A boron diffusion method and device for a topcon cell
By employing a four-stage temperature-progressive deposition and oxidation process, combined with high-pressure nitrogen purging, the problems of insufficient boron source and PN junction damage in the boron diffusion process were solved, achieving efficient selective emitter doping and improving the photoelectric conversion efficiency and production stability of TOPCon cells.
Patent Information
- Application Number
- CN202310348348.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-03
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-04-03
AI Technical Summary
Existing boron diffusion processes cannot provide sufficient boron diffusion sources, which leads to damage to the PN junction caused by laser direct doping technology. At the same time, it is impossible to achieve efficient doping of the selective emitter, which affects the photoelectric conversion efficiency of TOPCon cells.
A four-stage temperature-progressive deposition and oxidation process, combined with high-pressure nitrogen purging, forms a protective film and provides a sufficient source of boron diffusion, preventing laser damage to the PN junction and enabling heavy doping of the selective emitter.
This improved the open-circuit voltage and short-circuit current of TOPCon cells, enhancing photoelectric conversion efficiency while reducing contamination in diffusion equipment and silicon wafer fragmentation, thus ensuring production stability and quality.
Smart Images

Figure CN116387400B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of solar cell technology, and in particular to a boron diffusion method and apparatus for TOPCon cells. Background Technology
[0002] TOPCon cells, or Tunnel Oxide Passivated Contact cells, are a type of solar cell based on the selective carrier principle, using tunneled oxide passivated contacts. They are currently one of the most competitive types of mass-produced solar cells. The front side of a TOPCon cell typically uses a boron diffusion process to form a P-type emitter.
[0003] The application of selective emitters can improve the open-circuit voltage and short-circuit current of a battery, thereby enhancing its photoelectric conversion efficiency. Boron-diffused selective emitter (SE) cells are heavily doped (P++) in the contact region between the boron-diffused metal grid lines and the silicon wafer (i.e., the electrode contact area), while the non-metallic contact region between the metal electrodes is lightly doped (P+). Achieving this structure requires the use of boron diffusion laser direct doping technology. However, two challenges hinder its widespread application: firstly, direct laser contact with the PN junction surface can cause damage; secondly, sufficient boron atoms are required for laser propulsion to heavily dope the corresponding printed grid line areas. Solving these problems hinges on the boron diffusion process, which presents a significant challenge to the boron diffusion technology.
[0004] Although some studies have improved the boron diffusion process, they can only achieve the purpose of creating emitters, without obtaining a higher boron surface concentration. Furthermore, due to the difference in boron diffusion in silicon and silicon oxide and the phenomenon of impurity segregation, it is impossible to provide more boron atoms. In addition, in order to obtain a higher surface concentration, the driving temperature is high, which can easily cause problems such as oxygen rings and crystal defects. Summary of the Invention
[0005] To address the aforementioned problems, this invention provides a boron diffusion method for TOPCon cells. This method provides a sufficient boron diffusion source for laser propulsion, enabling heavy doping in the corresponding printed grid area. Simultaneously, it forms a protective film on the PN junction surface, preventing laser damage to the PN junction. This method is suitable for selective emitter laser doping and can improve the open-circuit voltage and short-circuit current of TOPCon cells, thereby enhancing their photoelectric conversion efficiency.
[0006] To achieve the above-mentioned objectives, the present invention adopts the following technical solution:
[0007] A boron diffusion method for TOPCon batteries, characterized by comprising the following steps: a silicon wafer is introduced into a diffusion furnace tube, and sequentially subjected to a first deposition, a first oxidation, a second deposition, a second oxidation, a third deposition, a fourth deposition, a cooling annealing, and the silicon wafer is removed from the diffusion furnace tube;
[0008] The temperature of the first deposition is 800–850°C;
[0009] The temperatures of the first oxidation, the second oxidation, and the third deposition are all 5 to 10°C higher than the temperature of the previous step, and the temperature of the fourth deposition is 10 to 20°C higher than the temperature of the third deposition.
[0010] The temperature of the second deposition is the same as the temperature of the first oxidation.
[0011] Compared to existing technologies, this invention utilizes a four-stage deposition process with progressively increasing temperature and two oxidation stages to provide a sufficient boron diffusion source for subsequent laser propulsion, resulting in heavy doping of the corresponding printed gate area. A protective film is also formed on the PN junction surface to prevent laser damage. The resulting non-metallic contact region has a shallow junction depth and high sheet resistance. The printed gate area undergoes secondary doping via laser propulsion in subsequent steps, achieving a deeper junction depth and lower sheet resistance for excellent ohmic contact. The entire boron diffusion process operates at temperatures not exceeding 900°C, and the high sheet resistance of the silicon wafer ensures the effectiveness of subsequent laser propulsion while extending the equipment's lifespan.
[0012] This invention performs oxidation and boron atom deposition on the silicon wafer surface through a first, second, and third deposition process. The first and second oxidation processes reduce the formation of a boron diffusion dead layer, while the increased temperature propels deep boron sources into the silicon wafer, achieving a "removing the surface and pushing inward" effect. The fourth deposition provides sufficient boron doping sources for subsequent laser heavy doping, contributing to improved cell conversion efficiency. The thicker borosilicate glass surface also forms a protective layer for the PN junction. Finally, cooling annealing reduces thermal stress on the silicon wafer caused by high temperatures, thereby reducing fragmentation. The first, first, second, and third deposition processes form light doping, while the fourth deposition prepares the surface for subsequent laser-driven secondary doping. This method is a boron diffusion method suitable for selective emitter laser doping, which can improve the open-circuit voltage and short-circuit current of TOPCon cells, thereby enhancing their photoelectric conversion efficiency.
[0013] Optionally, the silicon wafer undergoes empty tube purification before entering the diffusion furnace tube step, and silicon wafer purification is performed before the first deposition step begins. Empty tube purification removes metal ions such as sodium and iron from the diffusion furnace tube, preventing metal contamination of the silicon wafer. After the silicon wafer is cleaned in the previous texturing process, there is a certain risk of contamination by metal ions during its transport to the boron diffusion process; silicon wafer purification can effectively remove these contaminants.
[0014] It should be noted that after the silicon wafer purification step and before the first deposition step, evacuation, leak detection and stabilization are required; after the cooling annealing step and before the silicon wafer is removed from the diffusion furnace tube, nitrogen is also introduced into the diffusion furnace tube.
[0015] Optionally, the temperature for both the empty tube purification and the silicon wafer purification is 750–800°C, the time is 1–5 min, the nitrogen flow rate is 4500–5500 sccm, and the pressure is 1000–1050 mbar.
[0016] Optionally, the flow rate of boron trichloride for the empty pipe purification is 100–200 sccm, and the flow rate of boron trichloride for the silicon wafer purification is 50–100 sccm. At high temperatures, boron trichloride thermally decomposes to release chlorine gas, which has the function of removing metal ions such as sodium and iron.
[0017] Optionally, the time for the first deposition, the second deposition, and the third deposition is 5 to 10 minutes, the oxygen flow rate is 300 to 500 sccm, the nitrogen flow rate is 2500 to 3000 sccm, and the pressure is 80 to 120 mbar.
[0018] Optionally, the flow rate of boron trichloride in the first and second deposits is 100-200 sccm, and the flow rate of boron trichloride in the third deposit is 300-500 sccm.
[0019] Oxidation and boron atom deposition were performed on the silicon wafer surface through three deposition processes at different temperatures and boron trichloride flow rates. In the first and second deposition processes, the oxygen flow rate was higher than the boron trichloride flow rate to enhance oxidation and reduce the formation of diffusion dead layers. In the third deposition process, the increased boron trichloride flow rate resulted in more boron atoms adhering to the silicon wafer surface.
[0020] Optionally, the time for both the first oxidation and the second oxidation is 1 to 5 minutes, the flow rate of oxygen is 2000 to 3000 sccm, the flow rate of nitrogen is 2500 to 3000 sccm, and the pressure is 80 to 120 mbar.
[0021] Optionally, the first oxidizing gas may further include an inert gas, wherein the flow rate of the inert gas and the flow rate of oxygen are in the ratio of 1:9 to 11.
[0022] Further optionally, the inert gas includes at least one of argon, helium, or neon.
[0023] The formation of a diffusion dead layer can be reduced through the first and second oxidation processes. At the same time, the increased temperature promotes the deep boron source to enter the silicon, achieving the technical effect of "removing the surface and pushing inward". In the first oxidation process, an inert gas is introduced. The inert gas acts as a protective gas, which can reduce the oxidation of the silicon wafer, reduce heat loss, and also play a role in airflow circulation, carrying away volatile substances such as silicon and oxygen on the surface of the silicon wafer.
[0024] Optionally, the fourth deposition time is 20–40 min, the oxygen flow rate is 4500–5500 sccm, the nitrogen flow rate is 2500–3000 sccm, the boron trichloride flow rate is 500–1000 sccm, and the pressure is 80–120 mbar. By further increasing the flow rates of boron trichloride and oxygen, a thicker borosilicate glass is formed on the silicon wafer surface, providing sufficient boron atoms for selective emitter laser secondary doping, enabling heavy doping of the printed gate area, thereby achieving good ohmic contact; simultaneously, the thicker borosilicate glass forms a protective film on the inner surface of the silicon wafer, preventing damage to the PN junction during selective emitter laser secondary doping.
[0025] Optionally, the cooling annealing temperature is 700–750℃, the time is 10–20 min, the nitrogen flow rate is 5000–8000 sccm, and the pressure is 80–120 mbar.
[0026] In conjunction with the above technical solutions, as one embodiment of the present invention, the following steps are included:
[0027] (1) Silicon wafers enter the diffusion furnace tube
[0028] After the temperature inside the diffusion furnace tube reaches the preset temperature, the silicon wafer is placed in a quartz boat and sent into the diffusion furnace tube.
[0029] (2) First sediment
[0030] After the temperature inside the diffusion furnace tube reaches the preset temperature, boron trichloride, oxygen and nitrogen are introduced to oxidize the silicon wafer surface and deposit boron atoms.
[0031] (3) First oxidation
[0032] After raising the temperature inside the diffusion furnace tube by 5-10°C compared to the preset temperature in step (2), inert gas, oxygen and nitrogen are introduced to oxidize the surface of the silicon wafer.
[0033] (4) Second sediment
[0034] Under the first oxidation temperature conditions, boron trichloride, oxygen and nitrogen are introduced to oxidize the silicon wafer surface and deposit boron atoms;
[0035] (5) Second oxidation
[0036] After raising the temperature inside the diffusion furnace tube by 5-10°C compared to the second deposition temperature, oxygen and nitrogen are introduced to oxidize the silicon wafer surface.
[0037] (6) Third sediment
[0038] After raising the temperature inside the diffusion furnace tube by 5-10°C compared to the second oxidation temperature, boron trichloride, oxygen, and nitrogen are introduced to oxidize the silicon wafer surface and deposit boron atoms.
[0039] (7) Fourth sediment
[0040] After raising the temperature inside the diffusion furnace tube by 10-20°C compared to the third deposition temperature, boron trichloride, oxygen, and nitrogen are introduced to oxidize the silicon wafer surface and deposit boron atoms.
[0041] (8) Cooling and annealing
[0042] Nitrogen gas is introduced for cooling and annealing;
[0043] (9) The silicon wafer is removed from the diffusion furnace tube.
[0044] Optionally, the silicon wafer is purged with high-pressure nitrogen before entering the diffusion furnace tube and after exiting the diffusion furnace tube;
[0045] The outlet pressure of the high-pressure nitrogen pipeline is 0.1 to 1.0 MPa.
[0046] In another aspect, the present invention provides a boron diffusion device for a TOPCon battery, wherein a high-pressure nitrogen pipeline is provided at the diffusion furnace inlet of the boron diffusion device.
[0047] Compared to existing technologies, this invention establishes a high-pressure nitrogen pipeline at the furnace inlet of the boron diffusion device, forming an air curtain. This isolates the furnace tube from the outside when the door is opened, reducing the possibility of contamination and increasing the cleanliness of the furnace tube, thus improving diffusion quality. Simultaneously, since silicon wafers can stick together within the same tank during the high-temperature diffusion process, conventional diffusion equipment requires compressed air to purge the wafers in the loading / unloading area after diffusion to separate any stuck wafers. This prevents wafers from falling off or breaking during robotic unloading. However, compressed air contains water, oil, and other impurities, easily contaminating the wafers. This invention, by establishing a high-pressure nitrogen pipeline at the furnace inlet of the boron diffusion device and using high-pressure nitrogen to purge the wafers, not only avoids wafer sticking and fragmentation during automated unloading but also ensures wafer cleanliness.
[0048] It should be noted that the boron diffusion device of the TOPCon battery also includes a diffusion furnace tube, a quartz boat, an air inlet mechanism, and an exhaust mechanism; wherein, the first end of the diffusion furnace tube is provided with a furnace opening, and the second end of the diffusion furnace tube is provided with the air inlet mechanism and the exhaust mechanism; the quartz boat is located inside the diffusion furnace tube and is used to load silicon wafers.
[0049] Optionally, the high-pressure nitrogen pipeline is opened to purge the silicon wafer before it enters the diffusion furnace tube and after it exits the diffusion furnace tube. Attached Figure Description
[0050] To more clearly illustrate the technical solutions in the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0051] Figure 1 The graph shows the variation of boron surface concentration with silicon wafer depth after boron diffusion process in Example 3 and Comparative Example 2.
[0052] Curve 1 represents the change of boron surface concentration on the silicon wafer with the depth of the silicon wafer after the boron diffusion process in Example 3, and curve 2 represents the change of boron surface concentration on the silicon wafer with the depth of the silicon wafer after the boron diffusion process in Comparative Example 2. Detailed Implementation
[0053] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.
[0054] To better illustrate the present invention, further examples are provided below.
[0055] Traditional TOPCon cells use silver-aluminum paste on the front side to improve contact resistance. Aluminum reacts well with silicon, but aluminum is highly reactive, leading to aluminum penetration at great depths. To address this, the boron diffusion process typically raises the diffusion temperature to further deepen the junction and reduce surface recombination in non-metallic regions. This high-temperature diffusion process is therefore quite lengthy, which explains the extremely high requirements for boron diffusion equipment.
[0056] To address the aforementioned issues, the corresponding printed grid lines can be heavily doped to achieve good ohmic contact, while the non-electrode grid lines are lightly doped to reduce recombination in the diffusion layer. This optimization of the emitter increases the output current and voltage of the solar cell, thereby increasing photoelectric conversion efficiency. Achieving this structure requires boron diffusion laser direct doping technology, with laser doping performed after the boron diffusion process. However, two challenges hinder the widespread application of boron diffusion laser direct doping technology: firstly, direct contact with the PN junction surface can cause damage; secondly, a sufficient supply of boron atoms is required to propel the laser doping to heavily dope the corresponding printed grid lines. Solving these problems hinges on the boron diffusion process itself, which presents a significant challenge to the boron diffusion technology.
[0057] The boron diffusion principle involves gaseous boron trichloride being carried by nitrogen gas into a high-temperature quartz tube. At high temperature, it first reacts with oxygen to form particulate boron oxide. This particulate boron oxide is then carried by nitrogen gas and deposited on the silicon wafer surface, reacting with silicon to form boron atoms. The specific chemical reaction process is as follows:
[0058] 4BCl3 + 3O2 → 2B2O3 + 6Cl2
[0059] 2B₂O₃ + 3Si → 3SiO₂ + 4B
[0060] The boron diffusion method for TOPCon batteries provided by this invention includes the following steps: a silicon wafer enters a diffusion furnace tube, undergoes a first deposition, a first oxidation, a second deposition, a second oxidation, a third deposition, a fourth deposition, a cooling annealing, and the silicon wafer exits the diffusion furnace tube;
[0061] The temperature of the first deposition is 800–850°C;
[0062] The temperatures of the first oxidation, the second oxidation, and the third deposition are all 5 to 10°C higher than the temperature of the previous step, and the temperature of the fourth deposition is 10 to 20°C higher than the temperature of the third deposition.
[0063] The temperature of the second deposition is the same as the temperature of the first oxidation.
[0064] This invention provides a novel boron diffusion process that not only provides a sufficient boron diffusion source for laser propulsion to heavily dope the corresponding printed gate area, but also forms a protective film on the PN junction surface, thus preventing laser damage to the PN junction. This method is suitable for selective emitter laser doping of boron, and can improve the open-circuit voltage and short-circuit current of TOPCon cells, thereby enhancing their photoelectric conversion efficiency.
[0065] Furthermore, the inventors discovered during the production process that contamination at the diffusion furnace opening affects the performance of TOPCon cells. To avoid performance fluctuations caused by furnace opening contamination, TOPCon cell production needs to be stopped, the furnace tube thoroughly cooled after the silicon wafers exit the tube, and the tube openings manually cleaned, resulting in wasted production capacity. To solve the above problems, this invention also provides a boron diffusion device. A high-pressure nitrogen pipeline is installed at the furnace opening of the boron diffusion device to form an air curtain, which isolates the furnace tube from the high-pressure nitrogen when the door is opened, reducing contamination inside the furnace tube, increasing the cleanliness inside the furnace tube, and improving diffusion quality. At the same time, silicon wafers in the same tank may stick together during the high-temperature diffusion process. Currently, conventional diffusion equipment requires compressed air to blow each batch of silicon wafers in the loading and unloading area when unloading diffused silicon wafers. The purpose is to blow apart the silicon wafers stuck together in the same tank, so as to avoid the phenomenon of wafers falling off and breaking when the robotic arm picks up the stuck silicon wafers at the same time. However, compressed air contains impurities such as water and oil, which can contaminate the silicon wafers. Therefore, when the silicon wafers are finished and exiting the tubes, this device uses process nitrogen to purge the silicon wafers. This not only prevents the silicon wafers in the same tank from sticking together and causing them to become stuck or broken during automated unloading, but also ensures that the silicon wafers are clean and not contaminated.
[0066] Example 1
[0067] 1000 TOPCon solar cells were fabricated according to the following steps: texturing, boron diffusion, laser doping, oxidation, wet texturing, tunneling oxidation and polycrystalline silicon, annealing, wet processing, coating, screen printing, sintering and implantation. This process flow is a conventional process flow.
[0068] In the boron diffusion process, this embodiment provides a boron diffusion method for TOPCon cells, including the following steps: silicon wafer enters the diffusion furnace tube, evacuates, checks for leaks, stabilizes, performs a first deposition, a first oxidation, a second deposition, a second oxidation, a third deposition, a fourth deposition, cools and anneals, charges with nitrogen, and the silicon wafer exits the diffusion furnace tube. The process parameters for each step are detailed in Table 1, and the specific operations for each step are as follows:
[0069] (1) Silicon wafers enter the diffusion furnace tube
[0070] Once the temperature inside the diffusion furnace tube reaches 750°C, the silicon wafer is placed in a quartz boat and then fed into the diffusion furnace tube. The pressure inside the diffusion furnace tube is 1030 mbar.
[0071] (2) Evacuation
[0072] The temperature inside the diffusion furnace tube was raised to 800°C, and a vacuum process was performed.
[0073] (3) Leak detection
[0074] At the temperature in step (2), the diffusion furnace tube is leak-tested, and the pressure inside the diffusion furnace tube is 1030 mbar.
[0075] (4) Stable
[0076] At the temperature in step (3), oxygen is introduced into the diffusion furnace tube and stabilized for 5 minutes. The oxygen flow rate is 2000 sccm and the pressure inside the diffusion furnace tube is 100 mbar.
[0077] (5) First sediment
[0078] At the temperature in step (4), boron trichloride, oxygen, and nitrogen are introduced to oxidize and deposit boron atoms on the silicon wafer surface. The deposition time is 5 minutes, the oxygen flow rate is 300 sccm, the nitrogen flow rate is 2500 sccm, the boron trichloride flow rate is 100 sccm, and the pressure is 80 mbar.
[0079] (6) First oxidation
[0080] After raising the temperature inside the diffusion furnace tube to 805℃, inert gas, oxygen, and nitrogen were introduced to oxidize the silicon wafer surface. The oxidation time was 1 minute, the oxygen flow rate was 2000 sccm, the inert gas flow rate was 200 sccm, the nitrogen flow rate was 2500 sccm, and the pressure was 80 mbar.
[0081] (7) Second sediment
[0082] At the temperature in step (6), boron trichloride, oxygen, and nitrogen are introduced to oxidize and deposit boron atoms on the silicon wafer surface. The deposition time is 5 minutes, the oxygen flow rate is 300 sccm, the nitrogen flow rate is 2500 sccm, the boron trichloride flow rate is 100 sccm, and the pressure is 80 mbar.
[0083] (8) Second oxidation
[0084] After raising the temperature inside the diffusion furnace tube to 810℃, oxygen and nitrogen were introduced to oxidize the silicon wafer surface. The oxidation time was 1 minute, the oxygen flow rate was 2000 sccm, the nitrogen flow rate was 2500 sccm, and the pressure was 80 mbar.
[0085] (9) Third sediment
[0086] After raising the temperature inside the diffusion furnace tube to 815℃, boron trichloride, oxygen, and nitrogen were introduced to oxidize and deposit boron atoms on the silicon wafer surface. The deposition time was 5 minutes, the oxygen flow rate was 300 sccm, the nitrogen flow rate was 2500 sccm, the boron trichloride flow rate was 300 sccm, and the pressure was 80 mbar.
[0087] (10) Fourth sedimentary deposits
[0088] After raising the temperature inside the diffusion furnace tube to 825°C, boron trichloride, oxygen, and nitrogen were introduced to oxidize the silicon wafer surface and deposit boron atoms. The deposition time was 20 minutes, the oxygen flow rate was 4500 sccm, the nitrogen flow rate was 2500 sccm, the boron trichloride flow rate was 500 sccm, and the pressure was 80 mbar.
[0089] (11) Cooling and annealing
[0090] The temperature inside the diffusion furnace tube was reduced to 700℃ and annealed for 10 minutes. The nitrogen flow rate was 2500 sccm and the pressure was 80 mbar.
[0091] (12) Nitrogen purging
[0092] Nitrogen purging is performed at the temperature in step (11). The nitrogen flow rate is 2500 sccm and the pressure is 1030 mbar.
[0093] (13) Remove the silicon wafer from the diffusion furnace tube.
[0094] Table 1
[0095]
[0096]
[0097] Example 2
[0098] 1000 TOPCon cells were prepared according to the process flow in Example 1.
[0099] In the boron diffusion process, this embodiment provides a boron diffusion method for TOPCon cells, including the following steps: silicon wafer enters the diffusion furnace tube, evacuates, checks for leaks, stabilizes, performs a first deposition, a first oxidation, a second deposition, a second oxidation, a third deposition, a fourth deposition, cools and anneals, charges with nitrogen, and the silicon wafer exits the diffusion furnace tube. The process parameters for each step are detailed in Table 2.
[0100] Table 2
[0101]
[0102] Example 3
[0103] 1000 TOPCon cells were prepared according to the process flow in Example 1.
[0104] In the boron diffusion process, this embodiment provides a boron diffusion method for TOPCon cells, including the following steps: silicon wafer enters the diffusion furnace tube, evacuates, checks for leaks, stabilizes, performs a first deposition, a first oxidation, a second deposition, a second oxidation, a third deposition, a fourth deposition, cools and anneals, charges with nitrogen, and the silicon wafer exits the diffusion furnace tube. The process parameters for each step are detailed in Table 3.
[0105] Table 3
[0106]
[0107] Example 4
[0108] 1000 TOPCon cells were prepared according to the process flow in Example 1.
[0109] In the boron diffusion process, this embodiment provides a boron diffusion method for TOPCon cells, including the following steps: empty tube purification, silicon wafer entering the diffusion furnace tube, silicon wafer purification, evacuation, leak detection, stabilization, first deposition, first oxidation, second deposition, second oxidation, third deposition, fourth deposition, cooling annealing, nitrogen charging, and silicon wafer exiting the diffusion furnace tube. The process parameters for each step are detailed in Table 4.
[0110] Table 4
[0111]
[0112]
[0113] Example 5
[0114] 1000 TOPCon cells were prepared according to the process flow in Example 1.
[0115] In the boron diffusion process, this embodiment provides a boron diffusion method for TOPCon cells, including the following steps: the silicon wafer enters the diffusion furnace tube, evacuates, checks for leaks, stabilizes, performs a first deposition, a first oxidation, a second deposition, a second oxidation, a third deposition, a fourth deposition, cools and anneals, charges with nitrogen, and the silicon wafer exits the diffusion furnace tube. The process parameters for each step are the same as in Embodiment 3.
[0116] Unlike Example 3, the boron diffusion process is carried out in the boron diffusion device of the TOPCon cell provided by the present invention. Before the silicon wafer enters the diffusion furnace tube and after the silicon wafer exits the diffusion furnace tube, the high-pressure nitrogen pipeline located at the diffusion furnace opening is opened, and the silicon wafer is purged with high-pressure nitrogen. The outlet pressure of the high-pressure nitrogen pipeline is 0.5 MPa.
[0117] Example 6
[0118] 1000 TOPCon cells were prepared according to the process flow in Example 1.
[0119] In the boron diffusion process, this embodiment provides a boron diffusion method for TOPCon cells, including the following steps: empty tube purification, silicon wafer entering the diffusion furnace tube, silicon wafer purification, evacuation, leak detection, stabilization, first deposition, first oxidation, second deposition, second oxidation, third deposition, fourth deposition, cooling annealing, nitrogen charging, and silicon wafer removal from the diffusion furnace tube. The process parameters for each step are the same as in Embodiment 4.
[0120] Unlike Example 4, the boron diffusion process is carried out in the boron diffusion device of the TOPCon cell provided by the present invention. Before the silicon wafer enters the diffusion furnace tube and after the silicon wafer exits the diffusion furnace tube, the high-pressure nitrogen pipeline located at the diffusion furnace opening is opened, and the silicon wafer is purged with high-pressure nitrogen. The outlet pressure of the high-pressure nitrogen pipeline is 0.5 MPa.
[0121] Comparative Example 1
[0122] 1000 TOPCon cells were prepared according to the process flow in Example 1.
[0123] In the boron diffusion process, this comparative example provides a boron diffusion method for TOPCon cells, including the following steps: silicon wafer enters the diffusion furnace tube, evacuates, checks for leaks, stabilizes, performs a first deposition, a first oxidation, a second deposition, a third deposition, cools and anneals, charges with nitrogen, and the silicon wafer exits the diffusion furnace tube. The process parameters for each step are detailed in Table 5.
[0124] Table 5
[0125]
[0126] Comparative Example 2
[0127] 1000 TOPCon cells were prepared according to the process flow in Example 1.
[0128] In the boron diffusion process, this embodiment provides a boron diffusion method for TOPCon cells, including the following steps: silicon wafer enters the diffusion furnace tube, evacuates, checks for leaks, stabilizes, performs a first deposition, a first oxidation, a second deposition, a second oxidation, a third deposition, a fourth deposition, cools and anneals, charges with nitrogen, and the silicon wafer exits the diffusion furnace tube. The process parameters for each step are detailed in Table 6.
[0129] Table 6
[0130]
[0131]
[0132] Twenty silicon wafers from Examples 3 and 2 (after boron diffusion process) were taken respectively, and the boron surface concentration at different depths was measured. The average test results are detailed in [link to data]. Figure 1 .Depend on Figure 1 Analysis shows that within a thickness of 0.4 μm, the silicon wafer surface treated by the boron diffusion method provided in Example 3 has a higher boron surface concentration.
[0133] Twenty silicon wafers were taken from each of Example 3, Comparative Example 2 after the boron diffusion process, and after the laser doping process, and their sheet resistance was measured. The average test results are detailed in Table 7. Analysis of Table 7 shows that the silicon wafer treated with the boron diffusion method provided in Example 3 has a higher sheet resistance. The sheet resistance decreases even more in the region after laser doping, indicating that the boron diffusion method provided in Example 3 achieves better secondary doping after laser propulsion.
[0134] Table 7
[0135]
[0136] The performance and yield of the TOPCon cells finally prepared in Examples 1-6 and Comparative Examples 1-2 were tested. 100 cells were taken from each example / comparative example. The testing equipment was a photovoltaic simulation tester, and the testing conditions were the production environment (indoor cleanliness: ISO standard 7; ambient temperature: 23±3℃; relative humidity: 30%~50% (non-condensing)). The average test results are detailed in Table 8. Analysis of Table 8 shows that the TOPCon cells prepared in Examples 1-6 exhibit superior photoelectric conversion efficiency.
[0137] Table 8
[0138]
[0139]
[0140] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions or improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A boron diffusion method for a TOPCon battery, characterized in that, Includes the following steps: The silicon wafer enters the diffusion furnace tube and undergoes the first deposition, first oxidation, second deposition, second oxidation, third deposition, and fourth deposition in sequence. After cooling and annealing, the silicon wafer exits the diffusion furnace tube. The temperature of the first deposition is 800~850℃; The temperatures of the first oxidation, the second oxidation, and the third deposition are all 5-10°C higher than the temperature of the previous step, and the temperature of the fourth deposition is 10-20°C higher than the temperature of the third deposition. The temperature of the second deposition is the same as the temperature of the first oxidation; The deposition times for the first, second, and third depositions are all 5-10 min, the oxygen flow rate is 300-500 sccm, the nitrogen flow rate is 2500-3000 sccm, and the pressure is 80-120 mbar; the boron trichloride flow rate for the first and second depositions is 100-200 sccm, and the boron trichloride flow rate for the third deposition is 300-500 sccm. The fourth deposition time is 20-40 min, the oxygen flow rate is 4500-5500 sccm, the nitrogen flow rate is 2500-3000 sccm, the boron trichloride flow rate is 500-1000 sccm, and the pressure is 80-120 mbar.
2. The boron diffusion method for TOPCon batteries as described in claim 1, characterized in that, The silicon wafer is purified before entering the diffusion furnace tube step, and the silicon wafer is purified before starting the first deposition step.
3. The boron diffusion method for TOPCon batteries as described in claim 2, characterized in that, The temperature for both the empty tube purification and the silicon wafer purification is 750~800℃, the time is 1~5min, the nitrogen flow rate is 4500~5500sccm, and the pressure is 1000~1050mbar; and / or The flow rate of boron trichloride used for purifying the empty tube is 100~200 sccm, and the flow rate of boron trichloride used for purifying the silicon wafer is 50~100 sccm.
4. The boron diffusion method for TOPCon batteries as described in claim 1, characterized in that, The duration of both the first and second oxidation processes is 1–5 min, the oxygen flow rate is 2000–3000 sccm, the nitrogen flow rate is 2500–3000 sccm, and the pressure is 80–120 mbar; and / or The first oxidizing gas also includes an inert gas, and the flow rate of the inert gas is in the ratio of the flow rate of oxygen to 1:9~11.
5. The boron diffusion method for TOPCon batteries as described in claim 1, characterized in that, The cooling annealing temperature is 700~750℃, the time is 10~20min, the nitrogen flow rate is 5000~8000sccm, and the pressure is 80~120mbar.
6. The boron diffusion method for TOPCon batteries as described in claim 1, characterized in that, The silicon wafer is purged with high-pressure nitrogen before entering the diffusion furnace tube and after exiting the diffusion furnace tube. The outlet pressure of the high-pressure nitrogen pipeline is 0.1~1.0MPa.
Citation Information
Patent Citations
P diffusion method of silicon wafer and preparation method of solar cell
CN104409339A
Diffusion process method of selective emitter solar cell
CN112768346A