Method of processing quantum dot cells
By employing a quantum dot unit fabrication method that independently applies an electric field to the three-dimensional display element, the problems of low brightness, low contrast, and limited viewing angle in existing three-dimensional display technologies have been solved, achieving higher display effects and a wider viewing angle.
Patent Information
- Application Number
- CN202310441276.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-06-23
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2041-06-23
AI Technical Summary
Existing solid-state volumetric 3D display technologies, such as 3D display technologies based on upconversion materials and 3D display technologies based on liquid crystal stacking, suffer from problems such as low brightness, low contrast, low vertical resolution, and limited viewing angles. Furthermore, the display effects are reduced due to the mutual interference between quantum dot units.
The quantum dot unit fabrication method involves depositing first and second transparent conductive layers on a transparent substrate to form a transparent conductive layer, thereby enabling the independent application of an electric field to each quantum dot unit. The quantum dot layer and the conductive layer form a PN junction structure, allowing independent control of the quantum dot unit display.
It improves the display effect of 3D display elements, enhances brightness, contrast, vertical resolution and viewing angle, and reduces display interference between quantum dot units.
Smart Images

Figure CN116364815B_ABST
Abstract
Description
[0001] This case is a divisional application of application number 202110701334.1, application date June 23, 2021, entitled "Quantum dot composite, three-dimensional display element and processing method thereof". Technical Field
[0002] This invention relates to the field of display technology, and in particular to a method for fabricating quantum dot units. Background Technology
[0003] Existing solid-state volumetric 3D display technologies, such as upconversion material-based 3D display technology and liquid crystal stacking 3D display technology, each have their own problems. The former has low brightness and low contrast, while the latter has low vertical resolution and a limited viewing angle. In addition, the display of individual quantum dot units affects each other, reducing the display effect of display elements with quantum dot units. Summary of the Invention
[0004] This invention aims to at least solve one of the technical problems existing in the prior art. Therefore, one object of this invention is to propose a method for fabricating quantum dot units that enables the independent application of an electric field to the quantum dot unit layer, thereby enabling the independent display of the quantum dot unit layer.
[0005] Another object of the present invention is to provide a quantum dot unit fabricated using the above-described quantum dot unit fabrication method.
[0006] According to a first aspect of the present invention, a method for fabricating a quantum dot unit includes a transparent substrate, a first transparent conductive layer, a quantum dot layer, and a second transparent conductive layer. The first transparent conductive layer and the quantum dot layer are located on one side of the transparent substrate and are disposed sequentially away from the transparent substrate. The second transparent conductive layer is located on the other side of the transparent substrate, or on the side of the quantum dot layer away from the transparent substrate. The method for fabricating the quantum dot unit includes:
[0007] Prepare the transparent substrate;
[0008] A first photoresist layer is coated on one side of the transparent substrate;
[0009] Exposure and development occur, and a portion of the first photoresist layer is retained to form a first residual portion;
[0010] The first transparent conductive layer is deposited on the exposure and development side of the transparent substrate;
[0011] After peeling off the first residual portion, a first protrusion located on one side of the peeled area is formed on the first transparent conductive layer.
[0012] The quantum dot layer is coated on the side of the first transparent conductive layer away from the transparent substrate;
[0013] Apply the second photoresist layer;
[0014] Exposure and development are performed, and a portion of the second photoresist layer is retained to form a second residual portion, which is located near the same edge of the transparent substrate as the first residual portion.
[0015] A second transparent conductive layer is deposited on the exposure and development side of the transparent substrate;
[0016] After peeling off the second residual portion, the second transparent conductive layer is formed with a second protrusion located on one side of the second residual portion, and the second protrusion is offset from the first protrusion.
[0017] According to a method for fabricating quantum dot units based on a first aspect of the present invention, the quantum dot units are formed by depositing a first transparent conductive layer and a second transparent conductive layer to achieve independent application of an electric field to each quantum dot unit, thereby enabling independent display of the quantum dot units. When quantum dot units are applied to three-dimensional display elements, the display effect of the three-dimensional display elements is improved.
[0018] According to some embodiments of the present invention, the thickness of the quantum dot layer is d1, wherein d1 satisfies: 0.05μm≤d1≤10μm.
[0019] According to some embodiments of the present invention, the thickness of the transparent substrate is d2, wherein d2 satisfies: 0.1mm≤d2≤0.5mm, and the parallelism and flatness errors of the upper and lower light surfaces of the transparent substrate are controlled within ±2μm.
[0020] According to some embodiments of the present invention, the length of the transparent substrate is a, and the width of the transparent substrate is b, wherein a and b respectively satisfy: 1mm≤a≤500mm, 1mm≤b≤500mm.
[0021] According to some embodiments of the present invention, the transparent substrate is a glass plate, and the preparation of the transparent substrate includes: fabricating the glass plate using a float glass process, an overflow stretching process, a slit stretching process, or a secondary stretching process.
[0022] According to some embodiments of the present invention, the transparent substrate is a resin transparent plate.
[0023] According to some embodiments of the present invention, the first transparent conductive layer and the second transparent conductive layer are made of indium tin oxide.
[0024] According to some embodiments of the present invention, the difference in refractive index between any two of the first transparent conductive layer, the second transparent conductive layer and the transparent substrate is n, where n ≤ 0.01.
[0025] According to some embodiments of the present invention, depositing the first transparent conductive layer and the second transparent conductive layer includes: using magnetron sputtering, vacuum reactive evaporation, chemical vapor deposition, sol-gel method or pulsed laser deposition method.
[0026] According to some embodiments of the present invention, one of the first transparent conductive layer and the second transparent conductive layer is a P-type semiconductor, and the other of the first transparent conductive layer and the second transparent conductive layer is an N-type semiconductor. The quantum dot layer, together with the first transparent conductive layer and the second transparent conductive layer, forms a PN junction.
[0027] Additional aspects and advantages of the invention will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of the invention. Attached Figure Description
[0028] The above and / or additional aspects and advantages of the present invention will become apparent and readily understood from the description of the embodiments taken in conjunction with the following drawings, in which:
[0029] Figure 1 This is a schematic diagram of a method for fabricating quantum dot composites according to an embodiment of the present invention.
[0030] Figure 2 This is a schematic diagram of a processing method for a three-dimensional display element according to an embodiment of the present invention.
[0031] Figure 3 This is a schematic diagram of a processing method for a three-dimensional display element according to a specific embodiment of the present invention.
[0032] Figure 4 This is a process flow diagram of quantum dot composites processed by lamination according to an embodiment of the present invention.
[0033] Figure 5 This is a schematic diagram of a quantum dot composite according to an embodiment of the present invention.
[0034] Figure 6 This is a schematic diagram showing the disassembly of a quantum dot composite according to an embodiment of the present invention.
[0035] Figure 7 This is a schematic diagram of the spacer arrangement of a quantum dot composite according to an embodiment of the present invention.
[0036] Figure 8 This is a schematic diagram of the spacer arrangement of a quantum dot composite according to another embodiment of the present invention.
[0037] Figure 9 This is a schematic diagram of the spacer arrangement of a quantum dot composite according to yet another embodiment of the present invention.
[0038] Figure 10 This is a schematic diagram of the arrangement of quantum dot units and spacers in a quantum dot composite according to an embodiment of the present invention.
[0039] Figure 11 This is a schematic diagram of the quantum dot units and spacers of a quantum dot composite being pressurized according to an embodiment of the present invention.
[0040] Figure 12 This is a schematic diagram of the application of sealant to a quantum dot composite according to an embodiment of the present invention.
[0041] Figures 13-17 This is a schematic diagram illustrating the dispensing method of several embodiments of the present invention.
[0042] Figure 18 This is a schematic diagram of the display element.
[0043] Figures 19-21 This is a schematic diagram of a quantum dot composite bonded by lamination according to an embodiment of the present invention.
[0044] Figure label:
[0045] Quantum dot composite 100, electrode 200,
[0046] Quantum dot unit 10, transparent substrate 11, first transparent conductive layer 12, quantum dot layer 13, second transparent conductive layer 14
[0047] Spacer 20, sealant 30, rigid plate 40
[0048] Glue tank 51, adhesive a, vacuum chamber 52, adhesive 60, sealant 70. Detailed Implementation
[0049] The embodiments of the present invention will now be described in detail. The embodiments described with reference to the accompanying drawings are exemplary, and the embodiments of the present invention will be described in detail below. (Referring to...) Figures 4-6 A method for fabricating a quantum dot unit 10 according to an embodiment of the present invention is described.
[0050] Specifically, the quantum dot unit 10 includes a transparent substrate 11, a first transparent conductive layer 12, a quantum dot layer 13, and a second transparent conductive layer 14. The first transparent conductive layer 12 and the quantum dot layer 13 are located on one side of the transparent substrate 11 and are disposed sequentially away from the transparent substrate 11. The second transparent conductive layer 14 is located on the other side of the transparent substrate 11, or on the side of the quantum dot layer 13 away from the transparent substrate 11. For example, refer to... Figure 5 The quantum dot unit 10 includes a transparent substrate 11, a first transparent conductive layer 12, a quantum dot layer 13, and a second transparent conductive layer 14 arranged sequentially. The fabrication steps of the quantum dot unit 10 include:
[0051] S11. Coat one side of the transparent substrate 11 with a first photoresist layer;
[0052] S12, Exposure and development, a portion of the first photoresist layer is retained and forms the first residual portion;
[0053] S13. A first transparent conductive layer 12 is deposited on the exposure and development side of the transparent substrate 11;
[0054] S14. Peel off the first residual portion. The first transparent conductive layer 12 has a first protrusion located on one side of the peeled area. The first protrusion is used to connect with the first electrode.
[0055] S15. Coat the side where the first transparent conductive layer 12 is located with a quantum dot layer 13;
[0056] S16. Apply the second photoresist layer;
[0057] S17, Exposure and development, a portion of the second photoresist layer is retained and forms a second residual portion, the second residual portion and the first residual portion are disposed near the same edge of the transparent substrate 11;
[0058] S18. A second transparent conductive layer 14 is deposited on the exposure and development side of the transparent substrate 11;
[0059] S19. Peel off the second residual portion. The second transparent conductive layer 14 has a second protrusion located on one side of the second residual portion. The second protrusion is used to connect with the second electrode. The second protrusions are staggered from each other.
[0060] Therefore, the quantum dot unit 10 forms a transparent conductive layer by depositing a first transparent conductive layer 12 and a second transparent conductive layer 14, so as to achieve independent application of electric field to each quantum dot unit 10, thereby enabling independent display of the quantum dot unit 10. When the quantum dot unit 10 is applied to a three-dimensional display element, the display effect of the three-dimensional display element is improved.
[0061] In some embodiments, a solution containing quantum dots is spin-coated onto one side of a transparent substrate 11. The quantum dots can be oil-soluble or water-soluble. The thickness of the spin-coated quantum dot layer 13 is d1, where d1 satisfies the following condition: 0.05 μm ≤ d1 ≤ 10 μm. The spin-coating speed is determined by the required thickness and the viscosity of the solution.
[0062] Furthermore, the thickness of the transparent substrate 11 is d2, which satisfies: 0.1mm ≤ d2 ≤ 0.5mm. The parallelism and flatness errors of the upper and lower light surfaces of the transparent substrate 11 are controlled within ±2μm. The length of the transparent substrate 11 is a, and the width of the transparent substrate 11 is b, where a and b satisfy: 1mm ≤ a ≤ 500mm and 1mm ≤ b ≤ 500mm, respectively. For example, the transparent substrate 11 can be inspected to ensure that the parallelism and flatness errors of the upper and lower light surfaces do not exceed ±2μm. Therefore, the size of the transparent substrate 11 is suitable, which is beneficial to the production and processing of the quantum dot unit 10.
[0063] For example, the transparent substrate 11 can be a glass plate. Preparing the transparent substrate 11 includes fabricating the glass plate using a float glass process, overflow stretching process, slit stretching process, or double stretching process. For example, when preparing the transparent substrate 11, an ultra-thin glass plate fabricated using processes such as float glass process, overflow stretching process, slit stretching process, and double stretching process can be selected. The substrate thickness is 0.1-5mm, and the preferred length a and width b of the glass unit are: 1mm≤a≤500mm, 1mm≤b≤500mm. Alternatively, a resin-based transparent plate can also be selected as the transparent substrate 11.
[0064] In some embodiments, a transparent glass plate serves as the transparent substrate 11. Specifically, the first transparent conductive layer 12 and the second transparent conductive layer 14 can be made of indium tin oxide (i.e., ITO) or other transparent conductive materials. When an ITO layer is used as the transparent conductive layer, a first ITO layer is deposited on the transparent substrate 11, a layer of light-emitting quantum dots is spin-coated on the first ITO layer, and finally a second ITO layer is deposited on the light-emitting quantum dot layer 13. The majority carriers of the first ITO layer and the second ITO layer are different, i.e., one is n-type ITO and the other is p-type ITO. In this way, a PN junction structure of ITO-quantum dot-ITO is formed on a single transparent substrate 11. The refractive index (i.e., the refractive index of ITO) of the first transparent conductive layer 12 and the second transparent conductive layer 14 is similar to the refractive index of the transparent glass plate, with an error of no more than 0.01. The ITO deposition method can be magnetron sputtering, vacuum reactive evaporation, chemical vapor deposition, sol-gel deposition, or pulsed laser deposition. Preferably, magnetron sputtering is used because it is fast and produces a dense and highly uniform ITO film. A solution containing quantum dots is spin-coated onto one side of the ITO-coated transparent substrate 11. The quantum dots can be oil-soluble or water-soluble. The thickness of the spin-coated quantum dot layer 13 ranges from 0.05 μm to 10 μm, and the spin-coating speed is determined by the desired thickness and the viscosity of the solution.
[0065] like Figure 1 As shown, a method for fabricating a quantum dot composite 100 according to a second aspect embodiment of the present invention includes:
[0066] S1. A first transparent conductive layer 12, a quantum dot layer 13, and a second transparent conductive layer 14 are sequentially disposed on one side of the transparent substrate 11 to form a quantum dot unit 10. Specifically, when preparing the transparent substrate 11, an ultra-thin glass plate manufactured by processes such as float glass, overflow stretching, slit stretching, and double stretching can be selected. The substrate thickness is 0.1-5mm. The surface shape of the glass plate is inspected to ensure that the parallelism and flatness error of the upper and lower smooth surfaces does not exceed ±2μm. The preferred length a and width b of the glass unit are: 1mm≤a≤500mm, 1mm≤b≤500mm. Alternatively, a resin-based transparent plate can also be selected as the substrate.
[0067] Transparent glass serves as the transparent substrate 11. Specifically, the transparent conductive layer can be made of ITO or other transparent conductive materials. When an ITO layer is used as the transparent conductive layer, a first ITO layer is deposited on the transparent substrate 11, a layer of light-emitting quantum dots is spin-coated on the first ITO layer, and finally a second ITO layer is deposited on the light-emitting quantum dot layer 13. The majority carriers of the first ITO layer and the second ITO layer are different, that is, one is n-type ITO and the other is p-type ITO. In this way, a PN junction structure of ITO-quantum dot-ITO is formed on a single transparent substrate 11. The refractive index of ITO is similar to that of the transparent glass plate, with an error of no more than 0.01. The ITO deposition method can be magnetron sputtering, vacuum reactive evaporation, chemical vapor deposition, sol-gel method, and pulsed laser deposition. Magnetron sputtering is preferred because it has a fast ITO deposition speed and produces a dense and highly uniform film. A solution containing quantum dots is spin-coated onto one side of a transparent substrate 11 coated with ITO. The quantum dots can be oil-soluble or water-soluble. The thickness of the spin-coated quantum dot layer 13 ranges from 0.05 μm to 10 μm, and the spin-coating speed is determined by the desired thickness and the viscosity of the solution. Following this method, quantum dots of three different colors—red, green, and blue—are spin-coated onto different substrates.
[0068] S2. Bonding multiple quantum dot units 10 together.
[0069] S3. Trim the bonded quantum dot units 10 to obtain a quantum dot composite 100.
[0070] Trimming the bonded quantum dot units 10 may include leveling, curing, trimming, polishing, etc.
[0071] The processing technology proposed in this invention can significantly improve the uniformity of the luminescent surfaces of each layer of bulk material used for 3D display, increase luminous contrast, improve material transparency, enhance depth resolution, and increase the viewing angle of 3D images.
[0072] In some embodiments, a plurality of quantum dot units 10 are bonded together, the bonding method comprising:
[0073] S21. A spacer 20 is provided on at least one side of each quantum dot unit 10. The spacer 20 is a transparent polymer material, resin, optical glass, or optical crystal.
[0074] Specifically, the spacer 20 can be any one of the following shapes: frustum, cylinder, elliptical cylinder, oblong cylinder, cuboid, prism, sphere, or ellipsoid.
[0075] S22. Multiple quantum dot units 10 are stacked to form a laminate, with adjacent quantum dot units 10 separated by spacers 20 to form gaps for accommodating adhesive 60.
[0076] S23. Seal two opposing sides of the laminate, and form an inlet and outlet surface for the glue by forming two other opposing sides.
[0077] S24. Apply adhesive 60 to the injection surface to fill the gap, so that the cured adhesive layer containing spacers 20 is formed between adjacent quantum dot units 10.
[0078] In some embodiments, the height of the spacer 20 is 1μm-500μm, the distance between adjacent spacers 20 is 0.1mm-5mm, the height error of multiple spacers 20 is ≤2μm, and the spacers 20 are preferably distributed in a matrix pattern. Spacers 20 of equal thickness are pre-formed discretely in a regular array so that, after stacking, adjacent coating units are raised by the spacers 20 to form gaps of equal thickness.
[0079] This ensures the parallelism of each quantum dot unit 10, and also makes the final quantum dot composite 100 have better parallelism and flatness.
[0080] The spacer 20 can be set using any of the following methods:
[0081] 1) The spacer 20 is made of a material containing a fast-curing resin, using transparent UV adhesive spraying or screen printing. For example, after droplet formation, it can be rapidly cured by UV light to ensure the uniformity of the spacer 20's height. The shape of the spacer 20, viewed from above, can be circular, square, linear, or other patterns, preferably a circular dot pattern with a dot diameter of 0.05-2mm.
[0082] 2) Photolithography or etching method: Photoresist is applied to the surface to be etched, then exposed, developed, etched, and the remaining photoresist is removed. The photoresist can be positive or negative. Fabricating spacers 20 using photolithography or etching means directly applying photoresist to the surface to be etched, followed by exposure, development, etching, and removal of the remaining photoresist. The photoresist used can be positive or negative. The etching can be wet or dry. When fabricating spacers 20 using the photolithography-etching method, surfaces that do not require etching need to be protected with spin-coated photoresist.
[0083] 3) Nanoimprinting and nanotransfer.
[0084] In some embodiments, the distance between adjacent spacers 20 is 5μm-20mm, and the spacers 20 can be any one of silica microspheres, polystyrene microspheres, or polymethyl methacrylate microspheres. The spherical diameter of the spacers 20 is 1μm-200μm, and the uniformity error of the diameter is <10%.
[0085] Therefore, by using the above-mentioned spacer 20 dimensions, and with the spacer 20 layer impregnated and covered by adhesive, the spacer 20 will not interfere with the optical path.
[0086] Furthermore, before sealing or before the adhesive cures at 60°C, the parallelism and flatness of the laminate are adjusted to control the error within ±5μm. This ensures the processing accuracy of the laminate.
[0087] In some embodiments, the laminate is sealed using a liquid sealant or a solid sealant. The liquid sealant is an epoxy resin or an acrylic resin, while the solid sealant is a rubber sheet or silicone sealant. The viscosity of the liquid sealant is >20000 cps, and the curing method is natural curing at room temperature, heat curing, or ultraviolet light curing. The Shore hardness of the cured liquid sealant is 20A-70A. This results in a better sealing effect on the laminate and ensures the hardness and strength of the sealant region 30 of the laminate.
[0088] Furthermore, the adhesive 60 is degassed before injection. The viscosity of the adhesive 60 is <500cps. The adhesive 60 is an epoxy resin or acrylic resin. The volume shrinkage rate of the adhesive 60 after curing is <1.1%. The Shore hardness of the adhesive 60 after curing is 60D-80D. The refractive index of the adhesive 60 after curing is consistent with that of the transparent substrate 11. Thus, using the above-mentioned adhesive 60 results in better adhesion.
[0089] In some embodiments, potting is performed in any of the following ways:
[0090] 1) First gravity injection method: The glue inlet surface of the laminate is placed in the glue pool 51 of the gravity glue inlet device. The glue inlet device and the glue inlet surface are sealed by sealing material or tooling. The laminate together with the glue inlet device is placed in the vacuum chamber 52. The glue fills the gap under the combined action of gravity and capillary action. When it is observed that the adhesive 60 is uniformly seeping out from all parts of the glue outlet surface, the vacuum device is closed to complete the glue 60 injection.
[0091] 2) Second gravity injection method: The glue inlet surface of the laminate is placed in the glue pool 51 of the gravity glue inlet device. The glue inlet device and the glue inlet surface are sealed together by sealing material or tooling. A vacuum device is connected at the glue outlet surface. The vacuum device wraps the entire glue outlet surface of the laminate and isolates the glue outlet surface from the outside world by sealing material or tooling. The absolute vacuum degree of the vacuum device is <10 kPa. When it is observed that the adhesive 60 is uniformly seeping out from all parts of the glue outlet surface, the vacuum device is turned off to complete the glue 60 injection.
[0092] 3) First pressure injection method: The glue injection surface of the laminate is placed in the glue of the pressure injection device. The glue injection device and the glue injection surface are sealed by sealing material or tooling. Mechanical pressure is applied to the glue to fill the gap. The pressure injection device is equipped with a pressure sensor to monitor and adjust the pressure and control the injection speed. When it is observed that the adhesive 60 is uniformly seeping out from all parts of the glue injection surface, the pressure application device is turned off to complete the injection of adhesive 60.
[0093] 4) Second pressure injection method: Place the glue inlet surface of the laminate into the glue in the pressure injection device. The glue inlet device and the glue inlet surface are sealed together by sealing material or tooling. Apply atmospheric pressure to the glue to fill the gap. The pressure injection device is equipped with a gas flow valve to monitor and adjust the air pressure and control the glue injection speed. When it is observed that the adhesive 60 is uniformly seeping out from all parts of the glue outlet surface, turn off the pressure application device to complete the injection of adhesive 60.
[0094] 5) Vacuum infusion method: Immerse the glue inlet surface of the laminate in the glue pool 51 containing adhesive 60, so that the entire glue inlet surface is sealed by adhesive 60. Then, connect a vacuum device to the glue outlet surface. The vacuum device wraps the entire glue outlet surface of the laminate and isolates the glue outlet surface from the outside world by sealing material or tooling. The absolute vacuum degree of the vacuum device is <10 kPa. When it is observed that adhesive 60 is uniformly seeping out from all parts of the glue outlet surface, turn off the vacuum device to complete the glue 60 infusion.
[0095] Therefore, using the above method for glue application results in higher bonding efficiency.
[0096] In some embodiments, a plurality of quantum dot units 10 are bonded together, the bonding method comprising:
[0097] S25. After applying adhesive 60 to the first quantum dot unit 10, take the second quantum dot unit 10 and place it on the adhesive 60 for bonding, and so on, to form a stacked structure.
[0098] S26. Adjust the parallelism and flatness of the laminated structure before curing.
[0099] In this way, there is no need to set spacers 20. By using a spin coating method, the spacing between adjacent quantum dot units 10 is smaller, and the impact on the optical path is smaller.
[0100] In some embodiments, the adhesive 60 preferably has a viscosity of <1000 cps, is an epoxy resin or acrylic resin, has a volume shrinkage rate of <1.1% after curing, and has a Shore hardness of 60D-80D after curing. Therefore, using the aforementioned adhesive 60 in the above-described lamination bonding method results in better bonding performance.
[0101] A method for fabricating a three-dimensional display element according to a third aspect of the present invention includes: the method for fabricating the quantum dot composite 100 described above; and providing a first electrode electrically connected to a first transparent conductive layer 12 of each quantum dot unit 10 and a second electrode electrically connected to a second transparent conductive layer 14 of each quantum dot unit 10 outside the quantum dot composite 100; attaching a circuit board to one side of the quantum dot composite 100 and connecting the circuit board to the electrode 200.
[0102] In this way, by connecting the first and second electrodes to the circuit, the quantum dot can achieve a high photoluminescence quantum efficiency without an electric field. When a certain electric field is applied, the photoluminescence quantum efficiency decreases, even approaching zero. Almost all the photons absorbed by the quantum dot are emitted in a non-radiative relaxation manner. After the electric field is removed, the luminescence efficiency of the quantum dot can be restored to the initial state.
[0103] According to a fourth aspect of the present invention, a quantum dot composite 100 includes a plurality of quantum dot units 10 sequentially stacked and bonded in the thickness direction. Each quantum dot unit 10 includes a transparent substrate 11, a first transparent conductive layer 12, a second transparent conductive layer 14, and a quantum dot layer 13. The first transparent conductive layer 12 and the quantum dot layer 13 are located on one side of the transparent substrate 11 and are sequentially disposed away from the transparent substrate 11. The second transparent conductive layer 14 is located on the other side of the transparent substrate 11 or outside the quantum dot layer 13. The first transparent conductive layer 12 is a P-type semiconductor, and the second transparent conductive layer 14 is an N-type semiconductor. The quantum dot layer 13, the first transparent conductive layer 12, and the second transparent conductive layer 14 of the same quantum dot unit 10 or adjacent quantum dot units 10 together form a PN junction.
[0104] This invention proposes a novel quantum dot composite 100, which utilizes the effect of reduced luminescence efficiency of photoluminescent quantum dots under electric field modulation. By using a composite technique of quantum dots, transparent conductive materials and other transparent materials, a bulk structure with multi-layered multicolor luminescent quantum dot units 10 is fabricated. Then, a laser scanning system and an electric field modulation system are used to scan a three-dimensional pattern in the bulk structure.
[0105] Quantum dots exhibit high photoluminescence quantum efficiency without an applied electric field. However, when an electric field is applied, the photoluminescence quantum efficiency decreases, even approaching zero, as almost all photons absorbed by the quantum dots are emitted through non-radiative relaxation. After the electric field is removed, the photoluminescence efficiency returns to its initial state. This characteristic of quantum dots is called the quantum dot electric field modulation switching effect. The switching ratio is the ratio of the light emission intensity of the quantum dots without an applied electric field to that with an applied electric field, while keeping the excitation light parameters constant. Preferably, the switching ratio is greater than 20.
[0106] To ensure that the brightness of the luminescent points before and after the laser incident surface of the bulk material is the same under the same conditions, and to offset the energy loss of the laser through the quantum dot unit 10, the thickness of the quantum dot unit 10 on the laser incident surface of the bulk material must increase from front to back. In other words, one side surface of the quantum dot composite 100 is formed as the laser incident surface, and along the stacking direction of the quantum dot unit 10, the thickness of the quantum dot unit 10 increases the further away from the laser incident surface.
[0107] In some embodiments, the thickness of the quantum dot layer 13 is 0.05 μm-10 μm; and / or the thickness of the transparent substrate 11 is 0.1 mm-0.5 mm. The parallelism and flatness errors of the upper and lower optical surfaces of the transparent substrate 11 do not exceed ±2 μm, and the length a and width b of the transparent substrate 11 satisfy: 1 mm ≤ a ≤ 500 mm, 1 mm ≤ b ≤ 500 mm. Thus, by using the above-mentioned dimensions for the quantum dot layer 13, the quantum dot composite 100 fabricated has a more compact structure.
[0108] Optionally, each quantum dot unit 10's quantum dot layer 13 emits light of the same color when illuminated. The structure of the monochromatic quantum dot composite 100 is as follows: single-color emitting quantum dot light-emitting layer units are arranged periodically, and the layer units are bonded together with transparent adhesive. Electrodes 200 are fabricated on both sides of each quantum dot layer 13. The function of the electrodes 200 is to apply an electric field of adjustable magnitude and direction to the quantum dots.
[0109] Optionally, every three adjacent quantum dot units 10 are divided into a color adjustment group. When the quantum dot layer 13 of the three quantum dot units 10 in each group is irradiated, it emits red, green, and blue light, respectively. For example, the arrangement of the unit layers is as follows: red-emitting quantum dot units 10, green-emitting quantum dot units 10, and blue-emitting quantum dot units 10. The three colors of quantum dot units 10 are arranged periodically, and the unit layers are bonded together with transparent adhesive. Each quantum dot unit 10 has transparent electrodes 200 on both sides. The function of the electrodes 200 is to apply an electric field of adjustable magnitude and direction to the quantum dots.
[0110] According to a fifth aspect of the present invention, a three-dimensional display element includes: a quantum dot composite 100 as described above and a circuit board, wherein the circuit board is electrically connected to a first transparent conductive layer 12 and a second transparent conductive layer 14 of each quantum dot unit 10 via a first electrode and a second electrode, respectively.
[0111] Advantages of 3D display elements modulated by electric and light fields compared to 3D displays using liquid crystal stacks:
[0112] 1. Higher image frame rate: The modulation time of a single-layer electric field modulation quantum dot screen is less than 10μs, while the single refresh time of a liquid crystal layer is in the millisecond range.
[0113] 2. Higher vertical resolution in 3D imaging: Due to the slow refresh rate of the liquid crystal layer, the resolution in the 3D display depth direction is limited. For example, with a refresh rate of 1ms and a human visual persistence effect of 25Hz, the maximum number of liquid crystal layers that can be stacked is 40. To stack more layers, the frame rate must be sacrificed. A single-layer electric field modulated quantum dot screen has a modulation time of less than 10μs. Using 10μs and 25Hz as an example, 4000 layers can be stacked.
[0114] 3. Wider viewing angle: Due to the limitations of the LCD screen bezel, the viewing angle of the LCD stacked 3D display is limited to a small angle from the front, and cannot be viewed from the side or back. However, the 3D display system based on dual modulation of light and electric fields can be viewed from all directions except for a small area on the surface where the electrodes 200 are arranged.
[0115] 4. Higher color gamut: The light source of the liquid crystal stacked 3D display system is LED backlight, while the 3D display system based on dual modulation of light field and electric field uses photoluminescent quantum dots. As is well known, quantum dots have a higher color gamut than LEDs.
[0116] The manufacturing process of the quantum dot composite 100 in two specific embodiments is briefly described below.
[0117] Example 1: Fabrication of 100 quantum dot composites using the siphon method
[0118] like Figure 2 The fabrication process of the quantum dot composite 100 as an example
[0119] 1) Preparation of transparent base plate 11: Figure 3 For transparent substrates, ultra-thin glass sheets are manufactured using processes such as float glass, overflow stretching, slit stretching, and double stretching. The substrate thickness is 0.1-5mm. The glass sheets undergo surface inspection to ensure that the parallelism and flatness errors of the upper and lower smooth surfaces do not exceed ±2μm. The preferred dimensions of the transparent substrate 11 are: length a ≤ a ≤ 500mm, width b ≤ 1mm ≤ b ≤ 500mm. Alternatively, resin-based transparent sheets can also be used as the substrate.
[0120] 2) Quantum dot application process:
[0121] like Figure 4 Fabrication process for a single-layer quantum dot unit 10 structure. Figure 5 For the shape characteristics of each layer structure, the transparent substrate 11 is transparent glass. A first ITO layer is deposited on the transparent substrate 11, a quantum dot 13 is spin-coated on the first ITO layer, and finally a second ITO layer is deposited on the quantum dot layer 13. The majority carriers of the first ITO layer and the second ITO layer are different, that is, one is n-type ITO and the other is p-type ITO. In this way, an ITO-quantum dot-ITO PN junction structure is formed on a single transparent substrate 11. The refractive index of ITO is similar to that of the transparent glass plate, with an error of no more than 0.01. The ITO deposition method can be magnetron sputtering, vacuum reactive evaporation, chemical vapor deposition, sol-gel method and pulsed laser deposition. Magnetron sputtering is preferred because magnetron sputtering ITO deposition speed is fast and the film layer is dense and highly uniform. A solution containing quantum dots is spin-coated onto one side of a transparent substrate 11 coated with ITO. The quantum dots can be oil-soluble or water-soluble. The thickness of the spin-coated quantum dot layer 13 ranges from 0.05 μm to 10 μm, and the spin-coating speed is determined by the desired thickness and the viscosity of the solution. Using this method, quantum dots of three different colors are spin-coated onto different substrates: red-emitting quantum dots and green-emitting quantum dots.
[0122] In addition, N-type ITO can also be selected from other N-type transparent semiconductor materials, and P-type ITO can also be selected from other P-type transparent semiconductor materials.
[0123] To ensure that the brightness of the light-emitting points on the front and back of the laser incident surface of the bulk material is the same under the same conditions, and to offset the energy loss of the laser through the quantum dot unit 10, the thickness of the quantum dot layer 13 on the laser incident surface of the bulk material is required to increase from front to back.
[0124] 3) Fabrication of spacers 20: Spacer 20 forming process: Spacers 20 of equal thickness are formed in a regular array in advance, so that after stacking, adjacent coating units are raised by the spacers 20 to form gaps of equal thickness.
[0125] The spacer 20 can be formed by: spraying transparent UV adhesive and printing ( Figure 7 ), screen printing, photolithography-etching method ( Figure 8 Nanoimprinting, nanotransfer, etc. The height of the spacer 20 is 1-500μm, the distance between adjacent spacers 20 is 0.1-5mm, the height error of the spacer 20 is ≤2μm, and the spacer 20 is preferably distributed in a matrix.
[0126] UV adhesive printing is used. Figure 7 When manufacturing spacers 20 using processes such as screen printing, materials containing fast-curing resin are preferred for spacers 20. For example, after droplet molding, they can be rapidly cured by UV light to ensure the uniformity of the height of spacers 20. The shape of spacers 20, viewed from above, can be circular, square, linear, or other patterns, with circular dot patterns being preferred, and the diameter of the dots being 0.05-2mm.
[0127] Photolithography or etching methods are used. Figure 8 Fabricating spacer 20 refers to directly applying photoresist to the surface to be etched, followed by exposure, development, etching, and removal of excess photoresist. The photoresist used can be positive or negative. The etching can be wet or dry. When fabricating spacer 20 using the photolithography-etching method, the surfaces that do not need to be etched need to be protected by spin-coating with photoresist.
[0128] In addition, other uniformly sized granular materials can be used as spacers 20, uniformly dispersed between two layers of substrate units spin-coated with luminescent quantum dots. The distance between two adjacent particles is D, wherein D satisfies: 5μm≤D≤20mm. The external dimensions of the spacers 20 can be frustum-shaped, cylindrical, elliptical cylindrical, oblong cylindrical, cuboid, prism, spherical, or ellipsoidal. Preferably, they are spherical with a diameter of 1μm-200μm and a diameter uniformity error of <10%. The spacers 20 are applied by spraying microsphere spacers 20. Figure 9 The microsphere spacer 20 can be silica microspheres, polystyrene microspheres, or polymethyl methacrylate microspheres. In addition, the particulate spacer 20 can also be a polymer material component, resin component, optical glass component, or optical crystal component.
[0129] 4) Lay the transparent substrate 11 with the spacer 20 fabricated, such as... Figure 10 .
[0130] For full-color imaging: The stacking rules are as follows: ① The orientation of each quantum dot unit 10 is the same; ② The arrangement rules are as follows: the quantum dot emitting layer units of the three colors, namely red light emitting quantum dot unit 10, green light emitting quantum dot unit 10, and blue light emitting quantum dot unit 10, are arranged periodically.
[0131] For monochrome imaging: the stacking rules are as follows: ① Use quantum dot light-emitting layers of one color to stack; ② The orientation of each quantum dot unit 10 is the same.
[0132] 5) Adjusting the parallelism and flatness of the laminated body, such as... Figure 11 The stacked layers are clamped using a rigid plate 40 or an airbag. The parallelism and flatness of the top and bottom units are adjusted using a parallelism adjustment device to control the error within ±5μm. This corrects the cumulative parallelism and flatness errors caused by uneven thicknesses of the spacer 20, transparent substrate 11, and spin-coated quantum dot layer 13. This process can also be performed after potting but before the adhesive 60 cures.
[0133] 6) Sealing process: Select two opposite faces from the four surfaces of the laminate perpendicular to the lamination direction as sealing surfaces, and seal them with sealant 30. Figure 12 The sealant 30 can be a solid or liquid sealing material. If it is a liquid sealing material, the viscosity is preferably >20000cps. The liquid sealant 30 is made of epoxy resin or acrylic resin. The liquid sealant 30 can be cured by natural curing at room temperature, heat curing, or ultraviolet light curing. After curing, the liquid sealant 30 has a Shore hardness of 20A-70A. If it is a solid sealing material, a rubber sheet or silicone sealant with good ductility can be selected. By tightly pressing and adhering it to the sealing surface with tooling, a sealing effect can also be achieved.
[0134] 7) Glue application process
[0135] Two of the four faces of the laminate parallel to the lamination direction are selected, one as the adhesive inlet and the other as the adhesive outlet. The cured adhesive 60 enters the spacer layer in the middle of the substrate unit from the adhesive inlet and is led out from the adhesive outlet, achieving uniform filling of each spacer layer and completing the potting process. The adhesive 60 preferably has a viscosity <500 cps, and is cured by heat curing or natural curing at room temperature. The adhesive 60 is preferably epoxy resin or acrylic resin. Preferably, the volume shrinkage rate of the cured adhesive 60 is <1.1%, and the Shore hardness of the cured adhesive 60 is 60D-80D. The adhesive 60 is degassed before potting, and its color is preferably transparent. After curing, its refractive index is similar to that of the transparent substrate 11 with an error of less than 0.01.
[0136] There are gravity injection, pressure injection and vacuum injection methods for glue injection.
[0137] Gravity injection method 1: Place the glue injection surface of the laminate in the gravity injection device, and in the glue, such as... Figure 13 The glue injection device and the glue injection surface are sealed together by sealing material or tooling. The laminated body together with the gravity glue injection device is placed in the vacuum chamber 52. The adhesive a fills the spacer layer under the combined action of its own gravity and capillary action. When it is observed that the adhesive 60 is uniformly seeping out from all parts of the glue outlet, the pressure application device can be turned off to complete the injection of adhesive 60.
[0138] Gravity injection method 2: Place the glue injection surface of the laminate into the glue in the gravity injection device, such as... Figure 14 The glue inlet device and the glue inlet surface are sealed together using sealing material or tooling. A vacuum device is then connected to the glue outlet surface, enclosing the entire glue outlet surface of the laminate and isolating it from the outside environment using sealing material or tooling to ensure no air leakage occurs during vacuuming. The absolute vacuum level of the vacuum device is preferably <10 kPa. When adhesive 60 is observed to be uniformly seeping from all parts of the glue outlet surface, the vacuum device can be turned off, completing the adhesive 60 infusion.
[0139] Pressure injection method 1: Place the glue inlet surface of the laminate into the glue in the pressure injection device, such as... Figure 15 The glue dispensing device and the glue dispensing surface are sealed together using sealing material or tooling. Mechanical pressure is applied to the glue to fill the spacer layer. The pressure dispensing device is equipped with a pressure sensor to monitor and adjust the pressure, controlling the dispensing speed. When adhesive 60 is observed to be evenly seeping out from all parts of the glue dispensing surface, the pressure application device can be turned off, completing the glue 60 dispensing.
[0140] Pressure injection method 2: Place the glue inlet surface of the laminate into the glue in the pressure injection device, such as... Figure 16 The glue dispensing device and the glue dispensing surface are sealed together using sealing material or tooling. Atmospheric pressure is applied to the glue to fill the spacer layer. The pressure dispensing device is equipped with a gas flow valve to monitor and adjust the air pressure and control the glue dispensing speed. When it is observed that the adhesive 60 is evenly seeping out from all parts of the glue dispensing surface, the pressure application device can be turned off, completing the glue 60 dispensing.
[0141] Vacuum infusion method: The glue-injecting surface of the laminate is immersed in a glue tank 51 containing adhesive 60, such as... Figure 17The entire inlet surface is sealed with adhesive 60. A vacuum device is then connected to the outlet surface, enclosing the entire outlet surface of the laminate and isolating it from the outside environment using sealing material or tooling to ensure no air leakage occurs during vacuuming. The absolute vacuum level of the vacuum device is preferably <10 kPa. When adhesive 60 is observed to be uniformly seeping from all parts of the outlet surface, the vacuum device can be turned off, completing the adhesive 60 infusion process.
[0142] 8) Curing and heat treatment processes.
[0143] After the adhesive 60 is poured in, it can be cured by heating or placing it at a constant temperature for a period of time, and internal stress can be eliminated by necessary heat treatment to obtain the laminate. Before curing, the parallelism of the top and bottom coating units of the laminate can be corrected by a parallelism adjustment device. For example, the laminate can be pressed by a precision hydraulic device with a pressing force of not less than 20 kPa. The parallelism and flatness of the working surface of the press are corrected by the laminate and maintained until the adhesive 60 is cured.
[0144] 9) Trimming and polishing process: Trimming and polishing are carried out on the laminated blocks after curing. The purpose of trimming is to process the laminated blocks into an approximately standard cube. Then, each face of the laminated blocks is polished to maintain high light transmittance and prepare for the next process.
[0145] 10) Electrode 200 fabrication: Electrode 200 is fabricated by photolithography and film deposition on one of the four surfaces of the laminate perpendicular to the lamination direction. Electrode 200 is applied to each ITO layer. Figure 18 Furthermore, it is ensured that there is no short circuit between the ITO layers. The electrode 200 material can be gold or silver, with gold being the preferred material.
[0146] 11) Attaching the printed circuit board and bonding wires: Attach the circuit board according to specifications to the side where the electrode 200 is fabricated, and use an ultrasonic wire bonder to connect the electrode 200 on the laminate to the printed circuit board. To achieve a wider viewing angle, it is preferable to fabricate the electrode 200 on only one side. By applying voltage to the ITO layers on both sides of the quantum dot layer 13 through the control system, the luminous efficiency of the quantum dots in the electric field will decrease, even approaching zero. By controlling the magnitude of the applied electric field and the red, green, and blue quantum dots, full-color three-dimensional display can be achieved.
[0147] Example 2: Fabrication of laminated materials using lamination method
[0148] To complete Figure 5 The unit layer of the process is used to perform the stacked process.
[0149] The lamination process is as follows: Figure 19 , Figure 20 , Figure 21Take one piece to complete. Figure 5 One flat plate from the process is placed on a flat fixture, with the top side coated with an "I"-shaped adhesive at 60%. Then, another plate is taken out and completed. Figure 5 A plate in the process is placed on the adhesive 60, with the quantum dot units 10 on the first plate facing the same direction, i.e., all quantum dot units 10 are facing upwards or downwards. The adhesive 60 preferably has a viscosity of <1000cps, and is cured by heat curing or natural curing at room temperature. The adhesive 60 is an epoxy resin or an acrylic resin. Preferably, the volume shrinkage rate of the adhesive 60 after curing is <1.1%, and the Shore hardness of the adhesive 60 after curing is 60D to 80D. The adhesive 60 is degassed before being poured in. The adhesive 60 is transparent, and its refractive index after curing is similar to that of the transparent substrate 11, with an error of less than 0.01.
[0150] For full-color imaging: The stacking rules are ①. The orientation of each quantum dot unit 10 is the same; ② The arrangement rules are: the quantum dot emitting layer units of the three colors, namely red light emitting quantum dot unit 10, green light emitting quantum dot unit 10, and blue light emitting quantum dot unit 10, are arranged periodically.
[0151] For monochrome imaging: the stacking rules are as follows: ① use quantum dot light-emitting layers of one color stacked together; ② the orientation of each quantum dot unit 10 is the same.
[0152] 5) Adjustment of parallelism and flatness of the stacked body: The parallelism and flatness of the top and bottom units of the stacked body are adjusted by the parallelism adjustment device to control the error within ±5μm, so as to correct the cumulative parallelism and flatness error caused by the uneven thickness of the spacer 20, the transparent substrate 11 and the spin-coated quantum dot units 10.
[0153] 6) Curing and heat treatment processes.
[0154] After the adhesive 60 is poured, it can be cured by heating or placing it at a constant temperature for a period of time, and internal stress can be eliminated by using the necessary heat treatment methods to obtain the laminated block.
[0155] 7) Trimming and polishing process: Trimming and polishing are carried out on the laminated blocks after curing. The purpose of trimming is to process the laminated blocks into an approximately standard cube. Then, each face of the laminated blocks is polished to maintain high light transmittance and prepare for the next process.
[0156] 8) Electrode 200 fabrication: Electrode 200 is fabricated by photolithography and film deposition on one of the four surfaces of the stack perpendicular to the stacking direction. Electrode 200 is attached to each ITO layer, and it is ensured that there is no short circuit between ITO layers. The electrode 200 material can be gold or silver, with gold being the preferred material.
[0157] 9) Attaching printed circuit boards and wire bonding: Attach a circuit board made to specifications to the side of the electrode 200 that has been made, and use an ultrasonic wire bonding machine to connect the electrode 200 on the laminate to the printed circuit board. To achieve a wider viewing angle, it is preferable that the electrode 200 is made on an edge close to the bulk material.
[0158] In the description of this invention, it should be understood that the terms "center," "longitudinal," "lateral," "length," "width," "thickness," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," "outer," "clockwise," "counterclockwise," "axial," "radial," and "circumferential" indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are used only for the convenience of describing this invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this invention.
[0159] In the description of this invention, "first feature" and "second feature" may include one or more of the features. In the description of this invention, "a plurality of" means two or more. In the description of this invention, "above" or "below" the second feature may include direct contact between the first and second features, or it may include contact between the first and second features not being in direct contact but through another feature between them. In the description of this invention, "above," "over," and "on top" of the second feature includes the first feature being directly above or diagonally above the second feature, or simply indicating that the first feature is at a higher horizontal level than the second feature.
[0160] In the description of this specification, references to terms such as "one embodiment," "some embodiments," "illustrative embodiment," "example," "specific example," or "some examples," etc., refer to specific features, structures, materials, or characteristics described in connection with that embodiment or example, which are included in at least one embodiment or example of the present invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example.
[0161] Although embodiments of the invention have been shown and described, those skilled in the art will understand that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the claims and their equivalents.
Claims
1. A method for fabricating quantum dot units, characterized in that, The quantum dot unit includes a transparent substrate, a first transparent conductive layer, a quantum dot layer, and a second transparent conductive layer. The first transparent conductive layer and the quantum dot layer are located on one side of the transparent substrate and are sequentially disposed away from the transparent substrate. The second transparent conductive layer is located on the other side of the transparent substrate, or on the side of the quantum dot layer away from the transparent substrate. The processing method of the quantum dot unit includes: Prepare the transparent substrate; A first photoresist layer is coated on one side of the transparent substrate; Exposure and development occur, and a portion of the first photoresist layer is retained to form a first residual portion; The first transparent conductive layer is deposited on the exposure and development side of the transparent substrate; After peeling off the first residual portion, a first protrusion located on one side of the peeled area is formed on the first transparent conductive layer. The quantum dot layer is coated on the side of the first transparent conductive layer away from the transparent substrate; Apply the second photoresist layer; Exposure and development are performed, and a portion of the second photoresist layer is retained to form a second residual portion, which is located near the same edge of the transparent substrate as the first residual portion. A second transparent conductive layer is deposited on the exposure and development side of the transparent substrate; After peeling off the second residual portion, the second transparent conductive layer is formed with a second protrusion located on one side of the second residual portion, and the second protrusion is offset from the first protrusion.
2. The method for fabricating quantum dot units according to claim 1, characterized in that, The thickness of the quantum dot layer is d1, and d1 satisfies: 0.05μm≤d1≤10μm.
3. The method for fabricating quantum dot units according to claim 1, characterized in that, The thickness of the transparent substrate is d2, which satisfies: 0.1mm≤d2≤0.5mm, wherein the parallelism and flatness errors of the upper and lower light surfaces of the transparent substrate are controlled within ±2μm.
4. The method for fabricating quantum dot units according to claim 1, characterized in that, The transparent substrate has a length of a and a width of b, wherein a and b satisfy the following conditions: 1mm≤a≤500mm and 1mm≤b≤500mm, respectively.
5. The method for fabricating quantum dot units according to claim 1, characterized in that, The transparent substrate is a glass plate, and the preparation of the transparent substrate includes: The glass plate is manufactured using float glass, overflow stretching, slit stretching, or double stretching processes.
6. The method for fabricating quantum dot units according to claim 1, characterized in that, The transparent substrate is a resin transparent plate.
7. The method for fabricating quantum dot units according to claim 1, characterized in that, The first transparent conductive layer and the second transparent conductive layer are made of indium tin oxide.
8. The method for fabricating quantum dot units according to claim 7, characterized in that, The difference in refractive index between any two of the first transparent conductive layer, the second transparent conductive layer, and the transparent substrate is n, where n ≤ 0.
01.
9. The method for fabricating quantum dot units according to claim 7, characterized in that, The deposition of the first transparent conductive layer and the second transparent conductive layer includes: The methods employed include magnetron sputtering, vacuum reactive evaporation, chemical vapor deposition, sol-gel deposition, or pulsed laser deposition.
10. A method for fabricating quantum dot units according to any one of claims 1-9, characterized in that, One of the first transparent conductive layer and the second transparent conductive layer is a P-type semiconductor, and the other of the first transparent conductive layer and the second transparent conductive layer is an N-type semiconductor. The quantum dot layer, together with the first transparent conductive layer and the second transparent conductive layer, forms a PN junction.
Citation Information
Patent Citations
Quantum dot display device and preparation method and application thereof
CN112652649A
Quantum dot optoelectronic devices with enhanced performance
US20100090195A1