Hardcoat composition and window member
By using a multilayer coating technology based on norbornene compounds and polymers, the problems of insufficient fingerprint resistance and durability of hard coatings for window components have been solved, achieving higher fingerprint resistance and durability.
Patent Information
- Application Number
- CN202310002510.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2022-01-04
- Filing Date
- 2023-01-03
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-01-03
AI Technical Summary
Existing hard coatings for window components are insufficient in terms of fingerprint resistance and durability, making it difficult to meet the high requirements of use.
A hard coating composition comprising a norbornene-based compound and a polymer is used to form a multilayer coating through a cross-linking structure, including a first layer and a second layer. The first layer is formed from an epoxy, polyurethane, or acrylic resin, and the second layer is formed from a norbornene-based compound, thereby enhancing the anti-fingerprint function.
It improves the fingerprint resistance and durability of window components, and enhances the wear resistance and scratch resistance of the hard coating.
Smart Images

Figure CN116426201B_ABST
Abstract
Description
[0001] Cross-references to related applications
[0002] This application claims priority and benefit to Korean Patent Application No. 10-2022-0001004, filed with the Korean Intellectual Property Office on January 4, 2022, the disclosure of which is incorporated herein by reference. Technical Field
[0003] The embodiments relate to hard coating compositions and window components including a hard coating formed using said hard coating composition. Background Technology
[0004] Various types of display devices are used to provide image information. The display device may include a display panel for displaying images and a window component for protecting the display panel. For example, the display panel may include an organic light-emitting diode (OLED) display panel, a liquid crystal display (LCD) panel, etc. The user sees the image displayed on the display panel through the window component.
[0005] Additionally, the window component may include various layers to improve durability and prevent fingerprints. For example, the window component may include a substrate component and a hard coating disposed on the substrate component. The hard coating can be used to improve durability, such as the hardness of the substrate component. Summary of the Invention
[0006] The implementation provides a hard coating composition for forming a hard coating.
[0007] The implementation provides a window component comprising the hard coating formed using the hard coating composition.
[0008] The hard coating composition according to the embodiment may comprise: a norbornene-based compound represented by Formula 1, and a polymer comprising at least one selected from epoxy-based resins, polyurethane-based resins, and acrylic resins. In Formula 1, A may represent an ester group, an ether group, an amide group, or an alkyl group, and R... X It can represent a fluoroalkyl group or a fluoropolyether group, R Y It can represent an alkyl group having a crosslinkable functional group, and each of n and m can independently be about 1 to about 100.
[0009] Chemical Formula 1
[0010]
[0011] In the implementation scheme, the norbornene-based compound may be a block copolymer or a random copolymer.
[0012] In the implementation, the norbornene-based compound may have a bottle-brush polymer structure, as understood in the polymer field.
[0013] In the implementation scheme, the norbornene-based compound may be the product of ring-opening metathesis polymerization (ROMP) of a first monomer having a crosslinkable functional group and a second monomer having a fluoroalkyl group.
[0014] In the embodiments, the crosslinkable functional group may be a hydroxyl group, an epoxy group, an acrylate group, or a methacrylate group.
[0015] In the embodiments, the fluoroalkyl group may be 1H,1H,2H,2H-heptadecyl, 1,1,1,3,3,3-hexafluoroisopropyl, 1H,1H,3H-hexafluorobutyl, 1H,1H,3H-tetrafluoropropyl, 1H,1H,5H-octafluoropentyl, 1H,1H,7H-dodecylfluoroheptyl, 1H,1H-heptafluorobutyl, and 2,2,2-trifluoroethyl.
[0016] In the implementation scheme, in the norbornene-based compound, the compound containing R in Formula 1 X The first repeating group and containing R Y The molar ratio of the second repeating group can be from about 95:5 to about 50:50.
[0017] In an embodiment, if the polymer comprises a polyurethane-based resin, the hard coating composition may further comprise silica nanoparticles and a solvent. The silica nanoparticles may be dispersed in the solvent.
[0018] In an embodiment, the polyurethane-based resin may include at least one of a polyol and a polyisocyanate.
[0019] In an embodiment, if the polymer comprises an epoxy-based resin, the hard coating composition may further comprise silica nanoparticles, a solvent, a photoacid generator, and a crosslinking agent.
[0020] In an implementation scheme, the epoxy-based resin may include a composite of organic and inorganic resins.
[0021] In an embodiment, the crosslinking agent may have epoxy groups.
[0022] In an embodiment, the photoacid generator may have a fluoroalkyl group, for example, a perfluoroalkyl group.
[0023] In an embodiment, the solvent may include at least one of ketone-based solvents, ether-based solvents, and ester-based solvents.
[0024] A window component according to an embodiment of the present invention may include a substrate component and a rigid coating disposed on the substrate component, the rigid coating comprising a first layer and a second layer disposed on the first layer. The first layer may include a crosslinked structure formed by curing a polymer comprising at least one of an epoxy-based resin, a polyurethane-based resin, and an acrylic resin. The second layer may include a crosslinked structure formed by curing a compound based on norbornene represented by Formula 1. In Formula 1, A may represent an ester group, an ether group, an amide group, or an alkyl group, R... X It can represent a fluoroalkyl group or a fluoropolyether group, R Y It can represent an alkyl group having a crosslinkable functional group, and each of n and m can independently be about 1 to about 100.
[0025] Chemical Formula 1
[0026]
[0027] In one embodiment, the first layer may include a surface adjacent to the base member, and the second layer may be fixed to the opposite surface of the first layer.
[0028] In the implementation scheme, the norbornene-based compound may be a block copolymer or a random copolymer.
[0029] In an embodiment, the norbornene-based compound may be the product of ring-opening metathesis polymerization of a first monomer having a crosslinkable functional group and a second monomer having a fluoroalkyl group. The norbornene-based compound may have a bottle-brush polymer structure.
[0030] In the embodiments, the crosslinkable functional group may be a hydroxyl group, an epoxy group, an acrylate group, or a methacrylate group.
[0031] In the embodiments, the fluoroalkyl group may be 1H,1H,2H,2H-heptadecyl, 1,1,1,3,3,3-hexafluoroisopropyl, 1H,1H,3H-hexafluorobutyl, 1H,1H,3H-tetrafluoropropyl, 1H,1H,5H-octafluoropentyl, 1H,1H,7H-dodecylfluoroheptyl, 1H,1H-heptafluorobutyl, or 2,2,2-trifluoroethyl.
[0032] In the implementation scheme, the base component may comprise plastic.
[0033] According to embodiments of the present invention, a hard coating can be obtained from a hard coating composition comprising a norbornene-based compound obtained by reacting a norbornene-based monomer having a crosslinkable functional group with a norbornene-based monomer having a fluoroalkyl group. Therefore, the anti-fingerprint function of the hard coating can be improved. Attached Figure Description
[0034] Exemplary, non-limiting embodiments will be more clearly understood from the following detailed description taken in conjunction with the accompanying drawings.
[0035] Figure 1 This is a perspective view schematically illustrating a display device including window components according to an embodiment.
[0036] Figure 2 and Figure 3 This example shows the corresponding Figure 1 A cross-sectional view of the window component with line I-I'.
[0037] Figure 4 This is an example of manufacturing. Figure 1 A flowchart of an example of a method for using window components.
[0038] Figure 5 This is an example of manufacturing. Figure 1 A flowchart of another example of the window component method.
[0039] Figure 6 This is a view illustrating images of the surface of a hard coating according to embodiments of Examples 14, 15, 17, and 23. Detailed Implementation
[0040] In the following, embodiments of the present disclosure will be explained in detail with reference to the accompanying drawings. The same reference numerals are used for the same components in the drawings, and redundant descriptions of the same components will be omitted.
[0041] It should be understood that when a component is referred to as being "on" another component, it can be directly on the other component or there can be intermediate components in between. Conversely, when a component is referred to as being "directly" on another component, there are no intermediate components in between.
[0042] It should be understood that although the terms “first,” “second,” “third,” etc., may be used herein to describe various elements, components, areas, layers, and / or parts, these elements, components, areas, layers, and / or parts should not be limited by these terms. These terms are used only to distinguish one element, component, area, layer, or part from another element, component, area, layer, or part. Therefore, without departing from the teachings of this document, “first element,” “first component,” “first area,” “first layer,” or “first part” discussed below may be referred to as a second element, second component, second area, second layer, or second part.
[0043] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting. As used herein, the singular forms “a,” “an,” and “the” are intended to include the plural forms, including “at least one,” unless the content expressly indicates otherwise. “At least one” should not be construed as limiting “a” or “an.” “Or” means “and / or.” As used herein, the term “and / or” includes any and all combinations of one or more of the relevant listed items. It should be further understood that the terms “comprises” and / or “comprising” or “includes” and / or “including”, when used in this specification, specify the presence of the specified features, areas, integers, steps, operations, elements, and / or components, but do not exclude the presence or addition of one or more other features, areas, integers, steps, operations, elements, components, and / or groups thereof.
[0044] Furthermore, spatially relative terms such as “lower” or “bottom” and “upper” or “top” may be used herein to describe the relationship between one element and another, as illustrated in the accompanying drawings. It should be understood that spatially relative terms are intended to encompass different orientations of the device beyond those depicted in the drawings. For example, if a device in one drawing is flipped, an element described as being “below” the other element will be oriented “upper” the other element. Thus, depending on the specific orientation of the drawing, the exemplary term “lower” can encompass both “down” and “up” orientations. Similarly, if a device in one drawing is flipped, an element described as being “below” or “under” the other element will be oriented “above” the other element. Thus, the exemplary terms “below” or “under” can encompass both “upper” and “lower” orientations.
[0045] As used herein, “about” or “approximately” includes a specified value and means within an acceptable range of deviation from a specific value, as determined by a person skilled in the art considering the relevant measurements and the errors associated with the measurement of the specific quantity (i.e., the limits of the measurement system). For example, “about” may mean within one or more standard deviations, or within ±10% or ±5% of the specified value.
[0046] Unless otherwise defined, all terms used herein (including technical and scientific terms) have the same meaning as commonly understood by one of ordinary skill in the art to which this disclosure pertains. It should be further understood that terms (e.g., those defined in commonly used dictionaries) should be interpreted as having a meaning consistent with their meaning in the relevant field and the context of this disclosure, and should not be interpreted in an idealized or overly formal sense unless expressly defined herein.
[0047] This document describes exemplary embodiments with reference to cross-sectional views as illustrative examples of idealized embodiments. Thus, variations in the shape of the illustrations due to, for example, manufacturing techniques and / or tolerances should be expected. Therefore, the embodiments described herein should not be construed as limited to the specific shape of the areas illustrated herein, but should include, for example, deviations in shape resulting from manufacturing processes. For example, an illustrated or described flat area may generally have rough and / or non-linear characteristics. Furthermore, the illustrated acute angles may be rounded. Therefore, the areas illustrated in the drawings are schematic in nature, and their shapes are not intended to illustrate precise shapes of the areas, nor are they intended to limit the scope of these claims.
[0048] The term "fluoroalkyl" refers to an alkyl group in which at least one hydrogen atom (e.g., at least two or more hydrogen atoms, three or more hydrogen atoms) of the alkyl group is replaced or substituted with fluorine. The term "perfluoroalkyl" refers to an alkyl group in which every hydrogen atom of the alkyl group is replaced or substituted with fluorine.
[0049] The term "compound" refers to a compound having non-repeating units; or an oligomer having a small number of repeating units, such as an oligomer having at least 1 to 20 repeating units, wherein the repeating units may be the same or different, or a polymer having at least 20 repeating units, wherein the repeating units may be the same or different. Those skilled in the art recognize and understand that oligomers are in the form of polymers.
[0050] The term "alkyl" refers to a substituted or unsubstituted, branched or linear, acyclic, monovalent group comprising carbon and hydrogen. Optionally, the alkyl group may include a carbon atom substituted with a heteroatom. At least one heteroatom may be O, S, N, P, B, Si, or Se, preferably O, S, or N. The alkyl group may have 1 to 32 carbon atoms, 1 to 16 carbon atoms, or 1 to 8 carbon atoms.
[0051] The term "alkylene" refers to a substituted or unsubstituted, branched or straight-chain divalent alkyl group. Optionally, the divalent alkyl group may include a carbon atom substituted with a heteroatom. At least one heteroatom may be O, S, N, P, B, Si, or Se, preferably O, S, or N. The alkylene group may have 1 to 32 carbon atoms, 1 to 16 carbon atoms, or 1 to 8 carbon atoms.
[0052] The term "based on" refers to a compound that includes or is derived from a specified portion. For example, "polyurethane-based resin" contains repeating urethane groups, and "norbornene-based compound" is derived from a compound containing norbornene groups.
[0053] Figure 1 This is a perspective view schematically illustrating a display device including window components according to an embodiment. Figure 2 and Figure 3 This example shows the corresponding Figure 1 A cross-sectional view of the window component with line I-I'.
[0054] refer to Figure 1 , Figure 2 and Figure 3 The display device may include a display panel (DP) and a window component (CW) disposed on the display panel (DP). The display panel (DP) can display images. For example, in Figure 1 In this embodiment, the display panel DP can provide an image generated in direction DR3 as the front image side. The display panel DP may contain a flexible material. However, the configuration of the present invention is not limited thereto, and the display panel DP may contain a rigid material.
[0055] The display panel DP may include driving elements, insulating layers, and light-emitting elements. The driving elements can receive gate signals and data voltages to drive the light-emitting elements. For example, the driving elements may contain silicon semiconductors or oxide semiconductors, and each of the insulating layers may contain organic or inorganic materials. Furthermore, the light-emitting elements may include organic light-emitting elements. In this case, the display panel DP may include an organic light-emitting display panel.
[0056] As described above, the display panel DP can include an organic light-emitting display panel. However, the present invention is not limited thereto. For example, the display panel DP includes a liquid crystal display panel, an electrophoretic display panel, a quantum dot display panel, an inorganic light-emitting display panel, etc.
[0057] A window component (CW) can be disposed on the display panel (DP). The window component (CW) can be disposed on the display panel (DP) to protect it. Furthermore, the window component (CW) can provide the front surface of the display device, serving as an input surface, touch surface, display surface, etc., for user information input within the display device. For example, the window component (CW) can incorporate a flexible material.
[0058] However, despite Figure 1 The illustration shows a display device with a flat surface, but the invention is not limited thereto. For example, the display device may include a planar region and at least one curved region. In this case, the display device can be folded based on the curved region.
[0059] The window component CW may include a substrate component BL and a rigid coating HC disposed on the substrate component BL. In one embodiment, the substrate component BL may include a plastic substrate. For example, the substrate component BL may comprise polyimide, polyamide, polyethylene, polypropylene, polyacrylate, polycarbonate, etc. These materials may be used alone or in combination. In another embodiment, the substrate component BL may include a glass substrate, etc. However, the invention is not limited thereto, and the substrate component BL may comprise other materials.
[0060] The hard coating HC can be a product of the hard coating compositions described herein. In embodiments, the hard coating composition may comprise a polymer and a norbornene-based compound. For example, the polymer may include polyurethane-based resins, epoxy-based resins, acrylic resins, etc. Furthermore, the norbornene-based compound may include norbornene-based ester polymers comprising oligomers having crosslinkable functional groups, norbornene-based ester polymers having fluoroalkyl groups (e.g., perfluoroalkyl groups), etc. Each of these may be used alone or in combination with each other.
[0061] Because the hard coating HC contains polymers, it can improve the durability of the window component CW. Because the hard coating HC contains norbornene-based compounds, it can also have fingerprint-resistant properties. The norbornene-based compounds in the hard coating HC can perform additional functions.
[0062] The hard coating HC can be divided into a first layer 10 and a second layer 20 disposed on the first layer 10. In an embodiment, the first layer 10 may include a cross-linked structure formed by curing a polymer, and the second layer 20 may include a cross-linked structure formed by curing a norbornene-based compound. For example, the first layer 10 may include a surface adjacent to the substrate member BL, and the second layer 20 may be fixed to the opposite surface of the first layer 10.
[0063] The hard coating composition for forming the hard coating HC will be described in detail below.
[0064] Hard coating composition
[0065] As described above, the hard coating composition may comprise a polymer and a norbornene-based compound. For example, the polymer may include polyurethane-based resins, epoxy-based resins, acrylic resins, etc. The stated polymers may be used alone or in combination. However, the resins contained in the polymer are not limited thereto.
[0066] In the implementation scheme, the norbornene-based compound can be represented by chemical formula 1.
[0067] Chemical Formula 1
[0068]
[0069] In chemical formula 1, A can represent an ester group, an ether group, an amide group, or an alkyl group. Furthermore, R... X It can represent fluoroalkyl groups such as perfluoroalkyl groups, or perfluoropolyether groups. Furthermore, R... Y It can represent an alkyl group having a crosslinkable functional group. Furthermore, each of n and m can independently be an integer from about 1 to about 100.
[0070] In the embodiments, the crosslinkable functional group can be a hydroxyl group, an epoxy group, an acrylate group, or a methacrylate group. Furthermore, the fluoroalkyl group can be 1H,1H,2H,2H-heptadecyl, 1,1,1,3,3,3-hexafluoroisopropyl, 1H,1H,3H-hexafluorobutyl, 1H,1H,3H-tetrafluoropropyl, 1H,1H,5H-octafluoropentyl, 1H,1H,7H-dodecylfluoroheptyl, 1H,1H-heptafluorobutyl, or 2,2,2-trifluoroethyl. However, the invention is not limited thereto.
[0071] In the implementation plan, R Y The crosslinkable functional group can be a perfluoroalkyl group.
[0072] For example, in norbornene-based compounds containing R X The first repeating group and containing R Y The molar ratio of the second repeating group can be from about 95:5 to about 50:50. Preferably, it contains R X The first repeating group and containing R Y The molar ratio of the second repeating group can be from about 90:10 to about 80:20. Therefore, the surface contact angle of the hard coating formed from the hard coating composition shows a change with the presence of R... X The first repeating group and containing R Y The molar ratio of the second repeating group increases with the increase of the molar ratio.
[0073] For example, Rx can be a fluoroalkyl group represented by chemical formula 2-1.
[0074] Chemical formula 2-1
[0075]
[0076] For example, R Y It can be an alkyl group with a hydroxyl group represented by chemical formula 2-2, an alkyl group with an epoxy group represented by chemical formula 2-3, or an alkyl group with an epoxy group represented by chemical formula 2-4.
[0077] Chemical formula 2-2
[0078]
[0079] Chemical formula 2-3
[0080]
[0081] Chemical formula 2-4
[0082]
[0083] Norbornene-based compounds can be obtained by reacting a first monomer having a crosslinkable functional group with a second monomer having a fluoroalkyl group. In embodiments, the norbornene-based compounds can be products of ring-opening metathesis polymerization (ROMP) of the first and second monomers. For example, norbornene-based compounds can be obtained by reacting the first and second monomers with a ROMP catalyst such as a Grubbs catalyst, and therefore, the molecular weight of the norbornene-based compounds can be controlled by adjusting the reaction time.
[0084] Furthermore, using synthetic methods well known in the art, the norbornene-based compounds can be block copolymers or random copolymers formed during polymerization according to the order of addition of the first and second monomers.
[0085] Norbornene-based compounds can have a bottle-brush-like polymer structure. Therefore, the flowability of norbornene-based compounds contained in hard coating compositions can be increased.
[0086] When the polymer contains a polyurethane-based resin, the hard coating composition may further contain silica nanoparticles, for example, silica nanoparticles dispersed in a solvent. For example, the polyurethane-based resin may include polyols, polyisocyanates, etc. The polyurethane-based resin may be used alone or in combination. For example, when the polymer contains a polyurethane-based resin, the hard coating composition may have a cross-linked structure that cures by heat.
[0087] When the polymer comprises an epoxy-based resin, the hard coating composition may further comprise silica nanoparticles (e.g., silica nanoparticles dispersed in a solvent), a photoacid generator, and a crosslinking agent. For example, the epoxy-based resin may comprise a composite in which organic and inorganic resins are combined. For example, the epoxy-based resin may comprise an epoxy hybrid.
[0088] Photoacid generators can have perfluoroalkyl groups. For example, photoacid generators may include triphenylsulfonium perfluorobutanesulfonate, triphenylsulfonium perfluorooctanesulfonate, etc. These can be used alone or in combination.
[0089] The crosslinking agent may include an epoxy crosslinking agent or an acrylate crosslinking agent. Preferably, the crosslinking agent may include an epoxy crosslinking agent. For example, an epoxy crosslinking agent may contain two or more epoxy groups. For example, an epoxy crosslinking agent may include 4-vinylcyclohexene dioxide, cyclohexene vinyl monooxide, (3,4-epoxycyclohexane)methyl, 3,4-epoxycyclohexylcarboxylate, 3,4-epoxycyclohexylmethyl methacrylate, bis(3,4-epoxycyclohexylmethyl)adipate, 3,4-epoxycyclohexanecarboxylate, and 2-(3,4-epoxycyclohexyl)-1,3-dioxane. These can be used alone or in combination.
[0090] Solvents can include ketone-based solvents, ether-based solvents, or ester-based solvents. For example, ketone-based solvents can include methyl ethyl ketone, acetophenone, cyclopentanone, ethyl isopropyl ketone, 2-hexanone, isophorone, isopropylidene acetone, methyl isobutyl ketone, 3-methyl-2-pentanone, 2-pentanone, 3-pentanone, etc. Ether-based solvents can include cyclopentyl methyl ether (CPME), diethylene glycol diethyl ether, dimethoxymethane, methyl tert-butyl ether, 2-(2-methoxyethoxy)ethanol, propylene glycol ether, etc. Ester-based solvents can include propylene glycol monomethyl ether acetate (PGMEA), propylene glycol monoethyl ether acetate, ethyl lactate, etc. Each of these can be used alone or in combination.
[0091] Figure 4 This is an example of manufacturing. Figure 1 A flowchart illustrating an example of a method for defining a window component. For example, Figure 4 Examples of methods for manufacturing window components are shown if the polymer of the hard coating composition includes a polyurethane-based resin.
[0092] refer to Figure 2 , Figure 3 and Figure 4The method of manufacturing a window component may include: step S100 of applying a hard coating composition to a substrate component BL, step S110 of orienting a norbornene-based compound contained in the hard coating composition, and step S120 of curing the hard coating composition.
[0093] In step S100, where the hard coating composition is applied to the substrate component BL, the hard coating composition can be applied by methods such as spin coating, slot coating, bar coating, spraying, inkjet printing, etc. However, the present invention is not limited thereto, and the hard coating composition can be applied by other methods.
[0094] As described above, compositions for hard coatings may comprise a polymer and a norbornene-based compound. The polymer and the norbornene-based compound may be mixed.
[0095] In step S110, which orients the norbornene-based compound contained in the hard coating composition, the hard coating composition applied to the substrate member BL and the solvent can be located in a vacuum chamber. Then, when the solvent is slowly added to the applied hard coating composition, for example by vapor diffusion, the norbornene-based compound can separate from the polymer and float on top of the polymer. That is, the norbornene-based compound can be oriented in a specific direction (e.g., perpendicular to the polymer). For example, the solvent can include a fluorine-based solvent. However, step S110, which orients the norbornene-based compound using a solvent, is optional; that is, step S110 can be omitted.
[0096] In step S120, the hard coating composition can be cured by heating the applied hard coating composition. In this case, a second layer 20, comprising a cross-linked structure formed by cross-linking a norbornene-based compound, can be fixed to a first layer 10, comprising a cross-linked structure formed by cross-linking a polymer. Therefore, a hard coating HC comprising a polymer and a norbornene-based compound can be formed on the substrate member BL. That is, a window member CW comprising the substrate member BL and the hard coating HC can be formed on the substrate member BL. Figure 4 The method for manufacturing window components is illustrated in the example.
[0097] Figure 5 This is an example of manufacturing. Figure 1 A flowchart of another example of the method for using window components. For example, Figure 5 This example illustrates another method of manufacturing window components if the polymer of the hard coating composition includes an epoxy-based resin.
[0098] refer to Figure 2 , Figure 3 and Figure 5The method for manufacturing a window component may include: step S200 of applying a hard coating composition to a substrate component BL, step S210 of orienting a norbornene-based compound contained in the hard coating composition, step S220 of drying the hard coating composition, and step S230 of curing the hard coating composition.
[0099] In step S200, where the hard coating composition is applied to the substrate component BL, the hard coating composition can be applied by methods such as spin coating, slot coating, bar coating, spraying, inkjet printing, etc. However, the present invention is not limited thereto, and the hard coating composition can be applied by other methods.
[0100] As described above, the composition for a hard coating may comprise a polymer and a norbornene-based compound. The polymer and the norbornene-based compound may be mixed. In step S210, which orients the norbornene-based compound contained in the hard coating composition, the hard coating composition applied to the substrate member BL and the solvent may be located in a vacuum chamber. Then, when the solvent is slowly added to the applied hard coating composition, for example by vapor diffusion, the norbornene-based compound may separate from the polymer and float on top of the polymer. For example, the solvent may comprise a fluorine-based solvent. However, step S210, which uses a solvent to orient the norbornene-based compound contained in the hard coating composition, is optional; that is, step S210 may be omitted.
[0101] In step S220, the solvent contained in the hard coating composition (e.g., ketone-based, ether-based, or ester-based solvents) can be removed. However, after removal, a portion of the solvent may remain in the hard coating composition.
[0102] In step S230, the hard coating composition can be cured by light. In this case, a second layer 20, comprising a cross-linked structure formed by cross-linking a norbornene-based compound, can be fixed to a first layer 10, comprising a cross-linked structure formed by cross-linking a polymer. Therefore, a hard coating HC comprising a polymer and a norbornene-based compound can be formed on a substrate member BL. That is, a window member CW comprising a substrate member BL and a hard coating HC can be formed on the substrate member BL. Figure 5 The method for manufacturing window components is illustrated in the example.
[0103] The following will describe the process through... Figure 4 The method of manufacturing window components illustrated in the figure or Figure 5 The experimental results of the hard coating HC included in the window component CW manufactured by the method of manufacturing window components illustrated in the example.
[0104] Preparation of the first and second monomers
[0105] Synthesis Example 1 - Monomers with perfluoroalkyl groups
[0106] 1H,1H,2H,2H-heptadecane-1-ol (1.829 g, 3.94 mmol), p-5-norbornenic acid (0.544 g, 3.94 mmol), and dimethylaminopyridine-toluenesulfonate (DMAP-TsOH) (0.116 g, 0.4 mmol) were dissolved in 8 mL of anhydrous tetrahydrofuran (THF). Then, dicyclohexylcarbodiimide (DCC) (0.813 g, 3.94 mmol) dissolved in 3 mL of anhydrous tetrahydrofuran (THF) was added dropwise at 0 °C. The reaction mixture was stirred at room temperature. After 24 hours, the reaction mixture was cooled to 0 °C, and a white precipitate was filtered off. The filtrate was concentrated by rotary evaporation and purified by column chromatography to give a monomer with a fluoroalkyl group in approximately 80% yield.
[0107] Synthesis Example 2 - Monomers with hydroxyl groups
[0108] Diethylene glycol (0.938 g, 8.84 mmol), p-5-norborneol (0.610 g, 4.42 mmol), and DMAP-TsOH (0.130 g, 0.4 mmol) were dissolved in 4 mL of anhydrous THF. Then, DCC (0.912 g, 4.42 mmol) dissolved in 3 mL of anhydrous THF was added dropwise at 0 °C. The reaction mixture was heated to 80 °C and stirred. After 24 hours, the reaction mixture was cooled to 0 °C, and a white precipitate was filtered off. The filtrate was concentrated using a rotary evaporator and purified by column chromatography to give a monomer with a hydroxyl group in 96% yield.
[0109] Synthetic Example 3 - Monomers with Epoxy Groups
[0110] Glycidyl ether (0.160 g, 2.17 mmol), p-5-norborneolcarboxylic acid (0.3 g, 2.17 mmol), and DMAP-TsOH (0.032 g, 0.234 mmol, 0.05 equivalent) were dissolved in 3 mL of anhydrous THF. Then, DCC (0.447 g, 2.17 mmol) dissolved in 1 mL of anhydrous THF was added dropwise at 0 °C. The reaction mixture was stirred at room temperature. After 20 hours, the reaction mixture was cooled to 0 °C, and a white precipitate was filtered off. The filtrate was concentrated using a rotary evaporator and purified by column chromatography to give a monomer with epoxy groups in 55% yield.
[0111] Synthetic Example 4 - Monomers with Epoxy Groups
[0112] 3,4-Epoxy-1-(hydroxymethyl)cyclohexane (0.3 g, 2.34 mmol), exo-5-norborneolcarboxylic acid (0.323 g, 2.34 mmol), and DMAP-TsOH (0.689 g, 0.234 mmol, 0.1 equivalent) were dissolved in 4 mL of anhydrous THF. Then, DCC (0.483 g, 2.34 mmol) dissolved in 3 mL of anhydrous THF was added dropwise at 0 °C. The reaction mixture was stirred at room temperature. After 24 hours, the reaction mixture was cooled to 0 °C, and a white precipitate was filtered off. The filtrate was concentrated using a rotary evaporator and purified by column chromatography to give a monomer with epoxy groups in 93% yield.
[0113] Manufacturing of window components
[0114] Example 1 - Polyurethane-based resin matrix
[0115] A monomer with a hydroxyl group (0.225 g, 0.1 mmol) obtained by Synthesis Example 2, dissolved in 0.4 mL of THF, was added dropwise to a solution in which Grubbs' third-generation catalyst (0.044 g, 5 μmol) was dissolved in a mixed solvent of 0.7 mL of THF and 0.5 mL of ethyl nonafluorobutyl ether, and the mixture was stirred at 0 °C for 15 minutes. Then, a monomer with a fluoroalkyl group (0.233 g, 0.4 mmol) obtained by Synthesis Example 1, dissolved in 0.4 mL of THF, was added dropwise continuously, and the mixture was stirred at 0 °C for 15 minutes to obtain a norbornene-based compound as a block copolymer with a bottle-brush polymer structure.
[0116] The norbornene-based compound was prepared by mixing 1.0 wt% of silica nanoparticles (dispersed in methyl ethyl ketone). A hard coating composition was prepared by using 19.8 wt% polyol and 39.6 wt% hexamethylene diisocyanate (HDI).
[0117] The prepared hard coating composition was applied to a 5 cm x 7 cm polyethylene terephthalate (PET) film using a rod coating method. For solvent orientation, the film was placed in a glass Petri dish along with a small Petri dish containing 1,1,1,3,3,3-hexafluoro-2-propanol at room temperature. The Petri dish was sealed with a lid and allowed to stand for a certain period of time. The PET film coated with the prepared hard coating composition was then heat-cured in an oven at 80°C for 12 hours, and a window component with a hard coating formed on the PET film was manufactured.
[0118] Example 2
[0119] A monomer with hydroxyl groups (0.113 g, 0.05 mmol) obtained by Synthesis Example 2, dissolved in 0.2 mL of THF, was added dropwise to a solution in which Grubbs' third-generation catalyst (0.044 g, 5 μmol) was dissolved in a mixed solvent of 0.7 mL of THF and 0.5 mL of ethyl nonafluorobutyl ether, and the mixture was stirred at 0 °C for 15 minutes. Then, a monomer with fluoroalkyl groups (0.263 g, 0.45 mmol) obtained by Synthesis Example 1, dissolved in 0.536 mL of THF, was added dropwise continuously, and the mixture was stirred at 0 °C for 15 minutes to obtain a norbornene-based compound as a block copolymer with a bottle-brush polymer structure.
[0120] The norbornene-based compound was prepared by mixing 1.0 wt% of silica nanoparticles (dispersed in methyl ethyl ketone). A hard coating composition was prepared by using 19.8 wt% of polyol and 39.6 wt% of hexamethylene diisocyanate (HDI), and window components were manufactured in the same manner as in Example 1.
[0121] Example 3
[0122] A monomer with hydroxyl groups (0.056 g, 0.025 mmol) obtained by Synthesis Example 2, dissolved in 0.1 mL of THF, was added dropwise to a solution in which Grubbs' third-generation catalyst (0.044 g, 5 μmol) was dissolved in a mixed solvent of 0.7 mL of THF and 0.5 mL of ethyl nonafluorobutyl ether, and the mixture was stirred at 0 °C for 15 minutes. Then, a monomer with fluoroalkyl groups (0.276 g, 0.475 mmol) obtained by Synthesis Example 1, dissolved in 0.594 mL of THF, was added dropwise continuously, and the mixture was stirred at 0 °C for 15 minutes to obtain a norbornene-based compound as a block copolymer with a bottle-brush polymer structure.
[0123] The hard coating composition was prepared using the same method as in Example 1, and the window components were manufactured using the same method as in Example 1.
[0124] Example 4
[0125] The norbornene-based compound was obtained using the same method as in Example 1.
[0126] The mixture consisted of 0.3 wt% of a norbornene-based compound and 40 wt% of silica nanoparticles (dispersed in methyl ethyl ketone). A hard coating composition was prepared using 32 wt% polyol and 28 wt% hexamethylene diisocyanate (HDI). Window components were manufactured using the same method as in Example 1, but without solvent orientation. Here, "wt%" indicates the relative content of each component, assuming a total mass of 100 for the hard coating composition.
[0127] Example 5
[0128] The norbornene-based compound was obtained using the same method as in Example 1.
[0129] The hard coating composition was prepared using the same method as in Example 4, and the window components were manufactured using the same method as in Example 1.
[0130] Example 6
[0131] The norbornene-based compound was obtained using the same method as in Example 1.
[0132] The hard coating composition was prepared using the same method as in Example 4, but the content of the norbornene-based compound was 0.5 wt%, and the window components were manufactured using the same method as in Example 1, but without solvent orientation.
[0133] Example 7
[0134] The norbornene-based compound was obtained using the same method as in Example 1.
[0135] The hard coating composition was prepared using the same method as in Example 4, but the content of the norbornene-based compound was 0.5 wt%, and the window component was manufactured using the same method as in Example 1.
[0136] Example 8
[0137] The norbornene-based compound was obtained using the same method as in Example 1.
[0138] The hard coating composition was prepared using the same method as in Example 4, but the content of the norbornene-based compound was 0.7 wt%, and the window components were manufactured using the same method as in Example 1, but without solvent orientation.
[0139] Example 9
[0140] The norbornene-based compound was obtained using the same method as in Example 1.
[0141] The hard coating composition was prepared using the same method as in Example 4, but the content of the norbornene-based compound was 0.7 wt%, and the window component was manufactured using the same method as in Example 1.
[0142] Example 10
[0143] The norbornene-based compound was obtained using the same method as in Example 1.
[0144] The hard coating composition was prepared using the same method as in Example 4, but the content of the norbornene-based compound was 1.5 wt%, and the window components were manufactured using the same method as in Example 1, but without solvent orientation.
[0145] Example 11
[0146] The norbornene-based compound was obtained using the same method as in Example 1.
[0147] The hard coating composition was prepared using the same method as in Example 4, but the content of the norbornene-based compound was 1.5 wt%, and the window component was manufactured using the same method as in Example 1.
[0148] Example 12
[0149] The norbornene-based compound was obtained using the same method as in Example 1.
[0150] The hard coating composition was prepared using the same method as in Example 4, but the content of the norbornene-based compound was 2 wt%, and the window components were manufactured using the same method as in Example 1, but without solvent orientation.
[0151] Example 13 – Epoxy-based Resin Matrix
[0152] A monomer with an epoxy group (0.194 g, 0.1 mmol) obtained by Synthesis Example 3, dissolved in 0.5 mL of THF, was added dropwise to a solution in which Grubbs' third-generation catalyst (0.044 g, 5 μmol) was dissolved in a mixed solvent of 0.5 mL of THF and 0.3 mL of ethyl nonafluorobutyl ether, and the mixture was stirred at 0 °C for 15 minutes. Then, a monomer with a fluoroalkyl group (0.2337 g, 0.4 mmol) obtained by Synthesis Example 1, dissolved in 0.5 mL of THF, was added dropwise continuously, and the mixture was stirred at 0 °C for 15 minutes to obtain a norbornene-based compound as a block copolymer with a bottle-brush polymer structure.
[0153] The norbornene-based compound was prepared by mixing 1.0 wt% of silica nanoparticles (dispersed in methyl ethyl ketone). A hard coating composition was prepared by comprising 46.1 wt% of an epoxy organic / inorganic hybrid represented by Formula 3, 9.8 wt% of a crosslinking agent represented by Formula 4, and a photoacid generator represented by Formula 5. Here, "wt%" indicates the relative content of each component, assuming the total mass of the hard coating composition is 100.
[0154] Chemical formula 3
[0155]
[0156] Chemical Formula 4
[0157]
[0158] Chemical formula 5
[0159]
[0160] The prepared hard coating composition was applied to a 5 cm x 7 cm polyethylene terephthalate (PET) film using a rod coating method. For solvent orientation, the film was placed in a small Petri dish containing 1,1,1,3,3,3-hexafluoro-2-propanol in a glass Petri dish at room temperature. The dish was sealed with a lid and allowed to stand for 5 minutes. The applied hard coating composition was then dried at 60°C for 1 minute to remove methyl ethyl ketone. The PET film coated with the prepared hard coating composition was placed in a photoreactor and cured by light for 5 minutes to fabricate a window component with a hard coating formed on the PET film.
[0161] Example 14
[0162] The norbornene-based compounds were obtained using the same method as in Example 13.
[0163] The hard coating composition was prepared using the same method as in Example 13, and the window components were manufactured using the same method as in Example 13, but without solvent orientation.
[0164] Example 15
[0165] A monomer with an epoxy group (0.248 g, 0.1 mmol) obtained by Synthesis Example 4, dissolved in 0.5 mL of THF, was added dropwise to a solution in which Grubbs' third-generation catalyst (0.044 g, 5 μmol) was dissolved in a mixed solvent of 0.5 mL of THF and 0.3 mL of ethyl nonafluorobutyl ether, and the mixture was stirred at 0 °C for 15 minutes. Then, a monomer with a fluoroalkyl group (0.234 g, 0.4 mmol) obtained by Synthesis Example 1, dissolved in 0.5 mL of THF, was added dropwise continuously, and the mixture was stirred at 0 °C for 15 minutes to obtain a norbornene-based compound as a block copolymer with a bottle-brush polymer structure.
[0166] The norbornene-based compound was prepared by mixing 1.0 wt% of silica nanoparticles (dispersed in methyl ethyl ketone). A hard coating composition was prepared by comprising 41.7 wt% of an epoxy organic / inorganic hybrid represented by Formula 3, 16.7 wt% of a crosslinking agent represented by Formula 4, and a photoacid generator represented by Formula 5. Here, "wt%" represents the relative content of each component, and the total mass of the hard coating composition is assumed to be 100.
[0167] Chemical formula 3
[0168]
[0169] Chemical Formula 4
[0170]
[0171] Chemical formula 5
[0172]
[0173] The window component was manufactured using the same method as in Example 13, but without solvent orientation.
[0174] Example 16
[0175] The norbornene-based compound was obtained using the same method as in Example 15.
[0176] The hard coating composition was prepared using the same method as in Example 15, but the content of the norbornene-based compound was 0.2 wt%, and the window components were manufactured using the same method as in Example 13, but without solvent orientation.
[0177] Example 17
[0178] The norbornene-based compound was obtained using the same method as in Example 15.
[0179] The hard coating composition was prepared using the same method as in Example 15, but the content of the norbornene-based compound was 0.5 wt%, and the window components were manufactured using the same method as in Example 13, but without solvent orientation.
[0180] Example 18
[0181] The norbornene-based compound was obtained using the same method as in Example 15.
[0182] The hard coating composition was prepared using the same method as in Example 15, but the content of the norbornene-based compound was 0.7 wt%, and the window components were manufactured using the same method as in Example 13, but without solvent orientation.
[0183] Example 19
[0184] The norbornene-based compound was obtained using the same method as in Example 15.
[0185] The hard coating composition was prepared using the same method as in Example 15, and the window components were manufactured using the same method as in Example 13, but without solvent orientation.
[0186] Example 20
[0187] The norbornene-based compound was obtained using the same method as in Example 15.
[0188] The hard coating composition was prepared using the same method as in Example 15, and the window component was manufactured using the same method as in Example 13.
[0189] Example 21
[0190] The norbornene-based compound was obtained using the same method as in Example 15.
[0191] The hard coating composition was prepared using the same method as in Example 15, but the content of the norbornene-based compound was 1.5 wt%, and the window components were manufactured using the same method as in Example 13, but without solvent orientation.
[0192] Example 22
[0193] A monomer with an epoxy group (0.062 g, 0.25 mmol) obtained by Synthesis Example 4, uniformly dissolved in THF, and a monomer with a fluoroalkyl group (0.234 g, 0.4 mmol) obtained by Synthesis Example 1, were added dropwise to a solution in which the third-generation Grubbs catalyst (0.044 g, 5 μmol) was dissolved in a mixed solvent of 0.5 mL of THF and 0.3 mL of ethyl nonafluorobutyl ether. The mixture was stirred at 0 °C for 20 minutes to obtain a norbornene-based compound as a random copolymer with a bottle-brush polymer structure.
[0194] The hard coating composition was prepared using the same method as in Example 15, but the content of the norbornene-based compound was 1.5 wt%, and the window components were manufactured using the same method as in Example 13, but without solvent orientation.
[0195] Example 23
[0196] A monomer with an epoxy group (0.248 g, 0.1 mmol) obtained by Synthesis Example 4, uniformly dissolved in THF, and a monomer with a fluoroalkyl group (0.234 g, 0.4 mmol) obtained by Synthesis Example 1, were added dropwise to a solution in which the third-generation Grubbs catalyst (0.044 g, 5 μmol) was dissolved in a mixed solvent of 0.5 mL of THF and 0.3 mL of ethyl nonafluorobutyl ether. The mixture was stirred at 0 °C for 20 minutes to obtain a norbornene-based compound as a random copolymer with a bottle-brush polymer structure.
[0197] The hard coating composition was prepared using the same method as in Example 15, but the content of the norbornene-based compound was 1.5 wt%, and the window components were manufactured using the same method as in Example 13, but without solvent orientation.
[0198] Example 24
[0199] A monomer with an epoxy group (0.031 g, 0.125 mmol) obtained by Synthesis Example 4, uniformly dissolved in THF, and a monomer with a fluoroalkyl group (0.073 g, 0.125 mmol) obtained by Synthesis Example 1, were added dropwise to a solution in which Grubbs' third-generation catalyst (0.022 g, 2.5 μmol) was dissolved in a mixed solvent of 0.5 mL THF and 0.3 mL ethyl nonafluorobutyl ether. The mixture was stirred at 0 °C for 20 minutes to obtain a norbornene-based compound as a random copolymer with a bottle-brush polymer structure.
[0200] The hard coating composition was prepared using the same method as in Example 15, but the content of the norbornene-based compound was 1.5 wt%, and the window components were manufactured using the same method as in Example 13, but without solvent orientation.
[0201] Example 25
[0202] A monomer with an epoxy group (0.031 g, 0.125 mmol) obtained by Synthesis Example 4, dissolved in 0.5 mL of THF, was added dropwise to a solution in which Grubbs' third-generation catalyst (0.022 g, 2.5 μmol) was dissolved in a mixed solvent of 0.5 mL of THF and 0.3 mL of ethyl nonafluorobutyl ether, and the mixture was stirred at 0 °C for 15 minutes. Then, a monomer with a fluoroalkyl group (0.073 g, 0.125 mmol) obtained by Synthesis Example 1, dissolved in 0.5 mL of THF, was added dropwise continuously, and the mixture was stirred at 0 °C for 15 minutes to obtain a norbornene-based compound as a block copolymer with a bottle-brush polymer structure.
[0203] The hard coating composition was prepared using the same method as in Example 15, but the content of the norbornene-based compound was 1.5 wt%, and the window components were manufactured using the same method as in Example 13, but without solvent orientation.
[0204] Example 26
[0205] The norbornene-based compound was obtained using the same method as in Example 15.
[0206] The hard coating composition was prepared using the same method as in Example 15, but the content of the norbornene-based compound was 1.5 wt%, and the window components were manufactured using the same method as in Example 13, but without solvent orientation.
[0207] Evaluation of hard coatings included in window components
[0208] The pencil hardness, surface contact angle (°), thickness (μm), and surface roughness (Rq) of the hard coatings prepared in Examples 1 to 26 were measured.
[0209] First, the pencil hardness of the hard coatings prepared in Examples 1 to 21 was measured using a transverse pencil hardness tester. The pencils used for measurement were Mitsubishi Uni pencils 6B to 9H. When the Uni pencil was loaded with a load of 0.75 kg / 1 kg, it passed through the hard coating at a 45° angle. The maximum HB-type graphite grade that did not damage the hard coating was measured as the pencil hardness of the hard coating.
[0210] Referring to Table 1 below, it was confirmed that the pencil hardness of the hard coatings prepared in Examples 1 to 11 was B, and the pencil hardness of the hard coating prepared in Example 12 was H. Furthermore, referring to Table 2 below, it was confirmed that the pencil hardness of the hard coatings prepared in Examples 13 to 20 was B, and the pencil hardness of the hard coating prepared in Example 21 was H.
[0211] The surface contact angles of the hard coatings prepared in Examples 1 through 26 relative to water were then measured using a contact angle meter (CAX-150). The surface contact angles were measured by photographing water droplets, with 10 μL of water falling vertically onto a horizontally fixed hard coating. Photographs of the water droplets were taken using a USB digital microscope, and the surface contact angles of the hard coatings relative to water were measured using computer image analysis software.
[0212] Referring to Table 1 below, it is confirmed that the hard coating prepared in Example 1 exhibits the highest surface contact angle among Examples 1 to 12.
[0213] Table 1
[0214]
[0215]
[0216] Referring to Table 2 below, it is confirmed that the hard coatings prepared in Examples 19, 21, 24 and 26 exhibit high surface contact angles without solvent orientation.
[0217] Table 2
[0218] Example number Pencil hardness Surface contact angle (°) Thickness (μm) Example 13 B 108 9 Example 14 B 106 7 Example 15 B 70 9 Example 16 B 85 9 Example 17 B 85 8 Example 18 B 98 9 Example 19 B 110 8 Example 20 B 110 7 Example 21 H 110 9 Example 22 - 97 - Example 23 - 101 - Example 24 - 110 - Example 25 - 80 - Example 26 - 110 -
[0219] Figure 6 This is a view illustrating an image of a hard-coated surface according to an embodiment. Specifically, Figure 6 Examples are shown of images obtained by photographing the upper surface of the hard coatings prepared in Examples 14, 15, 17 and 23.
[0220] The surface roughness (Rq) of the hard coating was measured using a non-contact mode atomic force microscope (AFM). In this case, the atomic force microscope was used as the SIS Nanostation II.
[0221] Therefore, please refer to the following Figure 6 Table 3 confirms that the surface roughness of the hard coatings prepared in Examples 14, 15 and 17 is relatively small, while the surface roughness of the hard coating prepared in Example 23 is relatively large.
[0222] Table 3
[0223] Example number Surface roughness (Rq) Example 14 6.21mm Example 15 21.4mm Example 17 11.8mm Example 23 41.4mm
[0224] This disclosure is applicable to a variety of display devices, including display panels. For example, this disclosure is applicable to high-resolution smartphones, mobile phones, smart tablets, smartwatches, tablet PCs, in-vehicle navigation systems, televisions, computer monitors, laptops, etc.
[0225] The foregoing is illustrative of embodiments and should not be construed as limiting them. Although several embodiments have been described, those skilled in the art will readily understand that many modifications may be made to the embodiments without substantially departing from the new teachings and advantages of the inventive concept. Therefore, all such modifications are intended to be included within the scope of the inventive concept as defined in the claims. Accordingly, it should be understood that the foregoing is illustrative of various embodiments and should not be construed as limiting to the specific disclosed embodiments, and modifications to the disclosed embodiments and other embodiments are intended to be included within the scope of the appended claims.
Claims
1. A hard coating composition comprising: Compounds based on norbornene represented by chemical formula 1; and Polymers including at least one of epoxy-based resins, polyurethane-based resins, and acrylic resins: Chemical Formula 1 In chemical formula 1, A represents an ester group, ether group, amide group, or alkyl group, and R... X Indicates a fluoroalkyl group or a fluoropolyether group, R Y This indicates an alkyl group having crosslinkable functional groups, and each of n and m is independently 1 to 100. The crosslinkable functional group is a hydroxyl group, an epoxy group, an acrylate group, or a methacrylate group.
2. The hard coating composition of claim 1, wherein the norbornene-based compound is a block copolymer or a random copolymer.
3. The hard coating composition of claim 1, wherein the norbornene-based compound has a bottle-brush polymer structure.
4. The hard coating composition of claim 1, wherein the norbornene-based compound is the product of ring-opening metathesis polymerization of a first monomer having the crosslinkable functional group and a second monomer having the fluoroalkyl group.
5. The hard coating composition of claim 1, wherein the fluoroalkyl group is 1H,1H,2H,2H-heptadecyl, 1,1,1,3,3,3-hexafluoroisopropyl, 1H,1H,3H-hexafluorobutyl, 1H,1H,3H-tetrafluoropropyl, 1H,1H,5H-octafluoropentyl, 1H,1H,7H-dodecylfluoroheptyl, 1H,1H-heptafluorobutyl, or 2,2,2-trifluoroethyl.
6. The hard coating composition of claim 1, wherein in the norbornene-based compound, the first repeating group comprising Rx and the group comprising R... Y The molar ratio of the second repeating group is 95:5 to 50:
50.
7. The hard coating composition of claim 1, wherein if the polymer comprises the polyurethane-based resin, the hard coating composition further comprises silica nanoparticles and a solvent.
8. The hard coating composition of claim 7, wherein the polyurethane-based resin comprises at least one of a polyol and a polyisocyanate.
9. The hard coating composition of claim 1, wherein if the polymer comprises the epoxy-based resin, the hard coating composition further comprises silica nanoparticles, a solvent, a photoacid generator, and a crosslinking agent.
10. The hard coating composition of claim 9, wherein the epoxy-based resin comprises a composite of organic and inorganic resins.
11. The hard coating composition of claim 9, wherein the crosslinking agent has epoxy groups.
12. The hard coating composition of claim 9, wherein the photoacid generator has a fluoroalkyl group.
13. The hard coating composition of claim 9, wherein the solvent comprises at least one of ketone-based solvents, ether-based solvents, and ester-based solvents.
14. Window components, including: Matrix components; as well as A hard coating is disposed on the substrate component, the hard coating comprising a first layer and a second layer disposed on the first layer. The first layer comprises a cross-linked structure formed by curing a polymer comprising at least one of epoxy-based resins, polyurethane-based resins, and acrylic resins, and The second layer includes a cross-linked structure formed by curing a norbornene-based compound represented by chemical formula 1: Chemical Formula 1 In chemical formula 1, A represents an ester group, ether group, amide group, or alkyl group, and R... X Indicates a fluoroalkyl group or a fluoropolyether group, R Y This indicates an alkyl group having crosslinkable functional groups, and each of n and m is independently 1 to 100. The crosslinkable functional group is a hydroxyl group, an epoxy group, an acrylate group, or a methacrylate group.
15. The window member of claim 14, wherein the first layer has a surface adjacent to the base member, and the second layer is fixed to the opposite surface of the first layer.
16. The window component of claim 14, wherein the norbornene-based compound is a block copolymer or a random copolymer.
17. The window member of claim 14, wherein the norbornene-based compound is the product of a ring-opening metathesis polymerization of a first monomer having the crosslinkable functional group and a second monomer having the fluoroalkyl group, and The norbornene-based compound described therein has a bottle-brush polymer structure.
18. The window component of claim 14, wherein the fluoroalkyl group is 1H,1H,2H,2H-heptadecyl, 1,1,1,3,3,3-hexafluoroisopropyl, 1H,1H,3H-hexafluorobutyl, 1H,1H,3H-tetrafluoropropyl, 1H,1H,5H-octafluoropentyl, 1H,1H,7H-dodecylfluoroheptyl, 1H,1H-heptafluorobutyl, or 2,2,2-trifluoroethyl.
19. The window component of claim 14, wherein the substrate component comprises plastic.
Citation Information
Patent Citations
Sterilization device with disinfection water micro-injection structure
KR1020220001004A
Hard coating composition and flexible display device including the hard coating composition
CN108102540A
Hard coating resin composition
US20180334589A1