A black phosphorus / red phosphorus-cadmium sulfide heterojunction photocatalyst and its preparation method and application

CN116408111BActive Publication Date: 2024-11-05KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310581172.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-22
Publication Date
2024-11-05
Estimated Expiration
2043-05-22

Smart Images

  • Figure CN116408111B_ABST
    Figure CN116408111B_ABST
Patent Text Reader

Abstract

This invention provides a black phosphorus / red phosphorus-cadmium sulfide heterojunction photocatalyst, its preparation method, and its application, belonging to the field of photocatalytic materials technology. The invention involves mixing red phosphorus with water and performing a hydrothermal reaction, followed by solid-liquid separation to obtain purified red phosphorus. The purified red phosphorus is then mixed with a soluble cadmium source, a soluble sulfur source, and a primary diamine solvent, and subjected to a solvothermal reaction to obtain the black phosphorus / red phosphorus-cadmium sulfide heterojunction photocatalyst. The hydrothermal reaction of red phosphorus with water removes the oxide film layer on the surface of red phosphorus, achieving purification. The in-situ solvothermal method using primary diamine as a solvent allows for the phase transition of some red phosphorus to black phosphorus under the action of primary diamine, constructing a black phosphorus / red phosphorus-cadmium sulfide heterojunction. This improves the stability of black phosphorus, resulting in a highly stable catalyst that enables electron transfer within the catalyst material, thereby enhancing photocatalytic activity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of photocatalytic materials, and in particular to a black phosphorus / red phosphorus-cadmium sulfide heterojunction photocatalyst and a preparation method and application thereof. Background Art

[0002] The increasingly serious energy and environmental crises threaten the sustainable development of human society. In order to cope with the challenges of energy shortage and environmental pollution, it is urgent to develop new and environmentally friendly energy conversion methods. Inspired by plant photosynthesis, photocatalytic reactions driven by sunlight can achieve energy conversion in a green and environmentally friendly way and have attracted widespread attention. Currently, semiconductor photocatalysts are the most commonly used photocatalysts.

[0003] The principle of photocatalysis is mainly to use the electrons and holes of semiconductor materials. After external light irradiates the photocatalyst, the photogenerated electrons are stimulated to jump from the valence band of the catalyst to the conduction band, so that photogenerated electrons and holes are generated in the conduction band and valence band respectively. The photogenerated electrons and holes migrate to the surface of the photocatalyst and undergo redox reactions with the water molecules adsorbed on the surface of the catalyst. The photogenerated electrons on the conduction band convert H + Reduction to H2. Therefore, choosing the right semiconductor material as photocatalyst is the key part of photocatalytic application.

[0004] Among the catalysts for many photocatalytic reactions, cadmium sulfide (CdS) materials have the advantages of low cost and redox potential matching that of hydrogen, and have become a research hotspot in the field of photocatalytic hydrogen evolution at this stage. However, CdS also has many disadvantages as a photocatalyst, such as insufficient visible light absorption, high recombination rate of photogenerated electrons and holes, and insufficient reaction sites, which make its photocatalytic hydrogen production efficiency low, which limits the further application of CdS in the field of photocatalytic hydrogen evolution. Summary of the invention

[0005] In view of this, the present invention aims to provide a black phosphorus / red phosphorus-cadmium sulfide heterojunction photocatalyst and its preparation method and application. The black phosphorus / red phosphorus-cadmium sulfide heterojunction photocatalyst prepared by the present invention has good photocatalytic hydrogen production efficiency.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The present invention provides a method for preparing a black phosphorus / red phosphorus-cadmium sulfide heterojunction photocatalyst, comprising the following steps:

[0008] Mixing red phosphorus with water, performing a hydrothermal reaction, and obtaining purified red phosphorus after solid-liquid separation;

[0009] The purified red phosphorus is mixed with a soluble cadmium source, a soluble sulfur source and a primary diamine solvent, and a solvent thermal reaction is performed to obtain a black phosphorus / red phosphorus-cadmium sulfide heterojunction photocatalyst.

[0010] Preferably, the temperature of the hydrothermal reaction is 190-210° C., and the time is 11-13 hours.

[0011] Preferably, the soluble cadmium source is cadmium chloride, and the soluble sulfur source is one or more of thioacetamide, thiourea and glutathione.

[0012] Preferably, the primary diamine solvent is ethylenediamine and / or diethylenetriamine.

[0013] Preferably, the mass of the purified red phosphorus is 1-5% of the mass of the soluble cadmium source.

[0014] Preferably, the molar ratio of the soluble cadmium source to the soluble sulfur source is 1:2-4.

[0015] Preferably, the temperature of the solvent thermal reaction is 140-160° C., and the time is 12-20 hours.

[0016] The invention provides a black phosphorus / red phosphorus-cadmium sulfide heterojunction photocatalyst prepared by the preparation method, comprising cadmium sulfide nanorods and red phosphorus nanoparticles and black phosphorus nanoparticles distributed on the surfaces of the cadmium sulfide nanorods.

[0017] Preferably, the cadmium sulfide nanorods have a length of 100 to 300 nm and a diameter of 20 to 50 nm;

[0018] The particle sizes of the red phosphorus nanoparticles and the black phosphorus nanoparticles are independently 5 to 10 nm.

[0019] The present invention provides the use of the black phosphorus / red phosphorus-cadmium sulfide heterojunction photocatalyst in photocatalytic water decomposition to produce hydrogen.

[0020] The present invention provides a method for preparing a black phosphorus / red phosphorus-cadmium sulfide heterojunction photocatalyst, comprising the following steps: mixing red phosphorus with water, performing a hydrothermal reaction, and obtaining purified red phosphorus after solid-liquid separation; mixing the purified red phosphorus with a soluble cadmium source, a soluble sulfur source, and a primary diamine solvent, performing a solvothermal reaction, and obtaining a black phosphorus / red phosphorus-cadmium sulfide heterojunction photocatalyst (abbreviated as BP / RP-CdS). The present invention performs a hydrothermal reaction between red phosphorus and water, which can remove the oxide film layer on the surface of red phosphorus and achieve the effect of purifying red phosphorus; black phosphorus (BP) has the advantages of high carrier mobility, good conductivity, large specific surface area, and abundant photocatalytic active sites, which can well make up for the deficiency of cadmium sulfide, but black phosphorus itself is easily oxidized. The present invention adopts an in-situ solvothermal method and uses a primary diamine as a solvent. During the solvothermal reaction, part of the red phosphorus undergoes a phase change under the action of the primary diamine and is converted into black phosphorus, thereby constructing a black phosphorus / red phosphorus-cadmium sulfide heterojunction, which can improve the stability of black phosphorus. The obtained catalyst has high stability and can realize electron transfer inside the catalyst material, thereby improving the photocatalytic activity. The results of the embodiment show that the black phosphorus / red phosphorus-cadmium sulfide heterojunction photocatalyst provided by the present invention is used for photocatalytic decomposition of water to produce hydrogen, and its hydrogen production reaches 10.3mmol·g -1 ·h -1 , compared with cadmium sulfide, the hydrogen production is greatly improved.

[0021] At the same time, the present invention adopts a simple solvent thermal method, has a simple operation process, low cost, and is easy to realize industrial mass production. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a transmission electron microscope photo of the black phosphorus / red phosphorus-cadmium sulfide heterojunction photocatalyst obtained in Example 1;

[0023] Figure 2 The black phosphorus / red phosphorus-cadmium sulfide heterojunction photocatalyst obtained in Example 3 and cadmium sulfide as a catalyst for hydrogen production under the same conditions. DETAILED DESCRIPTION

[0024] The present invention provides a method for preparing a black phosphorus / red phosphorus-cadmium sulfide heterojunction photocatalyst, comprising the following steps:

[0025] Mixing red phosphorus with water, performing a hydrothermal reaction, and obtaining purified red phosphorus after solid-liquid separation;

[0026] The purified red phosphorus is mixed with a soluble cadmium source, a soluble sulfur source and a primary diamine solvent, and a solvent thermal reaction is performed to obtain a black phosphorus / red phosphorus-cadmium sulfide heterojunction photocatalyst.

[0027] Unless otherwise specified, the raw materials used in the present invention are all commercially available.

[0028] The present invention mixes red phosphorus with water, performs a hydrothermal reaction, and obtains purified red phosphorus after solid-liquid separation. In the present invention, the red phosphorus is preferably commercially available red phosphorus, and the purity of the red phosphorus is preferably 99.999%. During the storage process, a layer of oxide film will be formed on the surface of the commercially available red phosphorus, which needs to be further purified.

[0029] In the present invention, the water is preferably deionized water; in the present invention, the volume ratio of the mass of the red phosphorus to water is preferably 3-3.3 g: 60-66 mL, more preferably 3.1-3.2 g: 62-64 mL.

[0030] In the present invention, the hydrothermal reaction is preferably carried out in a hydrothermal reaction kettle. In the present invention, the temperature of the hydrothermal reaction is preferably 190-210°C, more preferably 200°C; the time is preferably 11-13h, more preferably 12h.

[0031] After the hydrothermal reaction, the present invention preferably performs post-treatment on the obtained hydrothermal reaction product, and the post-treatment preferably comprises the following steps:

[0032] The hydrothermal reaction product is sequentially cooled and solid-liquid separated, and the obtained solid is dried to obtain purified red phosphorus solid powder.

[0033] In the present invention, the cooling is preferably natural cooling to room temperature; the solid-liquid separation is preferably centrifugation, the centrifugal speed is preferably 10000-11000 rpm, the centrifugal time is preferably 5-10 min, more preferably 6-8 min. The present invention preferably performs the drying in a vacuum drying oven, the drying temperature is preferably 40-60°C, more preferably 50°C, the drying time is preferably 15-24 h, more preferably 18-20 h.

[0034] After obtaining the purified red phosphorus, the present invention mixes the purified red phosphorus with a soluble cadmium source, a soluble sulfur source, and a primary diamine solvent, and performs a solvothermal reaction to obtain a black phosphorus / red phosphorus-cadmium sulfide heterojunction photocatalyst. In the present invention, the soluble cadmium source is preferably cadmium chloride, and the soluble sulfur source is preferably one or more of thioacetamide, thiourea, and glutathione. In the present invention, the primary diamine solvent is preferably ethylenediamine and / or diethylenetriamine.

[0035] In the present invention, the mass of the purified red phosphorus is preferably 1-5% of the mass of the soluble cadmium source, and more preferably 2-4%.

[0036] In the present invention, the molar ratio of the soluble cadmium source to the soluble sulfur source is preferably 1:2-4, more preferably 1:3.

[0037] In the present invention, the volume ratio of the mass of the soluble cadmium source to the primary diamine solvent is preferably 1:15 to 20, more preferably 1:17.

[0038] In the present invention, the solvent thermal reaction is preferably carried out in a hydrothermal reactor; in the present invention, the temperature of the solvent thermal reaction is preferably 140-160°C, more preferably 150°C; the time is preferably 12-20h, more preferably 15-18h.

[0039] After the solvothermal reaction, the present invention preferably performs post-treatment on the obtained solvothermal reaction product, and the post-treatment preferably comprises the following steps:

[0040] The solvent thermal reaction product is sequentially cooled and solid-liquid separated, and the obtained solid is washed and dried.

[0041] In the present invention, the cooling is preferably natural cooling to room temperature. In the present invention, the solid-liquid separation is preferably centrifugation, the centrifugal speed is preferably 10000-11000 rpm, the centrifugal time is preferably 5-10 min, more preferably 6-8 min. In the present invention, the washing includes water washing and alcohol washing performed sequentially.

[0042] In the present invention, the drying is preferably carried out in a vacuum drying oven, the drying temperature is preferably 40 to 60° C., more preferably 50° C., the drying time is preferably 15 to 24 hours, more preferably 18 to 20 hours.

[0043] The invention provides a black phosphorus / red phosphorus-cadmium sulfide heterojunction photocatalyst prepared by the preparation method, comprising cadmium sulfide nanorods and red phosphorus nanoparticles and black phosphorus nanoparticles distributed on the surfaces of the cadmium sulfide nanorods.

[0044] In the present invention, the length of the cadmium sulfide nanorods is preferably 100-300 nm, more preferably 150-200 nm; the diameter is preferably 20-50 nm, more preferably 30-40 nm; in the present invention, the particle size of the red phosphorus nanoparticles and black phosphorus nanoparticles is independently preferably 5-10 nm.

[0045] The present invention provides the use of the black phosphorus / red phosphorus-cadmium sulfide heterojunction photocatalyst in photocatalytic water decomposition to produce hydrogen.

[0046] The black phosphorus / red phosphorus-cadmium sulfide heterojunction photocatalyst provided by the present invention and its preparation method and application are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0047] Example 1

[0048] The preparation method of black phosphorus / red phosphorus-cadmium sulfide heterojunction photocatalyst is as follows:

[0049] Step 1, 3 g of commercially available red phosphorus with a purity of 99.999% and 60 mL of deionized water are placed in a 100 mL stainless steel reactor lined with polytetrafluoroethylene, placed in an oven and hydroheated at 200° C. for 12 hours, cooled to room temperature, centrifuged at 10,000 rpm for 5 minutes to separate the red phosphorus solid, placed in a 60° C. vacuum drying oven and dried for 20 hours to obtain red phosphorus powder.

[0050] Step 2, 0.060g of the above red phosphorus powder and 3.49g of cadmium chloride hemipentahydrate are placed in a stainless steel reactor with a volume of 100mL and lined with polytetrafluoroethylene, 60mL of diethylenetriamine is added and stirred for 30min, then 3.66g of thiourea is added and stirred for 30min, the reactor is placed in a blast drying oven and heated at 160°C for 12h, the reaction is cooled to room temperature after the reaction is completed, and the solid is collected by centrifugation. The solid is washed with deionized water and anhydrous ethanol three times each, 10000 rpm, centrifuged for 5min, and finally vacuum dried at 60°C for 20h to obtain a black phosphorus / red phosphorus-cadmium sulfide heterojunction photocatalyst BP / RP-CdS.

[0051] Example 2

[0052] The preparation method of black phosphorus / red phosphorus-cadmium sulfide heterojunction photocatalyst is as follows:

[0053] Step 1, placing 3.3 g of commercially available red phosphorus with a purity of 99.999% and 66 mL of deionized water in a 100 mL stainless steel reactor lined with polytetrafluoroethylene, placing it in an oven and hydroheating it at 200° C. for 12 hours, cooling it to room temperature, centrifuging it at 11,000 rpm for 8 minutes to separate the red phosphorus solid, and placing it in a vacuum drying oven at 40° C. and drying it for 24 hours to obtain red phosphorus powder.

[0054] Step 2, 0.035g of the above red phosphorus powder and 3.49g of cadmium chloride hemipentahydrate are placed in a stainless steel reactor with a volume of 100mL and lined with polytetrafluoroethylene, 60mL of ethylenediamine is added and stirred for 30min, then 3.61g of thioacetamide is added, and stirring is continued for 30min, the reactor is placed in a blast drying oven and heated at 140°C for reaction for 20h, and the reaction is cooled to room temperature after the reaction is completed. The solid is collected by centrifugation, and the solid is washed with deionized water and anhydrous ethanol three times each, 11000 rpm, centrifuged for 8min, and finally vacuum dried at 60°C for 20h to obtain a black phosphorus / red phosphorus-cadmium sulfide heterojunction photocatalyst BP / RP-CdS.

[0055] The transmission electron microscopy image of the obtained black phosphorus / red phosphorus-cadmium sulfide heterojunction photocatalyst is shown in Figure 1 As shown, the energy spectrum analysis shows that Cd, S, and P elements are evenly distributed.

[0056] Example 3

[0057] The preparation method of black phosphorus / red phosphorus-cadmium sulfide heterojunction photocatalyst is as follows:

[0058] Step 1, 3 g of commercially available red phosphorus with a purity of 99.999% and 60 mL of deionized water are placed in a 100 mL stainless steel reactor lined with polytetrafluoroethylene, placed in an oven and hydroheated at 210° C. for 11 hours, cooled to room temperature, centrifuged at 11,000 rpm for 5 minutes to separate the red phosphorus solid, placed in a 50° C. vacuum drying oven and dried for 20 hours to obtain red phosphorus powder.

[0059] Step 2, 0.175g of the above-mentioned red phosphorus powder and 3.49g of cadmium chloride hemipentahydrate are placed in a stainless steel reactor with a volume of 100mL and lined with polytetrafluoroethylene, 60mL of ethylenediamine is added and stirred for 30min, then 15g of glutathione is added, and stirring is continued for 30min, and the reactor is placed in a blast drying oven and heated at 150°C for 16h. After the reaction is completed, it is cooled to room temperature and the solid is collected by centrifugation. The solid is washed with deionized water and anhydrous ethanol three times each by centrifugation, 11000 rpm, centrifuged for 5min, and finally vacuum dried at 60°C for 20h to obtain a black phosphorus / red phosphorus-cadmium sulfide heterojunction photocatalyst BP / RP-CdS.

[0060] Comparative Example 1

[0061] 3.49 g of cadmium chloride hemipentahydrate was placed in a 100 mL stainless steel reactor lined with polytetrafluoroethylene, 60 mL of diethylenetriamine was added and stirred for 30 min, then 3.66 g of thiourea was added and stirred for 30 min, the reactor was placed in a forced air drying oven and heated at 160 °C for 12 h. After the reaction was completed, it was cooled to room temperature and the solid was collected by centrifugation. The solid was washed with deionized water and anhydrous ethanol for 3 times each, and finally dried in vacuum at 60 °C for 20 h to obtain a cadmium sulfide photocatalyst CdS.

[0062] Performance Testing

[0063] The catalysts obtained in Examples 1 to 3 and Comparative Examples were used to produce hydrogen by photolysis of water, and the specific method was as follows:

[0064] Take 10 mg of the catalyst into a reaction glass container, add 45 mL of ultrapure water and 5 mL of lactic acid, connect to the reaction gas line, evacuate the system, and carry out the hydrogen evolution experiment under magnetic stirring conditions. The light source used is a 350 W xenon lamp (model: MC-PF300B). The amount of hydrogen produced is analyzed by gas chromatograph GC9790II (MC-01) (Zhejiang Fuli).

[0065] After testing, the hydrogen production of the black phosphorus / red phosphorus-cadmium sulfide heterojunction photocatalyst obtained in Example 1 was 6.8 mmol·g -1 ·h -1 .

[0066] The hydrogen production of the black phosphorus / red phosphorus-cadmium sulfide heterojunction photocatalyst obtained in Example 1 was 9.7 mmol·g -1 ·h -1 .

[0067] The results of hydrogen production using the black phosphorus / red phosphorus-cadmium sulfide heterojunction photocatalyst obtained in Example 3 and cadmium sulfide as a catalyst under the same conditions are as follows Figure 2 As shown by Figure 2 It can be seen that the hydrogen production of black phosphorus / red phosphorus-cadmium sulfide heterojunction photocatalyst reaches 10.3mmol·g -1 ·h -1 , compared with cadmium sulfide, the hydrogen production is greatly improved.

[0068] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a black phosphorus / red phosphorus-cadmium sulfide heterojunction photocatalyst, The following steps are involved: Mixing red phosphorus with water, performing a hydrothermal reaction, and obtaining purified red phosphorus after solid-liquid separation; The purified red phosphorus is mixed with a soluble cadmium source, a soluble sulfur source, and a primary diamine solvent, and subjected to a solvothermal reaction to obtain a black phosphorus / red phosphorus-cadmium sulfide heterojunction photocatalyst; The mass of the purified red phosphorus is 1-5% of the mass of the soluble cadmium source; The molar ratio of the soluble cadmium source to the soluble sulfur source is 1:2-4; The temperature of the solvent thermal reaction is 140-160° C. and the time is 12-20 hours.

2. The preparation method according to claim 1, It is characterized in that The temperature of the hydrothermal reaction is 190-210° C., and the time is 11-13 hours.

3. The preparation method according to claim 1, It is characterized in that The soluble cadmium source is cadmium chloride, and the soluble sulfur source is one or more of thioacetamide, thiourea and glutathione.

4. The preparation method according to claim 1 or 3, It is characterized in that The primary diamine solvent is ethylenediamine and / or diethylenetriamine.

5. The black phosphorus / red phosphorus-cadmium sulfide heterojunction photocatalyst prepared by the preparation method according to any one of claims 1 to 4, comprising cadmium sulfide nanorods and red phosphorus nanoparticles and black phosphorus nanoparticles distributed on the surface of the cadmium sulfide nanorods.

6. The black phosphorus / red phosphorus-cadmium sulfide heterojunction photocatalyst according to claim 5, It is characterized in that The cadmium sulfide nanorods have a length of 100 to 300 nm and a diameter of 20 to 50 nm; The particle sizes of the red phosphorus nanoparticles and the black phosphorus nanoparticles are independently 5 to 10 nm.

7. Use of the black phosphorus / red phosphorus-cadmium sulfide heterojunction photocatalyst according to claim 5 or 6 in photocatalytic water decomposition to produce hydrogen.