Lithium ion battery and electrolyte thereof
By using a combination of additives A, B, and C to form a composite interface film in lithium-ion batteries, the problem of insufficient lifespan and fast-charging performance of lithium-ion batteries under high-temperature environments was solved, thereby improving the high-temperature cycle life and fast-charging performance of the batteries.
Patent Information
- Application Number
- CN202310470268.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-27
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-04-27
AI Technical Summary
Existing lithium-ion batteries have shortcomings in balancing long lifespan and fast charging performance, especially in high-temperature environments where performance degradation is significant. Conventional film-forming additives lead to increased internal resistance, making it impossible to simultaneously meet the requirements of high-temperature tolerance and fast charging.
A combination of additives containing sodium ions, namely film-forming additives A and B, and ethylene sulfite C, is used to form a composite interface film containing SO, PO, BO, PF, and BF groups, which synergistically improve the high-temperature cycle life and fast-charging performance of lithium-ion batteries.
It significantly improves the high-temperature cycle life and fast-charging performance of lithium-ion batteries, suppresses gas generation during high-temperature storage, and improves the overall performance of the battery.
Smart Images

Figure QLYQS_1 
Figure QLYQS_2 
Figure BDA0004203710310000021
Abstract
Description
Technical Field
[0001] This invention belongs to the field of lithium-ion battery technology, specifically relating to a lithium-ion battery electrolyte and a lithium-ion battery using the electrolyte. Background Technology
[0002] Lithium-ion batteries are widely used in mobile electronic devices, electric vehicles, drones, and other fields due to their high energy density, long lifespan, and lack of memory effect. With the continuous development of products powered by lithium-ion batteries, higher demands are being placed on their energy density, lifespan, and fast-charging performance.
[0003] Electrolyte, as a crucial component of lithium-ion batteries, plays a vital role in their performance. With the increasing popularity of electric vehicles, consumers demand faster charging for electric cars and two-wheeled vehicles to reduce waiting time. This also necessitates lithium batteries with longer lifespans and higher tolerance to high temperatures. Currently, there is an urgent need to develop lithium-ion batteries that offer fast charging, long lifespan, and better high-temperature tolerance. In actual use, batteries undergo numerous charge-discharge cycles and may operate for extended periods in high-temperature environments. During this process, the accumulation of side reactions and gas production inevitably reduces battery lifespan. The conventional approach is to add film-forming additives to the electrolyte to suppress side reactions. However, these additives generally have low conductivity, and their addition can cause a rapid increase in internal resistance, making it impossible to simultaneously achieve both long lifespan and fast charging performance.
[0004] Therefore, it is necessary to develop an electrolyte that balances the long lifespan, fast charging performance, and high-temperature performance of lithium-ion batteries. Summary of the Invention
[0005] The purpose of this invention is to overcome the shortcomings of the prior art and provide a lithium-ion battery and its electrolyte that can balance the long life, fast charging performance and high temperature performance of lithium-ion batteries.
[0006] To achieve the above objectives, the technical solution adopted by the present invention is as follows:
[0007] In a first aspect, the present invention provides a lithium-ion battery electrolyte, characterized in that it comprises a lithium salt, an organic solvent, and a combination of additives, wherein the combination of additives comprises additive A, additive B, and additive C.
[0008] Additive A is a film-forming additive containing sodium ions, additive B contains a compound as shown in Formula I, and additive C is vinylene sulfite;
[0009]
[0010] In Formula I, R1 to R9 are alkyl groups with 1 to 4 carbon atoms or alkyl groups with 1 to 4 carbon atoms substituted by halogen atoms, wherein the halogen atom is any one of F, Cl, Br, and I; X is P or B element, and y is 0 or 1.
[0011] Preferably, additive A is any one or more of sodium difluorooxalate borate, sodium dioxalate borate, sodium difluorophosphate, and sodium difluorodioxalate phosphate, used for preferential film formation on the positive and / or negative electrodes of lithium-ion batteries.
[0012] Preferably, additive B is any one or more of tris(trimethylsilyl)phosphate, tris(trimethylsilyl)phosphite, and tris(trimethylsilyl)borate.
[0013] Preferably, the additive C has a mass fraction of 0.1% to 3% in the electrolyte, and its structural formula is shown in Formula II.
[0014]
[0015] Preferably, the mass fraction of additive A in the electrolyte is 0.1% to 3%; and the mass fraction of additive B in the electrolyte is 0.1% to 2%.
[0016] Preferably, the electrolyte further comprises other additives, which are at least one of carbonates, sulfonates, or nitriles.
[0017] Preferably, the other additives have a mass fraction of 0.1% to 2% in the electrolyte.
[0018] Preferably, the solvent in the electrolyte is a carbonate solvent and / or a carboxylic acid ester.
[0019] Preferably, the lithium salt in the electrolyte includes at least one of LiPF6, LiFSI, LiTFSI, and LiBF4.
[0020] In a second aspect, the present invention provides a lithium-ion battery, comprising a positive electrode, a negative electrode, a separator, and any of the lithium-ion battery electrolytes described above.
[0021] Compared with the prior art, the beneficial effects achieved by the present invention are as follows:
[0022] The combined additives provided by this invention can form a composite interface film containing SO, PO, BO, PF, and BF groups at the positive and negative electrode interfaces. This composite interface film is more dense and has lower impedance.
[0023] Since additive A is a film-forming additive containing sodium ions, the resulting composite interface film contains sodium ions. The resulting composite interface film is loose and has large pores, which is conducive to the transport and migration of lithium ions.
[0024] The silane groups in additive B can absorb hydrofluoric acid and moisture generated in the battery and electrolyte, suppress various gas production during battery use, further reduce the occurrence of side reactions, and improve battery life.
[0025] The electrolyte provided by this invention can significantly improve the high-temperature cycle life of lithium-ion batteries due to the synergistic effect of the combined additives, while also improving the fast-charging performance of lithium-ion batteries, as well as the high-temperature storage capacity recovery rate and suppressing gas generation during high-temperature storage.
[0026] The electrolyte provided by this invention also includes any one or more of carbonate, sulfonate, or nitrile additives, which can further protect the positive and negative electrode interfaces and improve the overall performance of the battery. Detailed Implementation
[0027] The following embodiments are only used to illustrate the technical solutions of the present invention more clearly, and should not be used to limit the scope of protection of the present invention.
[0028] Unless otherwise specified, all reagents, materials and instruments used in the following examples and comparative examples are commercially available.
[0029] This invention provides a lithium-ion battery electrolyte, comprising a lithium salt, an organic solvent, and a combination of additives, wherein the combination of additives includes additive A, additive B, and additive C;
[0030] Among them, additive A is a film-forming additive containing sodium ions, additive B contains a compound as shown in Formula I, and additive C is vinylene sulfite.
[0031]
[0032] In Formula I, R1 to R9 are alkyl groups with 1 to 4 carbon atoms or alkyl groups with 1 to 4 carbon atoms substituted by halogen atoms, wherein the halogen atom is any one of F, Cl, Br, and I; X is P or B element, and y is 0 or 1.
[0033] In practice, R1 to R9 in Formula I above are either alkyl groups having 1 to 2 carbon atoms, or any one of alkyl groups substituted with halogens.
[0034] It is feasible that additive B is any one or more of tris(trimethylsilyl)phosphate, tris(trimethylsilyl)phosphite, and tris(trimethylsilyl)borate, and the mass fraction of additive B in the electrolyte is 0.1% to 2%.
[0035] Additive B contains compounds with PO3 and / or BO3 and / or PO4 groups. This additive also participates in the formation of SEI, and the SEI it forms has low impedance. At the same time, the silane groups in additive B can absorb hydrofluoric acid and moisture generated in the battery and electrolyte, which can effectively suppress various gas generation during battery use, further reduce the occurrence of side reactions, and improve battery life.
[0036] In practice, the mass fraction of additive A in the electrolyte is 0.1% to 3%, preferably 0.1% to 2%. Additive A is any one or more of sodium difluorooxalate borate, sodium difluorooxalate borate, sodium difluorophosphate, and sodium difluorodifluorooxalate phosphate. It is used to preferentially form an interface film (SEI) on the positive and / or negative electrodes of lithium-ion batteries, which effectively suppresses the occurrence of battery side reactions. In addition, since sodium ions are present in additive A, the large radius of sodium ions results in larger internal pores in the formed SEI. Overall, the SEI film is more porous and less prone to clogging of SEI pores, which is beneficial to the transport and migration of lithium ions.
[0037] Additive C has a mass fraction of 0.1% to 3% in the electrolyte, and its structural formula is shown in Formula II.
[0038]
[0039] Preferably, in this invention, the mass fraction of additive C in the electrolyte is set to 0.1% to 2%, and the SO3 groups and unsaturated bonds contained in additive C can preferentially form dense SEI at the positive and negative electrodes.
[0040] Preferably, the electrolyte also contains other additives, with a mass fraction of 0.1% to 2% in the electrolyte, to further protect the positive and negative electrode interfaces and improve the overall performance of the battery.
[0041] Other additives are at least one of carbonates, sulfonates, or nitriles, specifically, carbonates, sulfonates, and nitriles are any one or more of fluoroethylene carbonate (FEC), 1,3-propanesulfonate lactone (PS), succinic acid nitrile (SN), adiponitrile (ADN), and 1,3,6-hexanetrionitrile (HTCN).
[0042] The solvent in the electrolyte is a carbonate solvent and / or a carboxylic acid ester, preferably containing at least one cyclic ester and one linear ester.
[0043] The solvent in the electrolyte of this invention is any one or more of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl formate, ethyl formate, propyl formate, methyl acetate, ethyl acetate, methyl propionate, ethyl propionate, and propyl propionate.
[0044] The lithium salt in the electrolyte includes at least one of LiPF6, LiFSI, LiTFSI, and LiBF4.
[0045] The present invention also provides a lithium-ion battery, comprising a positive electrode, a negative electrode, a separator, and a lithium-ion battery electrolyte. The positive electrode comprises any one or a combination of several of the following: nickel-cobalt-manganese ternary materials, nickel-cobalt-aluminum ternary materials, lithium iron phosphate, lithium manganese iron phosphate, and lithium manganese oxide; the negative electrode comprises any one or more of the following: artificial graphite, natural graphite, soft carbon, hard carbon, silicon materials, and lithium metal.
[0046] Preferably, the silicon material of the present invention comprises silicon-carbon material and silicon suboxide material.
[0047] In this embodiment of the invention, the materials used to prepare the electrolyte are as follows:
[0048] Organic solvents: ethylene carbonate (EC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC);
[0049] Lithium salt: LiPF6;
[0050] Additive A: Sodium difluorooxalate borate (NaDFOB), sodium difluorooxalate borate (NaBOB), sodium difluorophosphate (NaDFP), sodium difluorooxalate phosphate (NaDFOP);
[0051] Additive B: Tris(trimethylsilyl)phosphate (TMSP), Tris(trimethylsilyl)phosphite (TMSi), Tris(trimethylsilyl)borate (TMSB);
[0052] Additive C: Vinyl sulfite (VES);
[0053] Other additives: fluoroethylene carbonate (FEC), 1,3-propanesulfonate lactone (PS), succinate (SN), adiponitrile (ADN), 1,3,6-hexanetrionitrile (HTCN);
[0054] In addition, comparative additives were added: sodium hexafluorophosphate (NaPF6), to be compared with sodium ion film-forming additives; lithium difluorooxalate borate (LiDFOB), to be compared with NaDFOB; and ethylene ethylene carbonate (VEC), to be compared with VES.
[0055] The electrolytes in Examples 1 to 13 of this invention were all prepared using the following method:
[0056] First, lithium salt is slowly added to a mixture of EC, DMC, and EMC in a glove box. After the temperature in the container drops to room temperature, a combination additive is added. The combination additive includes additive A, additive B, and additive C, or other additives may be added simultaneously. After mixing evenly, an electrolyte is prepared. The mass ratio of EC, DMC, and EMC in the electrolyte is EC:DMC:EMC = 1:1:1, and the molar concentration of lithium salt in the electrolyte is 1 mol / L.
[0057] The types and contents of additives used in Examples 1 to 13 are shown in Table 1, where the content of additives is a weight percentage based on the total weight of the electrolyte.
[0058] Table 1: Composition of each additive in the electrolyte of Examples 1-13
[0059]
[0060]
[0061] Preparation of electrolytes in Comparative Examples 1–11:
[0062] In Comparative Examples 1 through 11, electrolytes were prepared sequentially according to the following preparation method:
[0063] First, lithium salt is slowly added to the mixture of EC, DMC, and EMC in a glove box. After the container temperature drops to room temperature, additives are added. The specific composition and content of the additives are shown in Table 2, and the additive content is a weight percentage calculated based on the total weight of the electrolyte. After thorough mixing, the electrolyte is prepared. The mass ratio of EC, DMC, and EMC in the electrolyte is EC:DMC:EMC = 1:1:1, and the molar concentration of lithium salt in the electrolyte is 1 mol / L.
[0064] Table 2: Proportions of additives in the electrolytes of Comparative Examples 1–11
[0065]
[0066]
[0067] Preparation of lithium-ion batteries:
[0068] The electrolytes obtained in the examples and comparative examples were applied to lithium-ion batteries for performance testing. The lithium-ion batteries were prepared using the following steps:
[0069] (1) Preparation of positive electrode
[0070] The cathode material is lithium nickel cobalt manganese oxide NCM622 (LiNi 0.6 Co 0.2 Mn0.2 O2), binder (polyvinylidene fluoride), and conductive agent (conductive carbon black) are mixed in a mass ratio of 96:2:2. N-methylpyrrolidone (NMP) is added and stirred to prepare a positive electrode slurry. The positive electrode slurry is then uniformly coated onto aluminum foil, with a single-sided coating weight of 20 mg / cm². 2 After the aluminum foil is dried at room temperature, it is transferred to a 120℃ oven to dry for 1 hour. Then it is dried at 85℃, cold-pressed, trimmed, cut into pieces, and slit. Finally, it is dried under vacuum at 85℃ for 4 hours, and the tabs are welded to produce the positive electrode sheet of the lithium-ion secondary battery that meets the requirements.
[0071] (2) Preparation of negative electrode
[0072] Artificial graphite (AG), sodium carboxymethyl cellulose (CMC) solution (thickener), styrene-butadiene rubber latex (SBR) binder, and conductive agent (conductive carbon black) were dissolved in deionized water at a mass ratio of 96:1:1.5:1.5 to prepare a negative electrode slurry. The negative electrode slurry was then uniformly coated onto the current collector copper foil at a coating weight of 10 mg / cm². 2 After drying at 85°C, the material is cold-pressed, trimmed, cut into sheets, and slit. Then, it is dried under vacuum at 110°C for 4 hours, and the tabs are welded to produce the negative electrode sheet for a lithium-ion secondary battery that meets the requirements.
[0073] (3) Preparation of lithium-ion batteries
[0074] The above-mentioned positive electrode, negative electrode and separator (PE film + 3um ceramic coating) are wound into a bare cell and then placed into an aluminum-plastic film. After being baked at 90°C to remove water, the corresponding electrolyte is injected and then sealed. After processes such as standing, hot and cold pressing, formation, degassing and capacity testing, a lithium-ion battery is obtained.
[0075] The lithium-ion batteries obtained above were subjected to lithium-ion battery performance testing.
[0076] (1) High-temperature cycle performance test of lithium-ion battery at 45℃
[0077] At 45℃, the lithium-ion battery was left to stand for 30 minutes, then charged at a constant current rate of 0.5C to 4.3V, followed by constant voltage charging at 4.3V to 0.05C, and left to stand for 5 minutes. Afterward, it was discharged at a constant current rate of 0.5C to 2.8V. This constitutes one charge-discharge cycle, and the resulting discharge capacity is the initial discharge capacity C1 of the lithium-ion battery. Subsequent charge-discharge cycles were performed 1000 times, and the discharge capacity of the 1000th cycle was recorded as C1. 1000 The lithium-ion battery cycle performance test data of the embodiments and comparative examples of this invention are shown in Table 3.
[0078] Capacity retention rate (%) of lithium-ion battery after 1000 cycles = C 1000 / C1.
[0079] (2) Lithium-ion battery 25℃ fast charging cycle performance test
[0080] At 25°C, the lithium-ion battery was left to stand for 30 minutes, then charged at a constant current rate of 3C to 4.3V, followed by constant voltage charging at 4.3V to 0.05C, and left to stand for 5 minutes. Finally, it was discharged at a constant current rate of 1C to 2.8V. This constitutes one charge-discharge cycle, and the resulting discharge capacity is the initial discharge capacity C of the lithium-ion battery. 1F Then, 1500 charge-discharge cycles were performed, and the discharge capacity of the 1500th cycle was recorded as C. 1500F The lithium-ion battery cycle performance test data for this embodiment and the comparative example are shown in Table 3.
[0081] Capacity retention rate (%) of lithium-ion battery after 1500 cycles = C 1500F / C 1F .
[0082] (3) High-temperature storage test of lithium-ion batteries at 70℃
[0083] First, allow the lithium-ion battery to stand at 25°C for 30 minutes; then charge it to 4.3V at a constant current of 0.5C, and further charge it to 0.5C at a constant voltage of 4.3V; finally, discharge the lithium-ion battery to 2.8V at a constant current of 0.5C. The discharge capacity at this point is denoted as C. 0s Then, it was charged to 4.3V at a constant current of 0.5C, and further charged to 0.5C at a constant voltage of 4.3V. Finally, the battery volume was tested using the water displacement method; this is the volume V0 before storage. The lithium-ion battery was then stored at 70℃ for 30 days. After storage, the lithium-ion rechargeable battery was placed at 25℃, and the battery volume was tested using the water displacement method; this is the volume V after storage. 30 Then, the lithium-ion battery is discharged to 2.8V at a constant current of 0.5C; then, the lithium-ion secondary battery is charged to 4.3V at a constant current of 0.5C, and further charged to a current of 0.5C at a constant voltage of 4.3V; then, the lithium-ion secondary battery is discharged to 2.8V at a constant current of 0.5C. The discharge capacity at this point is denoted as C. 30s .
[0084] Lithium-ion storage capacity recovery rate (%) after 30 days of storage = C 30S / C 0S ;
[0085] Volume expansion rate (%) of lithium-ion battery after 30 days of storage = (V 30 -V0) / V o .
[0086] Table 3: Test Results of Lithium-ion Batteries
[0087]
[0088]
[0089] As can be seen from Comparative Examples 1-4 and Example 2, the addition of three additives A, B, and C to the lithium-ion battery electrolyte significantly improved the 45°C cycling, 25°C fast-charge cycling, 70°C storage capacity recovery, and gas generation performance compared to adding a single component or both combinations. Additive A, a sodium ion film-forming additive, can form a low-impedance and dense SEI, achieving a good balance of various performance characteristics. Additive B can assist in film formation, forming a low-impedance SEI, and its trimethylsilyl group can capture the acid produced by battery decomposition at high temperatures, resulting in a more significant improvement in 25°C fast-charge cycling and high-temperature storage. Additive C can simultaneously undergo ring-opening and double-bond polymerization to form a dense SEI at both the positive and negative electrodes, resulting in a more significant improvement in 45°C cycling and high-temperature storage. The combined use of the three additives can better balance the high-temperature cycling, fast-charge, and high-temperature storage performance of lithium-ion batteries.
[0090] As can be seen from Comparative Examples 7-8 and Example 2, the overall performance of lithium-ion batteries with the addition of NaDFOB is significantly better than that of NaPF6 and LiDFOB. Firstly, NaPF6 cannot undergo an electrochemical reaction at the positive and negative electrodes to form a dense SEI, therefore its cycle and storage performance is inferior to NaDFOB. Furthermore, although NaPF6 can supplement sodium ions in the SEI component like NaDFOB, forming a low-resistance SEI with larger porosity, NaPF6 has better thermal stability below 60°C, and only a small portion undergoes a chemical reaction to deposit on the positive and negative electrode surfaces to modify the SEI. Therefore, its cycle performance at 25°C and 45°C is inferior to that of NaDFOB.
[0091] As can be seen from Comparative Example 11 and Example 2, the overall performance of adding VES to a lithium-ion battery is significantly better than that of VEC. Like VEC, VES contains five-membered rings and exocyclic double bonds, and both can form a dense SEI on the positive and negative electrode surfaces through electrochemical reactions. The difference is that VES replaces the C in the CO3 functional group of VEC with S. On the one hand, VES has a lower film-forming resistance than VEC, which is more conducive to fast-charging cycling. At the same time, sulfide compounds have a better protective effect on the positive electrode and a better effect on gas generation suppression than carbon compounds, which is beneficial for high-temperature cycling and storage. Furthermore, VES has a higher HOMO energy level than VEC and a lower LUMO energy level than VEC, preferentially forming SEI on both the positive and negative electrodes, which is more conducive to improved cycle life and increased capacity.
[0092] As can be seen from Examples 1-3 and Comparative Examples 4-6, as the mass fraction of additive A (NaDFOB) in the electrolyte gradually increases from 0% to 3%, the performance of 45°C cycling, 25°C fast-charge cycling, 70°C storage capacity recovery, and gas generation all first improve and then gradually deteriorate. Among them, the deterioration is more obvious when the gas generation content is too high in 45°C cycling and 70°C. NaDFOB preferentially forms a stable SEI at the positive and negative electrodes to protect the positive and negative electrode interfaces, but when the content is too high, there is excess during film formation, which will cause thermal decomposition at high temperatures and have a negative effect.
[0093] As can be seen from Examples 4-6, Example 9 and Comparative Example 9, the 25°C fast charge cycle improves sequentially with the increase of additive B content, but the improvement changes from significant to slow as the content increases; the 70°C storage capacity recovery and gas generation performance first improve and then gradually deteriorate with the increase of additive B; the main function of additive B is to assist film formation, forming a low-resistance SEI at the positive and negative electrodes, which is beneficial for 25°C fast charging, but additive A is more unstable than additive A and is more prone to thermal decomposition, especially when the content is too high, which significantly deteriorates the high-temperature performance.
[0094] As can be seen from Examples 4, 7-8, 10 and Comparative Example 10, the 45°C cycle performance of lithium-ion batteries improves with the increase of additive B content, but the trend slows down with the increase of content. The 25°C fast charge cycle performance, 70°C storage capacity recovery and gas generation performance all improve first and then gradually deteriorate. Additive C, ethylene sulfite, has good film density in both positive and negative electrodes, but the film resistance deteriorates with the increase of content. Therefore, when the content is high, the deterioration of the 25°C fast charge cycle is more obvious. In addition, when the content of additive C is too high, it also produces acidic substances in the solvent at high temperatures, which deteriorates the 70°C high-temperature storage performance.
[0095] As can be seen from Examples 9-13, the combined use of different additives A, B, and C in lithium-ion batteries can comprehensively regulate and improve the 25°C fast-charge cycle, 45°C cycle, 70°C storage capacity recovery, and gas generation of lithium-ion batteries. Furthermore, introducing other additives based on additives A, B, and C can further optimize the overall performance of the battery cell.
[0096] In summary, the combined additives in the electrolyte of this invention use additives A, B, and C in combination. In addition to the individual effects of each additive, the combined additives can also form a composite SEI containing SO, PO, BO, PF, and BF groups at the positive and negative electrode interfaces. This composite SEI is more dense and has a lower impedance compared to the SEI formed by a single or two combined additives.
[0097] Meanwhile, the presence of sodium ions in the composite SEI results in a loose SEI with large voids, which is beneficial for lithium ion transport and migration. The synergistic effect of additives A, B, and C in the electrolyte significantly improves the high-temperature cycle life of lithium-ion batteries, enhances their fast-charging performance, improves high-temperature storage capacity recovery, and suppresses gas generation during high-temperature storage.
[0098] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the technical principles of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A lithium-ion battery electrolyte, characterized in that, It includes lithium salts, organic solvents, and a combination of additives, wherein the combination of additives includes additive A, additive B, and additive C; Additive A is any one or more of sodium difluorooxalate borate, sodium difluorooxalate borate, and sodium difluorodifluorooxalate phosphate, with a mass fraction of 1% to 2% in the electrolyte; additive B comprises a compound as shown in Formula I, with a mass fraction of 0.1% to 2% in the electrolyte; additive C is vinylene sulfite, with a structural formula as shown in Formula II, with a mass fraction of 0.1% to 3% in the electrolyte; , Formula I, In Formula I, R1 to R9 are alkyl groups with 1 to 4 carbon atoms or alkyl groups with 1 to 4 carbon atoms substituted by halogen atoms, wherein the halogen atom is any one of F, Cl, Br, and I; X is P or B element, and y is 0 or 1; , Formula II.
2. The lithium-ion battery electrolyte according to claim 1, characterized in that, Additive A is sodium difluorooxalate borate.
3. The lithium-ion battery electrolyte according to claim 1, characterized in that, The additive B is any one or more of tris(trimethylsilyl)phosphate, tris(trimethylsilyl)phosphite, and tris(trimethylsilyl)borate.
4. The lithium-ion battery electrolyte according to claim 1, characterized in that, The electrolyte also contains other additives, which are at least one of carbonates, sulfonates, or nitrile compounds.
5. The lithium-ion battery electrolyte according to claim 4, characterized in that... The other additives have a mass fraction of 0.1% to 2% in the electrolyte.
6. The lithium-ion battery electrolyte according to claim 1, characterized in that, The solvent in the electrolyte is a carbonate solvent and / or a carboxylic acid ester.
7. The lithium-ion battery electrolyte according to claim 1, characterized in that, The lithium salt in the electrolyte includes at least one of LiPF6, LiFSI, LiTFSI, and LiBF4.
8. A lithium-ion battery, characterized in that, It includes a positive electrode, a negative electrode, a separator, and the lithium-ion battery electrolyte as described in any one of claims 1-7.
Citation Information
Patent Citations
Electrolyte for lithium ion battery and formation method thereof
CN113451655A
Rate type lithium ion battery electrolytic solution with high and low temperature performance and lithium ion battery
CN113471535A