89℃, 90℃, 91℃, 92℃, 93℃, 94℃, 95℃, 96℃, 97℃, 98℃, 99℃, or 100℃. In some embodiments, the reaction time between the silanized molecules and the chip surface is preferably 1–6 hours, more preferably 2–5 hours, and most preferably 4 hours. Other preferred reaction times are 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours, 4.5 hours, 5 hours, 5.5 hours, or 6 hours. In some embodiments, the silanized molecules react with the chip surface at 50°C to 100°C for 1 to 6 hours. In some preferred embodiments, the silanized molecules react with the chip surface at 60°C to 80°C for 2 to 5 hours. In one specific embodiment, the silanized molecules react with the chip surface under sealed conditions at 65°C for 4 hours.

[0009] In some embodiments, the functionalized molecule is a hydroxyl group containing a long carbon chain and an ester group. In other embodiments, the functionalized molecule is selected from one or more of succinic anhydride-modified base monomers, hydroxyethyl methacrylate, succinic acid-modified base monomers, and oxalic acid-modified base monomers, preferably succinic anhydride-modified base monomers. In some embodiments, the base monomer portion of the functionalized molecule is selected from one or more of adenine nucleoside, guanine nucleoside, cytosine nucleoside, thymine nucleoside, and uracil nucleoside. In one specific embodiment, the functionalized molecule is selected from one or more of succinic anhydride-modified adenine nucleoside, guanine nucleoside, cytosine nucleoside, thymine nucleoside, and uracil nucleoside.

[0010] In some implementations, the step of reinforcing the bonding molecules on the chip surface under appropriate conditions is included before modifying the bonding molecules with functionalized molecular reactions.

[0011] In some embodiments, the reinforcement conditions involve placing the item in a drying device at 60°C to 100°C for 1 to 6 hours, preferably at 75°C to 95°C, and most preferably at 90°C. Other preferred reinforcement temperatures are 75°C, 76°C, 77°C, 78°C, 79°C, 80°C, 81°C, 82°C, 83°C, 84°C, 85°C, 86°C, 87°C, 88°C, 89°C, 90°C, 91°C, 92°C, 93°C, 94°C, or 95°C; the reinforcement time is preferably 1 to 4 hours, most preferably 1 hour, and other preferred times are 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours, 3.5 hours, or 4 hours. In some specific embodiments, the reinforcement condition involves placing the item in a drying device at 90°C for 1 hour.

[0012] In some embodiments, the chip is a semiconductor chip. In some specific embodiments, the surface of the semiconductor chip comprises TiN (titanium nitride) or TiW (titanium tungsten), preferably TiN.

[0013] On the other hand, the present invention also provides a method for preparing a chip surface connector, comprising the following steps:

[0014] Step 1: Mix the silanized molecules with a suitable solvent at a certain volume ratio to obtain a mixture;

[0015] Step 2: The chip is brought into contact with the mixture from Step 1 to react and form bonded molecules attached to the chip surface;

[0016] Step 3: The chip surface with the bonded molecules after the reaction is brought into contact with functionalized molecules to modify it with hydroxyl and ester groups.

[0017] In some embodiments, the silanizing molecule described in step 1 above is selected from one or more of 3-aminopropyltriethoxysilane, dodecyltrimethoxysilane, vinyltriethoxysilane, bis(γ-trimethylsilylpropyl)amine and γ-(2,3-epoxypropoxy)propyltrimethoxysilane, preferably 3-aminopropyltriethoxysilane.

[0018] In some embodiments, the solvent in step 1 above is selected from one or more of toluene, ethanol and methanol, preferably toluene.

[0019] In some embodiments, the volume ratio of the solvent to the silanized molecules in step 1 above is 2:1 to 40:1, preferably 20:1 to 35:1, and more preferably 30:1. Other preferred volume ratios of the solvent to the silanized molecules are 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, 11:1, 12:1, 13:1, 14:1, 15:1, 16:1, 17:1, 18:1, 19:1, 20:1, 21:1, 22:1, 23:1, 24:1, 25:1, 26:1, 27:1, 28:1, 29:1, 30:1, 31:1, 32:1, 33:1, 34:1, 35:1, 36:1, 37:1, 38:1, 39:1, or 40:1.

[0020] In some embodiments, the reaction conditions between the silanized molecules and the chip surface in step 2 above are 50°C to 100°C for 1 to 6 hours. In some preferred embodiments, the reaction conditions between the silanized molecules and the chip surface are 60°C to 80°C for 2 to 5 hours. In one specific embodiment, the reaction conditions between the silanized molecules and the chip surface are 65°C with a sealed reaction for 4 hours.

[0021] In some embodiments, the functionalized molecule is a hydroxyl substance containing a long carbon chain and an ester group. In other embodiments, the functionalized molecule is selected from one or more of succinic anhydride-modified base monomers, hydroxyethyl methacrylate, succinic acid-modified base monomers, and oxalic acid-modified base monomers, preferably succinic anhydride-modified base monomers. In some embodiments, the base monomer portion of the functionalized molecule is selected from one or more of adenine nucleoside, guanine nucleoside, cytosine nucleoside, thymine nucleoside, and uracil nucleoside. In one specific embodiment, the functionalized molecule is selected from one or more of succinic anhydride-modified adenine nucleoside, guanine nucleoside, cytosine nucleoside, thymine nucleoside, and uracil nucleoside.

[0022] In some implementations, step 3 is preceded by a step of reinforcing the bonding molecules on the chip surface under suitable conditions.

[0023] In some embodiments, the reinforcement conditions involve placing the item in a drying device at 60℃ to 100℃ for 1 to 6 hours, preferably in a drying device at 75℃ to 95℃ for 1 to 3 hours, and most preferably in a drying device at 90℃ for 1 hour. The placement temperature for the reinforcement conditions can be selected from 75℃, 76℃, 77℃, 78℃, 79℃, 80℃, 81℃, 82℃, 83℃, 84℃, 85℃, 86℃, 87℃, 88℃, 89℃, 90℃, 91℃, 92℃, 93℃, 94℃, or 95℃; the reinforcement placement time is preferably 1 to 4 hours, most preferably 1 hour, and other preferred placement times can be selected from 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours, 3.5 hours, or 4 hours. In some specific embodiments, the reinforcement condition involves placing the item in a drying device at 90℃ for 1 hour.

[0024] In some embodiments, the chip is a semiconductor chip. In some specific embodiments, the surface of the semiconductor chip comprises TiN or TiW, preferably TiN.

[0025] The present invention also provides the application of the chip surface linker described above in nucleic acid synthesis or in the preparation of chip diagnostic kits. Invention Details

[0027] The present invention provides a chip surface connector, particularly a semiconductor chip connector, which is prepared by reacting silanized molecules with the chip surface in a suitable solvent to form a bonded molecule attached to the chip surface, and then reacting with functionalized molecules to modify hydroxyl and ester groups.

[0028] The silanizing molecule described in this invention can be 3-aminopropyltriethoxysilane, dodecyltrimethoxysilane, vinyltriethoxysilane, bis(γ-trimethylsilylpropyl)amine, or γ-(2,3-epoxypropoxy)propyltrimethoxysilane. In some embodiments of this invention, the silanizing molecule is 3-aminopropyltriethoxysilane. The bonding molecule described in this invention is a group covalently attached to the chip surface after the silanizing molecule reacts with the chip surface. In some embodiments of this invention, the silanizing molecule APTES (3-aminopropyltriethoxysilane) is dissolved in a suitable solvent such as toluene (the volume ratio of solvent to silanizing molecule is 2:1 to 40:1, preferably 30:1), and reacted with the TiN-containing semiconductor chip surface at a high temperature of 50°C to 100°C (preferably 65°C) for 1 to 6 hours (preferably 4 hours) to form a bonding molecule on the chip surface.

[0029] In some embodiments of the present invention, before modifying the bonding molecules with functionalized molecules, a step of reinforcing the bonding molecules on the chip surface under suitable conditions is included. In some embodiments of the present invention, the reinforcement conditions involve placing the chip, after reacting with the silanized molecules, in an oven at 60°C to 100°C for 1 to 6 hours, preferably in an oven at 90°C for 1 hour.

[0030] In this invention, the functionalized molecule is a hydroxyl substance containing a long carbon chain and an ester group. It can be a succinic anhydride-modified base monomer, hydroxyethyl methacrylate, a succinic acid-modified base monomer, or an oxalic acid-modified base monomer. In some embodiments of this invention, a solution of one or more of succinic anhydride-modified adenine, guanine, cytosine, or thymine is used. The long carbon chain referred to in this invention means a long-chain structure containing multiple carbon-carbon covalent bonds, and may contain two or more carbon atoms, preferably two to four. The longer the hydroxyl substance containing a long carbon chain and an ester group, the smaller the steric hindrance during subsequent nucleic acid synthesis, which is beneficial for synthesis. In some embodiments of this invention, a solution of succinic anhydride-modified adenine, guanine, cytosine, or thymine is used alone. In some embodiments, the functionalized molecule may also be selected from succinic anhydride-modified adenine, guanine, cytosine, thymine, or uracil nucleosides; hydroxyethyl methacrylate; succinic acid-modified adenine, guanine, cytosine, thymine, or uracil nucleosides; and oxalic acid-modified adenine, guanine, cytosine, thymine, or uracil nucleosides where the carboxylic acid reacts with an amino group to remove the hydroxyl group. In this invention, the functionalized molecule is modified onto the bonding molecule, forming a functionalized molecule group containing hydroxyl and ester groups, which facilitates subsequent electro-catalyzed DNA synthesis and cleavage on the chip.

[0031] In this invention, the hydroxyl group modified by the functionalized molecule reaction can be the hydroxyl group itself, i.e., -OH, or it can be a protected hydroxyl group, such as -ODMT. The hydroxyl protecting group is a hydroxyl group protected by a commonly used protecting group. In some embodiments of this invention, the hydroxyl group modified by the functionalized molecule reaction is a hydroxyl group. In other embodiments, the hydroxyl group modified by the functionalized molecule reaction is ODMT.

[0032] The chip surface connectors described in this invention are stably bonded to the chip surface via covalent bonds and can be used in applications such as electro-assisted chip synthesis of nucleic acids. The semiconductor chip described is a common chip in the art that incorporates semiconductor materials. The semiconductor chip in this invention can be selected from a typical sheet-like semiconductor chip with a surface containing TiN or TiW. In one specific embodiment of this invention, the chip is a semiconductor chip applicable to a CustomArray chip synthesizer. A chip cleaning step is included before the chip surface bonding reaction. In this invention, the chip cleaning step may include sequential rinsing with water, alcohol, and water, followed by drying to obtain a dry and clean chip surface. The water is generally distilled water, and the alcohol is ethanol or methanol, primarily removing contaminants such as other impurities, metal dust, inorganic particles, and small organic molecules.

[0033] This invention also provides a method for preparing a chip surface interconnect, comprising the following steps: mixing silanized molecules with a suitable solvent at a certain volume ratio to obtain a mixture; reacting a cleaned chip with the prepared mixture to form bonded molecules connected to the chip surface; and modifying the reacted chip surface with functionalized molecules to add hydroxyl and ester groups to obtain the interconnect. In some embodiments, the method further includes a step of strengthening the bonded molecules on the chip surface under suitable conditions before modifying the bonded molecules with functionalized molecules.

[0034] In some embodiments of the present invention, a mixture is prepared by mixing toluene as a solvent with silanizing molecules at a volume ratio of 2:1 to 40:1, preferably 30:1. The silanizing molecules may be 3-aminopropyltriethoxysilane, dodecyltrimethoxysilane, vinyltriethoxysilane, bis(γ-trimethylsilylpropyl)amine, or γ-(2,3-epoxypropoxy)propyltrimethoxysilane, preferably 3-aminopropyltriethoxysilane. The cleaned chip is reacted with the mixture at 50°C to 100°C, preferably 65°C, for 1 to 6 hours, preferably 4 hours. The specific reaction is shown below:

[0035]

[0036] After the reaction, the chip is removed and rinsed with water and alcohol in sequence, then rinsed with water and dried.

[0037] The reacted chip is then subjected to conditions that reinforce the bonded molecules attached to its surface. These reinforcement conditions involve placing the chip in a drying apparatus at 60°C–100°C for 1–6 hours, preferably at a temperature of 75°C–95°C, and most preferably at 90°C; the reinforcement time is preferably 1–4 hours, and most preferably 1 hour. In this invention, the chip reinforcement temperature is generally higher than the temperature at which the silanized molecules are attached to the chip surface.

[0038] The reinforced chip is then modified with functionalized molecules. The functionalized molecules are hydroxyl substances containing long carbon chains and ester groups, including but not limited to succinic anhydride-modified base monomers, hydroxyethyl methacrylate, and oxalic acid-modified base monomers. In some embodiments of the invention, solutions of succinic anhydride-modified adenine, guanine, cytosine, thymine, or uracil nucleosides are used individually. In some specific embodiments of the invention, solutions of two or more of succinic anhydride-modified adenine, guanine, cytosine, thymine, and uracil nucleosides are used. The functionalized molecules contain ester groups, which can be used for DNA synthesis and cleavage. These ester groups are cleavage sites, used to cut the DNA synthesized on the chip into a free-solution oligonucleotide pool. The hydroxyl groups in the functionalized molecules are the initiation sites for DNA synthesis. In some embodiments of the invention, the hydroxyl groups provided by the base monomer portion are used for DNA synthesis. In addition, the hydroxyl molecule solution may also contain activators for functionalization modification, such as NHS (N,N-hydroxysuccinimide) and EDC (1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride).

[0039] This invention also provides the application of the chip surface linkers as described above in DNA synthesis or chip preparation kits. The chip surface linkers of this invention have the following applications: DNA synthesis on a chip; chip detection of disease biomarkers; chip kits for developing point-of-care testing (POCT); and high-throughput chip screening kits.

[0040] The chip surface linker of this invention can be used to synthesize DNA. The synthesized DNA, after hybridization with oligonucleotides (such as DNA primers) and subsequent alkali and heat TE treatment, can also be used for hybridization with oligonucleotides (such as DNA primers). The DNA synthesized by the chip surface linker of this invention maintains good stability even after multiple nucleic acid hybridization, elution, and hybridization cycles. The chip surface linker prepared in the embodiments of this invention has good conductivity and electrical stability, and can be used for electro-assisted synthesis of nucleic acid molecules such as DNA. If the linker lacks this property, DNA synthesis will be affected. The chip surface linker of this invention is resistant to organic solvents required for DNA synthesis (including 4,5-dicyanimidazole, trichloroacetic acid, acetic anhydride, 1-methylimidazole, and iodine solution, etc.), and is resistant to acids, alkalis, and ammonolysis; otherwise, DNA synthesis cannot proceed. In the application of the chip linker for chip hybridization detection, this invention solves the problems of existing linkers being sensitive to the synthesis environment of water, acids, alkalis, and organic solvents, and being thermally unstable, thus allowing for reusable chips.

[0041] The term "chip" refers to a microarray formed of an inorganic material such as a semiconductor or a metal such as gold, silver, or platinum, on its surface with specific sites arranged in rows and columns, each site being usable for some type of chemical or biochemical analysis, synthesis, or method. These sites on the microarray are typically less than 100 micrometers. In some embodiments of the invention, the chip is a TiN-containing semiconductor chip.

[0042] The term "bonded molecule" refers to a chemical molecule located at the end of a linker, where one end of the molecule is covalently bonded to a solid surface (such as a TiN-containing semiconductor chip), and the other end has a reactive group. This reactive group is or can be bonded to an associated chemical substance, such as a small molecule, oligomer, or polymer; in this invention, it can be bonded to a functionalized molecule. The bonded molecule is already bound to a solid surface and / or its reactive group is attached to an associated chemical substance. The reactive group of the bonded molecule may be attached to a protecting group, which can be removed by chemical or electrochemical methods.

[0043] The term "functionalized molecule" refers to a chemical molecule located at the terminal portion of a linker, with one end of a group capable of being linked to a bonded molecule and the other end having a reactive group, which is linked to or can be linked to an associated chemical substance, such as a small molecule, oligomer, or polymer. In this invention, it can be linked to a deoxyribonucleotide molecule. The functionalized molecule may already have an associated chemical substance linked to the bonded molecule and / or its reactive group. The reactive group of the functionalized molecule may be linked to a protecting group, which can be removed by chemical or electrochemical methods. In this invention, the functionalized molecule may be adenosine, guanine, cytosine, thymine, or uracil modified with succinic anhydride; hydroxyethyl methacrylate; adenosine, guanine, cytosine, thymine, or uracil modified with succinic acid; or adenosine, guanine, cytosine, thymine, and uracil modified with oxalic acid, etc.

[0044] The term "base monomer" refers to a molecule that can polymerize to form a combination of basic structural units, such as oligomers, co-oligomers, polymers, or copolymers. Examples of monomers include A, C, T, G, adenine nucleoside, guanine nucleoside, cytosine nucleoside, thymine nucleoside, uracil nucleoside, adenosine acid, guanine acid, cytosine acid, uridine acid, amino acids, and other compounds.

[0045] The term "oligomery" refers to a molecule with an intermediate relative molecular mass whose structure essentially comprises a small number of units, either actually or conceptually derived from molecules with lower relative molecular mass. A molecule can be considered to have an intermediate relative molecular mass if removing one or more units significantly alters its properties. A molecule that has an intermediate relative molecular mass, either partially or entirely, and essentially comprises a small number of units, either actually or conceptually derived from molecules with lower relative molecular mass, can be described as oligomeric, or used as an adjective to describe it. Oligomers are typically composed of monomers.

[0046] Beneficial effects

[0047] This invention provides a stable linker for nucleic acid synthesis on the surface of a semiconductor TiN chip, its preparation method, and its applications. The invention uses silanized molecules as a solute and toluene as a solvent, reacting them with the TiN chip surface at high temperature for a certain time, followed by further consolidation at an even higher temperature. Finally, functionalized molecules containing ester and hydroxyl groups are modified onto the silanized molecules to complete the fabrication of this stable linker. This linker exhibits good stability, resisting organic solvents, strong acids, and strong bases. It can be used for in-situ nucleic acid synthesis on the TiN chip surface and can further facilitate in-situ hybridization on the chip surface, providing a possibility and laying the foundation for the development of related chip-based diagnostic products. Attached Figure Description

[0048] Figure 1 Flowchart of TiN chip linker fabrication;

[0049] Figure 2 Colorimetric test diagram for the feasibility of connecting a linker to a TiN chip;

[0050] Figure 3 This is a test result showing the organic solvent resistance of the linker in a TiN chip.

[0051] Figure 4 The image shows the stability test results of the linker of the TiN chip under ammonolysis conditions.

[0052] Figure 5 A graph showing the acid and alkali resistance stability test results of the linker for TiN chips;

[0053] Figure 6 The image shows the linker for the TiN chip used in DNA synthesis and hybridization. Detailed Implementation

[0054] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0055] To further understand this application, the chip surface interconnects, their preparation methods, and applications provided in this application are described in detail below with reference to embodiments. However, it should be understood that these embodiments are implemented based on the technical solution of this invention, providing detailed implementation methods and specific operating procedures, and are only for further illustrating the features and advantages of this invention, not for limiting the scope of the claims of this invention. The protection scope of this invention is not limited to the following embodiments.

[0056] Example 1: Linker preparation experiment

[0057] Specific experimental steps for linker preparation:

[0058] ① The TiN chip (IC foundry) is rinsed 5 times with distilled water, 5 times with ethanol, 5 times with methanol, then rinsed 5 times with distilled water, and dried with nitrogen.

[0059] ② Prepare a mixture of toluene and APTES (30:1, volume ratio), immerse the TiN chip in this mixture, seal it, and react at 65°C for 4 hours. The specific reaction is shown below:

[0060]

[0061] ③ Remove the chip, place it in a 90℃ oven, heat it for 1 hour, then clean it 3 times with ethanol, 3 times with distilled water, and dry it with nitrogen.

[0062] ④ The chip was immersed in a mixed solution of succinic anhydride-modified base monomers (the base monomers were adenine nucleoside, thymine nucleoside, guanine nucleoside or cytosine nucleoside 10.8 mg and NHS 1.53 mg, EDC 7.64 mg dissolved in 100 μL of water) and allowed to stand for 8 hours.

[0063] ⑤ The chip is rinsed five times in sequence with ethanol, acetone, ethanol, and distilled water, and then dried with nitrogen to obtain this stable linker. Figure 1 As shown; the linker includes a bonded molecule and a functionalized molecule, wherein the bonded molecule is a silanized molecule and the functionalized molecule is a molecule containing a hydroxyl group (or a protected hydroxyl group) and an ester group.

[0064] Linkers were fabricated on the TiN chip surface using the above method. The chip was rinsed with copious amounts of ethanol, then rinsed with distilled water and dried under nitrogen. 20 μL of trichloroacetic acid was applied to the linker-modified chip surface, and after 1 second, the trichloroacetic acid was rapidly collected into a centrifuge tube. Figure 2 As shown, compared with the original trichloroacetic acid solution, a significant color change (slightly red) was observed. This is due to the color reaction between the ODMT group (4,4'-dimethoxytriphenylmethyl, which is present on the monomer of the base molecule) at the top of the linker and trichloroacetic acid, indicating that the linker was successfully modified on the surface.

[0065] Example 2: Linker Stability Test

[0066] 2.1 Linker's stability against organic solvents

[0067] To test the stability of the linker against organic solvents, particularly the stability of the silanized molecules reacting with the TiN surface, the silanized molecules were first reacted onto the TiN chip surface according to the method in Example 1 (excluding the functionalization molecule modification step). The chip was then immersed in the organic solvent used for synthesizing the oligonucleotide (including 4,5-dicyanimidazole, trichloroacetic acid, acetic anhydride, 1-methylimidazole, and iodine solution, with a volume ratio of 1:1:1:1:1) and left at room temperature for two days. After rinsing with ethanol and distilled water, the probe DNA-H1 (2 μM, Nanjing Genscript Biotech Co., Ltd.) was linked to the silanized molecule using the reaction of carboxyl and amino groups. Then, the probe DNA-H2 (10 nM, Nanjing Genscript Biotech Co., Ltd.), modified with two fluorescent molecules, Cy5 and Cy3, was simultaneously hybridized with DNA-H1. Figure 3 As shown in a, the chip hybridization design is as follows: Figure 3 As shown in b, the sample is divided into four parts. The top two parts are hybridized, and the bottom two parts serve as controls. After hybridization, the sample is scanned under a microarray scanner (CustomArray, GenePix4000B) at 532nm / 635nm. It can be observed that only the hybridized portion exhibits significant fluorescence. Figure 3 As shown in c, this also indicates that the first step of silanization molecular modification remains stable on the TiN chip surface after being soaked in organic solvent, and can be used for subsequent reactions and applications.

[0068] The sequence of the DNA-H1 probe is as follows:

[0069] 5'-ACACTCTTTCCCTACACGACGCTCTTCCGATCTTTTTT-NH2-3'(SEQ ID NO:1)

[0070] The sequence of the DNA-H2-cy5 probe is as follows:

[0071] 5'-TAGGGAAAGAGTGT-Cy5-3'(SEQ ID NO:2)

[0072] The sequence of the DNA-H2-cy3 probe is as follows:

[0073] 5'-AGATCGGAAGAGCG-Cy3-3'(SEQ ID NO:3)

[0074] 2.2 Linker stability under ammonolysis conditions

[0075] To test the stability of the linker under ammonolysis conditions, particularly the stability of the silanized molecules reacting with the TiN surface, the silanized molecules were first reacted onto the TiN surface according to the method in Example 1 (excluding the functionalization molecule modification step). The chip was then immersed in 28% ammonia water and placed at 65°C for 16 hours. After rinsing with ethanol and distilled water, probe DNA-H1 (2 μM, Nanjing Genscript Biotech Co., Ltd., sequence same as in Example 2.1) was linked to the silanized molecules using the reaction of carboxyl and amino groups. Then, probe DNA-H2 (10 nM, Nanjing Genscript Biotech Co., Ltd., two probe sequences same as DNA-H2 in Example 2.1) modified with two fluorescent molecules, Cy5 and Cy3, was hybridized with DNA-H1. Figure 4 As shown in a, the chip hybridization design is as follows: Figure 4 As shown in b, the sample is divided into four parts. The top two parts are hybridized, and the bottom two parts serve as a control. After hybridization, the sample is scanned under a chip scanner (532nm / 635nm). It can be observed that only the hybridized parts show obvious fluorescence. Figure 4 As shown in c, this also indicates that the first step of silanization molecular modification remains stable on the TiN chip surface after immersion in ammonia water, and can be used for subsequent reactions and applications.

[0076] 2.3 Linker's acid and alkali resistance

[0077] To test the acid and alkali resistance of the linker, especially the stability of the silanized molecules reacting with the TiN surface, the silanized molecules were first reacted onto the TiN surface according to the method in Example 1 (excluding the functionalization molecule modification step). The chip was then immersed in 0.5M sodium hydroxide solution for 0.5 hours, rinsed with distilled water, and then placed in 0.5M hydrochloric acid solution for 0.5 hours. After rinsing with distilled water again, probe DNA-H1 (2 μM, Nanjing Genscript Biotech Co., Ltd., sequence same as SEQ ID NO:1 of Example 2.1) was linked to the silanized molecules using the reaction of carboxyl and amino groups. Then, probe DNA-H2 (10 nM, Nanjing Genscript Biotech Co., Ltd., two probe sequences same as DNA-H2 in Example 2.1, SEQ ID NO:2 and SEQ ID NO:3, respectively), modified with cy5 and cy3 fluorescent molecules, was hybridized with DNA-H1. Figure 5 As shown in a, the chip hybridization design is as follows: Figure 5 As shown in b, the sample is divided into four parts. The top two parts are hybridized, and the bottom two parts serve as a control. After hybridization, the sample is scanned under a chip scanner (532nm / 635nm). It can be observed that only the hybridized parts show obvious fluorescence. Figure 5 As shown in c, this also indicates that the first step of silanization molecular modification remains stable on the TiN chip surface after being soaked in strong alkali and strong acid, and can be used for subsequent reactions and applications.

[0078] Example 3: Linkers are used in DNA synthesis and hybridization

[0079] DNA was synthesized using a TiN chip modified with this linker. The TiN chip was divided into two parts: the upper part was modified with the linker, and the lower part was unmodified and served as a blank control. Figure 6 As shown in a. The chip was placed on a CustomArray chip synthesizer, and the DNA synthesis reagents were injected one by one into the chip surface using a column synthesis method (see reference [4]) to synthesize 38nt DNA (sequence is the same as DNA-H1 in Example 2.1, SEQ ID NO:1). After synthesis, the chip was placed on a chip scanner for scanning, and the results are shown in a. Figure 6 As shown in b, a clear color change is observed in the linker-modified portion, while no color change is observed in the blank portion, indicating successful DNA synthesis. To verify whether the synthesized DNA is the desired DNA, a DNA probe modified with cy3 fluorescent molecules (100 pM, Nanjing Genscript Biotech Co., Ltd., probe sequence same as DNA-H2-cy3 in Example 2.1, SEQ ID NO:3) can be hybridized with it. After hybridization, the chip is scanned on a chip scanner, and the results are as follows. Figure 6As shown in Figure c, the presence of a distinct red light indicates successful hybridization, and the sequence synthesized by the chip is the target sequence. This further demonstrates that this linker can be used for in situ DNA synthesis.

[0080] References:

[0081] 1.Malki, Maayan, et al. "Thin electroless Co(W,P)film growth ontitanium–nitride layer modified by self-assembled monolayer." Surface andCoatings Technology 252(2014):1-7.

[0082] 2.Zeb,Gul,et al."On the chemical grafting of titanium nitride bydiazonium chemistry."RSC Advances 5.62(2015):50298-50305.

[0083] 3.Qiu, Guangyu, Siu Pang Ng, and Chi-Man Lawrence Wu. "Label-free surfaceplasmon resonance biosensing with titanium nitride thin film." Biosensors and Bioelectronics 106 (2018): 129-135.

[0084] 4. H.Synthesis of oligonucleotides on a soluble support[J].Beilstein journal of organic chemistry, 2017,13(1):1368-1387.

Claims

1. A chip surface connector, characterized in that, The linker is formed by reacting silanized molecules with the chip surface to form bonded molecules attached to the chip surface, and the bonded molecules are further modified with functionalized molecules to add hydroxyl and ester groups. The chip is a semiconductor chip, and the surface of the semiconductor chip contains TiN or TiW. The silanized molecule is selected from one or more of 3-aminopropyltriethoxysilane, dodecyltrimethoxysilane, vinyltriethoxysilane, bis(γ-trimethylsilylpropyl)amine, and γ-(2,3-epoxypropoxy)propyltrimethoxysilane. The silanized molecules react with the chip surface in a solvent, wherein the solvent is selected from one or more of toluene, ethanol, and methanol. Wherein, the volume ratio of the solvent to the silanized molecules is 2:1 to 40:1, and The functionalized molecule is selected from one or more of the following: succinic anhydride-modified base monomers, hydroxyethyl methacrylate, succinic acid-modified base monomers, and oxalic acid-modified base monomers.

2. The chip surface connector according to claim 1, characterized in that, The silanized molecule is 3-aminopropyltriethoxysilane.

3. The chip surface connector according to claim 1 or 2, characterized in that, The solvent is toluene.

4. The chip surface connector according to claim 1, characterized in that, The volume ratio of the solvent to the silanized molecules is 30:

1.

5. The chip surface connector according to claim 1 or 2, characterized in that, The reaction temperature between silanized molecules and the chip surface is 50℃~100℃.

6. The chip surface connector according to claim 1 or 2, characterized in that, The reaction temperature between silanized molecules and the chip surface is 65℃.

7. The chip surface connector according to claim 1 or 2, characterized in that, The reaction time between the silanized molecules and the chip surface is 1 to 6 hours.

8. The chip surface connector according to claim 1 or 2, characterized in that, The reaction time between the silanized molecules and the chip surface is 4 hours.

9. The chip surface connector according to claim 1 or 2, characterized in that, The base monomer portion is selected from one or more of adenine nucleoside, guanine nucleoside, cytosine nucleoside, thymidine nucleoside, and uracil nucleoside.

10. The chip surface connector according to claim 9, characterized in that, The functionalized molecule is a base monomer modified with succinic anhydride.

11. The chip surface connector according to claim 1 or 2, characterized in that, Before modifying the bonding molecules with functionalized molecular reactions, the process also includes a step of reinforcing the bonding molecules on the chip surface.

12. The chip surface connector according to claim 11, wherein the step of reinforcing the chip surface bonding molecules includes placing it in a drying device at 60°C to 100°C for 1 to 6 hours.

13. The chip surface connector according to claim 11, wherein the step of reinforcing the chip surface bonding molecules includes placing it in a 90°C drying device for 1 hour.

14. The chip surface connector according to claim 1, wherein the semiconductor chip surface is TiN.

15. A method for preparing a chip surface interconnect, characterized in that, Includes the following steps: Step 1: Mix the silanized molecules with a solvent to obtain a mixture, wherein the silanized molecules are selected from one or more of 3-aminopropyltriethoxysilane, dodecyltrimethoxysilane, vinyltriethoxysilane, bis(γ-trimethylsilylpropyl)amine and γ-(2,3-epoxypropoxy)propyltrimethoxysilane, and the solvent is selected from one or more of toluene, ethanol and methanol, and the volume ratio of the solvent to the silanized molecules is 2:1 to 40:1; Step 2: The chip is brought into contact with the mixture from Step 1 to react and form bonded molecules attached to the chip surface; Step 3: The chip surface with the bonded molecules after the reaction is brought into contact with functionalized molecules to modify it with hydroxyl and ester groups. The chip is a semiconductor chip, and the surface of the semiconductor chip contains TiN or TiW. The functionalized molecule is selected from one or more of the following: succinic anhydride-modified base monomers, hydroxyethyl methacrylate, succinic acid-modified base monomers, and oxalic acid-modified base monomers.

16. The preparation method according to claim 15, characterized in that, The silanized molecule is 3-aminopropyltriethoxysilane.

17. The preparation method according to claim 15, characterized in that, The solvent in step 1 is toluene.

18. The preparation method according to claim 15, wherein the solvent to silanized molecules ratio is 30:

1.

19. According to the preparation method of claim 15, the conditions for the reaction between the chip surface and the mixture in step 2 are 50°C to 100°C for 1 to 8 hours.

20. According to the preparation method of claim 15, the conditions for the reaction between the chip surface and the mixture in step 2 are 65°C for 4 hours.

21. The preparation method according to claim 15, wherein, The base monomer portion is selected from one or more of adenine nucleoside, guanine nucleoside, cytosine nucleoside, thymidine nucleoside, and uracil nucleoside.

22. The preparation method according to claim 21, characterized in that, The functionalized molecule is a base monomer modified with succinic anhydride.

23. The preparation method according to claim 15, characterized in that, The step of reinforcing the bonding molecules on the chip surface is included before step 3.

24. The preparation method according to claim 23, wherein the step of reinforcing the chip surface by connecting the bonding molecules includes placing it in a drying device at 60°C to 100°C for 1 hour to 6 hours.

25. The preparation method according to claim 23, wherein the step of reinforcing the chip surface by connecting the bonding molecules includes placing it in a drying device at 90°C for 1 hour.

26. The preparation method according to claim 15, wherein the surface of the semiconductor chip is TiN.

27. The use of the chip surface connector according to any one of claims 1 to 14 in a nucleic acid synthesis or chip preparation kit.

Citation Information

Patent Citations

  • Microarray chip without solid wall based on LSPR (Localized Surface Plasmon Resonance) and application thereof

    CN103335984A

  • Substrate for Biochip, Biochip, Method for Manufacturing Substrate for Biochip and Method for Manufacturing Biochip

    US20100233429A1