A non-fluorinated supercritical CO2 thickener without additives and its preparation method
By preparing an additive-free, non-fluorinated supercritical CO₂ thickener, a spatial network structure is formed through polymer copolymerization, which solves the problems of high cost and low solubility of existing thickeners and achieves a highly efficient thickening effect, suitable for supercritical CO₂ oil displacement.
Patent Information
- Application Number
- CN202310327205.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-03-30
AI Technical Summary
Existing viscosity improvers suffer from high cost, significant environmental hazards, or low solubility, making them ineffective in increasing viscosity during CO₂ flooding. Furthermore, large amounts of co-solvents can damage the formation.
A non-fluorinated supercritical CO₂ thickener without additives is used, which is copolymerized from substances such as methoxy polyethylene glycol acrylate, ammonia-terminated polydimethylsiloxane and vinyl acetate to form a spatial network structure, thereby enhancing CO₂ viscosity and reducing the amount of thickener required.
Without additives, viscosity improvers can significantly increase the viscosity of supercritical CO₂. A viscosity improver concentration of 2% can increase it by 46 to 58 times, and a concentration of 5% can increase it by 57 to 75 times. It is suitable for supercritical CO₂ oil displacement.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention belongs to the field of thickener preparation technology, specifically relating to a supercritical CO2 thickener and its preparation method. This thickener is particularly suitable for thickening supercritical, liquid CO2. Background Technology
[0002] CO2 enhanced oil recovery (EOR) technology can achieve a win-win situation of CO2 emission reduction and utilization. Supercritical CO2 viscosity enhancers can effectively increase the viscosity of supercritical CO2, solving the "viscous fingering" phenomenon that easily occurs during CO2 displacement, and greatly improving displacement efficiency. Existing patents and literature disclose that viscosity enhancers are mainly fluorinated and non-fluorinated. Fluorinated viscosity enhancers have good viscosity-increasing effects, but their high cost, significant environmental harm, and tendency to adsorb onto rocks reduce extraction efficiency limit their use. Non-fluorinated viscosity enhancers suffer from low solubility in CO2 and excessive solvent pressure, requiring the addition of large amounts of co-solvents (approximately 20%) to achieve viscosity enhancement. Large amounts of co-solvents can damage the formation and are also expensive, making them impractical for field applications. Therefore, developing a non-fluorinated, additive-free supercritical CO2 viscosity enhancer with good viscosity-increasing effects is of great significance. Summary of the Invention
[0003] The purpose of this invention is to address the problems existing in the prior art by providing a method for preparing a non-fluorinated supercritical CO2 thickener without additives. This thickener is fluorine-free and can significantly improve the viscosity of supercritical CO2 without additives.
[0004] The additive-free, non-fluorinated supercritical CO2 thickener provided by this invention is made from the following substances in the indicated weight ratios:
[0005]
[0006] The degree of polymerization of the above-mentioned methoxy polyethylene glycol acrylate is 7 to 22.
[0007] The degree of polymerization of the above-mentioned amino-terminated polydimethylsiloxane is 3 to 18.
[0008] The structural formulas of the main components of the supercritical CO2 thickener of this invention are shown below:
[0009]
[0010] In the formula, m and n represent the degree of polymerization of ammonia-terminated polydimethylsiloxane and methoxy polyethylene glycol acrylate, respectively, and x, y, and z represent the degree of polymerization of methoxy polyethylene glycol acrylate monomer unit, ammonia-terminated polydimethylsiloxane monomer unit, and vinyl acetate monomer unit, respectively. The values of x, y, and z are determined by the proportion of raw materials added.
[0011] The preparation method of the additive-free non-fluorine supercritical CO2 thickener of the present invention is as follows: Nitrogen gas is introduced into a three-necked flask equipped with a condenser for protection. Methoxy polyethylene glycol acrylate, vinyl acetate, and ammonia-terminated polydimethylsiloxane are added sequentially, followed by cerium ammonium nitrate. Stirring is started, and the temperature is raised to 70–85°C. After reacting at this temperature for 5–8 hours, the crude product is removed and dissolved in anhydrous diethyl ether. Then, a 5% (w / w) sodium hydroxide aqueous solution is added, and the mixture is allowed to stand and separate into layers. Organic matter is extracted and washed 3–5 times with distilled water. Anhydrous diethyl ether is removed by vacuum distillation to obtain a pale yellow supercritical CO2 thickener product.
[0012] The beneficial effects of this invention are as follows:
[0013] 1. Among the comonomers used in the tackifier of this invention, vinyl acetate is currently the hydrocarbon compound with the best solubility in CO2; ammonia-terminated polydimethylsiloxane has more CO2-loving segments, relatively low surface tension and high main chain flexibility, and has higher solubility than oxygen-containing hydrocarbon polymers with similar molecular weight; methoxy polyethylene glycol acrylate contains ester and ether structures, the ester group is a CO2-loving group, which has a certain effect on promoting the solubility of polymers in carbon dioxide. The strong self-binding effect of the ether structure limits its solubility in CO2, but by introducing a methyl group at one end of the ether structure, the cohesive energy density can be reduced and the free volume can be increased, thereby improving its solubility in CO2.
[0014] 2. The tackifier of this invention utilizes the cross-twisting interaction between polymers to form a spatial network structure, which captures CO2 molecules and weakens their flow effect, thereby achieving a tackifying effect. By introducing long and short chain interlacing through structures such as amino-terminated polydimethylsiloxane, methoxy polyethylene glycol acrylate, and vinyl acetate, the amount of tackifier used can be reduced through long and short chain interaction and association, thereby reducing the cloud point pressure of the system and achieving tackification of CO2 under solvent-free conditions.
[0015] 3. The viscosity enhancer of this invention has a significant viscosity-enhancing effect. Without any additives, when the viscosity enhancer is added at a rate of 2%, it can increase the viscosity of supercritical CO2 by 46 to 58 times. When the viscosity enhancer is added at a rate of 5%, it can increase the viscosity of supercritical CO2 by 57 to 75 times. It is particularly suitable for use in supercritical CO2 oil displacement. Detailed Implementation
[0016] The present invention will be further described in detail below with reference to the embodiments, but the scope of protection of the present invention is not limited to these embodiments.
[0017] Example 1
[0018] Nitrogen gas was introduced into a three-necked flask equipped with a condenser for protection. 20g of methoxy polyethylene glycol acrylate (degree of polymerization n=8), 20g of vinyl acetate, and 60g of amino-terminated polydimethylsiloxane (degree of polymerization m=12) were added sequentially, along with 0.15g of cerium ammonium nitrate. The mixture was stirred and heated to 80℃. After reacting at this temperature for 6 hours, the crude product was removed and dissolved in 100g of anhydrous diethyl ether. Then, 100g of a 5% sodium hydroxide aqueous solution was added. The mixture was allowed to stand and separate into layers. The organic matter was extracted and washed five times with distilled water. The anhydrous diethyl ether was then removed by vacuum distillation to obtain a pale yellow supercritical CO2 thickener product.
[0019] Example 2
[0020] Nitrogen gas was introduced into a three-necked flask equipped with a condenser for protection. 30g of methoxy polyethylene glycol acrylate (degree of polymerization n=7), 20g of vinyl acetate, and 50g of amino-terminated polydimethylsiloxane (degree of polymerization m=18) were added sequentially, along with 0.3g of cerium ammonium nitrate. Stirring was started, and the temperature was raised to 70℃. After reacting at this temperature for 6 hours, the crude product was removed, dissolved in 100g of anhydrous diethyl ether, and then 100g of a 5% sodium hydroxide aqueous solution was added. The mixture was allowed to stand and separate into layers. The organic matter was extracted and washed five times with distilled water. Then, the anhydrous diethyl ether was removed by vacuum distillation to obtain a pale yellow supercritical CO2 thickener product.
[0021] Example 3
[0022] Nitrogen gas was introduced into a three-necked flask equipped with a condenser for protection. 15g of methoxy polyethylene glycol acrylate (degree of polymerization n=12), 40g of vinyl acetate, and 45g of amino-terminated polydimethylsiloxane (degree of polymerization m=8) were added sequentially, along with 0.1g of cerium ammonium nitrate. The mixture was stirred and heated to 85°C. After reacting at this temperature for 6 hours, the crude product was removed and dissolved in 100g of anhydrous diethyl ether. Then, 100g of a 5% sodium hydroxide aqueous solution was added. The mixture was allowed to stand and separate into layers. The organic matter was extracted and washed five times with distilled water. Anhydrous diethyl ether was then removed by vacuum distillation to obtain a pale yellow supercritical CO2 thickener product.
[0023] Example 4
[0024] Nitrogen gas was introduced into a three-necked flask equipped with a condenser for protection. 30g of methoxy polyethylene glycol acrylate (degree of polymerization n=20), 30g of vinyl acetate, and 40g of amino-terminated polydimethylsiloxane (degree of polymerization m=4) were added sequentially, along with 0.25g of cerium ammonium nitrate. Stirring was started, and the temperature was raised to 80℃. After reacting at this temperature for 6 hours, the crude product was removed, dissolved in 100g of anhydrous diethyl ether, and then 100g of a 5% sodium hydroxide aqueous solution was added. The mixture was allowed to stand and separate into layers. The organic matter was extracted and washed five times with distilled water. Then, the anhydrous diethyl ether was removed by vacuum distillation to obtain a pale yellow supercritical CO2 thickener product.
[0025] To demonstrate the beneficial effects of the product of this invention, the viscosity of supercritical CO2 liquid with added thickener was tested using a HAKKEMARS 60 rheometer (test accuracy 0.01mps) from ThermoFisher Scientific at a temperature of 35°C and a pressure of 8MPa. The viscosity was compared with that of pure supercritical CO2, and the thickening factor of supercritical CO2 was calculated.
[0026] Table 1. Viscosity enhancement factor of supercritical CO2
[0027] Tackifier Increase the amount of thickener viscosity increase factor Example 1 2% 50 Example 1 5% 67 Example 2 2% 58 Example 2 5% 75 Example 3 2% 46 Example 3 5% 57 Example 4 2% 48 Example 4 5% 61
[0028] As shown in Table 1, the thickeners in Examples 1-4 all exhibit good thickening ability for supercritical CO2. Without additives, a 2% thickener dosage increases the viscosity of supercritical CO2 by 46-58 times, and a 5% thickener dosage increases the viscosity by 57-75 times, demonstrating a significant thickening effect.
Claims
1. A non-fluorinated supercritical CO2 thickener without additives, characterized in that, The tackifier is made from the following substances in the indicated weight proportions: 15-30 parts of methoxy polyethylene glycol acrylate 20-40 parts of vinyl acetate 40-60 parts of ammonia-terminated polydimethylsiloxane 0.1 to 0.3 parts of cerium ammonium nitrate The preparation method of the thickener is as follows: nitrogen gas is introduced into a three-necked flask equipped with a condenser for protection, methoxy polyethylene glycol acrylate, vinyl acetate, and ammonia-terminated polydimethylsiloxane are added in sequence, and cerium ammonium nitrate is added. Stirring is started, the temperature is raised to 70-85°C, and the reaction is carried out at a constant temperature for 5-8 hours. The crude product is taken out and dissolved in anhydrous diethyl ether. Then, a 5% sodium hydroxide aqueous solution is added, and the mixture is allowed to stand and separate into layers. Organic matter is extracted and washed with distilled water 3-5 times. The mixture is then distilled under reduced pressure to obtain a light yellow supercritical CO2 thickener product. The degree of polymerization of the methoxy polyethylene glycol acrylate is 7 to 22; The degree of polymerization of the ammonia-terminated polydimethylsiloxane is 3 to 18.
Citation Information
Patent Citations
Fluorinated polyurethane thickener applied to supercritical CO2 tackification and preparation method thereof
CN105294948A
Thickening agent applied to supercritical CO2 dry fracturing and preparation method thereof
CN107794023A