Electrolyte and lithium ion battery
By using additives with specific structural compounds in lithium-ion batteries, the problems of volume expansion of silicon-carbon anodes and dissolution of cathode materials have been solved, forming a stable SEI film and siloxane, which improves the cycle and high-temperature performance of the battery.
Patent Information
- Application Number
- CN202310015835.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-04
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-01-04
AI Technical Summary
The volume expansion of silicon-carbon anodes leads to particle breakage and electrolyte consumption during lithium-ion battery cycling. The dissolution of transition metals in cathode materials causes side reactions, affecting the battery's cycle performance and high-temperature stability.
First and second additives containing compounds with specific structures are used. The first additive complexes transition metal ions on the positive electrode surface to form a uniform and dense SEI film. The second additive converts silanol groups into stable siloxanes, suppresses side reactions, and improves interface stability.
It effectively suppresses gas generation and interface corrosion in lithium-ion batteries, improves the cycle stability and high-temperature stability of batteries, and enhances electrochemical performance.
Smart Images

Figure QLYQS_1 
Figure QLYQS_2 
Figure QLYQS_3
Abstract
Description
Technical Field
[0001] This invention relates to the field of lithium-ion battery technology, and more specifically to electrolytes and lithium-ion batteries. Background Technology
[0002] Range anxiety has long hampered the driving convenience and user acceptance of electric vehicles, hindering their development. High-energy-density batteries can directly improve the driving range of electric vehicles, representing a key breakthrough in overcoming range anxiety. Lithium-ion batteries with silicon anodes are currently a popular research topic for high-energy-density batteries, but they suffer from the following problems:
[0003] The most prominent problem with silicon-carbon anodes is silicon-induced volume expansion, which exhibits a high volume expansion rate under full charge conditions. This volume expansion leads to particle breakage and powder shedding during cycling. Furthermore, the continuously exposed fresh electrode surface causes the electrolyte to undergo continuous reduction and decomposition, forming an SEI (solid electrolyte interface), resulting in the continuous consumption of electrolyte and lithium ions and accelerating battery failure. This problem will undoubtedly worsen with increasing silicon content in silicon-carbon anodes.
[0004] During the charging, discharging and storage processes, the cathode material may undergo transition metal dissolution and side reactions with the electrolyte interface, resulting in microcracks and a rapid decline in battery cycle performance and high-temperature stability.
[0005] How to effectively solve the aforementioned problems of lithium-ion batteries without sacrificing energy density has become an urgent technical challenge. Summary of the Invention
[0006] Based on the deficiencies of existing technologies, the purpose of this invention is to provide an electrolyte and a lithium-ion battery containing the electrolyte, which improves the stability of positive and negative electrode materials, suppresses interfacial side reactions, and effectively improves the gas generation problem of lithium-ion batteries as well as their electrochemical performance such as cycle stability and high-temperature stability.
[0007] In a first aspect, the present invention provides an electrolyte comprising a first additive and a second additive, wherein the first additive comprises at least one compound with a structure represented by Formula I or Formula II; and the second additive comprises at least one compound with a structure represented by Formula III.
[0008]
[0009] Wherein, R1 to R6 each independently contains a cyano group of C1 to C10; R7 to R9 each independently contains at least one of an alkyl group of C1 to C10 and an alkoxy group of C1 to C10; R 10 Includes C1 to C10 alkyl groups;
[0010] The mass ratio of the first additive to the second additive is (1-20):(1-10).
[0011] Furthermore, the first additive comprises at least one of the following compounds:
[0012]
[0013] The second additive comprises at least one of the compounds with the following structural formulas:
[0014]
[0015] Further, the first additive accounts for 0.1% to 6% of the total mass of the electrolyte; the second additive accounts for 0.1% to 3% of the total mass of the electrolyte.
[0016] Further, the electrolyte comprises lithium hexafluorophosphate and a second lithium salt, the second lithium salt comprising at least one of lithium tetrafluoroborate, lithium dioxaborate, lithium difluorooxaborate, lithium difluorodioxaborate, lithium bis(fluorosulfonyl)imide, lithium bistrifluoromethanesulfonylimide, lithium perchlorate, lithium difluorophosphate, lithium pentafluoroethyltrifluoroborate, and lithium 4,5-dicyano-2-trifluoromethyl-imidazolium.
[0017] Furthermore, the lithium hexafluorophosphate accounts for 12% to 15% of the total mass of the electrolyte, and the second lithium salt accounts for 0% to 15.0% of the total mass of the electrolyte.
[0018] Furthermore, the electrolyte further includes a solvent, which includes fluoroethylene carbonate and a second solvent, the second solvent including at least one of ethylene carbonate, propylene carbonate, butene carbonate, dimethyl carbonate, methyl ethyl carbonate, diethyl carbonate, methyl propyl carbonate, diphenyl carbonate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, γ-butyrolactone, acetonitrile, and sulfolane.
[0019] Furthermore, the mass ratio of the fluoroethylene carbonate and the second solvent includes (1-5):(5-15).
[0020] In a second aspect, the present invention provides a lithium-ion battery, comprising a positive electrode material, a negative electrode material, and the electrolyte.
[0021] Optionally, the cathode material is selected from at least one of nickel-cobalt-manganese ternary materials, nickel-aluminum-manganese ternary materials, lithium cobalt oxide materials, lithium iron phosphate materials, lithium manganese oxide materials, lithium manganese iron phosphate materials, and nickel-manganese spinel materials.
[0022] Optionally, the negative electrode material includes a silicon-carbon material, wherein the silicon-based material in the silicon-carbon material includes at least one of elemental silicon, silicon-carbon, silicon-oxygen, and silicon metal compounds; and the carbon-based material in the silicon-carbon material includes graphite.
[0023] Compared with the prior art, the beneficial effects of this application are as follows:
[0024] (1) This application utilizes the cyano group in the first additive to complex with the transition metal ions on the positive electrode surface, thereby inhibiting the dissolution of the positive electrode material and the side reactions at the positive electrode interface, reducing gas generation and interface corrosion. Moreover, the cyano group in the first additive can preferentially be reduced by the electrolyte solvent to form a uniform and dense SEI film on the negative electrode. At the same time, the branched structure in the first additive can promote the formation of the organic cross-linked polymer network in the SEI film, further improving the mechanical properties of the SEI film and effectively protecting the negative electrode / electrolyte interface.
[0025] (2) This application utilizes a second additive to convert the silanol groups (-SiOH) on the surface of the silicon-carbon anode into stable siloxanes and / or silicates, thereby inhibiting the interaction between the silanol groups and PF6. - The presence of anions can cause side reactions, increasing interfacial stability.
[0026] (3) This application utilizes the synergistic effect between the first additive and the second additive to improve the stability of the positive and negative electrode materials, suppress interfacial side reactions, reduce gas production, and effectively improve the electrochemical performance of lithium-ion batteries, such as gas production performance, cycle stability, and high temperature stability. Detailed Implementation
[0027] To better illustrate the purpose, technical solution, and advantages of this invention, the invention will be further described below with reference to specific embodiments and comparative examples. The purpose of this description is to provide a detailed understanding of the invention, not to limit its scope. All other embodiments obtained by those skilled in the art without inventive effort are within the protection scope of this invention. Unless otherwise specified, the experimental reagents and instruments involved in the implementation of this invention are commonly used reagents and instruments.
[0028] According to a first aspect of this application, an electrolyte is provided, comprising a first additive and a second additive.
[0029] The first additive includes at least one of the compounds with the structure shown in Formula I or Formula II; the second additive includes at least one of the compounds with the structure shown in Formula III;
[0030]
[0031] Wherein, R1 to R6 each independently contains a cyano group of C1 to C10; R7 to R9 each independently contains at least one of an alkyl group of C1 to C10 and an alkoxy group of C1 to C10; R10 Includes C1 to C10 alkyl groups;
[0032] The mass ratio of the first additive to the second additive is (1-20):(1-10).
[0033] In this application, the first additive, containing cyano unsaturated bonds, preferentially undergoes reduction in the electrolyte solvent to generate a uniform and dense passivation protective film—the SEI film—effectively protecting the interface. Simultaneously, its branched structure facilitates the formation of a cross-linked polymer network within the SEI film, further enhancing its mechanical properties and providing greater adaptability to the significant volume expansion of the silicon-carbon anode, thereby improving the structural stability of the silicon-carbon anode. It can also form a CEI film on the positive electrode surface, improving interfacial stability. The cyano groups in the first additive can also coordinate with transition metal ions on the positive electrode surface, stabilizing the positive electrode surface and inhibiting the dissolution of positive electrode materials and their deposition on the negative electrode surface, thus preventing damage to the negative electrode interface. This coordination effect also inhibits the catalytic effect of transition metal ions on gas-generating side reactions, effectively suppressing battery gas generation. The cyano, phosphite, and phosphate groups in the first additive improve the thermal stability of the electrolyte, and the phosphite and phosphate groups can also exert a flame-retardant effect by capturing free radicals, contributing to improved battery safety.
[0034] In this application, the second additive can react with the silanol groups on the surface of the silicon-carbon anode, converting the silanol groups into stable siloxanes and / or silicates, thereby inhibiting the reaction between the silanol groups and PF6. - The presence of anions in side reactions, coupled with their strong affinity for silicon-carbon anodes, is beneficial for enhancing interfacial stability.
[0035] In this application, the first additive and the second additive synergistically improve the stability of the material, suppress interfacial side reactions, reduce gas production, and effectively improve the electrochemical performance and safety performance of lithium-ion batteries, such as internal resistance, cycle stability, and high-temperature stability.
[0036] In some specific embodiments of this application, the first additive comprises at least one of the following compounds:
[0037]
[0038] In some specific embodiments of this application, the second additive comprises at least one of the compounds with the following structural formulas:
[0039]
[0040] In some specific embodiments of this application, the mass of the first additive accounts for 0.1% to 6% of the total mass of the electrolyte. Preferably, the mass of the first additive accounts for 0.5% to 3% of the total mass of the electrolyte, and more preferably, the mass of the first additive accounts for 1% to 2% of the total mass of the electrolyte.
[0041] As the content of the first additive in the electrolyte increases, its effect on improving the gas generation problem, internal resistance, cycle stability, and high-temperature stability of lithium-ion batteries initially increases and then decreases. To effectively improve these electrochemical performance characteristics, the content of the first additive in the electrolyte is selected to be in the range of 0.1% to 6%. Preferably, the content is in the range of 0.5% to 3% to better improve the gas generation problem and related electrochemical performance. Further, the content is optimized to be in the range of 1% to 2% to further improve these performance characteristics at a lower cost.
[0042] In some specific embodiments of this application, the mass of the second additive accounts for 0.1% to 3% of the total mass of the electrolyte. Preferably, the mass of the second additive accounts for 0.5% to 1.5% of the total mass of the electrolyte.
[0043] As the content of the second additive in the electrolyte increases, its effect on improving the gas generation problem, internal resistance, cycle stability, and high-temperature stability of lithium-ion batteries initially increases and then decreases. To effectively improve the gas generation problem and electrochemical performance of lithium-ion batteries, the content of the second additive in the electrolyte is selected to be in the range of 0.1% to 3%. Further optimization is achieved by selecting a content of the second additive in the electrolyte in the range of 0.5% to 1.5%, in order to further improve the gas generation problem, internal resistance, cycle stability, and high-temperature stability of lithium-ion batteries at a lower cost.
[0044] In some specific embodiments of this application, the electrolyte includes lithium hexafluorophosphate (LiPF6). Lithium hexafluorophosphate is the most commonly used lithium salt in lithium-ion batteries due to its moderate ion transport number and dissociation constant, good oxidation resistance, and excellent aluminum foil passivation capability, as well as its compatibility with various positive and negative electrode materials. In some embodiments of this application, the mass of lithium hexafluorophosphate accounts for 12% to 15% of the total mass of the electrolyte, such as 12%, 13%, 14%, 15%, or a combination of both.
[0045] In some specific embodiments of this application, the electrolyte further comprises a second lithium salt, that is, the electrolyte also contains a lithium salt other than lithium hexafluorophosphate. The second lithium salt includes at least one of lithium tetrafluoroborate (LiBF4), lithium dioxolane borate (LiBOB), lithium difluorooxolane borate (LiDFOB), lithium difluorodioxolane phosphate (LiDFOP), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium perchlorate (LiClO4), lithium difluorophosphate (LiDFPO2), lithium pentafluoroethyl trifluoroborate (LiFAB), and lithium 4,5-dicyano-2-trifluoromethyl-imidazolium (LiTDI), but is not limited thereto. In some embodiments of this application, the mass of the second lithium salt accounts for 0 to 15.0% of the total mass of the electrolyte.
[0046] In some specific embodiments of this application, the electrolyte further includes a solvent, including fluoroethylene carbonate (FEC). Fluoroethylene carbonate can be reduced to form a film at the electrode / electrolyte interface and increase the LiF content in the SEI and CEI, significantly improving the stability of the silicon anode and enhancing cycle performance.
[0047] In some specific embodiments of this application, the solvent further comprises a second solvent, that is, a solvent other than fluoroethylene carbonate. The second solvent may be selected from at least one of the following: ethylene carbonate (EC), propylene carbonate (PC), butenyl carbonate (BC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), methyl propyl carbonate (MPC), diphenyl carbonate (DPC), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), γ-butyrolactone (γ-GBL), acetonitrile (AN), and sulfolane (TMS), but is not limited thereto. In some embodiments of this application, the mass ratio of fluoroethylene carbonate to the second solvent is (1–5):(5–15).
[0048] According to a second aspect of this application, a lithium-ion battery is provided, comprising a positive electrode material, a negative electrode material, and the electrolyte described above.
[0049] In some embodiments of this application, the cathode material includes at least one of nickel-cobalt-manganese ternary materials, nickel-aluminum-manganese ternary materials, lithium cobalt oxide materials, lithium iron phosphate materials, lithium manganese oxide materials, lithium manganese iron phosphate materials, and nickel-manganese spinel materials.
[0050] In some embodiments of this application, the negative electrode material includes a silicon-carbon material, wherein the silicon-based material in the silicon-carbon material includes at least one of elemental silicon, silicon-carbon, silicon-oxygen, and silicon metal compounds; and the carbon-based material in the silicon-carbon material includes graphite.
[0051] The lithium-ion battery described in this application can be used in any electrical device, such as electric vehicles.
[0052] The present application will be further illustrated below through specific embodiments.
[0053] The sources of raw materials used in each embodiment and comparative example are as follows:
[0054] The synthesis of compound A1 was performed as follows: 24 mL of cyanoethoxytrimethylsilane (151 mmol, 3.2 eq.) was placed in a 100 mL round-bottom flask and sealed tightly with a PTFE screw cap. Phosphorus trichloride (4 mL, 45.9 mmol) and 40 mL of acetonitrile were added, and the mixture was stirred for 72 h. Volatile components were removed under vacuum (oil pump, 60 °C), leaving a colorless viscous oil (11 g). Compound A1 was obtained by column chromatography.
[0055] The synthesis of compound A2 was performed as follows: 2.13 g of 3-hydroxypropionitrile (0.03 mol, 1.7 eq.) and 4.24 g of cyanoethyl phosphite (17.6 mmol) were dissolved in 300 mL of a dichloromethane-pyridine (9:1, v / v) mixed solvent. The mixture was cooled to –40 °C using acetonitrile-dry ice, and then 7.02 g of tribromopyridinium (90% industrial grade, 20.6 mmol) was added and the mixture was stirred for 3 hours. Water (100 mL) was added at -20 °C, followed by ethyl acetate (1 L). The organic layer was washed with water (3 × 1 L), dried over sodium sulfate, and the solvent was removed under vacuum to obtain a foamy substance (13 g). The foamy substance was adsorbed onto silica and fractionated using rapid chromatography with an ether-methanol (1:0–7:3, v / v) gradient.
[0056] Examples and Comparative Examples
[0057] The examples and comparative examples each provide an electrolyte, the composition of which is shown in Table 1. The preparation methods for each electrolyte include the following steps: At room temperature, in an argon-filled glove box (H2O < 1 ppm, O2 < 1 ppm), the solvents are first mixed uniformly, then dehydrated to obtain a dehydrated mixed solvent. LiPF6 and a second lithium salt are then added sequentially to the dehydrated mixed solvent while stirring, controlling the system temperature rise to no more than 2°C to obtain a transparent solution. Additives are then added and stirred uniformly to obtain the corresponding electrolyte. The content of LiPF6 is 12.8% based on the total mass of the electrolyte.
[0058] Table 1
[0059]
[0060]
[0061] Note: The content of each substance in the table refers to its percentage of the total mass of the electrolyte.
[0062] The electrolytes of the various embodiments and comparative examples were used to prepare lithium-ion batteries. The specific preparation methods are as follows:
[0063] Preparation of the positive electrode: The positive electrode material Li(Ni) is used... 0.8 Mn 0.1 Co 0.1 O2 (NMC811), conductive agent acetylene black (Super P), and binder polyvinylidene fluoride (PVDF) are mixed evenly in a mass ratio of NMC811:Super P:PVDF = 94:3:3, and then uniformly dispersed in 1-methyl-2-pyrrolidone (NMP) to form a uniform positive electrode slurry. The resulting slurry is coated on both sides of an aluminum foil, and after baking, rolling, and cutting, a positive electrode sheet is obtained.
[0064] Preparation of negative electrode sheet: The negative electrode material silicon suboxide (SiO), artificial graphite (AG), conductive agent acetylene black (Super P) and binder SBR are mixed evenly in mass ratio SiO:AG:Super P:SBR=18:76:3:3 and evenly dispersed in deionized water to prepare negative electrode slurry. The obtained slurry is coated on both sides of copper foil, and then baked, rolled and cut to obtain negative electrode sheet.
[0065] Fabrication of pouch batteries: The positive electrode, separator, and negative electrode are stacked in sequence, with the separator positioned between the positive and negative electrodes. They are then wound, hot-pressed and shaped, and the tabs are welded to obtain a bare cell. The bare cell is placed in an outer aluminum-plastic film and baked in an oven at 85±10℃ for 24 hours. The electrolyte is then injected into the dried battery, and the battery is allowed to stand, form, and undergo capacity testing to obtain a pouch lithium-ion battery.
[0066] The soft-pack lithium-ion batteries prepared with the electrolytes of each embodiment and the comparative example were subjected to performance testing. The specific testing methods are as follows:
[0067] (1) DCR (DC internal resistance) test: At room temperature (25±2℃), the lithium-ion battery was charged to 4.4V at 1C, then discharged at 1C capacity for 30min. After adjusting to 50% SOC, it was pulsed discharged at 5C constant current for 10s and then charged for 10s. The DCR was calculated as (voltage before pulse discharge – voltage after pulse discharge) / discharge current × 100%. The results are shown in Table 2. Each soft-pack lithium-ion battery was stored at 60℃ for 30 days and then cooled. When the battery was completely cooled to 25±2℃, the DCR was tested again and the internal resistance change rate was calculated as (DCR after 30 days – DCR before 30 days) / DCR before 30 days × 100%. The results are shown in Table 2.
[0068] (2) Room temperature cycle performance test: At 25±2℃, the lithium-ion battery was subjected to charge-discharge cycle test at a charge-discharge rate of 1C / 1C within the range of 2.8–4.4V, and the discharge specific capacity of the battery in the first cycle and the discharge specific capacity after 500 cycles were recorded. The capacity retention rate after 500 cycles = discharge specific capacity of 500 cycles / discharge specific capacity in the first cycle × 100%. The recorded data are shown in Table 2.
[0069] (3) High-temperature storage performance: The lithium-ion battery was placed at 60±2℃ and charged and discharged at a rate of 1C / 1C within the range of 2.8–4.4V. The discharge specific capacity of the battery in the first week was recorded. Then, the battery was stored at 60±2℃ for 30 days, and the charge and discharge test was carried out again and the discharge specific capacity was recorded. High-temperature storage capacity retention rate = discharge specific capacity after 30 days / discharge specific capacity in the first week × 100%. The recorded data are shown in Table 2.
[0070] (4) High-temperature gas generation test: The lithium-ion battery was charged at 25±2℃ with a constant current rate of 1C to 4.4V, and then charged at 4.4V with a constant voltage until the current was below 0.05C, so that it was in a fully charged state of 4.4V. The volume of the fully charged battery before storage was measured and recorded as V0; then the fully charged battery was placed in an oven at 70±2℃. After 2 days, the battery was taken out and its volume after storage was measured immediately and recorded as V1. The volume expansion rate = (V1–V0) / V0×100%, and the results are shown in Table 2.
[0071] Table 2
[0072]
[0073]
[0074] As shown in Table 2, the lithium-ion batteries prepared in each embodiment have low internal resistance, low internal resistance change rate during high-temperature storage, low volume expansion rate during high-temperature storage, good cycle stability, and high capacity retention rate during high-temperature storage.
[0075] Compared to Comparative Example 3 (without the first additive and the second additive), Comparative Example 1 (without the second additive), and Comparative Example 2 (without the first additive), Example 5 exhibits significantly lower internal resistance, 60°C storage internal resistance change rate, and 70°C storage volume expansion rate due to the addition of the first additive and the second additive. It also shows significantly higher capacity retention rate after 500 cycles at 25°C and storage capacity retention rate at 60°C. This indicates that the first additive and the second additive can synergistically improve gas generation issues as well as electrochemical performance such as internal resistance, cycle stability, and high-temperature stability.
[0076] As can be seen from the comparison of Examples 2-7, 5 and 8-11, when the mass content of the first additive in the electrolyte is in the range of 0.1% to 6% and the mass content of the second additive in the electrolyte is in the range of 0.1% to 3%, the two additives play a synergistic role, which can improve the gas generation problem of lithium-ion batteries as well as the electrochemical performance such as internal resistance, cycle stability and high temperature stability.
[0077] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the essence and scope of the technical solutions of the present invention.
Claims
1. An electrolyte, characterized in that, Includes lithium hexafluorophosphate, solvent, first additive, and second additive. The first additive includes at least one of the compounds with the structure shown in Formula I or Formula II; The second additive includes at least one of the compounds with the structure shown in Formula III; ; ; Formula I Formula II Formula III Wherein, R1 to R6 each independently contains a cyano group of C1 to C10; R7 to R9 each independently contains at least one of an alkyl group of C1 to C10 and an alkoxy group of C1 to C10; R 10 Includes C1 to C10 alkyl groups; The mass ratio of the first additive to the second additive is (1-20):(1-10). The first additive accounts for 0.1% to 6% of the total mass of the electrolyte; the second additive accounts for 0.1% to 3% of the total mass of the electrolyte. The solvent includes fluoroethylene carbonate.
2. The electrolyte according to claim 1, characterized in that, The first additive comprises at least one of the following compounds: (A1) (A2) (A3) The second additive includes at least one of the following compounds: (B1) (B2) (B3) (B4) 3. The electrolyte according to claim 1, characterized in that, It includes lithium hexafluorophosphate and a second lithium salt, wherein the second lithium salt includes at least one of lithium tetrafluoroborate, lithium dioxaborate, lithium difluorooxaborate, lithium difluorodioxaborate, lithium bis(fluorosulfonyl)imide, lithium bistrifluoromethylsulfonylimide, lithium perchlorate, lithium difluorophosphate, lithium pentafluoroethyl trifluoroborate, and lithium 4,5-dicyano-2-trifluoromethyl-imidazolium.
4. The electrolyte according to claim 3, characterized in that, The lithium hexafluorophosphate accounts for 12% to 15% of the total mass of the electrolyte, and the second lithium salt accounts for 0% to 15.0% of the total mass of the electrolyte.
5. The electrolyte according to claim 1, characterized in that, The solvent includes fluoroethylene carbonate and a second solvent, the second solvent including at least one of ethylene carbonate, propylene carbonate, butene carbonate, dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, methyl propyl carbonate, diphenyl carbonate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, γ-butyrolactone, acetonitrile, and sulfolane.
6. The electrolyte according to claim 5, characterized in that, The mass ratio of the fluoroethylene carbonate and the second solvent is (1-5):(5-15).
7. A lithium-ion battery, characterized in that, It includes positive electrode material, negative electrode material and electrolyte as described in any one of claims 1 to 6.
8. The lithium-ion battery according to claim 7, characterized in that, The cathode material includes at least one of nickel-cobalt-manganese ternary materials, nickel-aluminum-manganese ternary materials, lithium cobalt oxide materials, lithium iron phosphate materials, lithium manganese oxide materials, lithium manganese iron phosphate materials, and nickel-manganese spinel materials.
9. The lithium-ion battery according to claim 7, characterized in that, The negative electrode material includes silicon-carbon material, wherein the silicon-based material in the silicon-carbon material includes at least one of elemental silicon, silicon-carbon, silicon-oxygen, and silicon metal compounds; and the carbon-based material in the silicon-carbon material includes graphite.
Citation Information
Patent Citations
Electrolyte for stabilizing silicon-carbon surface of lithium ion battery and preparation method thereof, and application of electrolyte for stabilizing silicon-carbon surface of lithium ion battery
CN110190331A
Electrolyte, electrochemical device comprising the electrolyte and electronic device
CN111628219A