electrode

By controlling the distribution and proportion of binder in the secondary battery electrode, the problem of insufficient adhesion between active material particles was solved, resulting in a highly stable and high-performance electrode that avoids battery performance degradation.

CN116325235BActive Publication Date: 2026-11-24LG ENERGY SOLUTION LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202180066634.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-09-28
Filing Date
2021-09-27
Publication Date
2026-11-24
Estimated Expiration
2041-09-27

AI Technical Summary

Technical Problem

In existing secondary batteries, the adhesion between active material particles and between the active material layer and the current collector is insufficient, leading to deterioration in battery stability and performance. Furthermore, increasing the proportion of binder will reduce battery performance.

Method used

By controlling the distribution of the adhesive in the active material layer, especially its concentrated distribution near the current collector surface, high interparticle adhesion and adhesion between the active material layer and the current collector are ensured. The area ratio of the adhesive to the proportion of the adhesive in the active material layer is adjusted using a standard peel test. Specific types of current collectors and adhesives are used to control particle diameter and solubility parameters.

Benefits of technology

A high level of adhesion was achieved with a low binder content, which improved the stability and performance of the electrode and avoided the problems of increased resistance and decreased conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116325235B_ABST
    Figure CN116325235B_ABST
Patent Text Reader

Abstract

This application relates to an electrode, and an electrochemical element and secondary battery including the electrode. Specifically, this application relates to an electrode comprising a current collector and an active material layer, which, compared to the binder content in the active material layer, provides an electrode capable of ensuring a high level of adhesion between particles and adhesion between the active material layer and the current collector. This application may also provide an electrochemical element and secondary battery including the electrode.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to an electrode. Background Technology

[0002] The application of energy storage technology has been expanded to mobile phones, cameras, laptops, electric vehicles, and the like.

[0003] One area of ​​research in energy storage technology is rechargeable and dischargeable secondary batteries, and research and development are underway to improve the energy density and specific energy of such secondary batteries.

[0004] Electrodes (positive or negative) used in secondary batteries are typically manufactured by forming an active material layer, including electrode active material and binder, on a current collector.

[0005] In order to successfully induce the movement of electrons between active materials and between the current collector and the active material layer in the electrodes of a secondary battery, it is necessary to ensure the adhesion between active material particles and the adhesion between the active material layer and the current collector.

[0006] In addition, when the adhesion between particles in the active material layer is insufficient, particles may detach from the electrodes, which degrades the stability and performance of the battery. For example, particles detached from the surfaces of the negative and positive electrodes due to insufficient adhesion can cause microshorts or similar issues inside the battery, which can lead to performance degradation and fire.

[0007] When the adhesion between the active material layer and the current collector decreases, the speed at which electrons move between the active material layer and the current collector decreases, which can lead to a deterioration in speed and cycle characteristics.

[0008] The adhesion between particles in the active material layer or the adhesion between the active material layer and the current collector is ensured by an adhesive.

[0009] Therefore, introducing a larger amount of adhesive into the active material layer can ensure higher adhesion.

[0010] However, in this case, the proportion of active material decreases as the proportion of binder increases, resulting in problems such as deterioration of battery performance due to increased electrode resistance, decreased conductivity, and the like. Summary of the Invention

[0011] Technical issues

[0012] This disclosure relates to an electrode. One objective of this application is to provide an electrode comprising a current collector and an active material layer, which ensures a high level of interparticle adhesion and adhesion between the active material layer and the current collector compared to the binder content in the active material layer.

[0013] Technical solution

[0014] Among the physical properties mentioned in this specification, those that affect the measurement results by temperature are measured at room temperature, unless otherwise explicitly stated.

[0015] The term room temperature refers to the natural temperature without heating or cooling, meaning, for example, any temperature in the range of 10°C to 30°C, or around 23°C or around 25°C. Otherwise, in this specification, the unit of temperature is degrees Celsius (°C) unless otherwise explicitly stated.

[0016] Among the physical properties mentioned in this specification, those that affect the measurement results under normal pressure are those measured under normal pressure, unless otherwise explicitly stated.

[0017] The term normal pressure is the natural pressure without pressurization or depressurization, which generally means about 1 atm at atmospheric pressure.

[0018] In cases where the physical properties affected by humidity are measured, the relevant physical properties are those measured under natural humidity conditions without deliberate control at room temperature and / or normal pressure.

[0019] The electrode of this application includes: a current collector; and an active material layer present on one side of the current collector. Figure 1 This is a cross-sectional view of such an electrode, showing a structure including a current collector (100) and an active material layer (200). In the electrode structure, the active material layer may be formed to contact the surface of the current collector, or another layer may exist between the current collector and the active material layer. For example, as described below, an intermediate layer may also exist between the current collector and the active material layer.

[0020] The active material layer may include at least electrode active material and binder.

[0021] By controlling the distribution of the adhesive in the active material layer, particularly in the active material layer adjacent to the current collector, this application ensures high adhesion between particles in the active material layer, and simultaneously ensures high adhesion between the active material layer and the current collector. The active material layer essentially comprises electrode active material and adhesive, with adhesion expressed by the adhesive. Therefore, to ensure adhesion, as much adhesive as possible must be placed at locations where adhesion is required.

[0022] However, for this purpose, careful consideration must be given to the affinity of the individual components in the slurry used to form the active layer, or the affinity of the individual components in the slurry to the current collector. Furthermore, controlling the position of the binder is not an easy task, as it migrates to the upper part of the active layer during electrode formation or after electrode fabrication, and this control is even more difficult when the binder content in the slurry is low. For example, as... Figure 2 As conceptually illustrated, due to the phenomenon that the adhesive (2001) present in the active material layer typically migrates to the upper part of the active material layer during and / or after the electrode manufacturing process, it is not easy to distribute the adhesive (2001) between the active material (1001) and the current collector (100). That is, among the adhesives distributed on the current collector, only a portion contributes to improving adhesion, and this tendency further increases when the proportion of this adhesive in the active material layer is small.

[0023] In this application, an electrode that can achieve excellent adhesion even with a small amount of adhesive can be provided by concentrating the adhesive in the parts where improved adhesion is required (e.g., between the surface of the current collector and the active material).

[0024] This application adjusts the area ratio of the adhesive, as confirmed by standard peel tests, to a high level compared to the amount of adhesive contained in the active material layer.

[0025] The term "adhesive area ratio" refers to the percentage (100 × A2 / A1) of the area (A2) on the current collector surface where the adhesive component is confirmed to be present after the standard peel test described below. Here, the area where the adhesive component is confirmed to be present is confirmed by FE-SEM (Field Emission Scanning Electron Microscope) analysis in the manner described in the examples. The adhesive is included in the area where the adhesive component is confirmed to be present during the confirmation process, and in some cases, other additional components (e.g., thickeners, etc.) may also be included.

[0026] In one example, the ratio (A / W) of the area occupied by the adhesive, as confirmed in the standard peel test performed on the electrode below, to the content (W) of the electrode active material in the active material layer can be 17 or greater.

[0027] That is, the electrode can satisfy the following equation 1 after the standard peel test.

[0028] [Equation 1]

[0029] 17≤A / W

[0030] In Equation 1, A is the percentage of the area occupied by the adhesive on the surface of the current collector (A2) relative to the total surface area of ​​the current collector (A1) (100×A2 / A1), and W is the adhesive content ratio in the active material layer (wt%).

[0031] Since the area ratio A in Equation 1 is in percentage (%) and the adhesive content ratio W is in weight percentage (wt%), the unit of the ratio A / W can be wt. -1 .

[0032] When the composition of the slurry in the electrode manufacturing process is known, the binder content is substantially the same as the binder content in the solids content of the relevant slurry (excluding the solvent portion). Furthermore, when the composition of the slurry in the electrode manufacturing process is unknown, the binder content can be confirmed by TGA (thermogravimetric analysis) of the active material. For example, when SBR (styrene-butadiene rubber) binder is used, the binder content can be confirmed by the SBR binder content obtained from a temperature-mass curve obtained by performing TGA analysis on the active material layer and decreasing the temperature from 370°C to 440°C at a rate of 10°C per minute.

[0033] In another example, the ratio A / W can be 17.5 or greater, 18 or greater, 18.5 or greater, 19 or greater, 19.5 or greater, 20 or greater, 20.5 or greater, 21 or greater, 21.5 or greater, 22 or greater, 22.5 or greater, 23 or greater, 23.5 or greater, 24 or greater, 24.5 or greater, 25 or greater, or 25.5 or greater, or it can also be 50 or less, 49 or less, 48 ​​or less, 47 or less, or 46 or less. 45 or smaller, 44 or smaller, 43 or smaller, 42 or smaller, 41 or smaller, 40 or smaller, 39 or smaller, 38 or smaller, 37 or smaller, 36 or smaller, 35 or smaller, 34 or smaller, 33 or smaller, 32 or smaller, 31 or smaller, 30 or smaller, 29 or smaller, 28 or smaller, 27 or smaller, 26 or smaller, 25 or smaller, 24 or smaller, 23 or smaller, 22 or smaller, 21 or smaller, 20 or smaller, 19 or smaller, or around 18 or smaller.

[0034] This A / W ratio provides electrodes that ensure a higher level of adhesion compared to the applied adhesive.

[0035] In this application, the A / W ratio can be achieved by controlling the composition of the slurry (e.g., the affinity of the solvent and binder), the affinity of each component in the slurry to the current collector surface, and / or the average particle diameter of the particulate matter in the slurry.

[0036] In this specification, the average particle diameter of the particulate material is the so-called D50 particle diameter or median diameter obtained by laser diffraction, and the method for obtaining this particle diameter is described in the embodiments. Furthermore, for example, when the active material layer is a rolled layer, the average particle diameter mentioned herein for the particulate binder and particulate active material used in the active material layer is the average particle diameter before rolling, unless otherwise explicitly stated.

[0037] In addition, in one example, when two types of particulate binders (or electrode active materials) with different average particle diameters are present in the active material layer, the average particle diameter, taking into account the weight fraction of the two types of particulate binders, can be defined as the average particle diameter of the particulate binder (or electrode active material). For example, when a particulate binder (or electrode active material) with an average particle diameter of D1 is present at a weight of W1, and a particulate binder (or electrode active material) with an average particle diameter of D2 is present at a weight of W2, the average particle diameter D can be defined as D = (D1 × W1 + D2 × W2) / (W1 + W2). In the above confirmation, the particle diameters D1 and D2, and the weights W1 and W2 are values ​​with the same units.

[0038] The standard peel test was performed using 3M Scotch® Magic™ Tape Cat. 810R. To perform the standard peel test, the electrodes were first cut to approximately 20 mm wide and 100 mm long. The Scotch® Magic™ Tape Cat. 810R was also cut to a horizontal length of 10 mm and a vertical length of 60 mm. After that, as... Figure 4As shown, Scotch® Magic™ tape Cat. 810R (300) is attached to the active material layer (200) of the electrode in a cross-attachment configuration. During this attachment, a standard peel test is performed so that a specific portion of the Scotch® Magic™ tape Cat. 810R (300) protrudes. This protruding portion is then held in place, and the Scotch® Magic™ tape Cat. 810R (300) is peeled off. There are no particular limitations on the peel rate and peel angle, but the peel rate can be approximately 20 mm / sec, and the peel angle can be approximately 30 degrees. Furthermore, regarding the attachment of the Scotch® Magic™ tape Cat. 810R (300), once the tape is attached, it is attached by reciprocating and pushing the surface of the tape with a roller weighing approximately 1 kg and having a radius and width of 50 mm and 40 mm, respectively.

[0039] Through the above process, when Scotch® Magic™ Tape Cat. 810R is peeled off, the components of the active material layer (200) are peeled off along with Scotch® Magic™ Tape Cat. 810R (300). Subsequently, the above process is repeated using new Scotch® Magic™ Tape Cat. 810R (300).

[0040] The standard peel test can be performed by performing this process until the components of the active material layer (200) have not detached from the Scotch® Magic™ tape Cat. 810R (300) and are therefore not observed.

[0041] Regarding the fact that components without the active material layer (200) have detached from Scotch® Magic™ tape Cat. 810R (300), it can be confirmed that the active material layer components have not detached when the surface of the Scotch® Magic™ tape from which the active material layer has been peeled off is compared with the surface of the unused Scotch® Magic™ tape and the two are substantially the same in color (visual observation).

[0042] The specific methods for enabling standard peel testing are described in the embodiments.

[0043] After the above standard peel test, the area occupied by the adhesive on the current collector can be confirmed.

[0044] There are no particular limitations on the type of current collector used in this application, and known current collectors may be used. To achieve the aforementioned A / W ratio, the surface characteristics of the current collector (water contact angle, etc.) can be controlled, as described below. For example, current collectors can be made of stainless steel, aluminum, nickel, titanium, calcined charcoal, copper, carbon, stainless steel surface-treated with nickel, titanium, or silver, aluminum-cadmium alloys, and the like, in the form of films, sheets, or foils. To achieve the desired network and blank areas, a current collector with the surface characteristics described below can be selected, or these surface characteristics can be adjusted through additional processing.

[0045] There are no particular restrictions on the thickness and shape of the current collector, or similar types, and a suitable shape can be selected within the known range.

[0046] The active material layer formed on the current collector includes electrode active material and binder.

[0047] Materials are known to be usable as adhesives, and components known to facilitate the bonding of components such as the active material in the active material layer and the bonding of the active material layer to the current collector can be used. As applicable adhesives, a selection from PVDF (polyvinylidene fluoride), PVA (polyvinyl alcohol), polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, SBR (styrene-butadiene rubber), fluororubber, and other known adhesives, or combinations of both or more thereof, can be used.

[0048] To form appropriate network areas, it is suitable to use granular adhesive as a binder.

[0049] When particulate materials are used as electrode active materials, the ratio of particle diameter between the particulate binder and the electrode active material layer can be controlled in order to control the distribution of the binder in the electrode active material layer.

[0050] For example, the ratio (D1 / D2) of the average particle diameter (D1, in nm) of the particulate electrode active material to the average particle diameter (D2, in nm) of the particulate binder can range from 10 to 1,000. In another example, the ratio (D1 / D2) can be 20 or greater, 30 or greater, 40 or greater, 50 or greater, 60 or greater, 70 or greater, 80 or greater, 90 or greater, 100 or greater, 110 or greater, 120 or greater, or 130 or greater, or it can be around 900 or less, 800 or less, 700 or less, 600 or less, 500 or less, 400 or less, 300 or less, 200 or less, or 150 or less.

[0051] Here, the adhesive may have an average particle diameter (D2) in the range of 50 nm to 500 nm. In another example, the average particle diameter (D2) of the adhesive may be about 70 nm or greater, about 90 nm or greater, about 110 nm or greater, about 130 nm or greater, or about 140 nm or greater, or it may be about 480 nm or less, about 460 nm or less, about 440 nm or less, about 420 nm or less, about 400 nm or less, about 380 nm or less, about 360 nm or less, about 340 nm or less, about 320 nm or less, about 300 nm or less, about 280 nm or less, about 260 nm or less, about 240 nm or less, about 220 nm or less, about 200 nm or less, about 180 nm or less, or about 160 nm or less.

[0052] Here, the electrode active material may have an average particle diameter (D1) in the range of 1 μm to 100 μm. In another example, the average particle diameter (D1) may be about 3 μm or greater, about 5 μm or greater, about 7 μm or greater, about 9 μm or greater, about 11 μm or greater, about 13 μm or greater, about 15 μm or greater, about 17 μm or greater, or about 19 μm or greater, or it may be about 90 μm or less, 80 μm or less, 70 μm or less, 60 μm or less, 50 μm or less, 40 μm or less, 30 μm or less, or about 20 μm or less.

[0053] The average particle diameters D1 and D2 are the average particle diameters of their respective materials in the slurry used to prepare the active material layer. Therefore, when the actual electrode is manufactured through a rolling process, there may be slight differences between the average particle diameters D1 and D2 of the respective components identified in the active material layer.

[0054] The reason is unclear, but it is expected that the dispersion state of the adhesive at the desired location can be achieved in the slurry during the electrode manufacturing process through this particle diameter ratio, and the migration of the adhesive is also properly controlled.

[0055] In addition, in order to form a suitable network region, it may be advantageous to use an adhesive having a solubility parameter within the range to be described below.

[0056] In this application, a high level of adhesion can be ensured while using a relatively small proportion of adhesive in the active material layer. For example, the proportion of adhesive in the active material layer can be from about 0.5% to about 10% by weight. In another example, this proportion can also be further controlled within the range of about 1% or more, 1.5% or more, 2% or more, 2.5% or more, 3% or more, 3.5% or more, or 4% or more and / or within the range of about 9.5% or less, 9% or less, 8.5% or less, 8% or less, 7.5% or less, 7% or less, 6.5% or less, 6% or less, 5.5% or less, 5% or less, or 4.5% or less.

[0057] The electrode active material included in the active material layer can be either a positive electrode active material or a negative electrode active material, and there are no particular restrictions on the specific type. For example, as a positive electrode active material, materials including LiCoO2, LiNiO2, LiMn2O4, LiCoPO4, LiFePO4, and LiNi can be used. 1-x-y-z Co x M1 y M2 z O2 (M1 and M2 are each independently selected from any one of the group consisting of Al, Ni, Co, Fe, Mn, V, Cr, Ti, W, Ta, Mg, and Mo, x, y, and z are each independently the atomic fractions of the constituent elements of the oxide, satisfying 0 ≤ x < 0.5, 0 ≤ y < 0.5, 0 ≤ z < 0.5, 0 < x + y + z ≤ 1), and similar active materials, and as negative electrode active materials, can include natural graphite, artificial graphite, carbonaceous materials; lithium-containing titanium composite oxide (LTO), Si, Sn, Li, Zn, Mg, Cd, Ce, Ni, or Fe metal (Me); alloys composed of metal (Me); oxides of metal (Me) (MeOx); and composites of metal (Me) and carbon, and similar active materials.

[0058] In this application, a relatively high proportion of active material can be maintained in the active material layer while ensuring excellent adhesion.

[0059] For example, the active material in the active material layer may be in the range of 1,000 parts by weight to 10,000 parts by weight relative to 100 parts by weight of the adhesive. In another example, the proportion could be 1500 parts by weight or more, 2000 parts by weight or more, 2500 parts by weight or more, 3000 parts by weight or more, 3500 parts by weight or more, 4000 parts by weight or more, or 4500 parts by weight or more, or it could be 9500 parts by weight or less, 9000 parts by weight or less, 8500 parts by weight or less, 8000 parts by weight or less, 7500 parts by weight or less, 7000 parts by weight or less, 6500 parts by weight or less, 6000 parts by weight or less, 5500 parts by weight or less, 5000 parts by weight or less, 4500 parts by weight or less, 4000 parts by weight or less, 3500 parts by weight or less, 3000 parts by weight or less, or about 2500 parts by weight or less.

[0060] In addition to the components mentioned above, the active material layer may further include other necessary components. For example, the active material layer may further include a conductive material. As a conductive material, for example, known components may be used without any particular limitation, as long as they exhibit conductivity without causing chemical changes in the current collector and electrode active materials. For example, as a conductive material, graphite selected from natural or artificial graphite; carbon black such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lampblack, or summer black; conductive fibers such as carbon fibers or metal fibers; fluorinated carbon powder; metal powders such as aluminum powder or nickel powder; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; polyphenylene derivatives; and mixtures of one or more of the like.

[0061] The content of conductive material is controlled where necessary and is not particularly limited, but it is generally included in an appropriate proportion in the range of 0.1 parts by weight to 20 parts by weight or 0.3 parts by weight to 12 parts by weight relative to 100 parts by weight of active material. Methods for determining the content of conductive material to an appropriate level taking into account the cycle life of the battery and the like are known.

[0062] In addition to the components mentioned above, the active material layer may also include other necessary and known components (e.g., thickeners such as carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, or regenerated cellulose).

[0063] There are no particular limitations on the thickness of the active material layer; it can be controlled to an appropriate level to take into account the desired performance.

[0064] For example, the thickness of the active material layer can range from about 10 μm to 500 μm. In another example, the thickness can be about 30 μm or more, 50 μm or more, 70 μm or more, 90 μm or more, or about 100 μm or more, or it can be about 450 μm or less, 400 μm or less, 350 μm or less, 300 μm or less, 250 μm or less, 200 μm or less, or about 150 μm or less.

[0065] The active material layer can be formed to have a specific level of porosity. Porosity is typically controlled by rolling during the electrode manufacturing process. The active material layer may have a porosity of approximately 35% or less. This porosity can also be further adjusted within the ranges of 33% or less, 31% or less, 29% or less, or 27% or less and / or within the ranges of 5% or more, 7% or more, 9% or more, 11% or more, 13% or more, 15% or more, 17% or more, 19% or more, 21% or more, 23% or more, or 25% or more. Controlling the rolling process to have this porosity helps to form the desired network and blank areas in this application, as described below. Here, porosity is a value calculated by comparing the ratio of the actual density of the active material layer to the density after rolling, and methods for calculating the porosity of the active material layer in this way are known.

[0066] In order to achieve proper binder distribution during electrode manufacturing, an additional layer may be present to control the surface properties of the current collector.

[0067] For example, an intermediate layer including silane compounds may exist between the active material layer in the electrode and the current collector.

[0068] At this point, there are no particular restrictions on the type of intermediate layer, as long as it can achieve the surface characteristics of the current collector to be described below.

[0069] For example, the intermediate layer may be a layer comprising a silane compound of Formula 1.

[0070] [Formula 1]

[0071]

[0072] In Formula 1, R1 is an alkyl group having 6 or fewer carbon atoms or an alkenyl group having 6 or fewer carbon atoms, wherein the alkyl group of R1 may be selectively substituted with one or more amino groups, and R2 to R4 are each independently an alkyl group having 1 to 4 carbon atoms.

[0073] The alkyl or alkenyl group in Formula 1 can be linear, branched, or cyclic, and in suitable examples, it can be a linear alkyl or alkenyl group.

[0074] In one example, R1 in Formula 1 may be a straight-chain alkyl group having 1 to 6 carbon atoms, 1 to 4 carbon atoms, or 2 to 4 carbon atoms, or a straight-chain alkenyl group having 2 to 6 carbon atoms, 2 to 4 carbon atoms, or 2 to 4 carbon atoms, or a straight-chain aminoalkyl group having 1 to 6 carbon atoms, 1 to 4 carbon atoms, or 2 to 4 carbon atoms.

[0075] The intermediate layer may include silane compounds as a major component, wherein, for example, the content of silane compounds in the intermediate layer may be approximately 70% by weight or more, 75% by weight or more, 80% by weight or more, 85% by weight or more, 90% by weight or more, or 95% by weight or more. The upper limit for the content of silane compounds in the intermediate layer is 100% by weight. When components other than silane compounds are present in the intermediate layer, these components may be components such as solvents used in the formation of the intermediate layer, or they may be components of the active material layer that have been reduced from the active material layer.

[0076] The thickness of the intermediate layer can be appropriately set with reference to the desired surface properties, for example, it can be in the range of about 0.5 μm to 50 μm.

[0077] In another example, the thickness could be about 1 μm or more, 3 μm or more, 5 μm or more, 7 μm or more, or about 9 μm or more, or it could be about 45 μm or less, 40 μm or less, 35 μm or less, 30 μm or less, 25 μm or less, 20 μm or less, or about 15 μm or less.

[0078] The electrodes described above can be manufactured in the manner described below. Generally, electrodes are manufactured by coating a slurry onto a current collector, drying it, and then performing a rolling process. In this application, desired network areas and blank areas can be formed by controlling the composition of the slurry, the surface characteristics of the current collector on which the slurry is coated, the drying conditions, and / or the rolling conditions during the above process.

[0079] For example, in the manufacturing process of this application, as a slurry, a relatively water-conducting binder (appropriately a particulate binder having a specific average particle diameter while being relatively hydrophobic) can be dispersed in a certain amount in a relatively polar solvent. This slurry is coated onto a current collector whose surface properties are controlled, as described below. The reason is unclear, but when this slurry is coated onto the current collector, it is expected that the dispersion state of the binder in the slurry, the affinity between the solvent of the slurry and the surface of the current collector, the affinity between the surface of the current collector and the binder in the slurry, and / or, in the case of particulate materials, the particle diameter relationship therebetween can be combined to control the position of the binder with the desired shape.

[0080] For example, the affinity between the solvent and the current collector surface affects the contact angle of the solvent on the current collector surface, where the contact angle can form forces in a specific direction in the slurry due to capillary action or the like during solvent evaporation. The affinity between the binder and the solvent and the amount of binder (i.e., the particle diameter in the case of particulate binders) affect the dispersion state of the binder in the slurry, and the affinity between the binder and the current collector surface affects the dispersion state of the binder in the slurry, or the shape of the binder distribution on the current collector surface, and the like.

[0081] In this application, it has been confirmed that the desired adhesive arrangement is achieved through the dispersion state of the adhesive and the evaporation of the solvent when a slurry of the composition described below is formed on a current collector having the surface properties described below, and the shear force in the slurry generated therefrom.

[0082] For example, the slurry used in this manufacturing process may include a solvent. As a solvent, one that can suitably disperse slurry components such as electrode active materials is typically used, and examples of such solvents include water, methanol, ethanol, isopropanol, acetone, dimethyl sulfoxide, formamide, and / or dimethylformamide, and the like.

[0083] In this application, it may be necessary to use a solvent with a dipole moment of approximately 1.3 D or greater. In another example, the dipole moment of the solvent can be further controlled within the range of approximately 1.35 D or greater, 1.4 D or greater, 1.45 D or greater, 1.5 D or greater, 1.55 D or greater, 1.6 D or greater, 1.65 D or greater, 1.7 D or greater, 1.75 D or greater, 1.8 D or greater, or approximately 1.85 D or greater and / or approximately 5 D or less, 4.5 D or less, 4 D or less, 3.5 D or less, 3 D or less, 2.5 D or less, 2 D or less, or approximately 1.9 D or less. The dipole moment of the solvent is known for each solvent.

[0084] As a binder included in the slurry, an appropriate type of binder from the aforementioned categories can be selected and used. To achieve the desired dispersion state in the solvent, it may be necessary to use a binder with a strength of approximately 10 MPa. 1 / 2 up to 30 MPa 1 / 2 The adhesive is used as a binder with a solubility parameter. In another example, this solubility parameter could be 11 MPa. 1 / 2 or larger, 12 MPa 1 / 2 Or larger, 13 MPa 1 / 2 Or larger, 14 MPa 1 / 2 or larger, 15 MPa 1 / 2 Or larger, or 16 MPa 1 / 2 Or larger, or it could be 28 MPa 1 / 2 or smaller, 26 MPa 1 / 2 or smaller, 24 MPa 1 / 2 or smaller, 22 MPa 1 / 2 or smaller, 20 MPa 1 / 2 Or smaller, or 18 MPa 1 / 2 Or even smaller. The solubility parameter of this adhesive can be confirmed by literature (e.g., Yanlong Luo et al., 2017, etc.). For example, among the types of adhesives mentioned above, those with this solubility parameter can be selected.

[0085] Particulate adhesives can be used as adhesives, and for example, particulate adhesives having an average particle diameter within the range mentioned above can be used.

[0086] The binder content in the slurry can be controlled with regard to the desired dispersion state. For example, the binder can be included in the slurry such that the binder concentration relative to the solvent (=100×B / (B+S), where B is the weight (g) of the binder in the slurry and S is the weight (g) of the solvent in the slurry) is about 0.1% to 10%. In another example, the concentration can be 0.5% or more, 1% or more, 1.5% or more, 2% or more, 2.5% or more, 3% or more, or 3.5% or more, or it can be about 9% or less, 8% or less, 7% or less, 6% or less, 5% or less, 4% or less, 3% or less, or 2.5% or less.

[0087] In addition to the components mentioned above, the slurry may include an electrode active material. As the electrode active material, a suitable type can be selected from the types described above, and considering its contribution to the desired dispersion state, an electrode active material in particulate form with an average particle diameter (D50 particle diameter) within the range described above and a ratio to the average particle diameter of the binder within the range described above can be used.

[0088] The proportion of electrode active materials in the slurry can be adjusted to achieve the desired proportion of electrode active materials in the active material layer.

[0089] In addition to the components mentioned above, the slurry may also include other components such as the conductive materials, thickeners, and similar components, depending on the purpose.

[0090] This slurry can be applied to the surface of the current collector. There are no particular limitations on the coating method used in this process, and known coating methods can be applied, such as spin coating, comma coating, or bar coating.

[0091] The surface characteristics of the current collector with applied slurry can be controlled.

[0092] For example, the surface of the current collector to which the slurry is applied may have a water contact angle of 50 degrees or greater. In another example, the water contact angle may be further controlled within the range of approximately 100 degrees or less, 95 degrees or less, 90 degrees or less, 85 degrees or less, 80 degrees or less, or 75 degrees or less and / or within the range of approximately 55 degrees or greater, 60 degrees or greater, 65 degrees or greater, 70 degrees or greater, 75 degrees or greater, 85 degrees or greater, or 90 degrees or greater.

[0093] For example, the surface of the current collector to which the slurry is applied may have a DM (diiodomethane) contact angle of 30 degrees or greater. In another example, the DM contact angle may be further controlled within the range of approximately 70 degrees or less, 65 degrees or less, 60 degrees or less, 55 degrees or less, 50 degrees or less, or 45 degrees or less and / or within the range of approximately 35 degrees or greater, 40 degrees or greater, 45 degrees or greater, 50 degrees or greater, 55 degrees or greater, or 60 degrees or greater.

[0094] For example, the surface of a current collector to which the slurry is applied may have a surface energy of 65 mN / m or less. This surface energy may be 60 mN / m or less, 55 mN / m or less, 50 mN / m or less, 45 mN / m or less, 40 mN / m or less, 35 mN / m or less, or around 30 mN / m or less, or it may be 25 mN / m or more, 27 mN / m or more, or around 29 mN / m or more.

[0095] For example, the surface of the current collector to which the slurry is applied may have a dispersion energy of less than 45 mN / m. In another example, the dispersion energy may be 40 mN / m or less, 35 mN / m or less, or about 30 mN / m or less, or about 23 mN / m or more, 25 mN / m or more, or about 27 mN / m or more.

[0096] For example, the surface of a current collector with applied slurry can have a polarity of 20 mN / m or less. In another example, the dispersion energy could be 18 mN / m or less, 16 mN / m or less, 14 mN / m or less, 12 mN / m or less, 10 mN / m or less, 8 mN / m or less, 6 mN / m or less, 4 mN / m or less, 2 mN / m or less, or 1.5 mN / m or less, or it could be 0.5 mN / m or more, 1 mN / m or more, 1.5 mN / m or more, 2 mN / m or more, 2.5 mN / m or more, 3 mN / m or more, 3.5 mN / m or more, 4 mN / m or more, 4.5 mN / m or more, 5 mN / m or more, 5.5 mN / m or more, 6 mN / m or more, 6.5 mN / m or more, or around 7 mN / m or more.

[0097] Here, surface energy, dispersion energy, and polar energy are physical quantities that can be obtained by the OWRK (Owens-Wendt-Rabel-Kaelble) method based on the water contact angle and DM contact angle.

[0098] The desired active material layer can be obtained by applying the slurry mentioned above to a current collector surface that satisfies at least one, two or more, or all of the surface properties described above.

[0099] Among the aforementioned current collectors, one can select a current collector that exhibits the water contact angle and the like. However, there are cases where the current collector does not normally meet the aforementioned characteristics, and surface treatment can still be performed to meet the desired surface characteristics.

[0100] For example, the surface properties can be satisfied by forming the aforementioned intermediate layer on the surface of the current collector, or by applying other known treatments such as plasma treatment (in particular, hydrophobic treatment).

[0101] The intermediate layer can be prepared, for example, using a coating solution in which the aforementioned silane compound is dispersed in a solvent, by a process of coating, annealing, washing, and drying. In addition, various treatment methods, such as plasma treatment, for controlling the surface properties of current collectors are known.

[0102] After the slurry is applied to the current collector surface where its surface properties are controlled, a drying process can be performed. There are no particular limitations on the conditions for performing the drying process, but adjusting the drying temperature within the range of approximately 150°C to 400°C may be suitable, taking into account the desired location of the adhesive and the like. In another example, the drying temperature may be approximately 170°C or greater, 190°C or greater, 210°C or greater, or around 225°C or greater, or it may be around 380°C or less, 360°C or less, 340°C or less, 320°C or less, 300°C or less, 280°C or less, 260°C or less, or around 240°C or less.

[0103] The drying time can also be adjusted taking into account the dispersion state, which takes into account the desired location of the adhesive and the like, and for example, it can be adjusted in the range of about 10 seconds to 200 seconds. In another example, the time can also be further controlled in the range of 20 seconds or more, 30 seconds or more, 40 seconds or more, 50 seconds or more, 60 seconds or more, 70 seconds or more, 80 seconds or less, or 85 seconds or more and / or in the range of about 190 seconds or less, 180 seconds or less, 170 seconds or less, 160 seconds or less, 150 seconds or less, 140 seconds or less, 130 seconds or less, 120 seconds or less, 110 seconds or less, 100 seconds or less, or 95 seconds or less.

[0104] After the drying process, a rolling process can be performed. In this case, the position of the binder and the like can even be adjusted by the rolling conditions (e.g., the pressure during rolling).

[0105] For example, the porosity of the slurry (active material layer) produced by rolling is approximately 35% or less. Desired network and blank areas can be effectively formed by applying pressure or the like during rolling to achieve this porosity. In another example, the porosity can also be further controlled within the ranges of 33% or less, 31% or less, 29% or less, or 27% or less and / or within the ranges of 5% or more, 7% or more, 9% or more, 11% or more, 13% or more, 15% or more, 17% or more, 19% or more, 21% or more, 23% or more, or 25% or more.

[0106] The thickness of the rolled slurry (i.e., the active material layer) is within the range of the active material layer thickness described above.

[0107] During the manufacturing process of the electrode in this application, in addition to slurry coating, drying, and rolling, necessary additional processes (e.g., cutting processes, etc.) may also be performed.

[0108] This application also relates to an electrochemical element including such an electrode, for example, a secondary battery.

[0109] The electrochemical element may include the electrode as a positive and / or negative electrode. There are no particular limitations on other configurations or manufacturing methods of the electrochemical element, provided that the electrode of this application is used as a negative and / or positive electrode, and known methods can be applied.

[0110] Beneficial effects

[0111] This application discloses an electrode comprising a current collector and an active material layer, wherein the amount of binder in the active material layer provides an electrode capable of ensuring a high level of interparticle adhesion and adhesion between the active material layer and the current collector. Attached Figure Description

[0112] Figure 1 This is a cross-sectional view of an exemplary electrode of this application.

[0113] Figure 2 This is a conceptual diagram of the formation state of the active material layer in existing technology.

[0114] Figure 3 This is a conceptual diagram of the state of performing standard stripping tests.

[0115] Figures 4 to 9 These are FE-SEM images of the current collector surface of Examples 1 to 6, respectively.

[0116] Figures 10 to 12 These are FE-SEM images of the current collector surfaces of Comparative Examples 1 to 3, respectively.

[0117] [Explanation of reference numerals in the attached diagram]

[0118] 100: Current collector

[0119] 200: Active material layer

[0120] 300: Scotch® Magic™ Tape

[0121] 1001: Electrode Active Materials

[0122] 2001: Adhesives Detailed Implementation

[0123] The present application will be described in more detail below with reference to embodiments and comparative examples, but the scope of the present application is not limited to the embodiments described below.

[0124] 1. Measurement of contact angle and surface energy

[0125] Contact angle and surface energy were measured using a KRUSS droplet shape analyzer (manufacturer: KRUSS, trade name: DSA100). 3 μL of water or DM (diiodomethane) droplets fell at a rate of approximately 3 μL / sec, and their respective contact angles were measured using the tangent angle method. Surface energy, disperse energy, and polar energy were calculated using the OWRK (Owens-Wendt-Rabel-Kaelble) method based on the contact angles of water and DM, respectively.

[0126] 2. Standard peel test

[0127] Standard peel tests were performed using 3M Scotch® Magic™ tape Cat. 810R. Electrodes prepared in the examples and comparative examples were each cut into pieces approximately 20 mm wide and 100 mm long to obtain samples. Scotch® Magic™ tape Cat. 810R was attached to the active material layer of the obtained samples by reciprocating and pushing a roller with a weight of approximately 1 kg, a radius of 50 mm, and a width of 40 mm. At this time, Scotch® Magic™ tape was cut into pieces approximately 10 mm wide and 60 mm long, and used as described above. Figure 3As shown, Scotch® Magic™ tape and the electrode active material layer are attached in an interlaced pattern to a length of approximately 20 mm, and the protruding portion is held and peeled off. At this point, the peeling rate and peeling angle are set to a speed of approximately 20 mm / sec and an angle of approximately 30 degrees. Replace and use a new Scotch® Magic™ tape each time it is peeled off. Repeat the above process until no components of the active material layer detach from the surface of the Scotch® Magic™ tape. Visually inspect for detachment of the active material layer components, and determine that no detachment of the active material layer components has occurred when the hue has not substantially changed compared to the unused hue.

[0128] 3. Confirmation of the area occupied by the adhesive

[0129] Following the standard peel test, the adhesive-occupied area on the current collector surface was confirmed. After the standard peel test, the current collector surface was photographed at 500x magnification using a FE-SEM (Field Emission Scanning Electron Microscope) device (manufacturer: HITACHI, trade name: S4800). Using the Trainable Weka Segmentation Plug-in of ImageJ software (manufacturer: ImageJ), the current collector surface was divided into areas where the adhesive was not observed and areas where the current collector surface was observed, and the adhesive-occupied area was measured based on these areas. In the above process, based on brightness, portions satisfying a brightness of 80 or less, and portions with a brightness of 160 or greater due to the height within the closed surface formed by the relevant portions, were defined as portions occupied by the adhesive, and other areas were designated as areas without adhesive.

[0130] 4. Confirmation of the average particle diameter (D50 particle diameter) of the particulate binder and electrode active material

[0131] The average particle diameter (D50 particle diameter) of the particulate binder and electrode active material was measured using a Marvern MASTERSIZER 3000 instrument according to ISO-13320 standard. Water was used as the solvent during the measurement. When the particulate binder or similar material is dispersed in the solvent and irradiated with a laser, the laser light is scattered by the binder dispersed in the solvent, and the intensity and directionality of the scattered laser light change with the particle size. These can be analyzed using Mie theory to obtain the average diameter. Through the above analysis, a cumulative curve of the volume-based particle size distribution was obtained by converting it into the diameter of spheres with the same volume as the dispersed binder, and the particle diameter at the 50% cumulative point of this curve (median diameter) was designated as the average particle diameter (D50 particle diameter).

[0132] 4. Measurement of adhesion force

[0133] After rolling, the electrodes were cut to a width of approximately 20 mm, and the adhesion force was measured using a known method for measuring the adhesion force of the active material layer. During the adhesion force measurement, the peel angle was 90 degrees, and the peel rate was approximately 5 mm / sec. After measurement, the stabilized portion of the peak was averaged and defined as the adhesion force.

[0134] Example 1

[0135] Copper foil (Cu foil) is used as a current collector and, after its surface properties are adjusted in the following manner, it is applied to the manufacture of electrodes.

[0136] First, a coating solution containing ethyltrimethoxysilane at a concentration of approximately 1% by weight in ethanol as a solvent is applied to the surface of a copper foil using a bar coater to a thickness of approximately 10 μm. After coating, the solution is annealed at 100°C for approximately 5 minutes, washed with ethanol, and then dried again at 100°C for approximately 5 minutes to form a silane coating. The silane coating has a surface energy of approximately 29.7 mN / m, a dispersion energy of approximately 28.3 mN / m, and a polar energy of approximately 1.4 mN / m. Additionally, the water contact angle is approximately 95 degrees, and the DM contact angle is approximately 60.4 degrees.

[0137] The slurry was prepared by mixing water, SBR (Styrene-Butadiene Rubber) binder, thickener (CMC, carboxymethyl cellulose), electrode active material (1) (artificial graphite (GT), average particle diameter (D50 particle diameter): 20 μm) and electrode active material (2) (natural graphite (PAS), average particle diameter (D50 particle diameter): 15 μm) in a weight ratio of 51:2:0.6:37.1:9.3 (water:SBR:CMC:active material (1):active material (2)). Here, water is a solvent with a dipole moment of approximately 1.84 D, and the SBR binder has a dipole moment of approximately 16.9 MPa. 1 / 2 The solubility parameters of this SBR adhesive are approximately [value missing]. The solubility parameters of this SBR adhesive are the values ​​described in Yanlong Luo et al., 2017. Furthermore, this SBR adhesive is a particulate adhesive with an average particle diameter (D50 particle diameter, median particle diameter) of approximately 150 nm.

[0138] The slurry was applied to the surface of the silane coating to a thickness of approximately 280 μm using a gap coating method and dried at a temperature of approximately 230°C for approximately 90 seconds. After drying, a slurry layer with a thickness of approximately 180 μm was obtained. The dried slurry layer was then rolled using a conventional electrode rolling mill to achieve a final thickness of approximately 110 μm and a porosity of approximately 26%, thereby forming the active material layer.

[0139] The porosity of the active material layer is calculated by comparing the ratio of the actual density to the density after rolling. In addition, when considering the slurry composition, the SBR binder content in the electrode's active material layer is approximately 4% by weight, and the electrode active material (GT+PAS) ​​content is approximately 95% by weight.

[0140] Example 2

[0141] Copper foil (Cu foil) is used as a current collector and, after its surface properties are adjusted in the following manner, it is applied to the manufacture of electrodes.

[0142] A coating solution containing allyltrimethoxysilane at a concentration of approximately 1% by weight in ethanol as a solvent was applied to the surface of a copper foil using a bar coater to a thickness of approximately 10 μm. After coating, the solution was annealed at 100°C for approximately 5 minutes, washed with ethanol, and then dried again at 100°C for approximately 5 minutes to form a silane coating. The silane coating has a surface energy of approximately 30.6 mN / m, a dispersion energy of approximately 29.5 mN / m, and a polar energy of approximately 1.1 mN / m. Furthermore, the water contact angle is approximately 95.8 degrees, and the DM contact angle is approximately 58.4 degrees.

[0143] Subsequently, the same slurry used in Example 1 was applied to the surface of the silane coating to a thickness of approximately 280 μm using a gap coating method, and dried at a temperature of approximately 230°C for approximately 90 seconds. After drying, a slurry layer with a thickness of approximately 180 μm was obtained, and the dried slurry layer was rolled using a conventional electrode rolling mill to achieve a final thickness of approximately 110 μm and a porosity of approximately 26%, thereby forming an active material layer.

[0144] The method for calculating the porosity of the active material layer, as well as the content of SBR binder in the active material layer of the electrode and the content of electrode active material, are the same as in Example 1.

[0145] Example 3

[0146] Copper foil (Cu foil) is used as a current collector and, after its surface properties are adjusted in the following manner, it is applied to the manufacture of electrodes.

[0147] A coating solution containing 3-aminopropyltrimethoxysilane at a concentration of approximately 1% by weight in ethanol as a solvent was applied to the surface of a copper foil using a bar coater to a thickness of approximately 10 μm. After coating, the solution was annealed at 100°C for approximately 5 minutes, washed with ethanol, and then dried again at 100°C for approximately 5 minutes to form a silane coating. The silane coating has a surface energy of approximately 28.3 mN / m, a dispersion energy of approximately 27.1 mN / m, and a polar energy of approximately 1.2 mN / m. Additionally, the water contact angle is approximately 96.8 degrees, and the DM contact angle is approximately 62.6 degrees.

[0148] Subsequently, the same slurry used in Example 1 was applied to the surface of the silane coating to a thickness of approximately 280 μm using a gap coating method, and dried at a temperature of approximately 230°C for approximately 90 seconds. After drying, a slurry layer with a thickness of approximately 180 μm was obtained, and the dried slurry layer was rolled using a conventional electrode rolling mill to achieve a final thickness of approximately 110 μm and a porosity of approximately 26%, thereby forming an active material layer.

[0149] The method for calculating the porosity of the active material layer, as well as the content of SBR binder in the active material layer of the electrode and the content of electrode active material, are the same as in Example 1.

[0150] Example 4

[0151] Copper foil (Cu foil) whose surface properties are controlled in the same manner as in Example 1 is used as a current collector.

[0152] The slurry was prepared by mixing water, SBR (Styrene-Butadiene Rubber) binder, thickener (CMC, carboxymethyl cellulose), electrode active material (1) (artificial graphite (GT), average particle diameter (D50 particle diameter): 20 μm) and electrode active material (2) (natural graphite (PAS), average particle diameter (D50 particle diameter): 15 μm) in a weight ratio of 48.5:1:0.5:45:5 (water:SBR:CMC:active material (1):active material (2)). Here, water is a solvent with a dipole moment of approximately 1.84 D, and the SBR binder has a dipole moment of approximately 16.9 MPa. 1 / 2The solubility parameters of this SBR adhesive are approximately [value missing]. The solubility parameters of this SBR adhesive are the values ​​described in Yanlong Luo et al., 2017. Furthermore, this SBR adhesive is a particulate adhesive with an average particle diameter (D50 particle diameter, median particle diameter) of approximately 150 nm.

[0153] The slurry was applied to the surface of the silane coating to a thickness of approximately 280 μm using a gap coating method and dried at a temperature of approximately 230°C for approximately 90 seconds. After drying, a slurry layer with a thickness of approximately 180 μm was obtained. The dried slurry layer was then rolled using a conventional electrode rolling mill to achieve a final thickness of approximately 110 μm and a porosity of approximately 26%, thereby forming the active material layer.

[0154] The method for calculating the porosity of the active material layer is the same as in Example 1. In addition, when considering the composition of the slurry, the SBR binder content in the active material layer of the electrode is approximately 2% by weight, and the content of the electrode active material is approximately 97% by weight.

[0155] Example 5

[0156] Copper foil (Cu foil) whose surface properties are controlled in the same manner as in Example 2 is used as a current collector.

[0157] Subsequently, the same slurry used in Example 4 was applied to the surface of the silane coating to a thickness of approximately 280 μm using a gap coating method, and dried at a temperature of approximately 230°C for approximately 90 seconds. After drying, a slurry layer with a thickness of approximately 180 μm was obtained, and the dried slurry layer was rolled using a conventional electrode rolling mill to achieve a final thickness of approximately 110 μm and a porosity of approximately 26%, thereby forming an active material layer.

[0158] The method for calculating the porosity of the active material layer, as well as the content of SBR binder in the active material layer of the electrode and the content of electrode active material, are the same as in Example 4.

[0159] Example 6

[0160] Copper foil (Cu foil) whose surface properties are controlled in the same manner as in Example 3 is used as a current collector.

[0161] Subsequently, the same slurry used in Example 4 was applied to the surface of the silane coating to a thickness of approximately 280 μm using a gap coating method, and dried at a temperature of approximately 230°C for approximately 90 seconds. After drying, a slurry layer with a thickness of approximately 180 μm was obtained, and the dried slurry layer was rolled using a conventional electrode rolling mill to achieve a final thickness of approximately 110 μm and a porosity of approximately 26%, thereby forming an active material layer.

[0162] The method for calculating the porosity of the active material layer, as well as the content of SBR binder in the active material layer of the electrode and the content of electrode active material, are the same as in Example 4.

[0163] Comparative Example 1

[0164] The copper foil (Cu foil) used as a current collector was directly applied to electrode manufacturing without any separate treatment. The surface energy of the untreated copper foil was approximately 71.2 mN / m, the dispersion energy was approximately 45 mN / m, and the polar energy was approximately 26.2 mN / m.

[0165] Subsequently, the same slurry used in Example 1 was applied to the surface of the copper foil layer to a thickness of approximately 280 μm using a gap coating method, and dried at a temperature of approximately 230°C for approximately 90 seconds. After drying, a slurry layer with a thickness of approximately 180 μm was obtained, and the dried slurry layer was rolled using a conventional electrode rolling mill to achieve a final thickness of approximately 110 μm and a porosity of approximately 26%, thereby forming an active material layer.

[0166] The method for calculating the porosity of the active material layer, as well as the content of SBR binder in the active material layer of the electrode and the content of electrode active material, are the same as in Example 1.

[0167] Comparative Example 2

[0168] Copper foil (Cu foil) is used as a current collector and, after its surface properties are adjusted in the following manner, it is applied to the manufacture of electrodes.

[0169] A coating solution containing dodecyltrimethoxysilane at a concentration of approximately 1% by weight in ethanol as a solvent was applied to the surface of a copper foil using a bar coater to a thickness of approximately 10 μm. After coating, the solution was annealed at 100°C for approximately 5 minutes, washed with ethanol, and then dried again at 100°C for approximately 5 minutes to form a silane coating. The silane coating has a surface energy of approximately 27.7 mN / m, a dispersion energy of approximately 27.4 mN / m, and a polar energy of approximately 0.3 mN / m. Additionally, the water contact angle is approximately 102.6 degrees, and the DM contact angle is approximately 62.2 degrees.

[0170] The same slurry used in Example 1 was applied to the surface of the silane coating to a thickness of approximately 280 μm using a gap coating method and dried at a temperature of approximately 230°C for approximately 90 seconds. After drying, a slurry layer with a thickness of approximately 180 μm was obtained. The dried slurry layer was then rolled using a conventional electrode rolling mill to achieve a final thickness of approximately 110 μm and a porosity of approximately 26%, thereby forming an active material layer.

[0171] The method for calculating the porosity of the active material layer, as well as the content of SBR binder in the active material layer of the electrode and the content of electrode active material, are the same as in Example 1.

[0172] Comparative Example 3

[0173] The copper foil (Cu foil) used as a current collector was directly applied to electrode manufacturing without any separate treatment. The surface energy of the untreated copper foil was approximately 71.2 mN / m, the dispersion energy was approximately 45 mN / m, and the polar energy was approximately 26.2 mN / m.

[0174] Subsequently, the same slurry used in Example 4 was applied to the surface of the copper foil layer to a thickness of approximately 280 μm using a gap coating method, and dried at a temperature of approximately 230°C for approximately 90 seconds. After drying, a slurry layer with a thickness of approximately 180 μm was obtained, and the dried slurry layer was rolled using a conventional electrode rolling mill to achieve a final thickness of approximately 110 μm and a porosity of approximately 26%, thereby forming an active material layer.

[0175] The method for calculating the porosity of the active material layer, as well as the content of SBR binder in the active material layer of the electrode and the content of electrode active material, are the same as in Example 4.

[0176] Test Example 1: Calculation of the area occupied by the adhesive

[0177] The electrodes of the examples and comparative examples were subjected to standard peel tests in the manner described above, and the area occupied by the adhesive was confirmed. Figures 4 to 9 These are FE-SEM images from Examples 1 to 6, Figures 10 to 12 The images are FE-SEM images of Comparative Examples 1 to 3, respectively.

[0178] The results are described in Table 1 below.

[0179] [Table 1]

[0180]

[0181] As can be confirmed from Table 1, in the case of the embodiments, a high adhesive coverage ratio is ensured relative to the adhesive content in the active material layer.

[0182] Test Example 2: Confirmation of Adhesion

[0183] The adhesion evaluation results for the embodiments and comparative examples are shown in Table 2 below.

[0184] [Table 2]

[0185]

[0186] As can be confirmed from Table 2, in the case of the embodiments, high adhesion was ensured relative to the adhesive content in the active material layer.

Claims

1. An electrode, comprising: Current collector; and The active material layer on one side of the current collector, The active material layer comprises an electrode active material and a binder, wherein the binder content in the active material layer ranges from 0.5% by weight to 10% by weight. The electrodes, after undergoing standard peel testing, satisfy the following equation 1. The standard peel test involves repeatedly attaching Scotch® Magic™ Tape Cat. 810R to the active material layer and then peeling off the Scotch® Magic™ Tape Cat. 810R until no components of the active material layer are observed on the Scotch® Magic™ Tape Cat. 810R. [Equation 1] 17≤A / W≤50 Where A is the percentage (100×A2 / A1) of the area occupied by the adhesive on the surface of the current collector (A2) relative to the total surface area of ​​the current collector (A1), and W is the adhesive content in the active material layer (wt%). This includes an intermediate layer of a compound of Formula 1 present between the active material layer and the current collector: [Formula 1] Wherein, R1 is an alkyl group having 6 or fewer carbon atoms or an alkenyl group having 6 or fewer carbon atoms, wherein the alkyl group of R1 is selectively substituted with one or more amino groups, and R2 to R4 are each independently an alkyl group having 1 to 4 carbon atoms. The adhesive is a granular adhesive. The ratio (D1 / D2) of the average particle diameter (D1) of the electrode active material to the average particle diameter (D2) of the adhesive is in the range of 10 to 1000.

2. The electrode according to claim 1, wherein the current collector is a film, sheet, or foil selected from one or more of the group consisting of stainless steel, aluminum, nickel, titanium, calcined charcoal, copper, carbon, stainless steel surface-treated with nickel, titanium, or silver, and aluminum-cadmium alloys.

3. The electrode according to claim 1, wherein the adhesive comprises one or more of the group consisting of PVDF (polyvinylidene fluoride), PVA (polyvinyl alcohol), polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, SBR (styrene-butadiene rubber), and fluororubber.

4. The electrode according to claim 1, wherein the adhesive has an average particle diameter in the range of 50 nm to 500 nm.

5. The electrode according to claim 1, wherein the electrode active material comprises selected from LiCoO2, LiMn2O4, LiCoPO4, LiFePO4, and LiNi. 1-x-y-z Co x M1 y M2 z O2, carbonaceous materials, M1 and M2 are each independently selected from any one of the group consisting of Al, Ni, Co, Fe, Mn, V, Cr, Ti, W, Ta, Mg, and Mo, x, y, and z are each independently the atomic fractions of the constituent elements of the oxide, satisfying 0 ≤ x < 0.5, 0 ≤ y < 0.5, 0 ≤ z < 0.5, and 0 < x + y + z ≤ 1; lithium-containing titanium composite oxides, Si, Sn, Li, Zn, Mg, Cd, Ce, Ni, or Fe metals; alloys composed of metals (Me); oxides of metals (Me) (MeOx); and one or more of the group consisting of metals (Me) and carbon composites.

6. The electrode of claim 1, wherein the electrode active material comprises in an amount of 1,000 to 10,000 parts by weight relative to 100 parts by weight of the adhesive.

7. The electrode according to claim 1, wherein the active material layer has a thickness in the range of 10 μm to 500 μm.

8. The electrode according to claim 1, wherein the active material layer has a porosity of 35% or less.

9. An electrochemical element, comprising: The electrode as described in claim 1, which can be used as a negative or positive electrode.

10. A secondary battery, comprising: The electrode as described in claim 1, which can be used as a negative or positive electrode.

Citation Information

Patent Citations

  • Method for producing battery electrode

    CN102106020A

  • Method of manufacturing negative electrode material for lithium ion secondary battery, and negative electrode material for lithium ion secondary battery