Negative active material and lithium secondary battery including the same
By using a silicon-carbon composite negative electrode active material with voids in the center of the lithium secondary battery, the problem of volume expansion during charging and discharging is solved, resulting in better cycle life and high capacity characteristics.
Patent Information
- Application Number
- CN202180065636.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-11-17
- Filing Date
- 2021-11-15
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2041-11-15
AI Technical Summary
The negative electrode active material of existing lithium secondary batteries suffers from volume expansion during charge and discharge, resulting in poor cycle life characteristics.
A silicon-carbon composite with voids in the center is used as the negative electrode active material, wherein the mixing ratio of silicon nanoparticles and amorphous carbon is 80:20 to 60:40. By controlling the particle size and aspect ratio of silicon nanoparticles and combining them with the distribution of amorphous carbon, a dense surface layer is formed to absorb volume expansion.
It effectively suppresses volume expansion during charging and discharging, improves the cycle life and high-rate characteristics of lithium secondary batteries, and maintains high capacity.
Smart Images

Figure CN116325220B_ABST
Abstract
Description
TECHNICAL FIELD
[0001] The present invention relates to a negative active material and a lithium secondary battery including the negative active material. BACKGROUND
[0002] Recently, a lithium secondary battery receiving attention as a power source for small portable electronic devices uses an organic electrolyte solution, and thus has a discharge voltage two times or more that of a conventional battery using an aqueous alkaline solution, and accordingly, has high energy density.
[0003] As for a positive active material of the lithium secondary battery, an oxide including lithium and a transition metal, which has a structure capable of intercalating / deintercalating lithium, such as LiCoO2, LiMn2O4, LiNi 1-x Co x O2 (0<x<1), and the like has been mainly used.
[0004] As for a negative active material, various carbon-based materials capable of intercalating and deintercalating lithium, such as artificial graphite, natural graphite, and hard carbon, have been used, but a graphite negative active material has low capacity of 360 mAh / g, and thus has low specific capacity, and in order to have higher capacity, studies on a non-carbon-based negative active material based on silicon or tin have been conducted. SUMMARY
[0005] Technical Problem
[0006] One embodiment provides a negative active material for a lithium secondary battery, which may suppress volume expansion during charge and discharge, thereby improving cycle-life characteristics.
[0007] Another embodiment provides a lithium secondary battery including the negative active material.
[0008] Technical Solution
[0009] According to an embodiment, provided is a negative active material for a lithium secondary battery, which includes a silicon-carbon composite having a void in a center portion, a radius of the center portion corresponding to 30% to 50% of a radius of the negative active material for a lithium secondary battery, and the silicon-carbon composite including silicon nanoparticles and amorphous carbon.
[0010] The center portion may include at least one silicon nanoparticle.
[0011] The silicon nanoparticles may have a particle size of 10 nm to 200 nm.
[0012] The negative active material may have a particle size of 5 μm to 20 μm.
[0013] Silicon nanoparticles can be in the form of thin sheets.
[0014] Silicon nanoparticles can have aspect ratios (width / thickness) from 5 to 20. X-ray diffraction using CuKα rays revealed that the silicon nanoparticles can have a full width at half maximum (FWHM) of 0.5 degrees (°) to 7 degrees (°) at the (111) plane.
[0015] According to another embodiment, a lithium secondary battery is provided, the lithium secondary battery comprising: a negative electrode including a negative electrode active material; a positive electrode including a positive electrode active material; and a non-aqueous electrolyte.
[0016] Other embodiments are included in the following detailed description.
[0017] Beneficial effects
[0018] The negative electrode active material used in lithium secondary batteries can reduce the stress caused by volume expansion during charging and discharging, thus exhibiting excellent cycle life characteristics. Attached Figure Description
[0019] Figure 1 This is a schematic diagram illustrating a negative electrode active material for a lithium secondary battery according to one embodiment.
[0020] Figure 2 This is a schematic diagram of a lithium secondary battery according to another embodiment.
[0021] Figure 3 This is a graph showing the X-ray photoelectron spectroscopy (XPS) analysis of the negative electrode active material according to Example 1. Detailed Implementation
[0022] Embodiments of the invention are described in detail below. However, these embodiments are merely examples, and the invention is not limited thereto; rather, it is defined by the scope of the claims.
[0023] According to one embodiment, the negative electrode active material for a lithium secondary battery may include a silicon-carbon composite having voids in a central portion, and the silicon-carbon composite may include silicon nanoparticles and amorphous carbon. In the negative electrode active material, the central portion may have a radius corresponding to 30% to 50% of the radius of the negative electrode active material for the lithium secondary battery.
[0024] Figure 1 The negative electrode active material is schematically shown. The negative electrode active material 1 includes a silicon-carbon composite with voids 4 in the central portion 3, and the silicon-carbon composite includes silicon nanoparticles 7 and amorphous carbon 9.
[0025] In addition, the radius a of the central portion 3 can correspond to 30% to 50% of the radius b of the active substance.
[0026] Thus, according to one embodiment, the negative electrode active material has voids in the central portion, and the central portion may substantially exclude amorphous carbon, but may only include silicon nanoparticles. In the case where the central portion excludes amorphous carbon and only includes silicon nanoparticles, the voids present in the central portion can absorb the volume expansion that may occur during charging and discharging, thereby effectively preventing the overall volume expansion of the negative electrode active material.
[0027] In one embodiment, the radius of the central portion can be 30% to 50% of the radius of the negative electrode active material. When the radius is smaller than this range, it is difficult to absorb the volume expansion caused during the initial charge and discharge, thus the initial expansion rate will increase significantly. Furthermore, when the radius of the central portion is larger than this range, with repeated charge and discharge, a large amount of SEI (solid electrolyte interface) will be generated due to side reactions between the negative electrode active material and the electrolyte, resulting in a significant increase in the total volume expansion of the negative electrode active material and a deterioration in cycle life characteristics.
[0028] The negative electrode active material can have a particle size of 5 μm to 20 μm. In one embodiment, the size and particle size can be the average particle size. In this case, the average particle size can be represented as the particle size (D50) as a cumulative volume measurement. Unless otherwise defined, the average particle size represents the average particle size (D50) of the cumulative volume in the particle distribution when it is about 50% by volume. The average particle size (D50) can be measured by methods known to those skilled in the art, such as by a particle size analyzer, or by a transmission electron microscope image or a scanning electron microscope image. Optionally, data analysis is performed using a dynamic light scattering measurement device, and the number of particles is counted for each particle size range, thereby allowing the average particle size (D50) value to be readily obtained by calculation.
[0029] When the particle size of the negative electrode active material is within this range, it can exhibit superior high-rate performance and cycle life characteristics.
[0030] The absence of voids in the central portion leads to extreme volume expansion of the negative electrode active material during charging and discharging.
[0031] In one embodiment, the central portion does not include amorphous carbon, and amorphous carbon may only be present in the surface portion of the negative electrode active material. Here, the surface portion refers to the region from the central portion of the negative electrode active material to its outermost surface. If the central portion includes the same amorphous carbon as the surface portion, there is no space to absorb the volume expansion of the negative electrode active material during charge and discharge; therefore, the volume expansion of the negative electrode active material during charge and discharge will occur extremely. In one embodiment, although amorphous carbon may be slightly included as an impurity in the central portion, it is present at a level close to zero, meaning it is essentially not present in the central portion.
[0032] Furthermore, silicon nanoparticles can be integrally, substantially, and uniformly incorporated into the negative electrode active material, i.e., present at a substantially uniform concentration in both the central and surface portions. When silicon nanoparticles are integrally, substantially, and uniformly present in the negative electrode active material, the amount of silicon is high, thereby achieving high capacity. If silicon nanoparticles are present only in the central portion and not in the surface portion, the capacity will deteriorate.
[0033] In the negative electrode active material according to one embodiment, silicon nanoparticles are present in both the central portion and the surface portion, while amorphous carbon is present only in the surface portion and not in the central portion. This indicates that the surface portion of the negative electrode active material includes a silicon-carbon composite. Therefore, the inclusion of a silicon-carbon composite in the surface portion results in increased capacity compared to an active material that only includes amorphous carbon.
[0034] According to one embodiment, the silicon-carbon composite includes secondary particles in which at least one silicon nanoparticle is aggregated, amorphous carbon positioned around the surface of the secondary particles, and amorphous carbon filling the spaces between the primary particles to be positioned on and around the surface of the primary particles. Filling the spaces between the primary particles with amorphous carbon effectively prevents the silicon nanoparticles from being directly exposed to the electrolyte, thereby forming a more stable interface and more effectively buffering the volume expansion of the silicon nanoparticles. Furthermore, since the amorphous carbon is positioned on the surface between the silicon nanoparticles, it acts as a channel for electron transport between the silicon nanoparticles and the electrolyte, thereby further improving conductivity and resulting in a further reduction in electrode resistance.
[0035] Additionally, the surface portion can be a dense layer in which no or substantially no voids exist. Thus, according to one embodiment, the negative electrode active material includes a dense surface portion in which no or substantially no voids exist, thereby inhibiting electrolyte permeation into the internal active material, thereby reducing side reactions with the electrolyte and maintaining cycle life characteristics.
[0036] Amorphous carbon can be soft carbon, hard carbon, mesophase pitch carbides, sintered coke, or a combination thereof.
[0037] Silicon nanoparticles can have particle sizes ranging from 10 nm to 200 nm. When the size of silicon nanoparticles is within this range, side reactions between the negative electrode active material and the electrolyte solution can be suppressed, and the expansion of Si nanoparticles can be reduced, thereby improving cycle life characteristics and initial efficiency.
[0038] In one embodiment, the secondary particles aggregated therein from the primary particles can have a particle size of 2 μm to 15 μm, or 5 μm to 10 μm. When the particle size of the secondary particles is within this range, superior high-rate performance and cycle life characteristics can be exhibited.
[0039] Silicon nanoparticles can be flake-type. That is, silicon nanoparticles can be flake-shaped with a long axis and a short axis. Here, the ratio of the long axis to the short axis of the Si nanoparticle (e.g., aspect ratio (width / thickness)) can be between 5 and 20. When the ratio of the long axis to the short axis of the Si nanoparticle is within this range, the expansion of the silicon nanoparticle can be reduced, thereby improving the cycle life characteristics and initial efficiency of the battery including this active material.
[0040] In one embodiment, X-ray diffraction using CuKα rays revealed that silicon primary particles can have a full width at half maximum (FWHM) (111) ranging from 0.5 degrees (°) to 7 degrees (°) at the (111) plane. When the FWHM (111) of the silicon primary particles is within this range, the cycle life characteristics of the battery can be improved.
[0041] X-ray diffraction measurements can be performed using CuKα rays as the target ray. The measurement conditions are 2θ = 40° to 50°, the scanning speed (° / s) is 0.04 to 0.06, and the step size (° / step) is 0.01 to 0.03.
[0042] In one embodiment, the mixing ratio of silicon nanoparticles and amorphous carbon included in the negative electrode active material can be from 80:20 to 60:40 by weight. When the mixing ratio of silicon nanoparticles to amorphous carbon meets this range, physical properties such as cycle life expansion rate and capacity retention rate can be effectively maintained.
[0043] According to one embodiment, the negative electrode active material can be prepared by the following steps.
[0044] First, silicon nanoparticles are prepared. These silicon nanoparticles can be nanoparticles with a particle size ranging from 10 nm to 200 nm. Such silicon nanoparticles can be prepared using common nanoparticle preparation techniques, such as pulverization. X-ray diffraction using CuKα rays revealed that the silicon nanoparticles can have a full width at half maximum (FWHM) (111) in the range of 0.5 (°) to 7 (°) at the (111) plane. The silicon nanoparticles can have an aspect ratio (width / thickness) of 5 to 20.
[0045] Silicon nanoparticles are added to a solvent to prepare a silicon particle liquid. The solvent can suitably be an alcohol that does not oxidize the silicon particles and is readily volatile; examples include isopropanol, ethanol, methanol, butanol, N-methylpyrrolidone, propylene glycol, or combinations thereof. The silicon particle liquid can have a concentration from 10 wt% to 30 wt%.
[0046] A dispersant may also be added during the addition of the solvent. The dispersant may be stearic acid, polyvinylpyrrolidone, polyvinyl alcohol, polyacrylic acid, gallic acid, carboxymethyl cellulose, sucrose, ethylene glycol, citric acid, or a combination thereof.
[0047] Mixing can be performed using a sand mill or a ball mill. Mixing can be performed for 0.5 to 3 hours, but is not limited to this. Furthermore, mixing can be performed at speeds from 1000 rpm to 3000 rpm, but is not limited to this.
[0048] When a dispersant is also used, the mixing ratio of silicon particles to dispersant can be from 3:1 to 9:1 by weight. When the mixing ratio is within this range, the dispersant can be more uniformly distributed on the surface of the silicon particles, thereby improving the efficiency during the mixing process, especially the grinding efficiency when using a mill. In addition, during the mixing process and the subsequent spray drying process, the dispersant can also prevent the oxidation of silicon and further promote the agglomeration of primary particles.
[0049] The resulting mixture can be further dispersed by using a homogenizer.
[0050] The prepared silicon particle liquid is then spray-dried. Spray drying allows silicon nanoparticles, which are primary particles, to aggregate to prepare secondary silicon particles. Spray drying can be performed at temperatures between 120°C and 170°C. When spray drying is performed within this temperature range, the primary silicon particles can aggregate more densely; that is, the primary silicon particles and the secondary silicon particles they aggregate with are densely clustered, and the distance between them is very narrow. Therefore, the voids between the primary silicon particles and the voids between the secondary silicon particles can be formed smaller, thus allowing for a suitable reduction in the amount of amorphous carbon included in the negative electrode active material at a desired level.
[0051] The resulting secondary particles were then mixed with an amorphous carbon precursor.
[0052] Here, the mixing ratio of secondary particles to amorphous carbon precursor can be from 80:20 to 60:40 by weight. When the mixing ratio of secondary particles to amorphous carbon precursor is within this range, there is no excess amorphous carbon in the final negative electrode active material, and no amorphous carbon layer is formed on the surface of the final negative electrode active material, which allows for a more suitable silicon utilization rate, thereby exhibiting excellent initial efficiency.
[0053] Amorphous carbon precursors can be coal tar pitch, mesophase pitch, petroleum pitch, mesophase carbon pitch, coal-based oil, petroleum-based heavy oil, or polymer resins (such as phenolic resins, furan resins, and polyimide resins).
[0054] The resulting mixture was subjected to heat treatment to prepare a negative electrode active material for lithium secondary batteries.
[0055] Heat treatment can be performed by raising the temperature to 700°C to 1000°C at a heating rate of 10°C / min to 15°C / min and then heat-treating at the raised temperature. The heat treatment time at the raised temperature can be from 1 hour to 4 hours.
[0056] Heat treatment melts the amorphous carbon precursor diffused within the active material, transforming it into amorphous carbon. Furthermore, when the heating rate is controlled in this process, the transformation to amorphous carbon can occur on the surface portion in a distributed state before the amorphous carbon precursor is distributed into the central portion. Therefore, amorphous carbon is not present in the central portion of the negative electrode active material, but can exist in the surface portion. Moreover, heat treatment at this heating rate prepares a surface portion containing distributed amorphous carbon and a central portion containing only silicon nanoparticles; here, the radius of the central portion can correspond to 30% to 50% of the radius of the negative electrode active material.
[0057] When the heating rate of heat treatment is below this range, it is undesirable for the amorphous carbon precursor to diffuse into the central part and then transform into amorphous carbon.
[0058] Furthermore, during heat treatment, the amorphous carbon precursor is located between the silicon nanoparticles on which the amorphous carbon precursor is positioned, with the primary particles surrounding the surface of the secondary particles. Here, when the heating rate of the heat treatment exceeds this range, the amorphous carbon precursor does not penetrate into the secondary particles at all, but is carbonized only on the outer surface of the secondary particles.
[0059] Heat treatment can be performed under a nitrogen (N2) atmosphere or an argon atmosphere. The atmosphere under these conditions prevents silicon oxidation and SiC formation, and effectively generates amorphous carbon, thereby reducing the electrical resistance of the active material.
[0060] The prepared negative electrode active material can then be further pulverized, and this pulverization can be performed using an air jet mill, a cutter mill, or a planetary mill. Pulverization can continue until the final particle size of the active material is between 5 μm and 20 μm.
[0061] According to one embodiment, a lithium secondary battery including a negative electrode, a positive electrode, and an electrolyte is provided.
[0062] The negative electrode includes a current collector and a negative electrode active material layer formed on the current collector and including a negative electrode active material according to one embodiment.
[0063] The negative electrode active material layer may also include crystalline carbon negative electrode active material. Examples of crystalline carbon negative electrode active material may be graphite (such as natural or artificial graphite in non-specific shapes, flakes, sheets, spheres, or fibers).
[0064] When the negative electrode active material layer comprises a negative electrode active material according to one embodiment as the first negative electrode active material and a crystalline carbon negative electrode active material as the second negative electrode active material, the first negative electrode active material is located between the particles of the second negative electrode active material to ensure good contact with the second negative electrode active material, thereby more effectively suppressing negative electrode expansion. Here, the mixing ratio of the first negative electrode active material to the second negative electrode active material can be from 1:99 to 40:60 by weight. When using the first and second negative electrode active materials within this range, the current density of the negative electrode can be further improved, and a thinner electrode can be fabricated. Furthermore, the first negative electrode active material, including silicon, can be more uniformly distributed in the negative electrode, thus more effectively suppressing negative electrode expansion.
[0065] In the negative electrode active material layer, the amount of negative electrode active material can be from 95 wt% to 99 wt%, based on the total weight of the negative electrode active material layer.
[0066] The negative electrode active material layer may include a binder and optionally a conductive material. In the negative electrode active material layer, the amount of binder may be from 1 wt% to 5 wt% based on the total weight of the negative electrode active material layer. Furthermore, when conductive material is also included, the negative electrode active material may comprise 90 wt% to 98 wt% of the total negative electrode active material, 1 wt% to 5 wt% of the binder, and 1 wt% to 5 wt% of the conductive material.
[0067] Binders improve the adhesion between negative electrode active material particles and between the negative electrode active material particles and the current collector. Binders can be non-aqueous binders, aqueous binders, or combinations thereof.
[0068] Non-aqueous adhesives may be ethylene-propylene copolymers, polyacrylonitrile, polystyrene, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamide-imide, polyimide, or combinations thereof.
[0069] Waterborne adhesives may include styrene-butadiene rubber, acrylated styrene-butadiene rubber, acrylonitrile-butadiene rubber, acrylic rubber, butyl rubber, fluororubber, ethylene oxide-containing polymers, polyvinylpyrrolidone, polyepoxychlorohydrin, polyphosphazene, ethylene propylene diene copolymer, polyvinylpyridine, chlorosulfonated polyethylene, latex, polyester resin, acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol, or combinations thereof.
[0070] When an aqueous binder is used as a negative electrode binder, a cellulose compound can also be used as a thickener to provide viscosity. Cellulose compounds include one or more of carboxymethyl cellulose, hydroxypropyl methyl cellulose, methyl cellulose, or their alkali metal salts. The alkali metal can be Na, K, or Li. Based on 100 parts by weight of the negative electrode active material, a thickener may be included in an amount from about 0.1 parts by weight to about 3 parts by weight.
[0071] Conductive materials are included to provide electrode conductivity. Any electrically conductive material can be used as a conductive material unless it causes a chemical change. Examples of conductive materials can be: carbon-based materials, such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, etc.; metal-based materials, including metal powders or fibers of copper, nickel, aluminum, silver, etc.; conductive polymers, such as polyphenylene derivatives; or mixtures thereof.
[0072] The current collector may include, but is not limited to, one selected from copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, polymer substrate coated with conductive metal, and combinations thereof.
[0073] A negative electrode can be formed by preparing an active material composition by mixing a negative electrode active material, a binder, and optionally a conductive material in a solvent, and then coating the active material composition onto a current collector. The solvent can be water.
[0074] Such a method of preparing the negative electrode is well known, and therefore will not be described in detail in this specification.
[0075] The positive electrode includes a current collector and a layer of positive electrode active material formed on the current collector.
[0076] The positive electrode active material may include lithiation compounds that reversibly insert and deintercalate lithium ions. Specifically, one or more composite oxides of lithium and metals selected from cobalt, manganese, nickel, and combinations thereof may be used. More specifically, compounds represented by one of the following chemical formulas may be used: Li a A 1-b X b D 1 2(0.90≤a≤1.8, 0≤b≤0.5); Li a A 1-b X b O 2-c1 D 1 c1 (0.90≤a≤1.8, 0≤b≤0.5, 0≤c1≤0.05); Li a E 1-b X b O 2-c1 D 1 c1 (0.90≤a≤1.8, 0≤b≤0.5, 0≤c1≤0.05); Li a E 2-b X b O 4-c1 D 1 c1 (0.90≤a≤1.8, 0≤b≤0.5, 0≤c1≤0.05); Li a Ni 1-b-c Co b X c D 1 α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α≤2); Li a Ni 1-b- c Co b X c O 2-α T α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α<2); Li a Ni 1-b-c Co b X c O 2-α T2(0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α<2); Li a Ni 1-b-c Mn b X c D 1 α(0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.5\0<α≤2);Li a Nor 1-b-c Mn b X c O 2-α T α (0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.5,0<α<2);Li a Nor 1-b-c Mn b X c O 2-α T2(0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.5\0<α<2);Li a Nor b E c G d O2(0.90≤a≤1.8,0≤b≤0.9,0≤c≤0.5,0.001≤d≤0.1);Li a Nor b Co c Mn d G e O2(0.90≤a≤1.8,0≤b≤0.9,0≤c≤0.5,0≤d≤0.5,0.001≤e≤0.1);Li a NiG b O2(0.90≤a≤1.8,0.001≤b≤0.1);Li a CoG b O2(0.90≤a≤1.8,0.001≤b≤0.1);Li a Mn 1-b G b O2(0.90≤a≤1.8,0.001≤b≤0.1);Li a Mn2G b O4(0.90≤a≤1.8,0.001≤b≤0.1);Li a Mn 1-g G g PO4(0.90≤a≤1.8,0≤g≤0.5);QO2;QS2;LiQS2;V2O5;LiV2O5;LiZO2;LiVO4;Li (3-f) J2(PO4)3(0≤f≤2);Li (3-f) Fe2(PO4)3(0≤f≤2);Li a FePO4(0.90≤a≤1.8)。
[0077] In the above chemical formulas, A is selected from Ni, Co, Mn and combinations thereof; X is selected from Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, rare earth elements and combinations thereof; D is selected from O, F, S, P and combinations thereof; E is selected from Co, Mn and combinations thereof; T is selected from F, S, P and combinations thereof; G is selected from Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V and combinations thereof; Q is selected from Ti, Mo, Mn and combinations thereof; Z is selected from Cr, V, Fe, Sc, Y and combinations thereof; and J is selected from V, Cr, Mn, Co, Ni, Cu and combinations thereof.
[0078] Furthermore, the compound can have a coating on the surface, or it can be mixed with another compound having a coating. The coating may include at least one coating element compound selected from the group consisting of oxides of coating elements, hydroxides of coating elements, hydroxy oxides of coating elements, oxy carbonates of coating elements, and hydroxy carbonates of coating elements. The compound used for the coating may be amorphous or crystalline. The coating elements included in the coating may include Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or mixtures thereof. By using these elements in the compound, the coating can be formed in a manner that does not adversely affect the properties of the positive electrode active material. For example, this method may include any coating method, such as spraying, dipping, etc., but since it is well known in the relevant art, it is not shown in more detail here.
[0079] In the positive electrode, the amount of positive electrode active material can be from about 90 wt% to about 98 wt%, based on the total weight of the positive electrode active material layer.
[0080] In one embodiment, the positive electrode active material layer may further include a binder and a conductive material. Here, based on the total amount of the positive electrode active material layer, the amounts of the binder and the conductive material may be from 1 wt% to 5 wt%, respectively.
[0081] The binder improves the adhesion between the positive electrode active material particles and between the positive electrode active material particles and the current collector. Examples of binders can be polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, nylon, etc., but are not limited to these.
[0082] Conductive materials are included to provide electrode conductivity; any conductive material can be used as the conductive material unless it causes a chemical change. Examples of conductive materials may include: carbon-based materials, such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, etc.; metal-based materials, including metal powders or metal fibers of copper, nickel, aluminum, silver, etc.; conductive polymers, such as polyphenylene derivatives; or mixtures thereof.
[0083] The current collector can be made of aluminum foil, nickel foil, or a combination thereof, but is not limited to these.
[0084] An active material composition is prepared by mixing an active material, a binder, and optionally a conductive material in a solvent, and then coating the active material composition onto a current collector to form a positive electrode active material layer and a negative electrode active material layer. Such methods for preparing active material layers are well known and therefore will not be described in detail in this specification. Solvents include, but are not limited to, N-methylpyrrolidone. Additionally, when the binder in the negative electrode active material layer is a water-soluble binder, the solvent can be water.
[0085] Electrolytes include non-aqueous organic solvents and lithium salts.
[0086] Non-aqueous organic solvents are used as media for transporting ions that participate in the electrochemical reactions of the battery.
[0087] Non-aqueous organic solvents can include carbonate solvents, ester solvents, ether solvents, ketone solvents, alcohol solvents, or aprotic solvents.
[0088] Carbonate solvents can include dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), methyl ethyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), and butyl carbonate (BC), etc. Ester solvents can include methyl acetate, ethyl acetate, n-propyl acetate, dimethyl acetate, methyl propionate, ethyl propionate, decanolactone, mevalonolactone, caprolactone, etc. Ether solvents can include dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, dimethoxyethane, 2-methyltetrahydrofuran, tetrahydrofuran, etc. Additionally, ketone solvents can include cyclohexanone, etc. In addition, alcohol solvents may include ethanol, isopropanol, etc., and examples of aprotic solvents may include nitriles such as R-CN (where R is a C2 to C20 straight-chain hydrocarbon, branched hydrocarbon or cyclic hydrocarbon, or may include double bond, aromatic ring or ether bond), amides such as dimethylformamide, dioxolane such as 1,3-dioxolane, sulfolane, etc.
[0089] Organic solvents can be used alone or in mixtures. When organic solvents are used in mixtures, the mixing ratio can be controlled according to the desired battery performance, which is easily understood by those skilled in the art.
[0090] Furthermore, carbonate solvents may include mixtures of cyclic carbonates and linear carbonates. Here, when a mixture of cyclic carbonates and linear carbonates mixed together in a volume ratio of about 1:1 to about 1:9 is used as an electrolyte, it can exhibit enhanced performance.
[0091] When mixing and using non-aqueous organic solvents, a mixture of cyclic carbonates and chain carbonates, a mixture of cyclic carbonates and propionate solvents, or a mixture of cyclic carbonates, chain carbonates, and propionate solvents can be used. Propionate solvents can be methyl propionate, ethyl propionate, propyl propionate, or combinations thereof.
[0092] Here, when cyclic carbonates and linear carbonates, or cyclic carbonates and propionate solvents, are mixed in a volume ratio of about 1:1 to about 1:9, the performance of the electrolyte solution can be improved. Alternatively, when cyclic carbonates, linear carbonates, and propionate solvents are mixed, they can be mixed in a volume ratio of about 1:1:1 to about 3:3:4. The mixing ratio of the solvents can be appropriately adjusted according to the desired properties.
[0093] In addition to carbonate solvents, organic solvents may also include aromatic hydrocarbon solvents. Here, carbonate solvents and aromatic hydrocarbon solvents may be mixed together in a volume ratio of about 1:1 to about 30:1.
[0094] Aromatic hydrocarbon organic solvents can be aromatic hydrocarbon compounds of chemical formula 1.
[0095] [Chemical Formula 1]
[0096]
[0097] (In Formula 1, R1 to R6 may be the same or different, and are selected from hydrogen, halogens, C1 to C10 alkyl groups, haloalkyl groups and combinations thereof)
[0098] Specific examples of aromatic hydrocarbon organic solvents may be selected from benzene, fluorobenzene, 1,2-difluorobenzene, 1,3-difluorobenzene, 1,4-difluorobenzene, 1,2,3-trifluorobenzene, 1,2,4-trifluorobenzene, chlorobenzene, 1,2-dichlorobenzene, 1,3-dichlorobenzene, 1,4-dichlorobenzene, 1,2,3-trichlorobenzene, 1,2,4-trichlorobenzene, iodobenzene, 1,2-diiodobenzene, 1,3-diiodobenzene, 1,4-diiodobenzene, 1,2,3-triiodobenzene, 1,2,4-triiodobenzene, toluene, and fluorotoluene. 2,3-Difluorotoluene, 2,4-Difluorotoluene, 2,5-Difluorotoluene, 2,3,4-Trifluorotoluene, 2,3,5-Trifluorotoluene, Chlorotoluene, 2,3-Dichlorotoluene, 2,4-Dichlorotoluene, 2,5-Dichlorotoluene, 2,3,4-Trichlorotoluene, 2,3,5-Trichlorotoluene, Iodotoluene, 2,3-Diiodotoluene, 2,4-Diiodotoluene, 2,5-Diiodotoluene, 2,3,4-Triiodotoluene, 2,3,5-Triiodotoluene, Xylene and combinations thereof.
[0099] Electrolytes may also include additives such as vinylene carbonate or ethylene carbonate compounds of formula 2 to improve battery cycle life.
[0100] [Chemical Formula 2]
[0101]
[0102] (In Formula 2, R7 and R8 may be the same or different and are selected from hydrogen, halogen, cyano (CN), nitro (NO2) and fluorinated C1 to C5 alkyl groups, provided that at least one of R7 and R8 is selected from halogen, cyano (CN), nitro (NO2) and fluorinated C1 to C5 alkyl groups, and R7 and R8 are not both hydrogen.)
[0103] Examples of ethylene carbonate compounds may include difluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, bromoethylene carbonate, dibromoethylene carbonate, nitroethylene carbonate, cyanoethylene carbonate, or fluoroethylene carbonate. The amount of additives used to improve cycle life may be used within appropriate limits.
[0104] Electrolytes may also include vinyl ethylene carbonate, propane sulfonyl lactone, succinate, or combinations thereof, and the amount used may be adjusted as appropriate.
[0105] Lithium salts dissolved in organic solvents supply lithium ions to the battery, enabling the basic operation of lithium secondary batteries and improving lithium ion transport between the positive and negative electrodes. Examples of lithium salts include those selected from LiPF6, LiBF4, LiSbF6, LiAsF6, LiN(SO2C2F5)2, Li(CF3SO2)2N, LiN(SO3C2F5)2, LiC4F9SO3, LiClO4, LiAlO2, LiAlCl4, LiPO2F2, and LiN(C x F 2x+1 SO2)(C y F 2y+1 One or more of the following lithium salts are used: SO2 (where x and y are natural numbers, for example, integers in the range of 1 to 20), lithium difluoro(dioxy)phosphate, LiCl, LiI, LiB(C2O4)2 (lithium bis(oxalate)borate: LiBOB), and lithium difluoro(oxalate)borate (LiDFOB). The concentration of the lithium salt can range from about 0.1 M to about 2.0 M. When lithium salts are included within the above concentration range, the electrolyte can exhibit excellent performance and lithium-ion mobility due to optimal electrolyte conductivity and viscosity.
[0106] Depending on the type of battery, lithium secondary batteries may also include a separator between the negative and positive electrodes. Examples of suitable separator materials include polyethylene, polypropylene, polyvinylidene fluoride, and their multilayers, such as polyethylene / polypropylene double-layer separators, polyethylene / polypropylene / polypropylene triple-layer separators, and polypropylene / polypropylene / polypropylene triple-layer separators.
[0107] Figure 2 This is an exploded perspective view of a lithium secondary battery according to one embodiment. The lithium secondary battery according to the embodiment is shown as a prismatic battery, but is not limited thereto, and may include batteries of various shapes, such as cylindrical batteries, pouch batteries, etc.
[0108] Reference Figure 2 The lithium secondary battery 100 according to an embodiment includes an electrode assembly 40 manufactured by winding a separator 30 disposed between a positive electrode 10 and a negative electrode 20, and a housing 50 housing the electrode assembly 40. An electrolyte (not shown) may be immersed in the positive electrode 10, the negative electrode 20, and the separator 30.
[0109] Method for carrying out the invention
[0110] Examples and comparative examples of the invention are described below. However, these embodiments should not be construed as limiting the scope of the invention in any way.
[0111] (Example 1)
[0112] Thin-film silicon nanoparticles with an average particle size D50 of 100 nm and polyvinylpyrrolidone dispersant were mixed in ethanol solvent and dispersed using a ball mill at 1500 rpm for 1 hour to prepare a silicon particle liquid with a concentration of 11 wt%. Here, the mixing ratio of silicon nanoparticles to polyvinylpyrrolidone dispersant was set to 5:1 by weight.
[0113] The obtained Si particles exhibited a full width at half maximum (FWHM) of 0.5 degrees (°) in the (111) plane using CuKα X-ray diffraction. X-ray diffraction analysis was performed within the range of 2θ = 10° to 50° at a scan rate (° / s) of 0.054, a step size (° / step) of 0.01313, and a step time of 62.475 s. Furthermore, the Si particles had an aspect ratio (width / thickness) of approximately 5.
[0114] Use a homogenizer to homogenize and disperse the resulting mixture for 30 minutes.
[0115] Subsequently, the resulting homogenized dispersion was spray-dried at 130°C. Spray drying was then used to aggregate the silicon nanoparticles, which were primary particles, to prepare secondary particles.
[0116] The prepared secondary particles were mixed with mesophase carbon pitch at a weight ratio of 77:23. After the temperature was increased to 800°C at a heating rate of 10°C / min, the resulting mixture was heat-treated at 800°C for 2 hours. The heat treatment was performed under a nitrogen atmosphere.
[0117] The heat-treated product was pulverized using an air jet mill to prepare a negative electrode active material with an average particle size D50 of 8 μm.
[0118] The prepared negative electrode active material is a silicon-carbon composite with voids formed in the central portion, where only silicon nanoparticles exist. The central portion has a size (diameter) of 3 μm, and the prepared negative electrode active material has an average particle size D50 of 8 μm. Therefore, the radius of the central portion corresponds to 37.5% of the radius of the negative electrode active material.
[0119] A negative electrode active material slurry was prepared by mixing 97.8 wt% of negative electrode active material, 1.2 wt% of styrene-butadiene rubber and 1.0 wt% of carboxymethyl cellulose in water. The slurry was then coated onto a Cu foil current collector and dried, followed by pressing to prepare the negative electrode.
[0120] A half-cell with a theoretical capacity of 530 mAh / g was constructed using a negative electrode, a lithium counter electrode, and an electrolyte. The electrolyte was used by dissolving 1.5 M LiPF6 in a mixed solvent of ethylene carbonate, ethyl methyl carbonate, and dimethyl carbonate (volume ratio 20:10:70).
[0121] (Example 2)
[0122] The negative electrode active material was prepared by the same steps as in Example 1, except that the prepared secondary particles and mesophase carbon pitch were mixed at a weight ratio of 80:20 and heat-treated at a heating rate of 15 °C / min to prepare a negative electrode active material for lithium secondary batteries with an average particle size D50 of 8 μm.
[0123] The prepared negative electrode active material is a silicon-carbon composite with voids formed in the central portion, where only silicon nanoparticles exist. The central portion has a size (diameter) of 3.6 μm, and the prepared negative electrode active material has an average particle size D50 of 8 μm. Therefore, the radius of the central portion corresponds to 45% of the radius of the negative electrode active material.
[0124] (Compare with Example 1)
[0125] The negative electrode active material was prepared by the same steps as in Example 1, except that the prepared secondary particles and mesophase carbon pitch were mixed at a weight ratio of 60:40 and heat-treated at a heating rate of 5 °C / min to prepare a negative electrode active material for lithium secondary batteries with an average particle size D50 of 8 μm.
[0126] The prepared negative electrode active material is a silicon-carbon composite as a whole, that is, a negative electrode active material in which silicon-carbon composite exists in both the central part and the surface part and there are no voids.
[0127] (Compare with Example 2)
[0128] The negative electrode active material was prepared by the same steps as in Example 1, except that the prepared secondary particles and mesophase carbon pitch were mixed at a weight ratio of 80:20 and heat-treated at a heating rate of 5 °C / min to prepare a negative electrode active material for lithium secondary batteries with an average particle size D50 of 8 μm.
[0129] The prepared negative electrode active material is a silicon-carbon composite as a whole, that is, a negative electrode active material in which silicon-carbon composite exists in both the central part and the surface part and there are no voids.
[0130] (Compare with Example 3)
[0131] The negative electrode active material was prepared by the same steps as in Example 1, except that the prepared secondary particles and mesophase carbon pitch were mixed at a weight ratio of 72:28 and heat-treated at a heating rate of 7 °C / min to prepare a negative electrode active material for lithium secondary batteries with an average particle size D50 of 8 μm.
[0132] The prepared negative electrode active material is a silicon-carbon composite with voids formed in the central portion, where only silicon nanoparticles exist. The central portion has a size (diameter) of 1.5 μm, and the prepared negative electrode active material has an average particle size D50 of 8 μm. Therefore, the radius of the central portion corresponds to 18.8% of the radius of the negative electrode active material.
[0133] (Compare with Example 4)
[0134] The negative electrode active material was prepared by the same steps as in Example 1, except that the prepared secondary particles and mesophase carbon pitch were mixed at a weight ratio of 90:10 and heat-treated at a heating rate of 20 °C / min to prepare a negative electrode active material for lithium secondary batteries with an average particle size D50 of 8 μm.
[0135] The prepared negative electrode active material is a silicon-carbon composite with voids formed in the central portion, where only silicon nanoparticles exist. The central portion has a size (diameter) of 5.5 μm, and the prepared negative electrode active material has an average particle size D50 of 8 μm. Therefore, the radius of the central portion corresponds to 68.5% of the radius of the negative electrode active material.
[0136] Experimental Example 1) Measurement of X-ray photoelectron spectroscopy (mapping test)
[0137] X-ray photoelectron spectroscopy (XPS) measurements were performed on the negative electrode active material according to Example 1 to obtain data from the surface portion ( Figure 3 The X-axis distance in the middle is 0 μm to the center part. Figure 3 The concentrations of Si and amorphous carbon (i.e., carbon) at the X-axis distance (4 μm) are shown in the results. Figure 3 In this study, X-ray photoelectron analysis (SiO2 conversion) was performed by sputtering argon ions into the active material at a sputtering rate of 0.5 nm / min.
[0138] like Figure 3 As shown, in the negative electrode active material according to Example 1, silicon is present completely uniformly, but amorphous carbon is present very little in the central portion.
[0139] Experimental Example 2) Assessment of the capacity of active substances
[0140] The half-cells according to Example 1, as well as Comparative Examples 1, 3, and 4, were charged and discharged once at 0.1C, and then the discharge capacity was measured. The results are shown in Table 1.
[0141] Experimental Example 3) Evaluation of Initial Efficiency
[0142] The half-cells according to Example 1 and Comparative Examples 1, 3, and 4 were charged and discharged once at 0.1C, and then the charging capacity and discharging capacity were measured. The ratio of discharging capacity to charging capacity was calculated, and the results are shown in Table 1.
[0143] Experimental Example 4) Evaluation of Initial Expansion Rate
[0144] The half-cells from Example 1 and Comparative Examples 1, 3, and 4 were charged and discharged once at 0.1C. The battery thickness before and after the charge and discharge were measured, and the ratio of the battery thickness after one charge and discharge cycle to the battery thickness before the charge and discharge cycle was obtained. The results are shown in Table 1 as the initial expansion rate.
[0145] Experimental Example 5) Evaluation of Cycle Life Expansion Rate
[0146] The half-cells from Example 1 and Comparative Examples 1, 3, and 4 were charged and discharged once at 0.1C, once at 0.2C, and 50 times at 0.5C. The battery thickness after 0.2C charge / discharge and after 50 cycles at 0.5C were measured, and the ratio of the battery thickness after 50 cycles at 0.5C to that after 0.2C charge / discharge was obtained. The results are shown in Table 1 as the cycle life expansion rate.
[0147] Experimental Example 6) Capacity Retention
[0148] The half-cells of Example 1 and Comparative Examples 1, 3, and 4 were charged and discharged at 1C for 100 cycles. The discharge capacity of the first cycle and the discharge capacity of the 100th cycle were measured. The ratio of the discharge capacity of the 100th cycle to the discharge capacity of the first cycle was obtained, and the results are shown in Table 1 as the capacity retention rate.
[0149] (Table 1)
[0150]
[0151] As shown in Table 1, the negative electrode active materials of Examples 1 and 2 exhibit excellent discharge capacity and suitable initial efficiency. Furthermore, their cycle lifetime expansion rate and capacity retention remain at 30% or less and 75% or more of the substantially useful levels, respectively, and they exhibit very low initial expansion rate. In contrast, Comparative Example 1 exhibits extremely low discharge capacity and deteriorated initial expansion rate, while Comparative Example 2 exhibits surprisingly deteriorated cycle lifetime expansion rate and capacity retention rate. Additionally, Comparative Example 3 exhibits slightly lower capacity and slightly higher initial expansion rate, while Comparative Example 4 exhibits deteriorated cycle lifetime expansion rate and capacity retention rate.
[0152] While the invention has been described in conjunction with exemplary embodiments now considered practical, it will be understood that the invention is not limited to the disclosed embodiments, but rather is intended to cover various modifications and equivalent arrangements included within the spirit and scope of the appended claims. Therefore, the foregoing embodiments should be understood as illustrative and not as limiting the invention in any way.
Claims
1. A negative electrode active material for a lithium secondary battery, the negative electrode active material for the lithium secondary battery comprising: Silicon-carbon composites, with voids in the central portion, The radius of the central portion corresponds to 30% to 50% of the radius of the negative electrode active material used in the lithium secondary battery. The silicon-carbon composite comprises silicon nanoparticles and amorphous carbon. The central portion includes at least one silicon nanoparticle, and the voids are spaces that absorb the volume expansion of the negative electrode active material during charging and discharging. The silicon nanoparticles and the amorphous carbon are included in a surface portion, which refers to the region from the central portion of the negative electrode active material to its outermost surface. The negative electrode active material has a particle size of 5 μm to 20 μm. The silicon-carbon composite comprises at least one secondary particle in which silicon nanoparticles are aggregated, at least amorphous carbon located on the secondary particle, and a portion of amorphous carbon filling the spaces between the primary particles. The secondary particles have a particle size of 5 μm to 10 μm.
2. The negative electrode active material for lithium secondary batteries according to claim 1, wherein, The silicon nanoparticles have a particle size of 10 nm to 200 nm.
3. The negative electrode active material for lithium secondary batteries according to claim 1, wherein, The silicon nanoparticles are in the form of thin sheets.
4. The negative electrode active material for lithium secondary batteries according to claim 1, wherein, The silicon nanoparticles have an aspect ratio of 5 to 20.
5. The negative electrode active material for lithium secondary batteries according to claim 1, wherein, X-ray diffraction using CuKα rays revealed that the silicon nanoparticles have a full width at half maximum (FWHM) of 0.5 degrees (°) to 7 degrees (°) at the (111) plane.
6. A lithium secondary battery, the lithium secondary battery comprising: The negative electrode comprises the negative electrode active material according to any one of claims 1 to 5; Positive electrode, including positive electrode active material; as well as Non-aqueous electrolyte.
Citation Information
Patent Citations
Negative active material composite, method of preparing the same, negative electrode, and lithium battery
CN111628160A
Lithium ion battery silicon-carbon negative electrode material and preparation method thereof
CN111653738A
Negative active material for lithium secondary battery, method of preparing same, and lithium secondary battery comprising same
KR1020090109225A
Composite electrode material and method for manufacturing the same
US20190067681A1