Preparation method of flexible light swim goggles and swim goggles
By using polyolefin copolymer injection molding and high-pressure autoclave depressurization foaming processes, combined with N₂ gas and SEBS/OBC ratio, the problems of insufficient softness and fit of swimming goggles were solved, and lightweight and durable swimming goggles were manufactured.
Patent Information
- Application Number
- CN202310402533.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-14
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-04-14
AI Technical Summary
Existing swimming goggle materials lack softness and fit, resulting in discomfort and easy water ingress.
Flexible and lightweight swimming goggles were prepared by using polyolefin copolymers through injection molding and high-pressure autoclave depressurization foaming process, using N₂ as supercritical gas, controlling the temperature at 135℃ and the pressure at 30MPa, and maintaining the pressure for 3 hours for depressurization foaming, combined with a weight ratio of SEBS to OBC of 4:1.
The prepared swimming goggles have good flexibility and tensile strength, and low density, which avoids poor fit and water ingress, thus improving wearing comfort.
Smart Images

Figure HDA0004180243540000011
Abstract
Description
Technical Field
[0001] This invention relates to the field of polymer materials technology, particularly to the field of IPC C08L51, and further to a method for preparing flexible and lightweight swimming goggles and the swimming goggles themselves. Background Technology
[0002] Currently, swimming is an ideal method for fitness and weight loss, suitable not only for teenagers but also for people of other ages, leading to a growing number of amateur swimming enthusiasts. Swimming goggles, as one of the core pieces of equipment in swimming, allow for clear underwater vision while preventing eye injuries. Since the inner lining of the goggles directly contacts the skin of the face, the choice of material is crucial for improving wearing comfort.
[0003] Chinese patent CN 02134444 discloses a swimming, diving, and surfing goggle and its manufacturing process. The goggle body consists of a frame, lenses, and connecting straps. The lenses and frame are formed by a one-time co-injection molding process using a mixture of high-strength polycarbonate and silicone materials. The manufacturing process of the goggle body is as follows: the polycarbonate and silicone material mixture is placed in a soft mask cavity, and soft mask silicone material is injected. The injection temperature is controlled at 250 degrees Celsius, and the injection pressure is controlled at 50 T / cm. 2 The silicone material used in this technical solution is not soft enough and cannot fit well on the face. Chinese patent CN201911049291 discloses a swimming goggle with memory and 3D shaping functions, including a goggle body and a pad. The rear end of the goggle body has a flange, and an annular groove is formed between the outer wall of the flange and the inner wall of the goggle body. The front end of the pad has a connecting part, which is embedded in the annular groove. The flange is located in the inner hole of the pad. The rear end of the pad has a fitting part with a curved surface from the inside out. However, this technical solution obtains the pad by hot melting, injection molding, pressure holding, mold locking, cooling, mold opening, and demolding of SEBS material, which can further improve the weight and softness of the pad. Summary of the Invention
[0004] To address the aforementioned technical problems, a first aspect of the present invention provides a method for manufacturing flexible, lightweight swimming goggles, comprising the following steps:
[0005] (1) The polyolefin copolymer is injection molded into a preform using an injection molding machine;
[0006] (2) The embryo is placed in a high-pressure autoclave and foamed using the depressurization method to obtain a flexible and lightweight swimming goggle.
[0007] In some preferred embodiments, the injection molding temperature is 220–260°C.
[0008] In some preferred embodiments, the depressurization foaming method is as follows: supercritical gas is introduced into the autoclave, the temperature of the autoclave is controlled at 100-160°C and the pressure is controlled at 20-50 MPa, and depressurization foaming is carried out after maintaining the pressure for 1-8 hours.
[0009] In some preferred embodiments, the supercritical gas is N2 or CO2.
[0010] Preferably, the supercritical gas is N2.
[0011] The applicant discovered that when the supercritical gas is N2, the prepared swimming goggles also have good tensile strength and are relatively lightweight. The applicant speculates that N2 can be fully and uniformly mixed / diffused in the polyolefin copolymer system, resulting in a large number of cells, small cell size, more uniform and dense cell structure, and moderate cell wall thickness, which maintains the good tensile strength of the swimming goggles while reducing their weight.
[0012] Preferably, the temperature of the autoclave is 125–145°C.
[0013] Preferably, the temperature of the autoclave is 135°C.
[0014] The applicant discovered that when the temperature of the autoclave is controlled at 125–145°C, especially at 135°C, the density and hardness of the swimming goggles are reduced while the polyolefin copolymer system forms a good network structure. This ensures the comfort of the goggles while preventing them from easily deforming, which could lead to insufficient fit between the goggles and the face, resulting in water ingress. The applicant hypothesizes that as the temperature increases, the viscosity of the polyolefin copolymer system decreases, and the diffusion rate of supercritical gas increases, making it easier for the gas to enter the polyolefin copolymer system. This results in more and larger bubbles, reducing the density of the goggles. However, excessively high temperatures may cause the bubbles to merge, rupture, or collapse due to their large size. The temperature under these conditions ensures that the viscosity and surface tension of the polyolefin copolymer system are moderate, the polyolefin copolymer system has a good network structure, is not easily deformed, and the goggles fit the face well, making water ingress less likely.
[0015] The applicant also discovered that when the supercritical gas is N2 and the autoclave temperature is controlled at 135°C, the swimming goggles prepared by depressurization foaming have both low density and good cell structure, thus improving the tensile strength of the goggles. The applicant hypothesizes that the specific temperature allows more N2 to dissolve in the polyolefin copolymer system, which is conducive to cell growth. The cells formed under these conditions are in a closed-cell state, thus exhibiting good tensile strength.
[0016] Preferably, the depressurization foaming method is as follows: supercritical gas is introduced into the high-pressure vessel, the temperature of the high-pressure vessel is controlled at 135°C, the pressure is 20-40 MPa, and after maintaining this for 2-4 hours, depressurization foaming is performed.
[0017] Preferably, the depressurization foaming method is as follows: supercritical gas is introduced into the high-pressure vessel, the temperature of the high-pressure vessel is controlled at 135°C and the pressure is 30MPa, and depressurization foaming is carried out after maintaining this for 3 hours.
[0018] In some preferred embodiments, the depressurization time is 25 to 40 seconds.
[0019] Preferably, the pressure relief time is 30 seconds.
[0020] In some preferred embodiments, the polyolefin copolymer is selected from one or a combination of two of SEBS (hydrogenated styrene-butadiene block copolymer) and OBC (olefin block copolymer).
[0021] In some preferred embodiments, the polyolefin copolymer is a combination of SEBS and OBC.
[0022] Preferably, the weight ratio of SEBS to OBC is (3-5):1.
[0023] Preferably, the weight ratio of SEBS to OBC is 4:1.
[0024] The applicant discovered that when SEBS and OBC are selected as the polyolefin copolymers, the prepared swimming goggles not only have good flexibility but also good tensile strength. When only SEBS is used, due to the large number of soft chain components in SEBS, the foaming ratio of the foamed goggles is large, the void volume between the cells is large, and the interaction between molecular chains is low, resulting in low tensile strength of the goggles. When OBC is added to the system, especially when the weight ratio of SEBS to OBC is controlled at 4:1, the tensile strength of the prepared goggles is improved while maintaining flexibility. The applicant speculates that since OBC is a novel ethylene-octene copolymer with a unique alternating "soft" and "hard" block structure synthesized by "chain shuttle" polymerization technology, the addition of OBC combines the plastic deformation of the SEBS phase with the plastic deformation of the OBC crystals, improving the tensile strength. However, if too much OBC is added, its melt index is relatively higher than that of SEBS, which will lead to poor flowability of the polyolefin copolymer material in the system, uneven material distribution in the molded preform, which is not conducive to the formation of cells during the foaming process, and thus affects the overall performance of the goggles.
[0025] In some preferred embodiments, the hardness (Shore A) of the SEBS is ≤50.
[0026] In some preferred embodiments, the SEBS is in the form of granules or fluffy granules.
[0027] Preferably, the SEBS is in the form of particles.
[0028] In some preferred embodiments, the density of the OBC is 0.866–0.877 g / cm³. 3 The melt mass flow rate is 0.5–1 g / 10 min (ASTM D1238).
[0029] Preferably, the density of the OBC is 0.866 g / cm³. 3 The melt mass flow rate is 1 g / 10 min (ASTM D1238).
[0030] A second aspect of the present invention provides a flexible, lightweight swimming goggle, which is prepared according to the above-described method.
[0031] Beneficial effects:
[0032] 1. The present invention selects N2 as the supercritical gas, which can not only reduce CO2 emissions and be more environmentally friendly, but also N2 can be fully and uniformly mixed / diffused in the polyolefin copolymer system, resulting in a large number of cells, small cell size, more uniform and dense cell structure, and moderate cell wall thickness, which maintains the good tensile strength of the swimming goggles while reducing its weight.
[0033] 2. The present invention controls the temperature of the autoclave to 125-145℃. In particular, when the temperature of the autoclave is controlled to 135℃, the density and hardness of the swimming goggles are reduced while the polyolefin copolymer system forms a good network structure. This ensures the comfort of the swimming goggles and prevents them from easily deforming, which would result in insufficient fit between the swimming goggles and the face and water ingress.
[0034] 3. In this invention, the supercritical gas is controlled to be N2 and the temperature of the autoclave is controlled to be 135°C. The swimming goggles prepared by depressurization foaming have both low density and good pore structure, which improves the tensile strength of the swimming goggles.
[0035] 4. The polyolefin copolymer of the present invention selects a combination of SEBS and OBC, and the resulting swimming goggles not only have good flexibility, but also good tensile strength.
[0036] 5. The present invention controls the weight ratio of SEBS and OBC to 4:1, which avoids poor flowability of polyolefin copolymer materials in the system and uneven distribution of materials in the molded preform, which is conducive to the formation of cells during the foaming process and thus improves the overall performance of the swimming goggles. Attached Figure Description
[0037] Figure 1This is a picture of the swimming goggles prepared in Example 1 of the present invention. Detailed Implementation
[0038] Example 1
[0039] Example 1 provides a method for preparing flexible and lightweight swimming goggles, including the following steps:
[0040] (1) The polyolefin copolymer is injection molded into a preform using an injection molding machine;
[0041] (2) The embryo is placed in a high-pressure autoclave and foamed using the depressurization method to obtain a flexible and lightweight swimming goggle.
[0042] The injection molding temperature is 240℃.
[0043] The pressure relief foaming method is as follows: supercritical gas is introduced into the high-pressure vessel, the temperature of the high-pressure vessel is controlled at 135℃ and the pressure is 30MPa, and pressure relief foaming is carried out after 3 hours.
[0044] The supercritical gas is N2.
[0045] The pressure relief time is 30 seconds.
[0046] The polyolefin copolymer is a combination of SEBS and OBC.
[0047] The weight ratio of SEBS to OBC is 4:1.
[0048] The hardness (Shore A) of the SEBS is 38.
[0049] The SEBS is in the form of particles.
[0050] The SEBS model is KETEN MD1646.
[0051] The density of the OBC is 0.866 g / cm³. 3 The melt mass flow rate is 1 g / 10 min (ASTM D1238).
[0052] The OBC model is Dow 9107.
[0053] Example 2
[0054] Example 2 provides a method for preparing flexible and lightweight swimming goggles, including the following steps:
[0055] (1) The polyolefin copolymer is injection molded into a preform using an injection molding machine;
[0056] (2) The embryo is placed in a high-pressure autoclave and foamed using the depressurization method to obtain a flexible and lightweight swimming goggle.
[0057] The injection molding temperature is 240℃.
[0058] The pressure relief foaming method is as follows: supercritical gas is introduced into the high-pressure vessel, the temperature of the high-pressure vessel is controlled at 140℃ and the pressure is 30MPa, and pressure relief foaming is carried out after 3 hours.
[0059] The supercritical gas is N2.
[0060] The pressure relief time is 30 seconds.
[0061] The polyolefin copolymer is a combination of SEBS and OBC.
[0062] The weight ratio of SEBS to OBC is 5:1.
[0063] The hardness (Shore A) of the SEBS is 38.
[0064] The SEBS is in the form of particles.
[0065] The SEBS model is KETEN MD1646.
[0066] The density of the OBC is 0.866 g / cm³. 3 The melt mass flow rate is 1 g / 10 min (ASTM D1238).
[0067] The OBC model is Dow 9107.
[0068] Example 3
[0069] Example 3 provides a method for preparing flexible and lightweight swimming goggles, the specific implementation of which is the same as that of Example 1, except that the supercritical gas is CO2.
[0070] Example 4
[0071] Example 4 provides a method for preparing flexible lightweight swimming goggles. The specific implementation method is the same as that in Example 1, except that the depressurization foaming method is as follows: supercritical gas is introduced into the high-pressure vessel, the temperature of the high-pressure vessel is controlled at 150°C and the pressure is 30MPa, and after maintaining this for 3 hours, depressurization foaming is performed.
[0072] Example 5
[0073] Example 5 provides a method for preparing flexible and lightweight swimming goggles, the specific implementation of which is the same as that of Example 1, except that the weight ratio of SEBS and OBC is 6:1.
[0074] Example 6
[0075] Example 6 provides a method for preparing flexible lightweight swimming goggles, the specific implementation of which is the same as that of Example 1, except that the polyolefin copolymer is SEBS.
[0076] Example 7
[0077] Example 7 provides a flexible, lightweight swimming goggle, the specific implementation of which is the same as in Example 1, except that the density of the OBC is 0.866 g / cm³. 3 The melt mass flow rate is 0.5 g / 10 min (ASTM D1238).
[0078] The OBC model is Dow 9007.
[0079] Performance testing:
[0080] 1. Density test: The density of the lightweight swimming goggles prepared in Examples 1 to 7 was tested according to GB / T6343 standard.
[0081] 2. Hardness test: The hardness of the lightweight swimming goggles prepared in Examples 1 to 7 was tested according to GB / T2411-2008 standard.
[0082] 3. Tensile strength test: The lightweight swimming goggles prepared in Examples 1 to 7 were tested for tensile strength in accordance with GB / T6344-2008 standard.
[0083] Test results:
[0084] Table 1:
[0085] <![CDATA[Density (kg / m 3 )]]> Hardness (Shore C) Tensile strength (MPa) Example 1 100 20 2.9 Example 2 80 16 2.1 Example 3 45 10 1.2 Example 4 63 13 1.5 Example 5 100 18 2.3 Example 6 92 16 1.9 Example 7 120 28 3.2
Claims
1. A method for preparing flexible, lightweight swimming goggles, characterized in that, Includes the following steps: (1) A preform is obtained by injection molding a polyolefin copolymer using an injection molding machine. The polyolefin copolymer is a combination of SEBS and OBC, and the weight ratio of SEBS to OBC is 4:
1. The injection molding temperature is 240℃. The SEBS has a Shore A hardness of 38 and is in granular form. The density of the OBC is 0.866 g / cm³. 3 The melt mass flow rate is 1 g / 10 min; (2) Place the preform in a high pressure vessel, introduce supercritical gas N2 into the high pressure vessel, control the temperature of the high pressure vessel to 135℃ and the pressure to 30MPa, maintain for 3h and then depressurize and foam to obtain a flexible lightweight swimming goggle; the depressurization time is 30s.
2. A flexible, lightweight swimming goggle, characterized in that, It is obtained according to the preparation method of claim 1.
Citation Information
Patent Citations
Swimming goggles with memory and 3D shaping function eyeshade protective pad and manufacturing process of swimming goggles
CN110652708A
Swiming, diving and surfing mirror and its manufacture process
CN1394658A
Thermoplastic elastomer composition and molded article of same
CN106661286A
Preparation process of foaming product and foaming product
CN110982110A
Elastomer composition for improving copolymer performance and preparation method thereof
CN113583377A