A method for preparing an anti-bleeding ionically conductive gelatin hydrogel

By mixing gelatin with sodium pyrrolidone carboxylate (PCA-Na), an ion-conductive gelatin hydrogel resistant to water loss was prepared, which solved the problems of easy water loss and poor conductivity of gelatin hydrogel and improved its mechanical and electrical properties.

CN116284863BActive Publication Date: 2026-11-24ZHEJIANG UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310306253.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2026-11-24
Estimated Expiration
2043-03-27

AI Technical Summary

Technical Problem

Existing gelatin hydrogels are prone to water loss when exposed to air for extended periods, leading to mechanical hardening and blocking ion transfer, thus failing to meet the requirements for long-term stable use.

Method used

A gelatin hydrogel with anti-dehydration and ionic conductivity was prepared by mixing gelatin with sodium pyrrolidone carboxylate (PCA-Na) to improve the hydrogel's resistance to dehydration and ionic conductivity through the formation of hydrogen bonds and ionic crosslinking.

Benefits of technology

This study improved the water loss resistance and ionic conductivity of gelatin hydrogels, enhancing their mechanical and electrical properties. The preparation method is simple and inexpensive.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116284863B_ABST
    Figure CN116284863B_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing a gelatin hydrogel with resistance to dehydration and ion conductivity. Gelatin is soaked and swollen in deionized water, then magnetically stirred in a water bath to obtain a gelatin solution. Sodium pyrrolidone carboxylate is added to the gelatin solution to obtain a gelatin-sodium pyrrolidone carboxylate mixed solution. The gelatin-sodium pyrrolidone carboxylate mixed solution is cooled at a certain temperature to obtain a gelatin-sodium pyrrolidone carboxylate hydrogel. The hydrogel of this invention uses gelatin as a framework and water as a solvent. Sodium pyrrolidone carboxylate is incorporated into the system to improve the hydrogel's resistance to dehydration and provide ion conductivity, thus improving the hydrogel's mechanical properties. The method is simple to operate, and the product simultaneously possesses elasticity, extensibility, conductivity, and resistance to dehydration, overcoming the characteristics of traditional hydrogels such as poor conductivity and easy dehydration.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for preparing hydrogels belonging to the field of polymer preparation, specifically to a method for preparing an ion-conductive gelatin hydrogel resistant to dehydration. Background Technology

[0002] Hydrogels are high-molecular-weight polymers with a three-dimensional network structure and a large number of water molecules. In recent years, their excellent flexibility, elasticity, and biocompatibility have led to their widespread application in various fields. Gelatin is a natural polymer extracted from animal connective tissues (such as skin, bone, and cartilage). It is mainly composed of collagen, a complex macromolecular polypeptide, whose main component is a trimer composed of three helical collagen chains. Gelatin's gelling property is one of its important characteristics; when a hot aqueous solution of gelatin cools, the gelatin molecular chains undergo a conformational change, causing gelatin to gelatinize and form a gelatin hydrogel.

[0003] The gelling property of gelatin solutions, which undergoes a phase transition with temperature, makes them widely applicable. In many applications, gelatin hydrogels are required to have ionic conductivity, and a common method is to add inorganic salts such as potassium chloride or sodium chloride to the gelatin solution to enhance its ionic conductivity.

[0004] However, when gelatin hydrogel is exposed to air for a long time, it will inevitably lose water, which will cause it to harden mechanically and block the transfer of ions within it. This will cause the gelatin hydrogel to lose its original mechanical properties and ionic conductivity, and it will not be able to meet the requirements for long-term stable use.

[0005] Therefore, preparing biocompatible gelatin hydrogels that simultaneously possess resistance to water loss and ionic conductivity is a major challenge. Summary of the Invention

[0006] To address the aforementioned problems, this invention provides a simple and easily implemented method for preparing gelatin / sodium pyrrolidone carboxylate conductive hydrogel. The method is simple to operate, and the prepared hydrogel simultaneously possesses elasticity, extensibility, conductivity, and resistance to water loss, overcoming the characteristics of traditional hydrogels such as poor conductivity and easy water loss.

[0007] The technical solution of the present invention is as follows:

[0008] Step 1: Place a certain amount of gelatin in a container, add deionized water, and immerse the gelatin in deionized water to allow it to swell for a period of time. Then, place the swollen gelatin in a water bath at a certain temperature and stir it magnetically for a period of time to obtain a gelatin solution.

[0009] Step 2: Add sodium pyrrolidone carboxylate to the gelatin solution to obtain a gelatin-sodium pyrrolidone carboxylate mixed solution;

[0010] Step 3: Pour the gelatin-pyrrolidone sodium carboxylate mixed solution into a mold and cool it at a certain temperature for a period of time to obtain gelatin-pyrrolidone sodium carboxylate hydrogel.

[0011] In step one, the concentration of gelatin after adding deionized water is 15-20 wt%, the soaking time of gelatin is 30-60 min, the water bath temperature is 50-55℃, and the stirring time is 60-120 min.

[0012] In step two, a sodium pyrrolidone carboxylate solution is added to the gelatin solution, and then the mixture is placed in a water bath at a certain temperature and magnetically stirred for a period of time to obtain a gelatin-sodium pyrrolidone carboxylate mixed solution.

[0013] In step two, the concentration of sodium pyrrolidone carboxylate in the gelatin-pyrrolidone carboxylate mixed solution is 0-40 wt%, the water bath temperature is 50-55℃, and the stirring time is 60-120 min.

[0014] In step three, the cooling temperature is 10-20℃ and the cooling time is 60-120 minutes.

[0015] The hydrogel of this invention uses gelatin as a skeleton and water as a solvent. Sodium pyrrolidone carboxylate is incorporated into the system as a substance to improve the hydrogel's resistance to water loss and provide ionic conductivity, which also improves the mechanical properties of the hydrogel.

[0016] Sodium pyrrolidone carboxylate (PCA-Na) is a naturally occurring substance in the stratum corneum of the skin. It is an amino acid derivative and a natural moisturizing factor. Its molecular structure contains a pyrrolidone ring and a carboxylic acid functional group.

[0017] PCA-Na exhibits extremely high hygroscopicity, capable of absorbing hundreds of times its own weight in water, thus providing excellent moisturizing properties. This gel, by incorporating PCA-Na as a biocompatible liquid, forms numerous hydrogen bonds with water molecules in the gelatin hydrogel, thereby slowing down water evaporation and contributing to its moisturizing effect. Furthermore, the carboxylic acid functional groups in PCA-Na can form ionic crosslinks with the amino groups on the gelatin molecular chains; the electrostatic interaction between these two groups significantly enhances the mechanical strength of the gelatin hydrogel. In addition, the sodium ions in the PCA-Na molecules can move freely within the hydrogel network, endowing the hydrogel with excellent ionic conductivity.

[0018] Therefore, the preparation method proposed in this invention improves the shortcomings of gelatin hydrogels, such as easy water loss, poor mechanical properties, and poor ionic conductivity, and can prepare gelatin hydrogels that are resistant to water loss and have good ionic conductivity.

[0019] The beneficial effects of this invention are as follows:

[0020] (1) The introduction of PCA-Na can form strong hydrogen bonds with water molecules to achieve a moisturizing effect, and at the same time improve the mechanical strength and ionic conductivity of gelatin hydrogel.

[0021] (2) The preparation method of the present invention is simple, inexpensive, practical and easy to promote. Attached Figure Description

[0022] Figure 1 Stress-strain diagrams for hydrogels with different PCA-Na contents are shown, where 0%-40wt% represents the PCA-Na content in the system.

[0023] Figure 2 The graph shows the composite viscosity of hydrogels with different PCA-Na contents as a function of temperature, where 0%-40% represents the PCA-Na content in the system.

[0024] Figure 3 The conductivity diagram shows the conductivity of hydrogels with different PCA-Na contents.

[0025] Figure 4 The graph shows the water retention properties of hydrogels with different PCA-Na contents, where 0%-40% represents the PCA-Na content in the system. Detailed Implementation

[0026] The present invention will be further described below with reference to the accompanying drawings and specific embodiments.

[0027] The embodiments of the present invention are as follows:

[0028] Example 1:

[0029] 0.4 g of gelatin was added to 1.88 mL of deionized water and soaked for 1 h, then stirred at 50 °C for 2 h to form a homogeneous gelatin solution; 0.12 g of sodium pyrrolidone carboxylate (PCA-Na) was added to the homogeneous gelatin solution, then stirred at 50 °C for 2 h to form a gelatin-sodium pyrrolidone carboxylate mixed solution; the gelatin-sodium pyrrolidone carboxylate mixed solution was poured into a mold and cooled at 20 °C for 1 h to obtain the anti-dehydration ion-conductive gelatin hydrogel.

[0030] Example 2:

[0031] 0.4 g of gelatin was added to 1.76 mL of deionized water and soaked for 1 h, then stirred at 50 °C for 2 h to form a homogeneous gelatin solution; 0.24 g of sodium pyrrolidone carboxylate (PCA-Na) was added to the homogeneous gelatin solution, then stirred at 50 °C for 2 h to form a gelatin-sodium pyrrolidone carboxylate mixed solution; the gelatin-sodium pyrrolidone carboxylate mixed solution was poured into a mold and cooled at 20 °C for 1 h to obtain an anti-dehydration ion-conductive gelatin hydrogel.

[0032] Example 3:

[0033] 0.4 g of gelatin was added to 1.52 mL of deionized water and soaked for 1 h, then stirred at 50 °C for 2 h to form a homogeneous gelatin solution; 0.48 g of sodium pyrrolidone carboxylate (PCA-Na) was added to the homogeneous gelatin solution, then stirred at 50 °C for 2 h to form a gelatin-sodium pyrrolidone carboxylate mixed solution; the gelatin-sodium pyrrolidone carboxylate mixed solution was poured into a mold and cooled at 20 °C for 1 h to obtain an anti-dehydration ion-conductive gelatin hydrogel.

[0034] Example 4:

[0035] 0.4 g of gelatin was added to 1.28 mL of deionized water and soaked for 1 h, then stirred at 50 °C for 2 h to form a homogeneous gelatin solution; 0.72 g of sodium pyrrolidone carboxylate (PCA-Na) was added to the homogeneous gelatin solution, then stirred at 50 °C for 2 h to form a gelatin-sodium pyrrolidone carboxylate mixed solution; the gelatin-sodium pyrrolidone carboxylate mixed solution was poured into a mold and cooled at 20 °C for 1 h to obtain an anti-dehydration ion-conductive gelatin hydrogel.

[0036] Example 5:

[0037] 0.4 g of gelatin was added to 1.04 mL of deionized water and soaked for 1 h, then stirred at 50 °C for 2 h to form a homogeneous gelatin solution; 0.96 g of sodium pyrrolidone carboxylate (PCA-Na) was added to the homogeneous gelatin solution, then stirred at 50 °C for 2 h to form a gelatin-sodium pyrrolidone carboxylate mixed solution; the gelatin-sodium pyrrolidone carboxylate mixed solution was poured into a mold and cooled at 20 °C for 1 h to obtain an anti-dehydration ion-conductive gelatin hydrogel.

[0038] Comparative Example 1:

[0039] Add 0.4g of gelatin to 2mL of deionized water and soak for 1h. Then stir at 50℃ for 2h to form a homogeneous gelatin solution. Pour the gelatin solution into a mold and cool at 20℃ for 1h to obtain gelatin hydrogel.

[0040] The above-mentioned Examples 1-5 and Comparative Document 1 have obtained results in various aspects such as stress-strain, composite viscosity, conductivity, and water retention through multiple tests. Figures 1-4 As shown.

[0041] In each figure, 0% PCA-Na refers to the PCA-Na mass content of Comparative Example 1, Examples 1-5, which increases sequentially to 5%, 10%, 20%, 30%, and 40%, respectively.

[0042] The stress-strain results obtained from the tests of Examples 1-5 and Comparative Document 1 are as follows: Figure 1 As shown in the figure, the Young's modulus of the hydrogel increases with the increase of PCA-Na content.

[0043] The results of testing the composite viscosity as a function of temperature in Examples 1-5 and Comparative Document 1 are as follows: Figure 2 As shown in the figure, the viscosity of the hydrogel increases with the increase of PCA-Na content.

[0044] The conductivity results obtained from the tests of Examples 1-5 and Comparative Document 1 are as follows: Figure 3 As shown in the figure, the conductivity of the hydrogel increases with the increase of PCA-Na content.

[0045] The water retention results obtained by testing Examples 1-5 and Comparative Document 1 are as follows: Figure 4 As shown in the figure, the water retention of the hydrogel increases with the increase of PCA-Na content.

[0046] As can be seen from this implementation, the present invention can improve the water loss resistance of the gel by adding sodium pyrrolidone carboxylate, and the addition of a substance with ionic conductivity into the system can improve the mechanical properties of the hydrogel.

[0047] It should be noted that the above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of them. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for preparing an ion-conductive gelatin hydrogel resistant to dehydration, characterized in that: The method, steps, and conditions are as follows: Step 1: Add a certain amount of gelatin to deionized water, that is, soak the gelatin in deionized water to make it swell for a period of time, and then place the swollen gelatin in a water bath at a certain temperature and stir it magnetically for a period of time to obtain a gelatin solution. Step 2: Add sodium pyrrolidone carboxylate to the gelatin solution to obtain a gelatin-sodium pyrrolidone carboxylate mixed solution; In step two, the concentration of sodium pyrrolidone carboxylate in the gelatin-pyrrolidone carboxylate mixed solution is greater than 0 wt% and less than or equal to 40 wt%, the water bath temperature is 50-55℃, and the stirring time is 60-120 min. In step two, a sodium pyrrolidone carboxylate solution is added to the gelatin solution, and then the solution is placed in a water bath at a certain temperature and magnetically stirred for a period of time to obtain a gelatin-sodium pyrrolidone carboxylate mixed solution. Step 3: Pour the gelatin-pyrrolidone sodium carboxylate mixed solution into a mold and cool it at a certain temperature for a period of time to obtain gelatin-pyrrolidone sodium carboxylate hydrogel; In step three, the cooling temperature is 10-20℃ and the cooling time is 60-120 min.

2. The method for preparing an anti-dehydration ion-conductive gelatin hydrogel according to claim 1, characterized in that: In step one, the concentration of gelatin after adding deionized water is 15-20 wt%, the soaking time of gelatin is 30-60 min, the water bath temperature is 50-55℃, and the stirring time is 60-120 min.

Citation Information

Patent Citations

  • Anti-freeze high-strength supramolecular organic hydrogel and preparation method thereof

    CN109796621A

  • Ionic cross-linked polysaccharide-based gel and application thereof

    CN115073823A