Secondary battery, battery pack, and electric device

By using lithium nickel cobalt manganese oxide and adding rubidium in lithium-ion secondary batteries, the oxygen release initiation temperature and the amount of lithium delithiation are controlled, thus solving the problems of insufficient energy density and high-temperature cycle performance of lithium-ion secondary batteries and achieving high energy density and good thermal stability.

CN116404111BActive Publication Date: 2026-11-24SUNWODA MOBILITY ENERGY TECHNOLOGY CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310399798.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-06
Publication Date
2026-11-24
Estimated Expiration
2043-04-06

AI Technical Summary

Technical Problem

Existing lithium-ion rechargeable batteries cannot simultaneously achieve high energy density and good high-temperature cycle performance.

Method used

Lithium nickel cobalt manganese oxide is used as the positive electrode active material. By controlling the oxygen release initiation temperature and active lithium removal amount of the positive electrode active material layer, rubidium element is added to form a specific structure, which suppresses phase transition during charging and discharging, reduces side reactions, and improves thermal stability.

Benefits of technology

This technology enables secondary batteries to achieve high energy density and good high-temperature cycling performance at high voltage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116404111B_ABST
    Figure CN116404111B_ABST
Patent Text Reader

Abstract

A secondary battery, battery pack, and power-consuming device are disclosed. The secondary battery includes a positive electrode sheet, which contains a positive active material layer. The positive active material layer contains a positive active material, which contains lithium nickel cobalt manganese oxide. The total molar amount of nickel, cobalt, and manganese in the lithium nickel cobalt manganese oxide is taken as 1, and the nickel content is x, where x > 0.5. The lithium nickel cobalt manganese oxide contains a first element, which includes at least one of rubidium, neodymium, or strontium. When the secondary battery is charged at UV, thermogravimetric mass spectrometry analysis of the positive active material layer satisfies 200 ≤ N ≤ 400, where N = T / b, T℃ is the oxygen release initiation temperature of the positive active material layer, b is the active delithiation amount of the positive active material, and 4.0 ≤ U ≤ 4.7. The secondary battery can simultaneously achieve high energy density and good high-temperature cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of secondary battery technology, specifically relating to a secondary battery, a battery pack, and an electrical device. Background Technology

[0002] Lithium-ion rechargeable batteries are a type of rechargeable battery and a widely used clean energy source. The positive electrode active material, as a crucial component of lithium-ion rechargeable batteries, provides lithium ions that move back and forth between the positive and negative electrodes during the charging and discharging process; therefore, the positive electrode active material is vital to the battery's performance.

[0003] Lithium nickel cobalt manganese oxide (LCO) possesses a high theoretical capacity, and lithium-ion secondary batteries using LCO as the positive electrode active material are expected to achieve high energy density. However, how to achieve both high energy density and good high-temperature cycling performance in this secondary battery remains a pressing technical challenge. Summary of the Invention

[0004] Therefore, the technical problem to be solved by the present invention is to overcome the shortcomings of existing secondary batteries in that they cannot achieve both high energy density and good high-temperature cycle performance, thereby providing a secondary battery, battery pack and power supply device.

[0005] The first aspect of this invention provides a secondary battery, including a positive electrode sheet, the positive electrode sheet comprising a positive electrode active material layer, the positive electrode active material layer comprising a positive electrode active material, the positive electrode active material comprising lithium nickel cobalt manganese oxide, wherein the total molar amount of nickel, cobalt and manganese in the lithium nickel cobalt manganese oxide is 1, the content of nickel is x, x>0.5, the lithium nickel cobalt manganese oxide comprises a first element, the first element comprising rubidium, and when the secondary battery is charged at UV, thermogravimetric mass spectrometry analysis of the positive electrode active material layer satisfies 200≤N≤400, where N=T / b, T℃ is the oxygen release initiation temperature of the positive electrode active material layer, b is the active delithiation amount of the positive electrode active material, and 4.0≤U≤4.7.

[0006] Optional, 200≤T≤250, 0.55≤b≤0.95.

[0007] Optionally, the oxygen release amount of the positive electrode active material layer is Z mL / g, M=b×Z×U, and 100≤M≤350.

[0008] Optional, Z≤90, b<0.9.

[0009] Optionally, when the voltage of the secondary battery is 4.0V, thermogravimetric mass spectrometry analysis is performed on the positive electrode active material layer, and the oxygen release amount of the positive electrode active material layer is Z1mL / g. When the voltage of the secondary battery is 4.7V, thermogravimetric mass spectrometry analysis is performed on the positive electrode active material layer, and the oxygen release amount of the positive electrode active material layer is Z2mL / g, satisfying 0.5≤Z1 / Z2≤1.

[0010] Optional, 40≤Z1≤60, 60≤Z2≤80.

[0011] Optionally, the positive electrode active material includes matrix particles, the matrix particles being made of lithium nickel cobalt manganese oxide, and the matrix particles containing a first element.

[0012] Optionally, the first element comprises at least one of sodium, potassium, magnesium, aluminum, zirconium, titanium, vanadium, antimony, yttrium, tungsten, niobium, nitrogen, fluorine, sulfur, or chlorine.

[0013] Optionally, the positive electrode active material further includes a coating layer located on the surface of the matrix particles, the coating layer containing a compound of a second element, the compound containing the second element comprising one or more of an oxide of the second element, a fluoride of the second element, or a phosphate of the second element, the second element comprising at least one of lithium, cobalt, zinc, magnesium, aluminum, zirconium, titanium, vanadium, antimony, yttrium, niobium, strontium, and tungsten.

[0014] Optionally, the nickel content on the surface of the matrix particles is lower than the nickel content at the center of the matrix particles.

[0015] A second aspect of the invention provides a battery pack comprising the secondary battery described in the first aspect.

[0016] In another aspect of the invention, an electrical device is provided, comprising the battery pack described in the second aspect.

[0017] The technical solution of this invention has the following advantages: The secondary battery provided by this invention includes a positive electrode sheet, the positive electrode sheet comprising a positive electrode active material layer, the positive electrode active material layer comprising a positive electrode active material, the positive electrode active material comprising lithium nickel cobalt manganese oxide, wherein the total molar amount of nickel, cobalt and manganese in the lithium nickel cobalt manganese oxide is 1, the content of nickel is x, x>0.5, the lithium nickel cobalt manganese oxide comprises a first element, the first element comprising rubidium, and when the secondary battery is charged at UV, thermogravimetric mass spectrometry analysis of the positive electrode active material layer satisfies 200≤N≤400, where N=T / b, T℃ is the oxygen release initiation temperature of the positive electrode active material layer, b is the active delithiation amount of the positive electrode active material, and 4.0≤U≤4.7. The lithium nickel cobalt manganese oxide contains rubidium, giving it a specific structure that suppresses phase transitions in the positive electrode active material during the charging and discharging process of the secondary battery, reducing side reactions. When the secondary battery operates at a voltage range of 4.0V to 4.7V, controlling the structure of the positive electrode active material and ensuring that the positive electrode sheet satisfies 200≤N≤400 enables the secondary battery to have better thermal stability at higher voltages, reducing oxygen release and thus improving the energy density and high-temperature cycle performance. Therefore, the secondary battery can simultaneously achieve both high energy density and good high-temperature cycle performance. Attached Figure Description

[0018] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.

[0019] Figure 1 The high-temperature cycling performance diagrams are for the positive electrode active material of Example 1 and the positive electrode active material of Comparative Example 1. Figure 2 Thermogravimetric mass spectra of the positive electrode active material of Example 1 and the positive electrode active material of Comparative Example 1 are shown. Detailed Implementation

[0020] The technical solution of the present invention will now be clearly and completely described with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0021] The present disclosure provides a secondary battery, including a positive electrode sheet, the positive electrode sheet includes a positive electrode active material layer, the positive electrode active material layer includes a positive electrode active material, the positive electrode active material includes a lithium nickel cobalt manganese oxide, based on the total molar amount of nickel element, cobalt element and manganese element in the lithium nickel cobalt manganese oxide being 1, the content of the nickel element is x, x > 0.5, the lithium nickel cobalt manganese oxide includes a first element, the first element includes rubidium, when the charging voltage of the secondary battery is U V, a thermogravimetric mass spectrometry analysis is performed on the positive electrode active material layer, and 200 ≤ N ≤ 400 is satisfied, wherein N = T / b, T°C is an oxygen release initial temperature of the positive electrode active material layer, b is an active delithiation amount of the positive electrode active material, and 4.0 ≤ U ≤ 4.7.

[0022] In the secondary battery provided by some embodiments of the present application, the lithium nickel cobalt manganese oxide includes rubidium, by controlling structural characteristics of the positive electrode active material, the phase transition of the positive electrode active material during charge and discharge of the secondary battery can be suppressed, and generation of side reactions can be reduced, so that when the voltage of the secondary battery is 4.0 V to 4.7 V, the positive electrode sheet satisfies 200 ≤ N ≤ 400, which can improve the thermal stability of the positive electrode sheet and reduce the oxygen release amount, thereby improving the energy density and the high-temperature cycle performance of the secondary battery. Therefore, the secondary battery can achieve both high energy density and good high-temperature cycle performance.

[0023] In some embodiments, x > 0.7.

[0024] In some embodiments, x > 0.75. When x is within this range, the secondary battery has a higher energy density.

[0025] In some embodiments, 241 ≤ N ≤ 300. When N is within this range, the secondary battery has better comprehensive performance.

[0026] In some embodiments, the lithium nickel cobalt manganese oxide includes a compound having a molecular formula of Li 1-a [Ni x Co y Mn z Me n O 2-b , wherein -0.2 ≤ a ≤ 0.1, 0 < x < 1, 0 < y < 1, 0 < z < 1, 0 < n < 0.05, 0 < b < 0.2, and Me is the first element.

[0027] In some embodiments, 200 ≤ T ≤ 250, for example, T may be any value of 200, 220, 230, 245, 250, or a range formed by any two thereof, T°C is an oxygen release initial temperature of the positive electrode active material layer, when the oxygen release initial temperature of the positive electrode active material layer is within this range, the thermal stability of the secondary battery during charge and discharge is relatively high, and the high-temperature cycle performance of the secondary battery is effectively improved.

[0028] In some embodiments, 0.55≤b≤0.95, for example, b can be any value among 0.55, 0.57, 0.64, 0.67, 0.70, 0.75, 0.79, 0.80, 0.82, 0.85, 0.87, 0.89, 0.90, 0.93, and 0.95, or a range of any two of them. b is the active lithium removal amount of the positive electrode active material at a voltage of UV, specifically the ratio of the lithium content in the positive electrode active material when the secondary battery is fully charged to the lithium content in the positive electrode active material when the secondary battery is at a voltage of UV. When the active lithium removal amount of the positive electrode active material is within this range, the stability of the positive electrode active material is better, and the overall system matching of the secondary battery material is better. The secondary battery has a high degree of thermal stability during charging and discharging, which can better improve the high-temperature cycle performance of the secondary battery.

[0029] In some embodiments, the oxygen release amount of the positive electrode active material layer is Z mL / g, M = b × Z × U, and 100 ≤ M ≤ 350. For example, M can be any value among 100, 120, 150, 180, 200, 230, 250, 280, 300, 320, and 350, or a range of any two of these values. When the secondary battery meets the above range, the structure of the positive electrode active material in the positive electrode active material layer is in a superior state, which can improve the overall performance of the secondary battery.

[0030] In some embodiments, the oxygen release amount of the positive electrode active material layer is Z mL / g, M = b × Z × U, and 141 ≤ M ≤ 330. When the oxygen release amount of the positive electrode active material layer is within this range, the structure of the positive electrode active material in the positive electrode active material layer is relatively stable and in a better state, which can make the overall performance of the secondary battery better.

[0031] In some embodiments, the oxygen release amount of the positive electrode active material layer is Z mL / g, M=b×Z×U, and 151≤M≤299.

[0032] In some embodiments, Z≤90, b<0.9, and the oxygen release of the positive electrode active material layer is less than 90 mL / g, which is beneficial to improving the thermal stability of the secondary battery during charge and discharge, improving the high-temperature cycle performance of the secondary battery, and improving the energy density of the secondary battery.

[0033] In some embodiments, when the voltage of the secondary battery is 4.0V, the oxygen release of the positive electrode active material layer is Z1mL / g, 40≤Z1≤60, for example, it can be any value among 40, 43, 45, 48, 50, 53, 55, 58, 60, or a range of any two of them.

[0034] In some embodiments, when the voltage of the secondary battery is 4.7V, the oxygen release of the positive electrode active material layer is Z2 mL / g, where 60 ≤ Z2 ≤ 80. For example, it can be any value among 60, 63, 65, 68, 70, 73, 75, 78, and 80, or a range of any two of these values. When Z2 is within the above range, the structure of the positive electrode active material is stable, and the overall performance of the secondary battery is improved.

[0035] In some embodiments, the condition 0.5 ≤ Z1 / Z2 ≤ 1 is satisfied. For example, Z1 / Z2 can be any value from 0.5, 0.7, 0.8, 0.9, 0.95, 1, or a range of any two of these values. When Z1 / Z2 satisfies the above range, the overall performance of the secondary battery is better.

[0036] In some embodiments, the positive electrode active material includes matrix particles, the material of which is lithium nickel cobalt manganese oxide, and the matrix particles contain a first element.

[0037] In some embodiments, the first element is distributed in the matrix particles.

[0038] In some embodiments, the first element comprises at least one of sodium, potassium, magnesium, aluminum, zirconium, titanium, vanadium, antimony, yttrium, tungsten, niobium, nitrogen, fluorine, sulfur, or chlorine.

[0039] In some embodiments, the first element is uniformly distributed in the matrix particles.

[0040] In some embodiments, the positive electrode active material further includes a coating layer located on the surface of the matrix particles, the coating layer containing a compound of a second element.

[0041] In some embodiments, the compound containing the second element comprises one or more of the following: an oxide of the second element, a fluoride of the second element, or a phosphate of the second element. Examples include aluminum oxide (Al₂O₃) and titanium dioxide (TiO₂).

[0042] In some embodiments, the second element comprises at least one of lithium, cobalt, zinc, magnesium, aluminum, zirconium, titanium, vanadium, antimony, yttrium, niobium, strontium, and tungsten.

[0043] In some embodiments, the nickel content on the surface of the matrix particles is lower than the nickel content at the center of the matrix particles. This configuration suppresses the phase transition of the positive electrode active material in the secondary battery during the charge and discharge process, improves the stability of the positive electrode active material structure, and thus improves the stability of the secondary battery performance.

[0044] The positive electrode also includes a positive current collector, and the positive active material layer is located on the surface of the positive current collector.

[0045] In some embodiments, the positive current collector comprises aluminum foil.

[0046] In some embodiments, the positive current collector includes a composite current collector, which comprises a polymer layer and a conductive layer disposed on at least one surface of the polymer layer. The conductive layer may be a metal layer. The metal of the metal layer may be aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, etc., and the polymer layer may contain at least one of polypropylene, polyethylene, polyethylene terephthalate, polybutylene terephthalate, polystyrene, polyaniline, poly(p-phenylene), polyacetylene, poly(p-phenylene acetylene), polypyrrole, and polythiophene.

[0047] In some embodiments, the positive electrode active material layer further includes a binder. As an example, the binder may include at least one of polyvinylidene fluoride, polytetrafluoroethylene, and a polyvinylidene fluoride-tetrafluoroethylene-propylene copolymer.

[0048] In some embodiments, the binder content is 0.5%-5% based on the total weight of the positive electrode active material layer.

[0049] In some embodiments, the positive electrode active material layer further includes a conductive agent. The conductive agent may include at least one selected from acetylene black, carbon black, Ketjen black, carbon nanotubes, graphene, and carbon nanofibers.

[0050] In some embodiments, the positive electrode active material layer further includes a conductive agent. The conductive agent may include at least two of acetylene black, carbon black, Ketjen black, carbon nanotubes, graphene, and carbon nanofibers.

[0051] In some embodiments, the content of the conductive agent is 1%-8% based on the total weight of the positive electrode active material layer. In some embodiments, the method for preparing the positive electrode active material includes: forming matrix particles and a coating layer located on the surface of the matrix particles, wherein the material of the matrix particles is a lithium nickel cobalt manganese oxide containing a first element, the first element including rubidium. Further, the first element also includes at least one of sodium, potassium, magnesium, aluminum, zirconium, titanium, vanadium, antimony, yttrium, tungsten, niobium, nitrogen, fluorine, sulfur, or chlorine.

[0052] In some embodiments, the step of forming matrix particles includes: forming a nickel cobalt manganese hydroxide precursor; providing a lithium source and a first element source, wherein the first element source is at least one of an oxide having a first element, a carbonate having a first element, and / or a hydroxide having a first element; mixing the nickel cobalt manganese hydroxide precursor, the lithium source, and the first element source together for a mixing process; and after mixing the nickel cobalt manganese hydroxide precursor, the lithium source, and the first element source together for a mixing process, sintering the nickel cobalt manganese hydroxide precursor, the lithium source, and the first element source.

[0053] In some embodiments, the sintering temperature for the nickel-cobalt-manganese hydroxide precursor, the lithium source, and the first dopant source is 600°C to 1000°C, for example, any value among 600°C, 630°C, 650°C, 680°C, 700°C, 750°C, 780°C, 800°C, 830°C, 850°C, 880°C, 900°C, 950°C, and 1000°C, or a range of any two of these values.

[0054] In some embodiments, the sintering temperature for the nickel-cobalt-manganese hydroxide precursor, the lithium source, and the first element source is 660°C to 950°C.

[0055] In some embodiments, the rate of temperature increase during the sintering process of the nickel-cobalt-manganese hydroxide precursor, the lithium source, and the first element source is 100℃ / h to 200℃ / h, for example, any value among 100℃ / h, 120℃ / h, 130℃ / h, 150℃ / h, 160℃ / h, 170℃ / h, 180℃ / h, 190℃ / h, and 200℃ / h, or a range of any two of them.

[0056] In some embodiments, the step of forming the nickel cobalt manganese hydroxide precursor includes: preparing a first solution using nickel salt, manganese salt and cobalt salt; and reacting the first solution with an alkaline solution to form the nickel cobalt manganese hydroxide precursor.

[0057] In some embodiments, the first solution includes a first sub-solution to an Nth sub-solution; N is an integer equal to or greater than 2; the molar content of nickel in the kth sub-solution is greater than the molar content of nickel in the (k+1)th sub-solution, and k is an integer greater than or equal to 1 and less than or equal to N-1; the step of reacting an alkaline solution with the first solution to form a nickel-cobalt-manganese hydroxide precursor includes: sequentially mixing the first sub-solution to the Nth sub-solution into the alkaline solution.

[0058] In some embodiments, the molar content of nickel in any j-th sub-solution accounts for 50% to 90% of the total molar content of nickel, manganese and cobalt in the j-th sub-solution. For example, it can be any value among 50%, 55%, 58%, 60%, 63%, 65%, 68%, 70%, 75%, 78%, 80%, 85%, 88%, 90%, or any range of two of these values, where j is an integer greater than or equal to 1 and less than or equal to N.

[0059] In some embodiments, the total molar concentration of nickel, manganese and cobalt in the j-th sub-solution is 0.8 mol / L to 1.2 mol / L, for example, it can be any value among 0.8 mol / L, 0.85 mol / L, 0.88 mol / L, 0.9 mol / L, 0.93 mol / L, 0.95 mol / L, 0.98 mol / L, 1 mol / L, 1.2 mol / L, or a range of any two of them.

[0060] In some embodiments, the pH value of the mixed solution formed during the process of sequentially mixing the first sub-solution to the Nth sub-solution into the alkaline solution is 10-12, for example, it can be any value among 10, 10.5, 11, 11.3, 11.5, 11.8, 12, or a range of any two of them.

[0061] In some embodiments, stirring and heating are performed during the mixing of any j-th sub-solution.

[0062] In some embodiments, the stirring speed is 500 rpm to 1100 rpm, for example, any value among 500 rpm, 550 rpm, 580 rpm, 600 rpm, 650 rpm, 670 rpm, 700 rpm, 730 rpm, 750 rpm, 800 rpm, 850 rpm, 900 rpm, 950 rpm, 1000 rpm, 1050 rpm, and 1100 rpm, or a range of any two of these values.

[0063] In some embodiments, the stirring time is 6h-9h, for example, any value among 6h, 6.5h, 6.8h, 7h, 7.2h, 7.5h, 7.8h, 8h, 8.5h, 8.8h, or a range of any two of them.

[0064] In some embodiments, the temperature of the heat treatment is 50°C to 65°C, for example, any value among 50°C, 53°C, 55°C, 58°C, 60°C, 62°C, and 65°C, or a range of any two of them.

[0065] In some embodiments, the step of forming a nickel-cobalt-manganese hydroxide precursor by reacting an alkaline solution with a first solution further includes: sequentially mixing the first sub-solution to the Nth sub-solution into the alkaline solution, and then performing an aging treatment for a time of 9h-14h, for example, any value among 9h, 10h, 10.5h, 11h, 11.5h, 12h, 13h, and 14h, or a range of any two of them.

[0066] In some embodiments, the diameter of the nickel cobalt manganese hydroxide precursor is 8 μm-12 μm, for example, any value among 8 μm, 8.5 μm, 9 μm, 9.5 μm, 10 μm, 10.5 μm, 11 μm, 11.5 μm, 12 μm, or a range of any two of these values.

[0067] In some embodiments, the step of forming a coating layer on the surface of the matrix particles includes: providing a coating source comprising a compound containing a second element, wherein the compound containing the second element is an oxide containing the second element, and the second element comprises at least one of lithium, cobalt, zinc, magnesium, aluminum, zirconium, titanium, vanadium, antimony, yttrium, niobium, strontium, and tungsten; mixing the matrix particles with the coating source; and then sintering the matrix particles with the coating source.

[0068] In some embodiments, the time for mixing the matrix particles with the coating source is 0.7h to 1.5h, for example, any value among 0.7h, 0.8h, 0.9h, 1h, 1.1h, 1.2h, 1.4h, and 1.5h, or a range of any two of them.

[0069] In some embodiments, during the sintering process of the matrix particles and the coating source, the temperature is 300°C to 500°C, for example, any value of 300°C, 320°C, 350°C, 370°C, 400°C, 420°C, 450°C, 480°C, 500°C, or a range of any two of these values.

[0070] In some embodiments, the sintering time for the matrix particles and the coating source is 6h-8h; the oxygen partial pressure in the chamber is 21kPa-50kPa.

[0071] In some embodiments, the temperature increases during the sintering process of the matrix particles and the coating source.

[0072] In some embodiments, the rate of temperature increase during the sintering process of the matrix particles and the coating source is 100℃ / h to 200℃ / h.

[0073] In some embodiments, O2 is introduced into the chamber during the sintering process of the matrix particles and the coating source, and the molar content of O2 accounts for 21% to 90% of the molar content of all gases in the chamber.

[0074] In some embodiments, O2 is introduced into the chamber during the sintering process of the matrix particles and the coating source, and the molar content of O2 accounts for 25% to 60% of the molar content of all gases in the chamber.

[0075] In other embodiments, the coating material includes lithium fluoride or lithium phosphate; the steps of forming the matrix particles and the coating layer located on the surface of the matrix particles include: forming a nickel cobalt manganese hydroxide precursor; providing a lithium source having a fluoride and / or phosphate having a first element; mixing the nickel cobalt manganese hydroxide precursor, the lithium source and the second dopant source together for a mixing process; and after mixing the nickel cobalt manganese hydroxide precursor, the lithium source and the second dopant source, sintering the nickel cobalt manganese hydroxide precursor, the lithium source and the second dopant source.

[0076] In some embodiments, the ratio of the molar content of lithium in the lithium source to the total molar content of nickel, manganese and cobalt in the nickel cobalt manganese hydroxide precursor is 0.95 to 1.1.

[0077] In one embodiment, the mixing time for mixing the nickel cobalt manganese hydroxide precursor, the lithium source, and the second dopant source together is 0.9 h to 1.2 h.

[0078] In one embodiment, the temperature increases during the sintering process of the nickel-cobalt-manganese hydroxide precursor, the lithium source, and the second doped source.

[0079] In one embodiment, the sintering time for the nickel-cobalt-manganese hydroxide precursor, lithium source, and second doping source is 9-11 hours.

[0080] In one embodiment, the oxygen partial pressure in the chamber during the sintering treatment of the nickel cobalt manganese hydroxide precursor, the lithium source, and the second doped source is 21 kPa to 50 kPa.

[0081] In one embodiment, the O2 concentration in the chamber is 21%-90% during the sintering process of the nickel cobalt manganese hydroxide precursor, lithium source, and second doped source.

[0082] Secondary batteries also include an electrolyte. The solvents of the electrolyte include ethylene carbonate (EC), diethyl carbonate (DEC), and dimethyl carbonate (DMC). The solvents are mixed in a certain proportion, and then lithium salts, such as lithium hexafluorophosphate (LiPF6), are added and dissolved in the above solvents to obtain the electrolyte.

[0083] In some embodiments, the negative electrode sheet includes a negative current collector and a negative active material layer on the surface of the negative current collector, the negative active material layer containing a negative active material.

[0084] In some embodiments, the negative current collector comprises aluminum foil.

[0085] This application also provides a battery pack including the aforementioned secondary battery. As a typical application, the battery pack can be used in, but is not limited to, electric toys, power tools, electric vehicles, electric cars, energy storage devices, ships, spacecraft, etc.

[0086] This application also provides an electrical device including the battery pack described above.

[0087] The preparation method of the secondary battery provided in this application is described below with reference to specific embodiments. It should be understood that these embodiments are only used to illustrate this application and are not intended to limit the scope of this application.

[0088] Example 1 The secondary battery provided in this embodiment includes a positive electrode, a negative electrode, a separator, and an electrolyte.

[0089] Preparation of the positive electrode sheet: The positive electrode active material, conductive agent carbon black, and binder polyvinylidene fluoride (PVDF) are mixed evenly at a mass ratio of 96.5:2:1.5. Then, they are thoroughly stirred and mixed in N-methylpyrrolidone (NMP) to form a uniform positive electrode slurry. The positive electrode slurry is uniformly coated on the surface of the positive electrode current collector aluminum foil. After drying, cold pressing, and die cutting, the positive electrode sheet is obtained.

[0090] The positive electrode active material is lithium nickel cobalt manganese oxide. Taking the total molar amount of nickel, cobalt and manganese in the lithium nickel cobalt manganese oxide as 1, the content of nickel is 0.8, the content of cobalt is 0.1 and the content of manganese is 0.1. The lithium nickel cobalt manganese oxide contains strontium, and the concentration of strontium is 3000 ppm. The positive electrode active material also includes a coating layer located on the surface of the matrix particles. The coating layer contains a second element, which is aluminum. The material of the coating layer is aluminum oxide (Al2O3), and the concentration of aluminum oxide is 3000 ppm.

[0091] The preparation method of the positive electrode active material is as follows: 1) Weigh out nickel sulfate, cobalt sulfate and manganese sulfate according to the elemental molar ratio Ni:Co:Mn=0.8:0.1:0.1 and dissolve them separately in deionized water. Transport each metal solution to the reaction vessel through pipeline to form a mixed metal solution. Introduce nitrogen gas as a protective gas. Add NaOH aqueous solution as a precipitant and ammonia water as a complexing agent to the mixed metal solution. Adjust the ammonia water concentration and pH value of the solution in stages. React for 10 hours to obtain the precursor.

[0092] 2) Mix the precursor, lithium hydroxide and strontium oxide evenly, and control the molar ratio of lithium to precursor to be 1.1:1. The mass percentage of strontium in the precursor is 0.3 wt%.

[0093] 3) Transfer the mixed materials to the sintering process, which includes two stages: the first stage is sintering at 500℃ for 6 hours; the second stage is sintering at 800℃ for 10 hours.

[0094] 4) Crush the sintered material and then mix the crushed material with alumina evenly. The mass ratio of aluminum to the crushed material is 0.3wt%.

[0095] 5) Transfer the mixed materials to the sintering process. The sintering temperature is 450℃ and the sintering time is 8 hours to obtain the positive electrode active material.

[0096] Preparation of negative electrode sheet: Graphite, conductive carbon SP, dispersant CMC, and binder SBR are mixed evenly in a ratio of 96.5:0.5:1.5:1.5, and then deionized water is added to coat the copper foil surface; then the negative electrode sheet is prepared by drying, cold pressing, die cutting and other processes. Separator membrane: Polypropylene membrane is used as the separator membrane.

[0097] Preparation of electrolyte: In an argon-atmospheric glove box, ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed evenly at a mass ratio of 3:7. Then, 12 wt% of lithium LiPF6 was added and dissolved in the organic solvent. 2 wt% of vinylene carbonate (VC) and 1 wt% of vinyl sulfate were added and stirred evenly to obtain the electrolyte.

[0098] Battery fabrication: The positive electrode, negative electrode, and separator are wound together to form a bare cell, which is then installed into a battery case. The lithium-ion battery is then fabricated through processes such as liquid injection, high-temperature settling, formation, aging, and capacity testing.

[0099] Example 2 The difference between the secondary battery provided in this embodiment and the secondary battery provided in Embodiment 1 is that the first element in the positive electrode active material is rubidium, and the concentration of rubidium is 3000ppm. When the charging voltage of the secondary battery is 4.35V, thermogravimetric mass spectrometry analysis of the positive electrode active material layer shows that the oxygen release initiation temperature of the positive electrode active material layer is 215.9℃, the oxygen release amount of the positive electrode active material layer is 72.58mL / g, the active delithiation amount of the positive electrode active material is 0.82, N=T / b =263.29, and M=b×Z×U=258.89.

[0100] Example 3 The difference between the secondary battery provided in this embodiment and the secondary battery provided in Embodiment 1 is that the first element in the positive electrode active material is neodymium, and the concentration of neodymium is 3000ppm. When the charging voltage of the secondary battery is 4.35V, thermogravimetric mass spectrometry analysis of the positive electrode active material layer shows that the oxygen release initiation temperature of the positive electrode active material layer is 217.4℃, the oxygen release amount of the positive electrode active material layer is 68.92mL / g, the active delithiation amount of the positive electrode active material is 0.82, N=T / b =265.12, and M=b×Z×U=245.84.

[0101] Example 4 The difference between the secondary battery provided in this embodiment and the secondary battery provided in Embodiment 1 is that the first element in the positive electrode active material is strontium and zirconium, the concentration of strontium is 2000 ppm and the concentration of zirconium is 1000 ppm. When the charging voltage of the secondary battery is 4.35V, thermogravimetric mass spectrometry analysis of the positive electrode active material layer shows that the oxygen release initiation temperature of the positive electrode active material layer is 219.7℃, the oxygen release amount of the positive electrode active material layer is 65.43 mL / g, the active delithiation amount of the positive electrode active material is 0.82, N = T / b = 267.93, and M = b × Z × U = 233.39.

[0102] Example 5 The difference between the secondary battery provided in this embodiment and the secondary battery provided in Embodiment 1 is that the first element in the positive electrode active material is strontium and sodium, with a strontium concentration of 2000 ppm and a sodium concentration of 1000 ppm. When the charging voltage of the secondary battery is 4.35V, thermogravimetric mass spectrometry analysis of the positive electrode active material layer shows that the oxygen release initiation temperature of the positive electrode active material layer is 218.4℃, the oxygen release amount of the positive electrode active material layer is 60.21 mL / g, the active delithiation amount of the positive electrode active material is 0.81, N = T / b = 269.63, and M = b × Z × U = 212.15.

[0103] Example 6 The difference between the secondary battery provided in this embodiment and the secondary battery provided in Embodiment 1 is that the first element in the positive electrode active material is strontium and magnesium, with a strontium concentration of 2000 ppm and a magnesium concentration of 1000 ppm. When the charging voltage of the secondary battery is 4.35V, thermogravimetric mass spectrometry analysis of the positive electrode active material layer shows that the oxygen release initiation temperature of the positive electrode active material layer is 217.8℃, the oxygen release amount of the positive electrode active material layer is 55.56 mL / g, the active delithiation amount of the positive electrode active material is 0.81, N = T / b = 268.89, and M = b × Z × U = 195.77.

[0104] Example 7 The difference between the secondary battery provided in this embodiment and the secondary battery provided in Embodiment 4 is that the coating material is titanium dioxide with a concentration of 3000 ppm. When the charging voltage of the secondary battery is 4.35 V, thermogravimetric mass spectrometry analysis of the positive electrode active material layer shows that the oxygen release initiation temperature of the positive electrode active material layer is 224.5 °C, the oxygen release amount of the positive electrode active material layer is 52.66 mL / g, the active delithiation amount of the positive electrode active material is 0.81, N = T / b = 277.16, and M = b × Z × U = 185.55.

[0105] Example 8 The difference between the secondary battery provided in this embodiment and the secondary battery provided in Embodiment 4 is as follows: the sintering temperature of the positive electrode active material is adjusted, and the total molar amount of nickel, cobalt and manganese in the precursor is 1, the content of nickel is controlled to be 0.7, the content of cobalt to be 0.1, and the content of manganese to be 0.2, the coating material is tungsten trioxide (WO3) with a concentration of 3000ppm, and when the charging voltage of the secondary battery is 4.35V, thermogravimetric mass spectrometry analysis of the positive electrode active material layer is performed. The oxygen release initiation temperature of the positive electrode active material layer is 220.4℃, the oxygen release amount of the positive electrode active material layer is 53.67mL / g, the active delithiation amount of the positive electrode active material is 0.79, N=T / b =278.99, M=b×Z×U=184.44.

[0106] Example 9 The difference between the secondary battery provided in this embodiment and the secondary battery provided in Embodiment 4 is that: the sintering temperature of the positive electrode active material is adjusted, and the total molar amount of nickel, cobalt and manganese in the precursor is 1, while the molar content of nickel is controlled to be 0.6, the molar content of cobalt is 0.2, and the molar content of manganese is 0.2. When the charging voltage of the secondary battery is 4.35V, thermogravimetric mass spectrometry analysis is performed on the positive electrode active material layer. The oxygen release initiation temperature of the positive electrode active material layer is 222.8℃, the oxygen release amount of the positive electrode active material layer is 50.26mL / g, the active delithiation amount of the positive electrode active material is 0.77, N=T / b =289.35, M=b×Z×U=168.35.

[0107] Example 10 The difference between the secondary battery provided in this embodiment and the secondary battery provided in Embodiment 4 is that: the sintering temperature of the positive electrode active material is adjusted, and the total molar amount of nickel, cobalt and manganese elements in the precursor is 1, while the molar content of nickel is controlled to be 0.6, the molar content of cobalt is 0.1 and the molar content of manganese is 0.3. When the charging voltage of the secondary battery is 4.35V, thermogravimetric mass spectrometry analysis is performed on the positive electrode active material layer. The oxygen release initiation temperature of the positive electrode active material layer is 223.6℃, ​​the oxygen release amount of the positive electrode active material layer is 49.73mL / g, the active delithiation amount of the positive electrode active material is 0.76, N=T / b =294.21, M=b×Z×U=164.41.

[0108] Example 11 The difference between the secondary battery provided in this embodiment and the secondary battery provided in Embodiment 1 is that the positive electrode active material does not include a coating layer. When the charging voltage of the secondary battery is 4.35V, thermogravimetric mass spectrometry analysis of the positive electrode active material layer shows that the oxygen release initiation temperature of the positive electrode active material layer is 212.6℃, the oxygen release amount of the positive electrode active material layer is 74.32mL / g, the active delithiation amount of the positive electrode active material is 0.82, N=T / b =259.27, and M=b×Z×U=265.10.

[0109] Example 12 The difference between the secondary battery provided in this embodiment and the secondary battery provided in Embodiment 11 is that the strontium concentration is 1000 ppm. When the charging voltage of the secondary battery is 4.35 V, thermogravimetric mass spectrometry analysis of the positive electrode active material layer shows that the oxygen release initiation temperature of the positive electrode active material layer is 209.3 °C, the oxygen release amount of the positive electrode active material layer is 75.47 mL / g, the active delithiation amount of the positive electrode active material is 0.82, N = T / b = 255.24, and M = b × Z × U = 269.20.

[0110] Example 13 The difference between the secondary battery provided in this embodiment and the secondary battery provided in Embodiment 11 is that the strontium concentration is 5000ppm. When the charging voltage of the secondary battery is 4.35V, thermogravimetric mass spectrometry analysis of the positive electrode active material layer shows that the oxygen release initiation temperature of the positive electrode active material layer is 214.7℃, the oxygen release amount of the positive electrode active material layer is 70.68mL / g, the active delithiation amount of the positive electrode active material is 0.82, N=T / b =261.83, and M=b×Z×U=252.12.

[0111] Example 14 The difference between the secondary battery provided in this embodiment and the secondary battery provided in Example 11 is that the strontium concentration is 500 ppm. When the charging voltage of the secondary battery is 4.35V, thermogravimetric mass spectrometry analysis of the positive electrode active material layer shows that the oxygen release initiation temperature of the positive electrode active material layer is 208.5℃, the oxygen release amount of the positive electrode active material layer is 76.83 mL / g, the active delithiation amount of the positive electrode active material is 0.82, N = T / b = 254.27, and M = b × Z × U = 274.05.

[0112] Example 15 The difference between the secondary battery provided in this embodiment and the secondary battery provided in Embodiment 4 is that the concentration of aluminum oxide is 1000 ppm. When the charging voltage of the secondary battery is 4.35V, thermogravimetric mass spectrometry analysis of the positive electrode active material layer shows that the oxygen release initiation temperature of the positive electrode active material layer is 216.9℃, the oxygen release amount of the positive electrode active material layer is 53.74 mL / g, the active delithiation amount of the positive electrode active material is 0.79, N = T / b = 274.56, and M = b × Z × U = 184.68.

[0113] Example 16 The difference between the secondary battery provided in this embodiment and the secondary battery provided in Embodiment 4 is that the concentration of aluminum oxide is 5000 ppm. When the charging voltage of the secondary battery is 4.35V, thermogravimetric mass spectrometry analysis of the positive electrode active material layer shows that the oxygen release initiation temperature of the positive electrode active material layer is 221.7℃, the oxygen release amount of the positive electrode active material layer is 48.63 mL / g, the active delithiation amount of the positive electrode active material is 0.78, N = T / b = 284.23, and M = b × Z × U = 165.00.

[0114] Example 17 The difference between the secondary battery provided in this embodiment and the secondary battery provided in Embodiment 1 is that the first element is sodium, strontium, and zirconium, with a sodium concentration of 500 ppm, a strontium concentration of 1500 ppm, and a zirconium concentration of 1000 ppm. When the secondary battery charging voltage is 4.35V, thermogravimetric mass spectrometry analysis of the positive electrode active material layer shows that the oxygen release initiation temperature of the positive electrode active material layer is 210.3℃, the oxygen release amount of the positive electrode active material layer is 73.78 mL / g, the active delithiation amount of the positive electrode active material is 0.82, N = T / b = 256.46, and M = b × Z × U = 263.17.

[0115] Example 18 The difference between the secondary battery provided in this embodiment and the secondary battery provided in Embodiment 1 is that the first element is magnesium, zirconium, and strontium, with a magnesium concentration of 500 ppm, a strontium concentration of 2000 ppm, and a zirconium concentration of 500 ppm. When the charging voltage of the secondary battery is 4.35 V, thermogravimetric mass spectrometry analysis of the positive electrode active material layer shows that the oxygen release initiation temperature of the positive electrode active material layer is 211.5 °C, the oxygen release amount of the positive electrode active material layer is 72.65 mL / g, the active delithiation amount of the positive electrode active material is 0.82, N=T / b =257.93, and M=b×Z×U=259.14.

[0116] Example 19 The difference between the secondary battery provided in this embodiment and the secondary battery provided in Embodiment 1 is that the first element is titanium and strontium, the concentration of titanium is 2000 ppm, and the concentration of strontium is 1000 ppm. When the charging voltage of the secondary battery is 4.35V, thermogravimetric mass spectrometry analysis of the positive electrode active material layer shows that the oxygen release initiation temperature of the positive electrode active material layer is 209.8℃, the oxygen release amount of the positive electrode active material layer is 69.58 mL / g, the active delithiation amount of the positive electrode active material is 0.82, N = T / b = 255.85, and M = b × Z × U = 248.19.

[0117] Example 20 The difference between the secondary battery provided in this embodiment and the secondary battery provided in Embodiment 19 is that: the sintering temperature of the positive electrode active material is adjusted, and the total molar amount of nickel, cobalt and manganese in the precursor is controlled to be 1, the content of nickel is 0.7, the content of cobalt is 0.1 and the content of manganese is 0.2. When the charging voltage of the secondary battery is 4.35V, thermogravimetric mass spectrometry analysis of the positive electrode active material layer is performed. The oxygen release initiation temperature of the positive electrode active material layer is 214.5℃, the oxygen release amount of the positive electrode active material layer is 67.36mL / g, the active delithiation amount of the positive electrode active material is 0.82, N=T / b =261.59, M=b×Z×U=240.27.

[0118] Example 21 The difference between the secondary battery provided in this embodiment and the secondary battery provided in Embodiment 19 is as follows: taking the total molar amount of nickel, cobalt and manganese as 1, the content of nickel is 0.6, the content of cobalt is 0.2, and the content of manganese is 0.2. When the charging voltage of the secondary battery is 4.35V, thermogravimetric mass spectrometry analysis of the positive electrode active material layer shows that the oxygen release initiation temperature of the positive electrode active material layer is 216.7℃, the oxygen release amount of the positive electrode active material layer is 65.57mL / g, the active delithiation amount of the positive electrode active material is 0.82, N=T / b =264.27, and M=b×Z×U=233.89.

[0119] Example 22 The difference between the secondary battery provided in this embodiment and the secondary battery provided in Embodiment 19 is as follows: taking the total molar amount of nickel, cobalt and manganese in the lithium nickel cobalt manganese oxide as 1, the content of nickel is 0.6, the content of cobalt is 0.1, and the content of manganese is 0.3. When the charging voltage of the secondary battery is 4.35V, thermogravimetric mass spectrometry analysis of the positive electrode active material layer shows that the oxygen release initiation temperature of the positive electrode active material layer is 218.4℃, the oxygen release amount of the positive electrode active material layer is 64.32mL / g, the active delithiation amount of the positive electrode active material is 0.82, N=T / b =266.34, and M=b×Z×U=229.43.

[0120] Comparative Example 1 This comparative example provides a secondary battery, including a positive electrode sheet, the positive electrode sheet comprising a positive electrode active material layer, the positive electrode active material layer comprising a positive electrode active material, the positive electrode active material comprising lithium nickel cobalt manganese oxide, with the total molar amount of nickel, cobalt and manganese in the lithium nickel cobalt manganese oxide being 1, the content of nickel being 0.8, the content of cobalt being 0.1, the content of manganese being 0.1, the lithium nickel cobalt manganese oxide not containing the first element, the positive electrode active material not including a coating layer, and when the secondary battery charging voltage is 4.35V, thermogravimetric mass spectrometry analysis of the positive electrode active material layer shows that the oxygen release onset temperature of the positive electrode active material layer is 202.4℃, the oxygen release amount of the positive electrode active material layer is 89.47mL / g, the active delithiation amount of the positive electrode active material is 0.83, N=T / b =243.86, M=b×Z×U=323.03.

[0121] Comparative Example 2 This comparative example provides a secondary battery, including a positive electrode sheet, the positive electrode sheet comprising a positive electrode active material layer, the positive electrode active material layer comprising a positive electrode active material, the positive electrode active material comprising lithium nickel cobalt manganese oxide, with the total molar amount of nickel, cobalt and manganese in the lithium nickel cobalt manganese oxide being 1, the content of nickel being 0.8, the content of cobalt being 0.1, the content of manganese being 0.1, the content of the first element being zirconium being 3000 ppm, the lithium nickel cobalt manganese oxide comprising a first element, the first element being zirconium, the concentration of zirconium being 3000 ppm, and the positive electrode active material excluding a coating layer. When the secondary battery is charged at a voltage of 4.35V, thermogravimetric mass spectrometry analysis of the positive electrode active material layer shows that the oxygen release onset temperature of the positive electrode active material layer is 202.9℃, the oxygen release amount of the positive electrode active material layer is 86.37 mL / g, the active delithiation amount of the positive electrode active material is 0.83, N = T / b = 244.46, M = b × Z × U = 311.84.

[0122] Comparative Example 3 This comparative example provides a secondary battery, including a positive electrode sheet, the positive electrode sheet comprising a positive electrode active material layer, the positive electrode active material layer comprising a positive electrode active material, the positive electrode active material comprising lithium nickel cobalt manganese oxide, wherein the total molar amount of nickel, cobalt and manganese in the lithium nickel cobalt manganese oxide is 1, the content of nickel is 0.8, the content of cobalt is 0.1, the content of manganese is 0.1, the lithium nickel cobalt manganese oxide does not contain a first element, the positive electrode active material further comprising a coating layer located on the surface of the matrix particles, the coating layer comprising a second element, the second element being aluminum, the material of the coating layer being aluminum oxide, and the concentration of aluminum oxide being 3000 ppm. When the secondary battery charging voltage is 4.35V, thermogravimetric mass spectrometry analysis of the positive electrode active material layer shows that the oxygen release initiation temperature of the positive electrode active material layer is 203.5℃, the oxygen release amount of the positive electrode active material layer is 85.29mL / g, the active delithiation amount of the positive electrode active material is 0.83, N=T / b =245.18, and M=b×Z×U=307.94.

[0123] Test method: Thermogravimetric mass spectrometry (TG-MS) tests, active lithium depletion tests, and high-temperature cycling performance tests were conducted on the positive electrode active materials under different charging states.

[0124] TG-MS testing includes: 1. At 25℃, charge the secondary battery at a constant current of 1C to the upper limit of the charge / discharge cutoff voltage, then charge it at a constant voltage until the current is less than or equal to 0.05C. After that, let it rest for 2 minutes, and then discharge it at a constant current of 1C to the lower limit of the charge / discharge cutoff voltage. The discharge capacity is the actual capacity C0 of the cell. 2. Charge the secondary battery at a constant current of 1 times C0 to the upper limit of the charge / discharge cutoff voltage, and then charge it at a constant voltage until the current is less than or equal to 0.05 times C0. 2. Take each charged secondary battery, disassemble the positive electrode in a dry room, and clean it with dimethyl carbonate (DMC) as a sample; 3. Weigh 100mg to 200mg of the charged positive electrode and place it in the crucible of the thermogravimetric mass spectrometer. Heat the sample to 500℃ at a heating rate of 5℃ / min. Use He gas as the test atmosphere and quantitatively record the changes in oxygen release with temperature (O2, H2O, CO2) to obtain the TG-MS spectrum. Obtain the initial temperature of oxygen release and calculate the amount of oxygen released.

[0125] The active lithium removal test includes: taking the positive electrode sheets before and after charging and punching them into round discs with a total mass greater than 0.5 g, weighing and recording the sample mass, placing them in a digestion vessel, slowly adding 10 mL of aqua regia as a digestion reagent, and then placing them in a microwave digester for digestion; transferring the digested and filtered sample solution to a volumetric flask and shaking well, taking a sample and placing it in an inductively coupled plasma atomic emission spectrometer (ICP-OES), and testing the elemental content of the positive electrode active material at 0.6 MPa argon pressure and 1300 W RF power. The difference in lithium elemental content before and after charging is the active lithium removal amount of the positive electrode (reference standard: positive electrode material: EPA 6010D-2018 Inductively Coupled Plasma Atomic Emission Spectrometry).

[0126] The high-temperature cycle performance test includes: charging the secondary battery at 45°C with a constant current of 1C to the upper limit of the charge / discharge cutoff voltage, then charging with a constant voltage until the current is less than or equal to 0.05C, then resting for 5 minutes, and then discharging at a constant current of 1C to the lower limit of the charge / discharge cutoff voltage. This constitutes one charge / discharge cycle, and the discharge capacity of this cycle is recorded as the discharge specific capacity D1 of the first cycle. The secondary battery is then subjected to 1000 charge / discharge cycles using the above method, and the discharge specific capacity D1 of the 1000th cycle is recorded. 1000 The capacity retention rate of the secondary battery after 1000 cycles was calculated.

[0127] Energy density testing includes recording the corresponding discharge energy data during a single charge-discharge cycle. The ratio of the discharge energy to the corresponding positive electrode active mass is the energy density of the positive electrode active material.

[0128] The performance parameters of the positive electrode active materials provided in Examples 1-22 and Comparative Examples 1-3 at the same voltage (4.35V) are shown in Table 1.

[0129] Table 1

[0130] refer to Figure 1 , Figure 1 The graph shows the high-temperature cycling performance of the positive electrode active material of Example 1 and the positive electrode active material of Comparative Example 1. The vertical axis represents the capacity retention rate, and the horizontal axis represents the number of cycles. The solid line represents the positive electrode active material of Example 1, and the dashed line represents the positive electrode active material of Comparative Example 1. It can be seen that the positive electrode active material of Example 1 has better high-temperature cycling stability than the positive electrode active material of Comparative Example 1.

[0131] refer to Figure 2 , Figure 2The thermogravimetric mass spectra of the positive electrode active material of Example 1 and the positive electrode active material of Comparative Example 1 are shown. The vertical axis represents the oxygen release, and the horizontal axis represents the heating temperature. The solid line represents the positive electrode active material of Example 1, and the dashed line represents the positive electrode active material of Comparative Example 1. It can be seen that the positive electrode active material of Example 1 has better thermal stability than the positive electrode active material of Comparative Example 1.

[0132] The comparison between Examples 1-7, Examples 11-19 and Comparative Examples 1-3 shows that when the lithium nickel cobalt manganese oxide in the positive electrode active material layer contains rubidium, neodymium or strontium, the thermal stability of the positive electrode active material layer can be improved.

[0133] A comparison between Example 1 and Example 11 shows that when the positive electrode active material is further covered with a coating layer, the stability of the positive electrode active material can be improved, and the positive electrode active material can be better bonded to other materials in the positive electrode active material layer, which can further improve the performance of the battery.

[0134] The comparison of Examples 1, 4, and 17-19 shows that when the positive electrode active material contains at least one of rubidium, neodymium, or strontium, the further inclusion of zirconium or titanium can further improve the overall performance of the secondary battery.

[0135] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.

Claims

1. A secondary battery, comprising a positive electrode, characterized in that, The positive electrode sheet includes a positive electrode active material layer, which contains a positive electrode active material. The positive electrode active material contains lithium nickel cobalt manganese oxide. Taking the total molar amount of nickel, cobalt, and manganese in the lithium nickel cobalt manganese oxide as 1, the content of nickel is x, where x>0.

5. The lithium nickel cobalt manganese oxide contains a first element, which contains rubidium. When the secondary battery charging voltage is UV, thermogravimetric mass spectrometry analysis is performed on the positive electrode active material layer to satisfy 200≤N≤400, where N=T / b, T℃ is the oxygen release initiation temperature of the positive electrode active material layer, b is the active delithiation amount of the positive electrode active material, and 4.0≤U≤4.

7.

2. The secondary battery according to claim 1, characterized in that, 200≤T≤250, 0.55≤b≤0.

95.

3. The secondary battery according to claim 1, characterized in that, The oxygen release capacity of the positive electrode active material layer is Z mL / g, M = b × Z × U, and 100 ≤ M ≤ 350.

4. The secondary battery according to claim 3, characterized in that, Z≤90, b<0.

9.

5. The secondary battery according to claim 1, characterized in that, When the voltage of the secondary battery is 4.0V, thermogravimetric mass spectrometry analysis is performed on the positive electrode active material layer, and the oxygen release amount of the positive electrode active material layer is Z1mL / g. When the voltage of the secondary battery is 4.7V, thermogravimetric mass spectrometry analysis is performed on the positive electrode active material layer, and the oxygen release amount of the positive electrode active material layer is Z2mL / g, satisfying 0.5≤Z1 / Z2≤1.

6. The secondary battery according to claim 5, characterized in that, 40≤Z1≤60, 60≤Z2≤80.

7. The secondary battery according to claim 1, characterized in that, The positive electrode active material includes matrix particles, the material of which is lithium nickel cobalt manganese oxide, and the matrix particles contain a first element.

8. The secondary battery according to claim 1 or 7, characterized in that, The first element further comprises at least one of sodium, potassium, magnesium, aluminum, zirconium, titanium, vanadium, antimony, yttrium, tungsten, niobium, nitrogen, fluorine, sulfur, or chlorine.

9. The secondary battery according to claim 7, characterized in that, The positive electrode active material further includes a coating layer located on the surface of the matrix particles. The coating layer contains a compound of a second element. The compound containing the second element includes one or more of the oxides, fluorides, or phosphates of the second element. The second element includes at least one of lithium, cobalt, zinc, magnesium, aluminum, zirconium, titanium, vanadium, antimony, yttrium, niobium, strontium, and tungsten.

10. The secondary battery according to claim 7, characterized in that, The nickel content on the surface of the matrix particles is lower than the nickel content at the center of the matrix particles.

11. A battery pack, characterized in that, The secondary battery comprising any one of claims 1 to 10.

12. An electrical appliance, characterized in that, It includes the battery pack as described in claim 11.

Citation Information

Patent Citations

  • POSITIVE ELECTRODE ACTIVE MATERIAL FOR Lithium SECONDARY BATTERY, METHOD FOR PREPARING THE SAME AND LITHIUM SECONDARY BATTERY

    CN108336326A

  • Positive electrode active material, positive electrode plate and lithium ion secondary battery

    CN112447967A

  • Method and systems for metal doping on battery cathode materials

    US20200365874A1