Silicon-based negative electrode sheet and preparation method and application thereof

By coating the surface of nano-silicon particles with a lithium aluminate layer, a core-shell structured silicon-based anode material is constructed, solving the problems of low silicon content and poor cycle stability in sulfide all-solid-state batteries. This enables the efficient preparation and application of high energy density and stability in all-solid-state batteries.

CN116417573BActive Publication Date: 2026-11-20SHENZHEN JIECHUANG NEW ENERGY CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310241985.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-06
Publication Date
2026-11-20
Estimated Expiration
2043-03-06

AI Technical Summary

Technical Problem

In existing sulfide all-solid-state batteries, silicon-based anode plates have low silicon content and poor cycle stability. The reaction between sulfide electrolyte and polar solvent is difficult to avoid during the preparation process, which makes it difficult for silicon-based anode materials to be used on a large scale.

Method used

A core-shell silicon-based anode material is constructed by coating the surface of nano-silicon particles with a lithium aluminate layer. A silicon-based anode sheet with high silicon content is prepared by wet coating to avoid direct contact with the sulfide solid electrolyte. The lithium-ion conductivity and mechanical strength of the lithium aluminate layer are used to suppress volume expansion.

Benefits of technology

A silicon-based anode sheet with high silicon content has been achieved, which improves cycle stability and battery energy density, avoids the reaction of sulfides with polar solvents, and is suitable for large-scale preparation and application in all-solid-state batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116417573B_ABST
    Figure CN116417573B_ABST
Patent Text Reader

Abstract

The application relates to the technical field of batteries, in particular to a silicon-based negative electrode sheet and a preparation method and application thereof. The silicon-based negative electrode sheet comprises a negative electrode current collector and a negative electrode material layer loaded on the negative electrode current collector, and the negative electrode material layer comprises a silicon-based negative electrode material, a conductive agent and a binder. The silicon-based negative electrode material comprises nanosilicon and a lithium meta-aluminate layer coated on the surface of the nanosilicon. The silicon-based negative electrode sheet is prepared by coating a lithium meta-aluminate layer on the surface of nanosilicon particles without adding sulfide solid-state electrolyte, so that the problem of reaction between sulfide and polar solvent is avoided, and the expansion of silicon in the cycle process is inhibited. The silicon-based negative electrode sheet has a high silicon content, is beneficial to exerting the advantages of high capacity of silicon, improving the energy density of a battery system, and improving the cycle stability and rate performance of the silicon negative electrode.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of battery technology, specifically to a silicon-based negative electrode sheet, its preparation method, and its application. Background Technology

[0002] In recent years, with the depletion of fossil fuels and the serious environmental pollution they cause, the demand for developing clean new energy sources has been growing. Lithium-ion batteries, as an important energy storage method for achieving clean energy storage and use, are crucial for promoting the development of new energy sources. They possess characteristics such as long cycle life, high energy density, and environmental friendliness, and are widely used in portable electronic devices, electric vehicles, and grid energy storage. However, currently commercially available lithium-ion batteries use liquid electrolytes and graphite anode materials, which are gradually failing to meet the demands of development in terms of energy density and safety. Therefore, developing high-safety, high-energy-density lithium-ion batteries is imperative. All-solid-state batteries use non-flammable solid electrolytes, greatly improving battery safety during use and are considered the next-generation direction for lithium-ion battery development. Among various solid electrolytes, sulfide solid electrolytes have the highest room-temperature ionic conductivity (10⁻⁶). -3 -10 -2 With its good processability and S / cm ratio, it is considered one of the most promising solid electrolytes.

[0003] Silicon-based anode materials have attracted widespread attention from researchers and industry due to their ultra-high theoretical specific capacity. At room temperature, their theoretical specific capacity reaches 3579 mAh / g, close to that of lithium metal, and about 10 times that of commercial graphite materials (372 mAh / g). Their operating potential is 0.3V vs. Li / Li + Around, compared to graphite's 0.1V vs. Li / Li + Compared to other materials, silicon can effectively prevent lithium metal deposition and reduce short circuits. Furthermore, silicon is the second most abundant element on Earth and has a relatively low cost. However, silicon-based anode materials have encountered many difficulties in commercialization. Firstly, silicon in its lithium-intercalated state will alloy to form Li. 15Si4 expands by up to 280% in volume. Such massive expansion generates enormous stress, causing silicon particles to crack, leading to silicon pulverization and detachment from the current collector. Ultimately, the active material loses electrical contact, resulting in rapid capacity decay. Although nano-sizing silicon to a diameter of less than 150 nm can effectively prevent particle cracking, the problem of volume expansion still exists. Repeated volume expansion also causes the solid electrolyte interphase (SEI) film formed on the surface of silicon particles to rupture. When the exposed new surface comes into contact with the electrolyte, SEI is re-formed, causing irreversible lithium loss. This repeated formation of SEI leads to low coulombic efficiency and capacity decay in the full cell, resulting in generally poor cycle life of silicon-based anode materials. Silicon is also a semiconductor material with poor conductivity, lower than that of graphite anode materials.

[0004] Combining silicon-based anode materials with sulfide solid electrolytes enables the achievement of high energy density and safety. Firstly, the moderate Young's modulus of sulfides effectively mitigates the volume expansion of silicon. Secondly, in solid-state battery systems, the contact between the silicon-based anode material and the sulfide electrolyte primarily occurs at the interface, resulting in less SEI formation during charge and discharge compared to liquid batteries. Furthermore, although silicon-based anode materials expand continuously during cycling, leading to SEI rupture, the newly exposed silicon in a solid-state system does not continue to contact the sulfide solid electrolyte, thus preventing repeated SEI formation. Therefore, higher coulombic efficiency can be achieved compared to liquid batteries.

[0005] To realize the application of silicon-based anode materials in sulfide-based all-solid-state battery systems, large-scale fabrication of electrodes with high silicon content is crucial. Currently, research on silicon-based anode materials in solid-state batteries, both domestically and internationally, is still in its initial stages. Effective methods for improving silicon are limited, and the cycle life is generally poor. Furthermore, most reports involve combining silicon, sulfide electrolytes, and conductive carbon black to prepare composite anodes. However, due to the severe reactions between sulfide electrolytes and polar solvents, and the fact that most binders used in silicon-based anode materials contain strongly polar groups and are insoluble in non-polar solvents, electrode fabrication is extremely difficult. Therefore, most reports use silicon-based anode materials in powder form, which is detrimental to large-scale fabrication. In addition, the mass percentage of silicon in composite silicon-based anode materials is generally low, between 5% and 60%, failing to fully utilize the high specific capacity advantage of silicon-based anode materials.

[0006] Masanari Takahashi et al. from the Materials Science Research Institute of the Nara Institute of Science and Technology in Japan prepared a composite silicon-based anode sheet using PPC as a binder and anisole as a solvent via a wet coating method. They further removed the PPC binder by heat treatment at 225°C, reducing the battery's internal resistance. In an all-solid-state half-cell, this composite silicon-based anode sheet exhibited excellent cycle stability. However, the silicon-based anode material prepared by this method only contains 53% silicon as the active material, failing to fully utilize the high specific capacity advantage of silicon.

[0007] Yoon Seok Jung et al. from the Department of Energy Engineering at Hanyang University in South Korea first prepared silicon-based anode sheets by uniformly mixing silicon, conductive agents, and binders (PVDF or CMC) in a solvent (water or NMP) and then preparing them using a conventional wet coating method. They then obtained composite silicon-based anode sheets by immersing the silicon-based anode sheets in a sulfide solid electrolyte-ethanol solution and subjecting them to further heat treatment. The composite silicon-based anode material prepared by this method exhibits a higher specific capacity than powdered composite silicon-based anode materials prepared by direct ball milling. However, the silicon content of this anode is still relatively low, and some aqueous binders may decompose during the heat treatment process.

[0008] Recently, Yong Min Lee and colleagues at the Department of Energy Science and Engineering, Daegu Gyeongbuk Institute of Science and Technology (DGIST) in South Korea, prepared Si / C anode sheets by combining graphite and silicon using a conventional wet coating process. Because graphite possesses excellent lithium-ion diffusion and electronic conductivity, there is no need to add electrolytes and conductive agents to the anode, avoiding the problems associated with the reaction between sulfide solid electrolytes and polar solvents. However, the anode prepared by this method exhibits rapid capacity decay when the silicon content is high (mass fraction > 10%).

[0009] Therefore, existing technologies still need to be improved and developed. Summary of the Invention

[0010] In view of the shortcomings of the prior art, the present invention provides a silicon-based anode sheet, its preparation method and application, aiming to solve the problems of low silicon content and poor cycle stability of silicon-based anode sheets in existing sulfide all-solid-state batteries.

[0011] To address the technical problems of existing silicon-based anodes in lithium-ion batteries, the inventors devised a method of coating the surface of silicon-based anode materials with an inorganic solid electrolyte layer possessing lithium-ion conductivity and high mechanical strength. This was combined with a wet coating method to prepare silicon-based anode sheets with high silicon content. This invention uses lithium aluminate as the inorganic solid electrolyte layer, constructing an ion-conducting network within the electrode. By constructing such a coating layer, a very high silicon content (90%) is achieved in the silicon-based anode material. Furthermore, the hardness of the coating layer effectively suppresses the expansion of the silicon core, significantly improving the cycle stability of the silicon-based anode.

[0012] Meanwhile, the silicon-based negative electrode sheet provided by this invention can be applied to all-solid-state batteries with sulfide solid electrolytes, eliminating the need to add sulfide electrolytes to the silicon-based negative electrode, thus avoiding the problem of sulfide electrolytes reacting with polar solvents. It also provides a new approach to the preparation of silicon-based negative electrode sheets, and its preparation method is compatible with the existing preparation process of all-solid-state lithium-ion battery electrode sheets, making it suitable for mass production.

[0013] Specifically, the technical solution of the present invention is as follows:

[0014] The present invention provides a silicon-based negative electrode sheet, the silicon-based negative electrode sheet comprising a negative electrode current collector and a negative electrode material layer loaded on the negative electrode current collector, the negative electrode material layer comprising a silicon-based negative electrode material, a conductive agent and a binder.

[0015] The silicon-based anode material includes nano-silicon and a lithium aluminate layer coating the surface of the nano-silicon core.

[0016] Preferably, the lithium aluminate layer of the silicon-based anode material is amorphous, and the thickness of the lithium aluminate layer is 1-5 nm.

[0017] Preferably, the nano-silicon is spherical in shape and has a particle size of 50-150 nm.

[0018] Preferably, the conductive agent is one of acetylene black, vapor-grown carbon fiber, carbon nanotubes, and Super P.

[0019] Preferably, the adhesive is one of polyvinylidene fluoride, carboxymethyl cellulose, and polyacrylic acid.

[0020] This invention also provides a method for preparing a silicon-based negative electrode sheet, comprising the following steps:

[0021] Preparation of alumina-coated silicon nanoparticles;

[0022] The alumina is converted into lithium aluminate to obtain a silicon-based anode material;

[0023] The silicon-based anode material is wet-coated to obtain the silicon-based anode sheet.

[0024] The method for preparing alumina-coated nano-silicon includes the following steps:

[0025] Prepare buffer solutions;

[0026] An ethanol solution of nano-silicon was mixed with the buffer solution, and aluminum salt was added to react, resulting in alumina-coated nano-silicon.

[0027] Optionally, the aluminum salt is one of aluminum nitrate, aluminum sulfate, and aluminum chloride.

[0028] The method for converting alumina into lithium aluminate to obtain the silicon-based anode material includes the following steps:

[0029] The alumina-coated nano-silicon was ground and mixed with lithium salt, and then heat-treated under an inert atmosphere to obtain the silicon-based anode material.

[0030] Optionally, the lithium salt is one of lithium hydroxide, lithium hydroxide monohydrate, and lithium carbonate.

[0031] Optionally, the heat treatment temperature is 550-750℃, and the heat treatment time is 1-5h.

[0032] The method for obtaining the silicon-based anode sheet by wet coating of the silicon-based anode material includes the following steps:

[0033] The silicon-based anode material, conductive agent, and binder are mixed and wet-coated onto the anode current collector. After drying, the silicon-based anode sheet is obtained.

[0034] Optionally, the mass ratio of the silicon-based anode material, conductive agent, and binder is (80-90):(5-10):(5-10).

[0035] The present invention also provides an application of a silicon-based negative electrode sheet in a sulfide all-solid-state lithium battery or a halide all-solid-state lithium battery.

[0036] The present invention also provides a sulfide all-solid-state lithium battery, including the aforementioned silicon-based negative electrode sheet.

[0037] Compared with the prior art, the present invention has the following beneficial effects:

[0038] (1) The present invention prepares silicon-based negative electrode sheets by coating the surface of nano-silicon particles with lithium aluminate layer without adding sulfide solid electrolyte, thus avoiding the problem of sulfide reacting with polar solvent.

[0039] (2) In the silicon-based anode electrode prepared by the present invention, the lithium aluminate layer coated on the surface of the nano-silicon particles has lithium-ion conductivity and high mechanical strength, which suppresses the volume expansion of silicon during cycling and improves the cycling stability of the silicon anode.

[0040] (3) The silicon-based negative electrode of the present invention has a high silicon content (mass fraction reaches 90%), which is conducive to giving full play to the high specific capacity of silicon and improving the energy density and rate performance of sulfide all-solid-state batteries. Attached Figure Description

[0041] Figure 1 A schematic diagram of the structure of the silicon-based negative electrode sheet provided by the present invention;

[0042] Figure 2 The image shows a scanning electron microscope (SEM) image of the silicon-based anode material prepared in Example 1 of this invention.

[0043] Figure 3 This is a scanning electron microscope image of the surface of the silicon-based negative electrode sheet prepared in Example 1 of the present invention;

[0044] Figure 4 The results of cycle performance tests of sulfide all-solid-state half-cells prepared from silicon-based anode material sheets in Examples 1 and 3 of this invention;

[0045] Figure 5 The results show the cycle performance of the sulfide all-solid-state full cell prepared from the silicon-based anode material in Example 1 of this invention. Detailed Implementation

[0046] This invention provides a silicon-based negative electrode sheet, its preparation method, and its application. To make the objectives, technical solutions, and effects of this invention clearer and more explicit, the invention is further described in detail below. It should be understood that the specific embodiments described herein are merely illustrative of the invention and are not intended to limit the scope of protection of the invention.

[0047] This invention provides a silicon-based negative electrode sheet, the schematic diagram of which is shown below. Figure 1 As shown. The silicon-based negative electrode includes a negative current collector and a negative electrode material layer loaded on the negative current collector, wherein the negative electrode material layer includes a silicon-based negative electrode material, a conductive agent, and a binder.

[0048] The silicon-based anode material comprises nano-silicon and a lithium aluminate layer coating the surface of the nano-silicon. The silicon-based anode material has a core-shell structure, with nano-silicon as the core and the lithium aluminate layer as the outer shell.

[0049] In some embodiments, the nano-silicon is spherical in shape and has a particle size of 50-150 nm.

[0050] In some embodiments, the lithium aluminate layer of the silicon-based anode material is amorphous. Compared with the pure crystalline phase, the amorphous lithium aluminate layer is more conducive to ion conduction.

[0051] In some implementations, the thickness of the lithium aluminate layer is 1-5 nm. As the thickness of the lithium aluminate layer increases, the battery capacity decreases, but its cycle stability improves.

[0052] The lithium aluminate layer coated on the surface of nano-silicon is mainly used to replace the sulfide solid electrolyte in the composite silicon anode. It also helps to alleviate volume expansion. In this way, silicon-based anode sheets can be prepared and used in sulfide-based all-solid-state batteries.

[0053] In some embodiments, the conductive agent is one of acetylene black, vapor-grown carbon fiber (VGCF), carbon nanotubes (CNTs), and Super P. When carbon materials come into contact with sulfide electrolytes, they induce the decomposition of the sulfide electrolyte, leading to a decrease in battery efficiency. In this embodiment of the invention, the conductive agent is mixed with silicon anode material to form a silicon anode sheet, avoiding large-area contact caused by powdery mixing with sulfide solid electrolytes, thereby further improving battery efficiency.

[0054] In some embodiments, the adhesive is one of polyvinylidene fluoride (PVDF), carboxymethyl cellulose (CMC), and polyacrylic acid (PAA).

[0055] This invention also provides a method for preparing a silicon-based negative electrode sheet, comprising the following steps:

[0056] Preparation of alumina-coated silicon nanoparticles;

[0057] The alumina is converted into lithium aluminate to obtain a silicon-based anode material;

[0058] The silicon-based anode material is wet-coated to obtain the silicon-based anode sheet.

[0059] The method for preparing alumina-coated silicon nanoparticles in this embodiment of the invention includes the following steps:

[0060] Prepare buffer solutions;

[0061] An ethanol solution of nano-silicon was mixed with the buffer solution, and aluminum salt was added to react, resulting in alumina-coated nano-silicon.

[0062] Specifically, in this embodiment of the invention, an ammonium formate-formic acid buffer solution is prepared and the pH value is adjusted. Nano-silicon particles are dispersed in anhydrous ethanol, and the dispersed nano-silicon ethanol suspension is poured into the ammonium formate-formic acid buffer solution. Aluminum salt is then added to the mixture and reacted for a period of time. Finally, alumina-coated nano-silicon is obtained by centrifugation and drying.

[0063] In some embodiments, the aluminum salt is one of aluminum nitrate, aluminum sulfate, and aluminum chloride, but is not limited thereto.

[0064] The method for converting alumina into lithium aluminate to obtain the silicon-based anode material includes the following steps:

[0065] The alumina-coated nano-silicon was ground and mixed with lithium salt, and then heat-treated under an inert atmosphere to obtain the silicon-based anode material.

[0066] Specifically, the process of transforming the surface-coated alumina layer into the inorganic solid electrolyte lithium aluminate involves grinding and mixing alumina-coated nano-silicon particles and lithium salt, transferring the mixture into a crucible, placing the crucible into a tube furnace, and heat-treating it for a period of time in an inert gas atmosphere and at a certain temperature to obtain lithium aluminate-coated nano-silicon particles, i.e., silicon-based anode material.

[0067] In some embodiments, the lithium salt is one of lithium hydroxide, lithium hydroxide monohydrate, and lithium carbonate, but is not limited thereto.

[0068] In some embodiments, the heat treatment temperature is 550-750°C and the heat treatment time is 1-5 hours.

[0069] In some implementations, nitrogen or argon is selected as the inert gas, but it is not limited to these.

[0070] The method for obtaining the silicon-based anode sheet by wet coating of the silicon-based anode material includes the following steps:

[0071] The silicon-based anode material, conductive agent, and binder are mixed and wet-coated onto the anode current collector. After drying, the silicon-based anode sheet is obtained.

[0072] In this embodiment of the invention, a solvent is added to the mixture of silicon-based anode material, conductive agent, and binder before wet coating. In some embodiments, NMP or water is used as the solvent, but it is not limited thereto.

[0073] In some embodiments, the mass ratio of the silicon-based anode material, conductive agent, and binder is (80-90):(5-10):(5-10). More preferably, the mass ratio of the silicon-based anode material, conductive agent, and binder is 90:5:5.

[0074] After wet coating onto the negative electrode current collector, the drying temperature can be selected as 80-110℃.

[0075] The silicon-based negative electrode sheet prepared in the embodiments of the present invention can be used in sulfide all-solid-state lithium batteries or halide all-solid-state lithium batteries.

[0076] The embodiments of the present invention have prepared silicon-based negative electrode sheets without the need to add sulfide solid electrolytes, thus avoiding the problem of sulfide reacting with polar solvents. Moreover, the silicon-based negative electrode sheets of the embodiments of the present invention have a high silicon content (mass fraction reaches 90%), giving full play to the advantages of silicon's high specific capacity, which helps to improve the energy density and rate performance of sulfide all-solid-state batteries.

[0077] The sulfide-based all-solid-state lithium battery of this invention includes the silicon-based negative electrode sheet.

[0078] In the embodiments, the specific process for preparing a sulfide-based all-solid-state lithium battery includes: first, pouring a certain amount of sulfide solid electrolyte into a polyether ether ketone (PEEK) mold, cold-pressing it into a sheet under a certain pressure, then attaching the silicon anode sheet and the high-nickel ternary single-crystal composite cathode NCM83 sheet to both sides, and cold-pressing again under a certain pressure to make the positive and negative electrodes and the solid electrolyte in close contact, thereby preparing a sulfide-based all-solid-state lithium battery containing a silicon-based anode sheet.

[0079] In some embodiments, the sulfide solid electrolyte is Li3PS4 or Li7PS4. 11 It is one of Li6PSCl5, but not limited to it.

[0080] The present invention will be further described below with reference to specific embodiments.

[0081] Example 1

[0082] (1) Preparation of silicon-based anode materials

[0083] First, prepare an ammonium formate-formic acid buffer solution with a pH of 4.4: Dissolve 7.56g of ammonium formate in 400mL of deionized water, and then add formic acid dropwise until the pH reaches 4.4.

[0084] 1.6 g of silicon nanoparticles (average diameter 100 nm) were added to 100 mL of ethanol and sonicated for 30 minutes. The ethanol solution of silicon nanoparticles was then added to ammonium formate-formate buffer to obtain a mixed solution. 1.6 g of aluminum sulfate hexadecahydrate was added to the mixed solution, and the mixture was reacted at 70 °C for 30 minutes. After centrifugation, washing with water and ethanol, alumina-coated silicon nanoparticles were obtained.

[0085] The alumina-coated silicon nanoparticles were mixed with lithium hydroxide monohydrate (mass ratio 30:1) and ground for 10 minutes. The mixture was then heat-treated at 650°C for 3 hours under an argon atmosphere to obtain lithium aluminate-coated silicon nanoparticles, i.e., silicon-based anode material.

[0086] Scanning electron microscope images of the obtained silicon-based anode material are as follows: Figure 2As shown, the silicon-based anode material consists of uniformly sized nanoparticles with an average particle size of around 100 nm.

[0087] (2) Preparation of silicon-based negative electrode sheet

[0088] Silicon-based anode material, conductive carbon black Super P, and binder PVDF are mixed in a mass ratio of 90:5:5, then added to NMP solvent with a solid content of 20wt%. After stirring on a magnetic stirrer for 12 hours, the mixture is coated onto copper foil, dried at 80°C in air for 4 hours, and then dried at 80°C in vacuum for more than 12 hours to obtain a silicon-based anode sheet.

[0089] Scanning electron microscope images of the surface of a silicon-based negative electrode sheet, as shown below Figure 3 As shown,

[0090] (3) Preparation of sulfide all-solid-state half-cells

[0091] 150 mg of sulfide solid electrolyte Li6PS5Cl was poured into a PEEK mold and cold-pressed at 300 MPa.

[0092] The silicon-based negative electrode sheet prepared in step (2) is attached to one side of the sulfide solid electrolyte and cold-pressed at 370 MPa to make the silicon-based negative electrode sheet and the sulfide solid electrolyte in close contact. A lithium indium alloy is attached to the other side of the sulfide solid electrolyte and cold-pressed at 120 MPa to obtain a sulfide all-solid-state half cell containing a silicon-based negative electrode sheet.

[0093] Example 2

[0094] The difference between this embodiment and embodiment 1 is that in step (1) of the preparation of silicon-based anode material in this embodiment, the amount of aluminum sulfate hexadecahydrate added is 1.2g.

[0095] The remaining preparation process is the same as in Example 1.

[0096] Example 3

[0097] The difference between Example 3 and Example 1 is that this example does not involve the preparation of lithium aluminate-coated silicon nanoparticles in step (1) of Example 1. Instead, pure silicon nanoparticles are directly used as the silicon-based anode material in step (2) to prepare the silicon-based anode sheet. The rest of the preparation process is the same as in Example 1.

[0098] Next, the electrochemical performance of the sulfide all-solid-state half-cells prepared in steps 1-3 was tested.

[0099] Test conditions: Test voltage 0.025-1.5V vs Li + / Li was activated once at a rate of 0.1C, and then cycled at a rate of 0.33C, where 1C equals 3500 mAh / g, and the test temperature was room temperature. The test results of the cycling performance are shown in Table 1.

[0100] Table 1

[0101]

[0102] First, comparing the test results of Examples 1 and 2 in Table 1, it can be seen that the capacity of the sulfide all-solid-state half-cell in Example 1 is lower than that in Example 2, but it has better cycle stability. The difference lies in the thickness of the coating layer of the silicon-based anode material core-shell structure. In Example 1, the thickness of the lithium aluminate layer is within 2-3 nm, while in Example 2, the thickness of the lithium aluminate layer is within 1-2 nm. Combined with the electrochemical test results of the sulfide all-solid-state half-cell, it can be seen that as the thickness of the lithium aluminate layer of the silicon-based anode material increases, the capacity of the sulfide all-solid-state half-cell decreases, but the cycle stability significantly improves.

[0103] Analysis of the test results shows that, on the one hand, the lithium aluminate coating of silicon-based anode materials inhibits the volume expansion of the core silicon; on the other hand, increasing the thickness of the lithium aluminate coating leads to lower capacity and may even hinder ion conduction. Therefore, when preparing silicon-based anode materials, the core-shell structure of the lithium aluminate coating needs to be controlled within a suitable thickness range to obtain optimal electrochemical performance.

[0104] Meanwhile, comparing the test results of Examples 1-2 and Example 3 in Table 1, it can be seen that the initial discharge capacity of the silicon-based anode material with a lithium aluminate coating is reduced compared to pure nano-silicon anode material. This is because the coating can suppress the volume expansion of silicon, reduce lithium intercalation, and the coating, being an inactive material, occupies a certain mass. However, in terms of cycle stability, the silicon-based anode material with a lithium aluminate coating shows a significant improvement compared to pure nano-silicon. Figure 4 As shown, the good lithium-ion conductivity and high mechanical strength of the lithium aluminate coating are beneficial to improving the cycle stability of the battery.

[0105] The silicon-based negative electrode sheet prepared in Example 1 was used to prepare a sulfide all-solid-state full cell. The specific process is as follows:

[0106] 100 mg of sulfide solid electrolyte Li6PS5Cl was poured into a PEEK mold and cold-pressed at 300 MPa.

[0107] The silicon-based negative electrode sheet and the dry-processed ternary NCM83 composite positive electrode prepared in Example 1 were respectively attached to both sides of the sulfide solid electrolyte and cold-pressed at 300 MPa to make them in close contact, thus obtaining a sulfide all-solid-state full cell containing a silicon-based negative electrode sheet.

[0108] Electrochemical testing conditions: test voltage 2.4-4.2V vs Li + / Li, first lap at 0.28mA / cm 2 At a current density of 0.14 mA / cm², it was charged with a constant current to 4.2 V and then charged with a constant voltage to a current density of 0.14 mA / cm². 2 Then at 0.28 mA / cm 2 Discharged to 4.2V, then maintained at 0.92mA / cm. 2 Cyclic testing was conducted. During charging, constant current charging was first applied to 4.2V, followed by constant voltage charging to a current density of 0.14mA / cm². 2 The test temperature was room temperature, and the test results of its cycling performance are as follows: Figure 5 As shown, the sulfide all-solid-state full cell prepared from the silicon-based negative electrode sheet provided in Example 1 exhibits good cycle stability.

[0109] In summary, this invention provides a silicon-based anode sheet, its preparation method, and its application. This invention prepares a silicon-based anode material by coating a lithium aluminate layer onto the surface of nano-silicon particles, and prepares a silicon-based anode sheet without the need for a sulfide solid electrolyte, which can then be applied in a sulfide all-solid-state battery system. The core-shell structure of the silicon-based anode material allows for the construction of an ion-conducting network within the electrode, thus avoiding the problem of sulfides reacting with polar solvents. Simultaneously, the lithium aluminate layer not only possesses excellent lithium-ion conductivity, but its high mechanical strength also suppresses the volume expansion of silicon during cycling, thereby improving the cycle stability of the silicon anode. Furthermore, the silicon-based anode sheet of this invention has a high silicon content (reaching 90% by mass), which is beneficial for leveraging the high capacity of silicon and improving the energy density and rate performance of the battery system.

[0110] It should be understood that the application of the present invention is not limited to the examples above. Those skilled in the art can make improvements or modifications based on the above description, and all such improvements and modifications should fall within the protection scope of the appended claims.

Claims

1. A method for preparing a silicon-based negative electrode sheet, characterized in that, Including the following steps: Preparation of alumina-coated silicon nanoparticles; The alumina-coated silicon nanoparticles are mixed with lithium salt and heat-treated at 550-750℃ for 1-5 hours under an inert atmosphere to convert the alumina into lithium aluminate, thereby obtaining a silicon-based anode material; wherein the lithium salt is one of lithium hydroxide, lithium hydroxide monohydrate, and lithium carbonate. The silicon-based anode material, conductive agent, and binder are mixed in a polar solvent to form a slurry, wherein no electrolyte is added during the mixing step. The slurry is wet-coated onto the anode current collector and dried to obtain the silicon-based anode sheet. The mass ratio of the silicon-based anode material, conductive agent, and binder is (80~90):(5~10):(5~10). In the silicon-based negative electrode sheet prepared by the method, the lithium aluminate layer is amorphous and the thickness of the lithium aluminate layer is 1-5 nm; the nano-silicon is spherical and the particle size of the nano-silicon is 50-150 nm; the silicon-based negative electrode sheet is used in sulfide all-solid-state lithium batteries. The method for preparing alumina-coated nano-silicon includes the following steps: Prepare an ammonium formate-formic acid buffer solution; An ethanol solution of nano-silicon was mixed with the buffer solution, and aluminum salt was added to react, resulting in alumina-coated nano-silicon. The aluminum salt is one of aluminum nitrate, aluminum sulfate, and aluminum chloride.

2. A silicon-based negative electrode sheet, characterized in that, The silicon-based negative electrode sheet is prepared by the preparation method described in claim 1; the silicon-based negative electrode sheet includes a negative electrode current collector and a negative electrode material layer loaded on the negative electrode current collector, the negative electrode material layer includes a silicon-based negative electrode material, a conductive agent and a binder, and the negative electrode material layer does not contain a sulfide solid electrolyte. The mass ratio of the silicon-based anode material, conductive agent and binder is (80~90):(5~10):(5~10); The silicon-based anode material includes nano-silicon and a lithium aluminate layer coated on the surface of the nano-silicon; The lithium aluminate layer is amorphous, and the thickness of the lithium aluminate layer is 1-5 nm; The nano-silicon is spherical in shape and has a particle size of 50-150 nm.

3. The silicon-based negative electrode sheet according to claim 2, characterized in that, The conductive agent is one of acetylene black, vapor-grown carbon fiber, carbon nanotubes and Super P. And / or, the adhesive is one of polyvinylidene fluoride, carboxymethyl cellulose, and polyacrylic acid.

4. A sulfide-based all-solid-state lithium battery, characterized in that, The sulfide all-solid-state lithium battery includes a silicon-based negative electrode as described in any one of claims 2-3.

Citation Information

Patent Citations

  • Lithium titanate composite negative electrode piece and lithium titanate battery

    CN106099041A

  • Solid electrolyte coated silicon-based negative electrode material and preparation method thereof

    CN110071280A

  • Pure silicon negative electrode and preparation method and application thereof

    CN115377355A