Compositions and elastomers
By using three block copolymers with different structures and waxes in specific weight ratios, the problems of high elastic modulus, low permanent elongation and moldability in hygiene products were solved, achieving excellent moldability and ozone crack resistance, while improving color and low odor.
Patent Information
- Application Number
- CN202310514811.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-08-28
- Filing Date
- 2019-08-28
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2039-08-28
AI Technical Summary
Existing technologies struggle to simultaneously achieve high elastic modulus, low permanent elongation, and excellent formability in hygiene products, while also presenting issues with color and ozone cracking.
By using three block copolymers with different structures, adjusting the weight-average molecular weight and aromatic vinyl monomer unit content of each block, and adding waxes of straight-chain hydrocarbons and branched hydrocarbons in specific weight ratios, a composition with excellent moldability is formed.
It has achieved an elastomer with excellent formability, small film thickness variation, low permanent elongation, and excellent color and ozone crack resistance.
Smart Images

Figure BDA0004218699850000341 
Figure BDA0004218699850000351 
Figure BDA0004218699850000361
Abstract
Description
[0001] This application is a divisional application of the invention patent application with application number 201980053821.2, the original application being filed on August 28, 2019, and the invention being entitled "Composition and Elastomer". Technical Field
[0002] The present invention relates to compositions comprising block copolymers having aromatic vinyl polymer blocks and conjugated diene polymer blocks, and more specifically, to compositions capable of producing elastomers with excellent formability, small film thickness variation and low permanent elongation, and elastomers obtained from the compositions. Background Technology
[0003] Among thermoplastic elastomers, aromatic vinyl-conjugated diene-aromatic vinyl block copolymers are particularly elastic and soft, so one of their representative uses is as a material for stretch films used in hygiene products such as diapers and sanitary products.
[0004] Hygiene products such as diapers and sanitary pads require adaptability and fit to the wearer's movements, thus using stretch membranes in various parts. For example, short-sleeved diapers, a type of diaper, need to remain in place even during vigorous activity or prolonged wear, therefore the stretch membrane used must have both high elastic modulus and low permanent elongation.
[0005] In Patent Document 1, a block copolymer composition was proposed that, after being molded into a film, achieves both high elastic modulus and low permanent elongation at a high level and can be molded with good moldability. The block copolymer composition contains 25 to 150 parts by weight of an aromatic vinyl polymer and 0.2 to 10 parts by weight of a fatty acid amide relative to 100 parts by weight of a block copolymer having at least one aromatic vinyl polymer block and at least one conjugated diene polymer block.
[0006] Existing technical documents
[0007] Patent documents
[0008] Patent Document 1: Japanese Patent Application Publication No. 2016-69565. Summary of the Invention
[0009] The problem the invention aims to solve
[0010] The primary objective of this invention is to provide a composition that yields an elastomer with excellent formability, minimal film thickness variation, and low permanent elongation.
[0011] Furthermore, a second objective of the present invention is to provide a composition that yields an elastomer with excellent color and low odor, and excellent resistance to ozone cracking.
[0012] Solution for solving the problem
[0013] In order to achieve the first objective, the inventors conducted in-depth research and found that when three block copolymers with different structures are used in combination and the weight-average molecular weight of the blocks constituting each block copolymer and the content of aromatic vinyl monomer units in each block copolymer are appropriately adjusted, a composition with excellent moldability can be obtained, and an elastomer with small film thickness variation and small permanent elongation can be obtained, thus completing the present invention.
[0014] That is, according to the present invention, a composition (hereinafter, sometimes referred to as the "first composition") is provided, comprising:
[0015] General formula (A): Ar1 a -D a -Ar2 a The block copolymer A represented by Ar1 (where Ar1 is a molecule) is a molecule that ... a D represents aromatic vinyl polymer blocks with a weight-average molecular weight of 5000–20000. a Ar2 represents a conjugated diene polymer block. a (This refers to aromatic vinyl polymer blocks with a weight-average molecular weight exceeding 20,000 and below 400,000);
[0016] General formula (B): Ar1 b -D b -Ar2 b The block copolymer B represented by the formula (where Ar1) b and Ar2 b D represents aromatic vinyl polymer blocks with a weight-average molecular weight of 5000–20000. b (representing conjugated diene polymer blocks); and
[0017] General formula (C): (Ar c -D c ) n -X represents the block copolymer C (where Ar is the value of C). c D represents an aromatic vinyl polymer block. c This indicates a conjugated diene polymer block, where n represents an integer greater than 2, and X represents a residual group of the coupling agent.
[0018] The content of aromatic vinyl monomer units in the above-mentioned block copolymer A is 40-50% by weight relative to all monomer units constituting the above-mentioned block copolymer A.
[0019] The content of aromatic vinyl monomer units in the block copolymer B is 20-30% by weight relative to all monomer units constituting the block copolymer B.
[0020] The content of aromatic vinyl monomer units in the above-mentioned block copolymer C is less than 20% by weight relative to all the monomer units constituting the above-mentioned block copolymer C.
[0021] In the first composition of the present invention, a conjugated diene polymer block (D) is preferred. a The vinyl bond content of the conjugated diene polymer block (D) is 1–20 mol%. a The weight-average molecular weight is 40,000 to 400,000.
[0022] In the first composition of the present invention, a conjugated diene polymer block (D) is preferred. b The vinyl bond content of the conjugated diene polymer block (D) is 1–20 mol%. b The weight-average molecular weight is 40,000 to 400,000.
[0023] In the first composition of the present invention, it is preferred that the block copolymer A and the block copolymer B are obtained by the following manufacturing method: polymer blocks are formed by stepwise polymerization of aromatic vinyl monomers, conjugated diene monomers, and then aromatic vinyl monomers.
[0024] In the first composition of the present invention, n in the general formula (C) is preferably an integer from 2 to 4.
[0025] In the first composition of the present invention, a conjugated diene polymer block (D) is preferred. c The vinyl bond content of the conjugated diene polymer block (D) is 1–20 mol%. c The weight-average molecular weight is 20,000 to 200,000.
[0026] In the first composition of the present invention, the block copolymer C is preferably obtained by the following manufacturing method: polymerizing an aromatic vinyl monomer and a conjugated diene monomer to form a diblock chain, and then coupling the diblock chain with a coupling agent.
[0027] The first composition of the present invention preferably further comprises general formula (D): Ar d -D d The block copolymer D (where Ar) represents d Indicates aromatic vinyl polymer blocks, D d (representing a conjugated diene polymer block), wherein the content of aromatic vinyl monomer units in the block copolymer D is less than 20% by weight relative to all monomer units constituting the block copolymer D.
[0028] The first composition of the present invention preferably further contains a wax containing straight-chain hydrocarbons and branched hydrocarbons, wherein the weight ratio (normal / iso-) of the straight-chain hydrocarbons and the branched hydrocarbons isomers is 30 / 70 to 99 / 1, the melting point of the wax is less than 80°C, and the content of the wax in the composition is 0.1 to 5 parts by weight relative to a total of 100 parts by weight of the block copolymer in the composition.
[0029] Furthermore, the inventors conducted in-depth research to achieve the second objective and discovered that by adding a wax containing linear hydrocarbons and branched hydrocarbons with a low melting point in a specific weight ratio to the block copolymer, a composition with excellent color and low odor can be obtained, and an elastomer with excellent ozone crack resistance can be obtained, thereby completing the present invention.
[0030] Furthermore, according to the present invention, a composition (hereinafter sometimes referred to as "second composition") is provided, comprising: a block copolymer having at least one aromatic vinyl polymer block and at least one conjugated diene polymer block, and a wax containing linear hydrocarbons and branched hydrocarbons, wherein the weight ratio (linear / isolinear) of linear hydrocarbons (normal-phase) and linear hydrocarbons (iso-phase) is 30 / 70 to 99 / 1, the melting point of the wax is less than 80°C, and the content of the wax in the composition is 0.1 to 5 parts by weight relative to 100 parts by weight of the block copolymer.
[0031] Furthermore, according to the present invention, an elastomer obtained from the above-described first and second compositions can be provided.
[0032] The elastomer described above is preferably an elastomer for sanitary materials.
[0033] The elastomer described above or the elastomer used in the sanitary materials described above is preferably a film or a thread.
[0034] Invention Effects
[0035] According to the present invention, a first composition is provided that can produce an elastomer with excellent formability, small film thickness variation, and low permanent elongation.
[0036] Furthermore, according to the present invention, a second composition can be provided that yields an elastomer with excellent color and low odor, and excellent resistance to ozone cracking. Detailed Implementation
[0037] The first composition of the present invention contains block copolymer A, block copolymer B and block copolymer C.
[0038] (Block copolymer A)
[0039] Block copolymer A is a copolymer represented by the following general formula (A).
[0040] General formula (A): Ar1 a -D a -Ar2 a
[0041] (where Ar1) a D represents aromatic vinyl polymer blocks with a weight-average molecular weight of 5000–20000. a Ar2 represents a conjugated diene polymer block. a (This refers to aromatic vinyl polymer blocks with a weight-average molecular weight exceeding 20,000 and below 400,000)
[0042] Aromatic vinyl polymer block (Ar1) a ) and aromatic vinyl polymer blocks (Ar2) a () is a polymer block composed of aromatic vinyl monomer units obtained by polymerizing aromatic vinyl monomers as the main repeating units.
[0043] Used to form aromatic vinyl polymer blocks (Ar1) a ) and aromatic vinyl polymer blocks (Ar2) a The aromatic vinyl monomer unit is not particularly limited to any aromatic vinyl compound, and examples include styrene, α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2-ethylstyrene, 3-ethylstyrene, 4-ethylstyrene, 2,4-diisopropylstyrene, 2,4-dimethylstyrene, 4-tert-butylstyrene, 5-tert-butyl-2-methylstyrene, 2-chlorostyrene, 3-chlorostyrene, 4-chlorostyrene, 4-bromostyrene, 2-methyl-4,6-dichlorostyrene, 2,4-dibromostyrene, vinylnaphthalene, etc. Among these, styrene is preferred. These aromatic vinyl monomers can be used alone or in combination of two or more. Furthermore, the two aromatic vinyl polymer blocks can be composed of the same aromatic vinyl monomer unit or different aromatic vinyl monomer units.
[0044] In addition, aromatic vinyl polymer blocks (Ar1) a ) and aromatic vinyl polymer blocks (Ar2) a As long as aromatic vinyl monomer units are the main repeating units, other monomer units may also be included. As constituent blocks of aromatic vinyl polymers (Ar1... a ) and aromatic vinyl polymer blocks (Ar2) aMonomers that can be included in aromatic vinyl monomer units, excluding aromatic vinyl monomer units, include, for example, conjugated diene monomers such as 1,3-butadiene and isoprene (2-methyl-1,3-butadiene), α,β-unsaturated nitrile monomers, unsaturated carboxylic acid or anhydride monomers, unsaturated carboxylic acid ester monomers, and non-conjugated diene monomers. Monomer units other than aromatic vinyl monomer units are found in aromatic vinyl polymer blocks (Ar1... a ) and aromatic vinyl polymer blocks (Ar2) a The content of aromatic vinyl polymer blocks (Ar1) is preferably 20% by weight or less, more preferably 10% by weight or less, and particularly preferably substantially 0% by weight. a ) and aromatic vinyl polymer blocks (Ar2) a Preferably, it is formed of only one or two or more aromatic vinyl monomer units, and particularly preferably, it is formed of only styrene units.
[0045] In block copolymer A, aromatic vinyl polymer blocks (Ar1) a ) and aromatic vinyl polymer blocks (Ar2) a The weight-average molecular weights of the components are different. Because the first composition of the present invention contains such an asymmetric block copolymer A, it is possible to obtain an elastomer with excellent formability, small film thickness variation, and low permanent elongation.
[0046] Aromatic vinyl polymer block (Ar1) a The weight-average molecular weight is 5,000 to 20,000, more preferably 6,000 to 18,000, and even more preferably 7,000 to 16,000.
[0047] Aromatic vinyl polymer block (Ar2) a The weight-average molecular weight of the substance is greater than 20,000 and less than 400,000, more preferably 25,000 to 300,000, and even more preferably 30,000 to 200,000.
[0048] Conjugated diene polymer block (D a () is a polymer block composed of conjugated diene monomer units obtained by polymerizing conjugated diene monomers as the main repeating units.
[0049] Used to form conjugated diene polymer blocks (D aThe conjugated diene monomer of the conjugated diene monomer unit is not particularly limited as long as it is a conjugated diene compound, and examples include 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 2-chloro-1,3-butadiene, 1,3-pentadiene, 1,3-hexadiene, myrcene, farnesene, etc. Among these, 1,3-butadiene and / or isoprene are preferred, and isoprene is particularly preferred. These conjugated diene monomers can be used alone or in combination of two or more. Furthermore, conjugated diene polymer blocks (D... a A portion of the unsaturated bonds in the ) undergoes a hydrogenation reaction.
[0050] In addition, conjugated diene polymer blocks (D a As long as the conjugated diene monomer unit is the main repeating unit, it can also include other monomer units. As a component of the conjugated diene polymer block (D... a Monomers that can be included in a conjugated diene monomer unit, excluding conjugated diene monomer units, include, for example, aromatic vinyl monomers such as styrene and α-methylstyrene, α,β-unsaturated nitrile monomers, unsaturated carboxylic acid or anhydride monomers, unsaturated carboxylic acid ester monomers, and non-conjugated diene monomers. Monomer units other than conjugated diene monomer units are included in the conjugated diene polymer block (D...). a The content of the conjugated diene polymer block (D) is preferably 20% by weight or less, more preferably 10% by weight or less, and particularly preferably substantially 0% by weight. a Preferably, it is formed from only one or two or more conjugated diene monomer units, and particularly preferably from only isoprene units.
[0051] Conjugated diene polymer block (D a The vinyl bond content (1,2-vinyl bond units and 3,4-vinyl bond units in the conjugated diene polymer block (D)) a The proportion of all conjugated diene monomer units in the elastomer is not particularly limited, but is preferably 1 to 20 mol%, more preferably 2 to 15 mol%, and particularly preferably 3 to 10 mol%. When the vinyl bond content is too high, there is a tendency for the softness of the resulting elastomer to be impaired.
[0052] Conjugated diene polymer block (D a The weight-average molecular weight of the product is preferably 40,000 to 400,000, more preferably 45,000 to 350,000, and even more preferably 50,000 to 300,000.
[0053] The weight-average molecular weight (i.e., the weight-average molecular weight of the block copolymer A as a whole) is preferably 65,000 to 800,000, more preferably 70,000 to 700,000, and even more preferably 75,000 to 650,000.
[0054] It should be noted that, in this invention, the weight-average molecular weight of each polymer block and the weight-average molecular weight of the block polymer as a whole are calculated as values converted from polystyrene measured by high performance liquid chromatography.
[0055] Furthermore, the weight-average molecular weight of each polymer block and the weight-average molecular weight of the block polymer as a whole can be adjusted by regulating the amount of each monomer used to form each polymer block and the amount of polymerization initiator used when obtaining the block copolymer through polymerization.
[0056] The content of aromatic vinyl monomer units in block copolymer A is 40 to 50% by weight relative to all monomer units constituting block copolymer A. Since the first composition of the present invention contains an asymmetric block copolymer A comprising aromatic vinyl monomer units in the above-mentioned amount, it is possible to obtain an elastomer with excellent formability, small film thickness variation, and low permanent elongation.
[0057] Block copolymer A is preferably obtained by a manufacturing method that forms polymer blocks by stepwise polymerization of aromatic vinyl monomers, conjugated diene monomers, and then aromatic vinyl monomers. Therefore, block copolymer A preferably does not contain residual coupling agent groups. Details of such a manufacturing method are described below.
[0058] (Block copolymer B)
[0059] Block copolymer B is a copolymer represented by the following general formula (B).
[0060] General formula (B): Ar1 b -D b -Ar2 b
[0061] (where Ar1) b and Ar2 b These represent aromatic vinyl polymer blocks with a weight-average molecular weight of 5000–20000, and D, respectively. b (representing conjugated diene polymer blocks)
[0062] Aromatic vinyl polymer block (Ar1) b ) and aromatic vinyl polymer blocks (Ar2) b () is a polymer block composed of aromatic vinyl monomer units obtained by polymerizing aromatic vinyl monomers as the main repeating units.
[0063] Used to form aromatic vinyl polymer blocks (Ar1) b ) and aromatic vinyl polymer blocks (Ar2) bThe aromatic vinyl monomer unit of the aromatic vinyl monomer is not particularly limited as long as it is an aromatic vinyl compound. Examples include, for instance, aromatic vinyl polymer blocks (Ar1) mentioned above. a ) and aromatic vinyl polymer blocks (Ar2) a The same monomer.
[0064] Aromatic vinyl polymer block (Ar1) b ) and aromatic vinyl polymer blocks (Ar2) b As long as the aromatic vinyl monomer unit is the main repeating unit, it may also include other monomer units. Examples of monomers constituting monomer units other than the aromatic vinyl monomer unit include, for example, those that are associated with the aforementioned aromatic vinyl polymer blocks (Ar1). a ) and aromatic vinyl polymer blocks (Ar2) a The same monomers can be present in the same amounts. Furthermore, aromatic vinyl polymer blocks (Ar1) b ) and aromatic vinyl polymer blocks (Ar2) b It is also preferred that it is substantially formed of only one or two or more aromatic vinyl monomer units, and particularly preferred that it is formed of only styrene units.
[0065] In block copolymer B, aromatic vinyl polymer blocks (Ar1) b ) and aromatic vinyl polymer blocks (Ar2) b All of them have a weight-average molecular weight in the range of 5,000 to 20,000. The first composition of the present invention contains such a symmetrical block copolymer B, so it is possible to obtain an elastomer with excellent formability, small film thickness variation and low permanent elongation.
[0066] Aromatic vinyl polymer block (Ar1) b ) and aromatic vinyl polymer blocks (Ar2) b The weight-average molecular weight is 5,000 to 20,000, more preferably 6,000 to 18,000, and even more preferably 7,000 to 16,000.
[0067] If aromatic vinyl polymer block (Ar1) b ) and aromatic vinyl polymer blocks (Ar2) b If the weight-average molecular weights of the aromatic vinyl polymer blocks (Ar1) are within the above-mentioned range, they can be equal or different from each other, but are preferably substantially equal. Furthermore, aromatic vinyl polymer blocks (Ar1) b ) and aromatic vinyl polymer blocks (Ar2) b The weight-average molecular weight of the aromatic vinyl polymer block (Ar1) of the block copolymer A is preferably lower than that of the block copolymer A.a The weight-average molecular weights of the two molecules are essentially equal.
[0068] Conjugated diene polymer block (D b () is a polymer block composed of conjugated diene monomer units obtained by polymerizing conjugated diene monomers as the main repeating units.
[0069] Used to form conjugated diene polymer blocks (D b The conjugated diene monomer unit of the conjugated diene monomer is not particularly limited as long as it is a conjugated diene compound. Examples include, for instance, the conjugated diene polymer block (D) mentioned above. a The same compound.
[0070] In addition, conjugated diene polymer blocks (D b As long as the conjugated diene monomer unit is the main repeating unit, it can also include other monomer units. Examples of monomers constituting monomer units other than the conjugated diene monomer unit include, for example, those with conjugated diene polymer blocks (D...). a The same monomers can have the same content and vinyl bond content. Furthermore, conjugated diene polymer blocks (D...) b It is also preferred that it is substantially formed of only one or two or more conjugated diene monomer units, and particularly preferred that it is formed of only isoprene units.
[0071] Conjugated diene polymer block (D b The vinyl bond content of ) is preferably similar to that of the conjugated diene polymer block (D) of block polymer A. a The vinyl bond content of the two groups is essentially the same.
[0072] Conjugated diene polymer block (D b The weight-average molecular weight of the substance is 40,000 to 400,000, more preferably 45,000 to 350,000, and even more preferably 50,000 to 300,000.
[0073] Conjugated diene polymer block (D b The weight-average molecular weight of the preferred polymer is that of the conjugated diene polymer block (D) of the block polymer A. a The weight-average molecular weights of the two molecules are essentially equal.
[0074] The weight-average molecular weight (i.e., the weight-average molecular weight of the block copolymer B as a whole) is preferably 65,000 to 800,000, more preferably 70,000 to 700,000, and even more preferably 75,000 to 600,000.
[0075] The content of aromatic vinyl monomer units in block copolymer B is 20 to 30% by weight relative to all monomer units constituting block copolymer B. Since the first composition of the present invention contains a symmetrical block copolymer B comprising aromatic vinyl monomer units in the above-mentioned amount, an elastomer with excellent formability, small film thickness variation, and low permanent elongation can be obtained.
[0076] Block copolymer B is preferably obtained by a manufacturing method that forms polymer blocks by stepwise polymerization of aromatic vinyl monomers, conjugated diene monomers, and then aromatic vinyl monomers. Therefore, block copolymer B preferably does not contain residual coupling agent groups. Details of such a manufacturing method are described below.
[0077] (Block copolymer C)
[0078] Block copolymer C is a copolymer represented by the following general formula (C).
[0079] General formula (C): (Ar c -D c ) n -X
[0080] (where Ar) c Indicates aromatic vinyl polymer blocks, D c (This represents a conjugated diene polymer block, n represents an integer greater than 2, and X represents a residual group of the coupling agent.)
[0081] Block copolymer C has n diblocks (Ar) c -D c The structure is formed by the residual groups (X) of the coupling agent bonded together. In the general formula (C), n represents the number of branches in the block copolymer C. The block copolymer C can be a mixture of two or more block copolymers in which diblocks are bonded in different quantities. n is an integer of 2 or more, preferably an integer from 2 to 8, and more preferably an integer from 2 to 4. The residual groups (X) of the coupling agent are not particularly limited as long as they are residual groups of an n-valent coupling agent, but are preferably residual groups of silicon-containing coupling agents, and more preferably residual groups of halogenated silanes or alkoxysilanes. Examples of coupling agents constituting the residual groups of the coupling agent can be given later.
[0082] As block copolymer C, a mixture of block copolymer C1 with n=2, block copolymer C2 with n=3, and block copolymer C3 with n=4 is particularly preferred. As the weight ratio (C1 / C2 / C3) of block copolymers C1 to C3 in this case, it is preferably 40 to 80 / 30 to 10 / 30 to 10.
[0083] Aromatic vinyl polymer block (Ar) c() is a polymer block composed of aromatic vinyl monomer units obtained by polymerizing aromatic vinyl monomers as the main repeating units.
[0084] Used to form aromatic vinyl polymer blocks (Ar c The aromatic vinyl monomer unit of the aromatic vinyl monomer is not particularly limited as long as it is an aromatic vinyl compound. Examples include, for instance, aromatic vinyl polymer blocks (Ar1) mentioned above. a ) and aromatic vinyl polymer blocks (Ar2) a The same monomer.
[0085] Aromatic vinyl polymer block (Ar) c As long as the aromatic vinyl monomer unit is the main repeating unit, it may also include other monomer units. Examples of monomers constituting monomer units other than the aromatic vinyl monomer unit include, for example, those with aromatic vinyl polymer blocks (Ar1). a ) and aromatic vinyl polymer blocks (Ar2) a The same monomers can have the same content. Furthermore, the aromatic vinyl polymer blocks in block copolymer C can be composed of the same aromatic vinyl monomer units or different aromatic vinyl monomer units. Additionally, aromatic vinyl polymer blocks (Ar... c It is also preferred that it is substantially formed of only one or two or more aromatic vinyl monomer units, and particularly preferred that it is formed of only styrene units.
[0086] Aromatic vinyl polymer block (Ar) c The weight-average molecular weight of the product is preferably 4,000 to 18,000, more preferably 5,000 to 16,000, and even more preferably 6,000 to 14,000.
[0087] Block copolymer C has multiple aromatic vinyl polymer blocks (Ar c As long as the weight-average molecular weights are within the above-mentioned range, they can be equal or different from each other, but preferably substantially equal.
[0088] Conjugated diene polymer block (D c () is a polymer block composed of conjugated diene monomer units obtained by polymerizing conjugated diene monomers as the main repeating units.
[0089] Used to form conjugated diene polymer blocks (D c The conjugated diene monomer unit of the conjugated diene monomer is not particularly limited as long as it is a conjugated diene compound. Examples include, for instance, the conjugated diene polymer block (D) mentioned above. aThe same monomers. In addition, the individual conjugated diene polymer blocks in the block copolymer C can be composed of the same conjugated diene monomer units or different conjugated diene monomer units.
[0090] In addition, conjugated diene polymer blocks (D c As long as the conjugated diene monomer unit is the main repeating unit, it can also include other monomer units. Examples of monomers constituting monomer units other than the conjugated diene monomer unit include, for example, those with conjugated diene polymer blocks (D...). a The same monomers can have the same content and vinyl bond content. Furthermore, conjugated diene polymer blocks (D...) c It is also preferred that it is substantially formed of only one or two or more conjugated diene monomer units, and particularly preferred that it is formed of only isoprene units.
[0091] Conjugated diene polymer block (D c The weight-average molecular weight of the product is preferably 20,000 to 200,000, more preferably 25,000 to 180,000, and even more preferably 30,000 to 150,000.
[0092] Block copolymer C has multiple conjugated diene polymer blocks (D c As long as the weight-average molecular weights are within the above-mentioned range, they can be equal or different from each other, but it is preferred that they are substantially equal.
[0093] The weight-average molecular weight (i.e., the weight-average molecular weight of the block copolymer C as a whole) is preferably 60,000 to 800,000, more preferably 80,000 to 600,000.
[0094] The content of aromatic vinyl monomer units in block copolymer C is less than 20% by weight, more preferably less than 18% by weight, and even more preferably less than 16% by weight, relative to all monomer units constituting block copolymer C. The lower limit is not particularly limited and can be 5% by weight or more. Because the first composition of the present invention contains block copolymer C containing aromatic vinyl monomer units in the above-mentioned amount and also containing residual groups of coupling agents, it is possible to obtain an elastomer with excellent formability, small film thickness variation, and low permanent elongation.
[0095] Block copolymer C is preferably obtained by a manufacturing method in which an aromatic vinyl monomer and a conjugated diene monomer are polymerized to form a diblock chain, and the diblock chain is coupled by reacting with a coupling agent. Therefore, block copolymer C contains residual groups of the coupling agent. Details of this manufacturing method are described below.
[0096] (Block copolymer D)
[0097] The first composition of the present invention may further contain a block copolymer D. The block copolymer D is a copolymer represented by the following general formula (D).
[0098] General formula (D): Ar d -D d
[0099] (where Ar) d Indicates aromatic vinyl polymer blocks, D d (representing conjugated diene polymer blocks)
[0100] Aromatic vinyl polymer block (Ar) d () is a polymer block composed of aromatic vinyl monomer units obtained by polymerizing aromatic vinyl monomers as the main repeating units.
[0101] Used to form aromatic vinyl polymer blocks (Ar d The aromatic vinyl monomer unit of the aromatic vinyl monomer is not particularly limited as long as it is an aromatic vinyl compound. Examples include aromatic vinyl polymer blocks (Ar1) mentioned above. a ) and aromatic vinyl polymer blocks (Ar2) a The same monomer.
[0102] Aromatic vinyl polymer block (Ar) d As long as the aromatic vinyl monomer unit is the main repeating unit, it may also include other monomer units. Examples of monomers constituting monomer units other than the aromatic vinyl monomer unit include, for example, those that are associated with the aforementioned aromatic vinyl polymer blocks (Ar1). a ) and aromatic vinyl polymer blocks (Ar2) a The same monomers can be present in the same amounts. Furthermore, aromatic vinyl polymer blocks (Ar...) d It is also preferred that it is substantially formed of only one or two or more aromatic vinyl monomer units, and particularly preferred that it is formed of only styrene units.
[0103] Aromatic vinyl polymer block (Ar) d The weight-average molecular weight of the product is preferably 4,000 to 18,000, more preferably 5,000 to 16,000, and even more preferably 6,000 to 14,000.
[0104] Aromatic vinyl polymer block (Ar) d The weight-average molecular weight of ) is preferably the same as that of the aromatic vinyl polymer block (Ar) of the block polymer C. c The weight-average molecular weights of the two molecules are essentially equal.
[0105] Conjugated diene polymer block (Dd () is a polymer block composed of conjugated diene monomer units obtained by polymerizing conjugated diene monomers as the main repeating units.
[0106] Used to form conjugated diene polymer blocks (D d The conjugated diene monomer unit of the conjugated diene monomer is not particularly limited as long as it is a conjugated diene compound. Examples include, for instance, the conjugated diene polymer block (D) mentioned above. a The same monomer.
[0107] In addition, conjugated diene polymer blocks (D d As long as the conjugated diene monomer unit is the main repeating unit, it can also include other monomer units. Examples of monomers constituting monomer units other than the conjugated diene monomer unit include, for example, those with conjugated diene polymer blocks (D...). a The same monomers can have the same content and vinyl bond content. Furthermore, conjugated diene polymer blocks (D...) d It is also preferred that it is substantially formed of only one or two or more conjugated diene monomer units, and particularly preferred that it is formed of only isoprene units.
[0108] Conjugated diene polymer block (D d The vinyl bond content of the ) is preferably similar to that of the conjugated diene polymer block (D) of the block polymer C. c The vinyl bond content of the two groups is essentially the same.
[0109] Conjugated diene polymer block (D d The weight-average molecular weight of the product is preferably 20,000 to 200,000, more preferably 25,000 to 180,000, and even more preferably 30,000 to 150,000.
[0110] Conjugated diene polymer block (D d The weight-average molecular weight of the preferred polymer is that of the conjugated diene polymer block (D) of the block polymer C. c The weight-average molecular weights of the two molecules are essentially equal.
[0111] The weight-average molecular weight (i.e., the weight-average molecular weight of the block copolymer D as a whole) is preferably 30,000 to 200,000, more preferably 40,000 to 180,000.
[0112] The content of aromatic vinyl monomer units in block copolymer D is less than 20% by weight, preferably less than 18% by weight, more preferably less than 16% by weight, relative to all monomer units constituting block copolymer D. The lower limit is not particularly limited and can be 5% by weight or more. When the first composition of the present invention contains block copolymer D comprising aromatic vinyl monomer units in the above-mentioned amount, an elastomer with superior formability, smaller film thickness variation, and smaller permanent elongation can be obtained.
[0113] The first composition of the present invention contains the block copolymers A to C described above, and optionally also contains block copolymer D. The weight ratio (A / B / C) of the block copolymers A to C in the first composition of the present invention is preferably 10–40 / 10–40 / 80–20, more preferably 15–40 / 15–40 / 70–25, and even more preferably 20–35 / 20–35 / 60–30.
[0114] When the first composition of the present invention further contains block copolymer D, the content of block copolymer D in the first composition of the present invention containing block copolymers A to C is preferably 1 to 20% by weight, more preferably 2 to 18% by weight, and even more preferably 3 to 16% by weight.
[0115] Block copolymers A through D can be manufactured using conventional methods. The most common manufacturing method includes: forming polymer blocks by stepwise polymerization of aromatic vinyl monomers and conjugated diene monomers using anionic living polymerization, followed by coupling with a coupling agent as needed. Alternatively, a method can be used to form polymer blocks by stepwise polymerization of aromatic vinyl monomers, conjugated diene monomers, and then aromatic vinyl monomers. Furthermore, they can be manufactured by separately producing each polymer using existing polymerization methods, incorporating other polymer components as needed, and then mixing them using conventional methods such as compounding or solution mixing. Additionally, block copolymers A and B, or block copolymers C and D, can be manufactured simultaneously as described below.
[0116] Furthermore, commercially available block copolymers can also be used in this invention, such as Quintac (registered trademark) (manufactured by Zeon Corporation, Japan), JSR-SIS (registered trademark) (manufactured by JSR Corporation), Vector (registered trademark) (manufactured by DEXCO polymers), Asaprene (registered trademark), Tufprene (registered trademark), Tuftec (registered trademark) (manufactured by Asahi Kasei Chemicals Corporation), SEPTON (registered trademark) (manufactured by KURARAY CO.,LTD.), and KRATON (registered trademark) (manufactured by Kraton Corporation).
[0117] Block copolymer A and block copolymer B are preferably manufactured by a method of forming polymer blocks by stepwise polymerization of aromatic vinyl monomers, conjugated diene monomers, and then aromatic vinyl monomers.
[0118] More specifically, block copolymer A and block copolymer B are preferably manufactured by the following method. That is, a manufacturing method having the following steps is preferred:
[0119] In the first polymerization step, monomers containing aromatic vinyl monomers are polymerized in a solvent in the presence of a polymerization initiator, thereby obtaining a solution containing aromatic vinyl polymer block chains.
[0120] In the second polymerization step, a monomer containing a conjugated diene monomer is added to a solution containing aromatic vinyl polymer block chains, and polymerization is carried out to obtain a solution containing diblock chains.
[0121] In the third polymerization step, a monomer containing an aromatic vinyl monomer is added to a solution containing a diblock chain and polymerized to obtain a solution containing a triblock chain.
[0122] The termination process involves adding a polymerization terminator to a solution containing triblock chains in an amount less than 1 molar equivalent relative to the active ends of the triblock chains, thereby deactivating a portion of the active ends and obtaining a solution containing block copolymer B and triblock chains; and
[0123] In the fourth polymerization step, a monomer containing an aromatic vinyl monomer is added to a solution containing a triblock chain and a block copolymer B, and polymerization is carried out to obtain a solution containing block copolymer A and block copolymer B.
[0124] In the above-described manufacturing method, firstly, a polymerization initiator is used in a solvent to polymerize a monomer containing an aromatic vinyl monomer as the main component (first polymerization step). As the polymerization initiator used, for both aromatic vinyl monomers and conjugated diene monomers, known anionic polymerization activities such as organoalkali metal compounds, organoalkaline earth metal compounds, and organolanthanide rare earth metal compounds can generally be used. As the organoalkali metal compound, organolithium compounds having one or more lithium atoms in their molecules are particularly preferred. Specific examples include organomonal lithium compounds such as ethyllithium, n-propyllithium, isopropyllithium, n-butyllithium, sec-butyllithium, tert-butyllithium, hexyllithium, phenyllithium, stilbeneyllithium, dialkylaminolithium, diphenylaminolithium, and bis(trimethylsilyl)aminolithium; organodilithium compounds such as methylene dilithium, tetramethylene dilithium, hexamethylene dilithium, isoprene dilithium, and 1,4-dilithium-ethylcyclohexane; and further organotrilithium compounds such as 1,3,5-trilithiumbenzene. Among these, organic single-lithium compounds are particularly preferred.
[0125] Examples of organoalkaline earth metal compounds used as polymerization initiators include n-butylmagnesium bromide, n-hexylmagnesium bromide, calcium ethoxylate, calcium stearate, tert-butoxystrontium, barium ethoxylate, barium isopropoxylate, barium ethylthiolate, barium tert-butoxylate, barium phenoxylate, barium diethylamino, barium stearate, and barium ethyllate. Other specific examples of polymerization initiators include composite catalysts formed from lanthanide rare earth metal compounds containing neodymium, samarium, gadolinium, etc., / alkylaluminum / alkylhalide / alkylaluminum hydride, and metallocene catalysts containing titanium, vanadium, samarium, gadolinium, etc., which form a homogeneous system in organic solvents and exhibit active polymerization properties. It should be noted that these polymerization initiators can be used alone or in combination of two or more.
[0126] The amount of polymerization initiator used can be determined according to the target molecular weight and is not particularly limited. The total amount of monomer used per 100g is preferably 0.01 mmol to 20 mmol, more preferably 0.05 mmol to 15 mmol, and even more preferably 0.1 mmol to 10 mmol.
[0127] The solvent used for polymerization is not particularly limited as long as it is inactive to the polymerization initiator; for example, linear hydrocarbon solvents, cyclic hydrocarbon solvents, or mixtures thereof can be used. Examples of linear hydrocarbon solvents include: n-butane, isobutane, 1-butene, isobutene, trans-2-butene, cis-2-butene, 1-pentene, trans-2-pentene, cis-2-pentene, n-pentane, isopentane, neopentane, n-hexane, and other linear alkanes and alkenes with 4 to 6 carbon atoms. Specific examples of cyclic hydrocarbon solvents include: aromatic compounds such as benzene, toluene, and xylene; and alicyclic hydrocarbon compounds such as cyclopentane and cyclohexane. These solvents can be used individually or in mixtures of two or more.
[0128] The amount of solvent used for polymerization is not particularly limited, but it is preferably set such that the concentration of the block copolymer in the final block copolymer solution is preferably in the range of 5 to 60% by weight, more preferably in the range of 10 to 55% by weight, and particularly preferably in the range of 20 to 50% by weight.
[0129] Furthermore, to control the structure of each polymer block, Lewis base compounds can be added to the reactor used for polymerization. Examples of Lewis base compounds include ethers such as tetrahydrofuran, diethyl ether, dioxane, ethylene glycol dimethyl ether, ethylene glycol dibutyl ether, diethylene glycol dimethyl ether, and diethylene glycol dibutyl ether; tertiary amines such as tetramethylethylenediamine, trimethylamine, triethylamine, pyridine, and quinine rings; alkali metal alkoxides such as potassium tert-amyloxide and potassium tert-butoxide; and phosphines such as triphenylphosphine. These Lewis base compounds can be used individually or in combination of two or more, and can be appropriately selected without prejudice to the purpose of the present invention.
[0130] There is no particular limitation on the timing of adding Lewis base compounds during the polymerization reaction, as long as it is appropriately determined according to the structure of the target block copolymers. For example, they can be added before the start of polymerization, or after the polymerization of a portion of the polymer blocks. Furthermore, they can be added before the start of polymerization and then further added after the polymerization of a portion of the polymer blocks.
[0131] The polymerization temperature is preferably 10–150°C, more preferably 30–130°C, and even more preferably 40–90°C. The polymerization time varies depending on the conditions, but is usually within 48 hours, preferably 0.5–10 hours. The polymerization pressure is not particularly limited as long as it is sufficient to maintain the monomer and solvent in a liquid phase within the above-mentioned polymerization temperature range.
[0132] By polymerizing monomers containing aromatic vinyl monomers as the main component in a solvent under the conditions described above, a solution containing aromatic vinyl polymer block chains can be obtained. Furthermore, the aromatic vinyl polymer block chains obtained by polymerization typically have active ends. In addition, the obtained aromatic vinyl polymer block chains, due to the formation of aromatic vinyl polymer blocks (Ar1... a ) or aromatic vinyl polymer blocks (Ar1) b Therefore, the amount of monomer used in this first polymerization step can be determined based on the aromatic vinyl polymer block (Ar1). a ) and aromatic vinyl polymer blocks (Ar1 b The weight-average molecular weight is used to determine this.
[0133] Next, a monomer containing a conjugated diene monomer as the main component is added to the solution containing aromatic vinyl polymer block chains obtained in the first polymerization step, and polymerization is carried out (second polymerization step). This yields a solution containing diblock chains. Furthermore, the diblock chains obtained by polymerization typically have active ends. Moreover, the diblock chains obtained in the second polymerization step are formed from aromatic vinyl polymer blocks (Ar1) obtained in the first polymerization step. a ) or aromatic vinyl polymer blocks (Ar1) b The polymer chain of ) further incorporates conjugated diene polymer blocks (D) to form conjugated diene polymer blocks. a ) or conjugated diene polymer block (D b The monomers used in this second polymerization step are diblock chains formed from the polymer chains of the conjugated diene polymer block (D). a ) and conjugated diene polymer blocks (D b The weight-average molecular weight is determined by the polymerization reaction temperature, polymerization time, and polymerization pressure. Furthermore, the polymerization temperature, polymerization time, and polymerization pressure can be controlled within the same range as the first polymerization step described above.
[0134] Next, a monomer containing an aromatic vinyl monomer as the main component is added to the solution containing diblock chains obtained in the second polymerization step, and polymerization is carried out (third polymerization step). This yields a solution containing triblock chains. Furthermore, the triblock chains obtained through polymerization typically have active ends. Moreover, the triblock chains obtained in the third polymerization step are formed from aromatic vinyl polymer blocks (Ar1) obtained in the second polymerization step. a ) or aromatic vinyl polymer blocks (Ar1) b ) and conjugated diene polymer blocks (D a ) or conjugated diene polymer block (D bThe polymer chain further incorporates aromatic vinyl polymer blocks (Ar2) to form aromatic vinyl polymer blocks. a Part of or aromatic vinyl polymer block (Ar2) b The polymer chain is a triblock chain composed of aromatic vinyl polymer blocks (Ar2). Therefore, the amount of monomer used in this third polymerization step can be determined according to the amount of aromatic vinyl polymer blocks (Ar2). b The weight-average molecular weight is determined by the polymerization reaction temperature, polymerization time, and polymerization pressure. Furthermore, the polymerization temperature, polymerization time, and polymerization pressure can be controlled within the same range as the first polymerization step described above.
[0135] Next, in the solution containing triblock chains obtained in the third polymerization step, a polymerization terminator is added in an amount less than 1 molar equivalent relative to the active ends of the triblock chains (termination step). This deactivates a portion of the active ends of the triblock chains, resulting in a block copolymer with deactivated active ends. This block copolymer has the general formula (B): Ar1 b -D b -Ar2 b The block copolymer B is represented.
[0136] The polymerization terminator is not particularly limited as long as it can react with the active end to deactivate it and does not react with other active ends after reacting with one. From the viewpoint of suppressing the hygroscopicity of the resulting composition, polymerization terminators containing compounds without halogen atoms are preferred, and polymerization terminators that form metal alkoxides, metal aromatic oxides, or metal hydroxides upon reaction with the active end are particularly preferred. Examples of compounds that are particularly preferred as polymerization terminators include water; monohydric alcohols such as methanol and ethanol; and monohydric phenols such as phenol and cresol.
[0137] The amount of polymerization terminator used is determined based on the weight ratio of block copolymer A and block copolymer B constituting the first composition. There is no particular limitation as long as the amount is less than 1 molar equivalent relative to the active end of the triblock chain. Generally, the amount of polymerization terminator relative to the active end is in the range of 0.18 to 0.91 molar equivalents, preferably in the range of 0.35 to 0.80 molar equivalents.
[0138] As described above, when a polymerization terminator is added to a solution containing triblock chains with active ends in an amount less than 1 molar equivalent relative to the active ends, a portion of the active ends of the triblock chains with active ends are deactivated, and the polymer with deactivated active ends becomes block copolymer B. Then, the remaining portion of the triblock chains with active ends that have not reacted with the polymerization terminator remains unreacted in the solution.
[0139] Next, in the solution containing triblock chains and block copolymer B obtained in the termination step, a monomer containing aromatic vinyl monomers as the main component is added, and polymerization is carried out (fourth polymerization step). This yields a solution containing the general formula (A): Ar1 a -D a -Ar2 a The solutions represented are block copolymer A and block copolymer B. Block copolymer A obtained in the fourth polymerization step is formed by further bonding the active ends of the triblock chains obtained in the third step to form aromatic vinyl polymer blocks (Ar2). a The monomers used in this fourth polymerization step are block copolymers formed from a portion of the polymer chain of the aromatic vinyl polymer block (Ar2). a The weight-average molecular weight is determined by the polymerization reaction temperature, polymerization time, and polymerization pressure. Furthermore, the polymerization temperature, polymerization time, and polymerization pressure can be controlled within the same range as the first polymerization step described above.
[0140] After the fourth polymerization step, the polymer components can be recovered from the solution containing block copolymer A and block copolymer B (recovery step). The recovery method is not particularly limited and can be any conventional method. For example, recovery can be carried out by adding polymerization terminators such as water, methanol, ethanol, propanol, hydrochloric acid, and citric acid as needed after the reaction is terminated, and then adding additives such as antioxidants as needed. The solution can then be recovered using known methods such as direct drying or stripping. When recovering the polymer components as a slurry using methods such as stripping, dehydration can be performed using any dehydrator such as an extrusion press to produce granules with a moisture content below a specified value. These granules can then be dried using any dryer such as a belt dryer or an extrusion dryer. The block copolymers obtained as described above can be processed into granules or the like using conventional methods for use.
[0141] As described above, block copolymer A and block copolymer B can be manufactured.
[0142] The block copolymer C is preferably manufactured by polymerizing an aromatic vinyl monomer and a conjugated diene monomer to form a diblock chain, and then coupling the diblock chain with a coupling agent.
[0143] More specifically, the block copolymer C is preferably manufactured by the following method. That is, a manufacturing method having the following steps is preferred:
[0144] In the first polymerization step, monomers containing aromatic vinyl monomers are polymerized in a solvent in the presence of a polymerization initiator, thereby obtaining a solution containing aromatic vinyl polymer block chains.
[0145] In the second polymerization step, a monomer containing a conjugated diene monomer is added to a solution containing aromatic vinyl polymer block chains, and polymerization is carried out to obtain a solution containing diblock chains; and
[0146] In the reaction process, a coupling agent is added to a solution containing diblock chains to obtain block copolymer C.
[0147] In the above-described manufacturing method, firstly, a polymerization initiator is used in a solvent to polymerize a monomer containing an aromatic vinyl monomer as the main component (first polymerization step). The solvent used and its amount, as well as the polymerization initiator and its amount, in the first polymerization step can be the same as in the first polymerization step of the preferred manufacturing method for block copolymer A and block copolymer B described above. Furthermore, a Lewis base compound can be added in the same manner as in the first polymerization step of the preferred manufacturing method for block copolymer A and block copolymer B described above. Moreover, the same polymerization reaction temperature, polymerization time, and polymerization pressure as in the first polymerization step of the preferred manufacturing method for block copolymer A and block copolymer B described above can be used.
[0148] By polymerizing monomers containing aromatic vinyl monomers as the main component in a solvent under the above conditions using a polymerization initiator, a solution containing aromatic vinyl polymer block chains can be obtained. Furthermore, the aromatic vinyl polymer block chains obtained by polymerization typically have active ends. Moreover, the obtained aromatic vinyl polymer block chains form aromatic vinyl polymer blocks (Ar... c The amount of monomer used in this first polymerization step can be determined based on the polymer block chain of aromatic vinyl polymer blocks (Ar). c The weight-average molecular weight is used to determine this.
[0149] Next, a monomer containing a conjugated diene monomer as the main component is added to the solution containing aromatic vinyl polymer block chains obtained in the first polymerization step, and polymerization is carried out (second polymerization step). This yields a solution containing diblock chains. Furthermore, the diblock chains obtained by polymerization typically have active ends. Moreover, the diblock chains obtained in the second polymerization step are formed from aromatic vinyl polymer blocks (Ar) obtained in the first step described above. c The polymer chain of ) further incorporates conjugated diene polymer blocks (D) to form conjugated diene polymer blocks. c The monomers used in this second polymerization step are diblock chains formed from the polymer chains of the conjugated diene polymer block (D). c The weight-average molecular weight is determined by the polymerization reaction temperature, polymerization time, and polymerization pressure. Furthermore, the polymerization temperature, polymerization time, and polymerization pressure can be controlled within the same range as the first polymerization step described above.
[0150] Next, a coupling agent is added to the solution containing diblock chains (reaction step). The active ends of the diblock chains react with the coupling agent, and two or more diblock chains combine via the residual groups of the coupling agent to form a block copolymer C.
[0151] The coupling agent is not particularly limited as long as it has two or more functional groups in one molecule that can react with the active ends of the diblock chain. Preferably, it is a coupling agent with 2 to 8 functional groups in one molecule that can react with the active ends of the diblock chain; more preferably, it is a coupling agent with 2 to 4 functional groups in one molecule that can react with the active ends of the diblock chain. Furthermore, the coupling agent preferably contains silicon atoms, and more preferably, it contains silane halides and alkoxysilanes.
[0152] As coupling agents having two functional groups in one molecule capable of reacting with the active ends of a diblock chain (difunctional coupling agents), examples include: difunctional silane halides such as dichlorosilane, monomethyldichlorosilane, and dimethyldichlorosilane; difunctional alkoxysilanes such as diphenyldimethoxysilane and diphenyldiethoxysilane; difunctional alkyl halides such as dichloroethane, dibromoethane, dichloromethane, and dibromomethane; difunctional tin halides such as tin dichloride, monomethyltin dichloride, dimethyltin dichloride, monoethyltin dichloride, diethyltin dichloride, monobutyltin dichloride, and dibutyltin dichloride; dibromobenzene, benzoic acid, CO, and 2-chloropropene. Among these, difunctional silane halides or difunctional alkoxysilanes are particularly preferred. These difunctional coupling agents can be used alone or in combination of two or more.
[0153] Examples of trifunctional coupling agents (trifunctional coupling agents) are those having three functional groups in one molecule that can react with the active ends of a diblock chain. Examples include trifunctional halogenated alkanes such as trichloroethane and trichloropropane; trifunctional halogenated silanes such as methyltrichlorosilane and ethyltrichlorosilane; and trifunctional alkoxysilanes such as methyltrimethoxysilane, phenyltrimethoxysilane, and phenyltriethoxysilane. These trifunctional coupling agents can be used alone or in combination of two or more.
[0154] Examples of four-functional coupling agents (quadratic coupling agents) that have four functional groups in one molecule capable of reacting with the active ends of a diblock chain include: carbon tetrachloride, carbon tetrabromide, tetrachloroethane, and other four-functional halogenated alkanes; tetrachlorosilane, tetrabromosilane, and other four-functional halogenated silanes; tetramethoxysilane, tetraethoxysilane, and other four-functional alkoxysilanes; and tin tetrachloride, tin tetrabromide, and other four-functional tin halides. These four-functional coupling agents can be used alone or in combination of two or more.
[0155] The value of n in block copolymer C, i.e., the number of branches in block copolymer C, can be adjusted by regulating the type, amount, timing of addition, and amount of Lewis base compound used. Furthermore, the coupling ratio and the number of branches in block copolymer C can be adjusted using reaction terminators such as methanol. Additionally, the number of branches in block copolymer C can also be adjusted by using two or more coupling agents with different numbers of functional groups that react with the active ends of the diblock chains. Furthermore, these methods can be used to ensure that the diblock chains obtained in the second polymerization step remain in an unreacted state and are ultimately recovered as block copolymer D.
[0156] The amount of coupling agent used can be adjusted to an appropriate amount based on the number of branches of the block copolymer C targeted. The amount of coupling agent used is preferably 0.05 to 0.9 molar equivalents, more preferably 0.20 to 0.70 molar equivalents, relative to the active ends of the diblock chains.
[0157] The reaction temperature is preferably 10–150°C, more preferably 30–130°C, and particularly preferably 40–90°C. The reaction time varies depending on the conditions, but is usually within 48 hours, preferably 0.5–10 hours.
[0158] After the reaction process, the polymer components can be recovered from the solution containing block copolymer C and optionally block copolymer D (recovery process). The recovery method is not particularly limited and can be any conventional method. For example, recovery can be performed by adding polymerization terminators such as water, methanol, ethanol, propanol, hydrochloric acid, and citric acid as needed after the reaction is terminated, and then adding additives such as antioxidants as needed. The solution is then recovered using known methods such as direct drying or stripping. When recovering the polymer components as a slurry using methods such as stripping, dehydration can be performed using any dehydrator such as an extrusion press to produce granules with a moisture content below a specified value. These granules are then dried using any dryer such as a belt dryer or an extrusion dryer. The block copolymers obtained as described above can be processed into granules or the like using conventional methods for use.
[0159] As described above, block copolymer C and block copolymer D can be manufactured arbitrarily.
[0160] In addition to containing block copolymers A to C, the first composition of the present invention may also contain a polyolefin thermoplastic resin. A stretchable film can be readily obtained from the first composition containing block copolymers A to C and a polyolefin thermoplastic resin. Furthermore, by laminating the stretchable film and a nonwoven fabric, a stretchable laminate can be obtained, in which case the stretchable film and the nonwoven fabric are firmly bonded. The stretchable laminate can be manufactured, for example, by extruding the composition onto a nonwoven fabric using extrusion molding. As the polyolefin thermoplastic resin used in the present invention, there is no particular limitation on any thermoplastic resin with olefins as the main repeating unit; it can be any of the following: a homopolymer of α-olefins, a copolymer of two or more α-olefins, or a copolymer of α-olefins with monomers other than α-olefins. Furthermore, it can also be a polymer modified from these (co)polymers.
[0161] Specific examples of polyolefin-based thermoplastic resins include: homopolymers or copolymers of α-olefins such as ethylene and propylene, such as linear low-density polyethylene (LLDPE), low-density polyethylene (LDPE), medium-density polyethylene (MDPE), high-density polyethylene (HDPE), metallocene polyethylene, etc.; α-olefin homopolymers such as polypropylene, metallocene polypropylene, polymethylpentene, and polybutene; copolymers of ethylene with other α-olefins, such as ethylene-propylene random copolymers, ethylene-propylene block copolymers, ethylene-butene-1 copolymers, ethylene-propylene-butene-1 copolymers, and ethylene-cyclic olefin copolymers; copolymers of α-olefins as the main component with carboxylic acid unsaturated alcohols and their saponifications, such as ethylene-vinyl acetate. Ester copolymers, ethylene-vinyl alcohol copolymers; copolymers of α-olefins as the main body with α,β-unsaturated carboxylic acid esters or α,β-unsaturated carboxylic acids, such as ethylene-α,β-unsaturated carboxylic acid ester copolymers (ethylene-ethyl acrylate copolymers, ethylene-methyl methacrylate copolymers, etc.), ethylene-α,β-unsaturated carboxylic acid copolymers (ethylene-acrylic acid copolymers, ethylene-methacrylic acid copolymers, etc.); acid-modified olefin resins that modify α-olefin (co)polymers such as polyethylene and polypropylene with unsaturated carboxylic acids such as acrylic acid, methacrylic acid, maleic acid, maleic anhydride, fumaric acid, itaconic acid and / or their anhydrides; ionomer resins that allow copolymers of ethylene and methacrylic acid to react with Na ions, Zn ions, etc.; mixtures of these. Among these, polyethylene or copolymers of ethylene with other α-olefins are preferred, and polyethylene or copolymers of ethylene with other α-olefins manufactured using metallocene catalysts are particularly preferred.
[0162] The weight-average molecular weight of polyolefin thermoplastic resins is not particularly limited, and is generally selected in the range of 10,000 to 5,000,000, preferably in the range of 50,000 to 800,000. Furthermore, the specific gravity and melt flow index of polyolefin thermoplastic resins are not particularly limited, with specific gravity typically ranging from 0.80 to 0.95 g / cm³. 3 The concentration should be selected within the range of 0.85–0.94 g / cm³, preferably between 0.85 and 0.94 g / cm³. 3 The melt index is selected within the range specified in ASTM D-1238 (G conditions, 200°C, 5kg), and is typically selected within the range of 1 to 1000 g / 10 minutes, preferably within the range of 3 to 500 g / 10 minutes.
[0163] The content of the polyolefin thermoplastic resin relative to a total of 100 parts by weight of block copolymers A to C is preferably 3 to 50 parts by weight, more preferably 5 to 40 parts by weight, and even more preferably 8 to 30 parts by weight. Furthermore, the polyolefin thermoplastic resin may be used alone or in combination of two or more types.
[0164] The first composition of the present invention may also contain, as needed, fatty acid amides, polyethylene wax, antioxidants, tackifying resins, softeners, antibacterial agents, light stabilizers, ultraviolet absorbers, dyes, lubricants, etc.
[0165] Aliphatic amides can be either aliphatic monoamides or aliphatic diamides. There are no particular limitations on aliphatic monoamides as long as they are compounds formed by the combination of a hydrocarbon group and one amide group (-NHCO). Monoamides of higher saturated fatty acids with 12 or more carbon atoms (i.e., compounds formed by the combination of a chain alkyl group with 12 or more carbon atoms and one amide group (-NHCO)) are preferred.
[0166] Specific examples of fatty acid monoamides include saturated fatty acid monoamides such as laurylamide, tetradecylamide, palmitamide, stearamide, behenamide, and hydroxystearamide; and unsaturated fatty acid monoamides such as oleamide and erucamide.
[0167] The content of fatty acid amide relative to a total of 100 parts by weight of block copolymers A to C is preferably 0.2 to 10 parts by weight, more preferably 0.3 to 8 parts by weight, and even more preferably 0.5 to 6 parts by weight.
[0168] Polyethylene wax is a wax whose main constituent unit is vinyl monomer units. There are no particular limitations on the polyethylene wax used in this invention, but a polyethylene wax with a viscosity of 20–6000 mPa·s at 140°C is preferred.
[0169] Polyethylene wax is typically manufactured through the polymerization of ethylene or the decomposition of polyethylene, and any type of polyethylene wax can be used in this invention. Furthermore, commercially available polyethylene waxes can be used; specific examples include "AC Polyethylene" (manufactured by Honeywell International Inc.), "Mitsui Hi-WAX" (manufactured by Mitsui Chemicals), "SANWAX" (manufactured by Sanyo Chemical Industries), and "Epolene" (manufactured by Eastman Chemical Company).
[0170] There are no particular limitations on antioxidants, and hindered phenolic compounds such as pentaerythritol tetra[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 2,6-di-tert-butyl-p-cresol, and di-tert-butyl-4-methylphenol can be used; thiodicarboxylic acid esters such as dilauryl thiopropionate; and phosphites such as tris(nonylphenyl) phosphite can be used.
[0171] The content of antioxidant relative to a total of 100 parts by weight of block copolymers A to C is preferably 10 parts by weight or less, more preferably 0.05 to 5 parts by weight.
[0172] The first composition of the present invention preferably further contains a wax comprising linear hydrocarbons and branched hydrocarbons. By containing a wax comprising linear hydrocarbons and branched hydrocarbons, the first composition of the present invention can not only obtain an elastomer with excellent formability, small film thickness variation, and low permanent shrinkage, but also an elastomer with excellent color and low odor, and excellent resistance to ozone cracking.
[0173] The wax used in this invention can be natural wax or synthetic wax, preferably natural wax, and more preferably petroleum wax.
[0174] Alternatively, a compound wax can be used, which is mainly composed of petroleum wax and mixed with a portion of other natural waxes and synthetic waxes. Furthermore, a wax obtained by further compounding a small amount of resin or the like into the wax to improve its function and processability can also be used. In addition, the first composition of the present invention may contain waxes other than those containing linear and branched hydrocarbons, but from the viewpoint of obtaining an elastomer with excellent color, low odor, and excellent ozone crack resistance, it is preferable not to contain other waxes.
[0175] Straight-chain hydrocarbons are preferably straight-chain aliphatic saturated hydrocarbons. Straight-chain hydrocarbons are sometimes referred to as n-chain alkanes. Branched-chain hydrocarbons are preferably branched-chain aliphatic saturated hydrocarbons. Branched-chain hydrocarbons are sometimes referred to as iso-chain alkanes. As straight-chain and branched hydrocarbons, those contained in petroleum waxes are preferred.
[0176] In addition to straight-chain hydrocarbons and branched hydrocarbons, the wax used in this invention may also contain cyclic hydrocarbons. However, the total amount of straight-chain hydrocarbons and branched hydrocarbons in the wax is preferably 50% by mass or more, more preferably 70% by mass or more, further preferably 80% by mass or more, and most preferably 90% by mass or more.
[0177] The weight ratio (normal / iso-) of straight-chain hydrocarbons (positive) and branched-chain hydrocarbons (negative) in the wax is 30 / 70 to 99 / 1, preferably 50 / 50 to 97 / 3, more preferably 70 / 30 to 95 / 5, and most preferably 75 / 25 to 90 / 10. By keeping the weight ratio (normal / iso-) within the above range, an elastomer with excellent ozone crack resistance can be obtained.
[0178] The melting point of the wax is less than 80°C, preferably below 76°C, more preferably below 73°C, preferably above 30°C, more preferably above 40°C, and even more preferably above 45°C. The melting point of the wax can be determined using a differential scanning calorimeter or the like. When the melting point of the wax is too high, it is difficult to obtain an elastomer with excellent ozone crack resistance. When the melting point of the wax is too low, it is prone to sticking during transportation and storage, and it is also prone to melting during processing, resulting in poor handleability.
[0179] The wax content in the first composition of the present invention is preferably 0.1 to 5 parts by weight, more preferably 0.3 to 3.5 parts by weight, and even more preferably 0.5 to 2 parts by weight, relative to 100 parts by weight of the block copolymers in the composition. If the wax content is too high, it may be difficult to obtain an elastomer with low permanent elongation; if the wax content is too low, it may be difficult to obtain an elastomer with excellent ozone resistance. Regarding the weight of the block copolymers in the composition, for example, in the case where the first composition of the present invention contains block copolymers A to C, it refers to the total weight of block copolymers A to C; and in the case where the first composition of the present invention contains block copolymers A to D, it refers to the total weight of block copolymers A to D.
[0180] When obtaining the first composition of the present invention, the method for mixing the block copolymers A to C and other components is not particularly limited. Examples include methods such as dissolving each component in a solvent and uniformly mixing it, then removing the solvent by heating, or melt mixing the components using a screw extruder, kneader, or the like. Among these, melt mixing is preferred from the viewpoint of more efficient mixing. Furthermore, the temperature during melt mixing is not particularly limited, and is typically in the range of 100 to 250°C.
[0181] When block copolymers A to C are melt-mixed with other components, to ensure a more uniform mixing of the other components and block copolymers A to C, it is preferable to pre-mix all or part of one or more components of block copolymers A to C with the other components using a single-spindle extruder, a two-spindle extruder, a Banbury mixer, or the like to produce masterbatch granules. Of the above, a two-spindle extruder is particularly preferred from the viewpoints of mixability, cleanliness, and cost.
[0182] When manufacturing elastomers, by supplying the aforementioned masterbatch particles simultaneously with the block copolymers A to C, and mixing them uniformly, an elastomer with good productivity and highly uniform dispersion of other components in the block copolymers A to C can be obtained.
[0183] One or more of the block copolymers A to C used to make masterbatch particles can be supplied only in the amount required for making masterbatch particles. By adjusting the supply amount of block copolymers A to C and the supply amount of masterbatch particles during the production of elastomer, the composition ratio of the block copolymers A to C described above can be achieved.
[0184] The second composition of the present invention comprises: a block copolymer having at least one aromatic vinyl polymer block and at least one conjugated diene polymer block, and a wax.
[0185] (block copolymer)
[0186] The block copolymer used in the second composition of the present invention has at least one aromatic vinyl polymer block and at least one conjugated diene polymer block. The aromatic vinyl polymer block contains aromatic vinyl monomer units formed from aromatic vinyl monomers, and the conjugated diene polymer block contains conjugated diene monomer units formed from conjugated diene monomers.
[0187] The aromatic vinyl monomers forming the aromatic vinyl monomer units are not particularly limited to any aromatic vinyl compound, and examples include styrene, α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2-ethylstyrene, 3-ethylstyrene, 4-ethylstyrene, 2,4-diisopropylstyrene, 2,4-dimethylstyrene, 4-tert-butylstyrene, 5-tert-butyl-2-methylstyrene, 2-chlorostyrene, 3-chlorostyrene, 4-chlorostyrene, 4-bromostyrene, 2-methyl-4,6-dichlorostyrene, 2,4-dibromostyrene, vinylnaphthalene, etc. Among these, styrene is preferred. These aromatic vinyl monomers can be used alone or in combination of two or more. Furthermore, in the case where the block copolymer has multiple aromatic vinyl polymer blocks, each aromatic vinyl polymer block can be composed of the same aromatic vinyl monomer unit or different aromatic vinyl monomer units.
[0188] Furthermore, aromatic vinyl polymer blocks may also include monomer units other than aromatic vinyl monomer units, provided that the aromatic vinyl monomer unit is the main repeating unit. Examples of monomer units other than aromatic vinyl monomer units that can be included in aromatic vinyl polymer blocks include, for example, conjugated diene monomers such as 1,3-butadiene and isoprene (2-methyl-1,3-butadiene), α,β-unsaturated nitrile monomers, unsaturated carboxylic acid or anhydride monomers, unsaturated carboxylic acid ester monomers, and non-conjugated diene monomers. The content of monomer units other than aromatic vinyl monomer units in the aromatic vinyl polymer block is preferably 20% by mass or less, more preferably 10% by mass or less, and particularly preferably substantially 0% by mass.
[0189] The conjugated diene monomer forming the conjugated diene monomer unit is not particularly limited as long as it is a conjugated diene compound, and examples include 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 2-chloro-1,3-butadiene, 1,3-pentadiene, and 1,3-hexadiene. Among these, 1,3-butadiene and / or isoprene are preferred, and isoprene is particularly preferred. These conjugated diene monomers can be used alone or in combination of two or more. Furthermore, in the case where the block copolymer has multiple conjugated diene polymer blocks, each conjugated diene polymer block can be composed of the same conjugated diene monomer unit or different conjugated diene monomer units. Furthermore, a portion of the unsaturated bonds in the conjugated diene polymer block can be hydrogenated.
[0190] Furthermore, the conjugated diene polymer block may also include monomer units other than the conjugated diene monomer unit, as long as the conjugated diene monomer unit is the main repeating unit. Examples of monomer units other than the conjugated diene monomer unit that can be included in the conjugated diene polymer block include aromatic vinyl monomers such as styrene and α-methylstyrene, α,β-unsaturated nitrile monomers, unsaturated carboxylic acid or anhydride monomers, unsaturated carboxylic acid ester monomers, and non-conjugated diene monomers. The content of monomer units other than the conjugated diene monomer unit in the conjugated diene polymer block is preferably 20% by mass or less, more preferably 10% by mass or less, and particularly preferably substantially 0% by mass.
[0191] The vinyl bond content (the proportion of 1,2-vinyl bond units and 3,4-vinyl bond units in all conjugated diene monomer units in the conjugated diene polymer block) is not particularly limited, but is preferably in the range of 1 to 20 mol%, more preferably in the range of 2 to 15 mol%, and particularly preferably in the range of 3 to 10 mol%.
[0192] If the block copolymer used in the second composition of the present invention is a block copolymer having at least one aromatic vinyl polymer block and one conjugated diene polymer block respectively, the number of each polymer block and their combination form are not particularly limited. Specific examples of the form of the block copolymer used in the second composition of the present invention include: aromatic vinyl-conjugated diene block copolymers represented as Ar-D, aromatic vinyl-conjugated diene-aromatic vinyl block copolymers represented as Ar-D-Ar or (Ar-D)nX, conjugated diene-aromatic vinyl-conjugated diene block copolymers represented as D-Ar-D or (D-Ar)nX, aromatic vinyl-conjugated diene-aromatic vinyl-conjugated diene block copolymers represented as Ar-D-Ar-D, and mixtures of block copolymers formed by mixing two or more of these in any combination, but are not limited to these. In the second composition of the present invention, block copolymers that are particularly preferred include: aromatic vinyl-conjugated diene block copolymers represented as Ar-D and those represented as Ar-D-Ar or (Ar-D). n -X aromatic vinyl-conjugated diene-aromatic vinyl block copolymers, and block copolymers in mixtures thereof.
[0193] Furthermore, it is represented as Ar-D-Ar or (Ar-D) n In the aromatic vinyl-conjugated diene-aromatic vinyl block copolymer of -X, the molecular chain length of each aromatic vinyl block (Ar) can be the same, or it can contain components with different molecular chain lengths.
[0194] The weight-average molecular weight of the block copolymer used in the second composition of the present invention is not particularly limited, but is usually selected in the range of 40,000 to 500,000, and preferably in the range of 50,000 to 400,000.
[0195] The content of aromatic vinyl monomer units in the block copolymer used in the second composition of the present invention is not particularly limited, but is preferably in the range of 5 to 60% by mass, more preferably in the range of 7 to 55% by mass, and even more preferably in the range of 10 to 50% by mass. Furthermore, if the block copolymer is substantially composed only of aromatic vinyl monomer units and conjugated diene monomer units, if the block copolymer is subjected to ozone decomposition according to the method described in Rubber Chem. Technol., 45, 1295 (1972), followed by reduction with lithium aluminum hydride, the conjugated diene monomer unit portion can be decomposed, and the aromatic monovinyl monomer unit portion can be removed. Therefore, the content of aromatic vinyl monomer units can be determined by such a method.
[0196] Block copolymers having aromatic vinyl polymer blocks and conjugated diene polymer blocks as described above can be manufactured by conventional methods. One of the most common manufacturing methods is to form polymer blocks by stepwise polymerization of aromatic vinyl monomers and conjugated diene monomers using anionic living polymerization, and then couple them with a coupling agent as needed. Alternatively, a method can be used to form polymer blocks by stepwise polymerization of aromatic vinyl monomers, conjugated diene monomers, and then aromatic vinyl monomers.
[0197] Furthermore, the block copolymer used in the second composition of the present invention can also be a commercially available block copolymer, such as Quintac (registered trademark) (manufactured by Zeon Corporation of Japan), JSR-SIS (registered trademark) (manufactured by JSR Corporation), Vector (registered trademark) (manufactured by DEXCO polymers), Asaprene (registered trademark), Tufprene (registered trademark), Tuftec (registered trademark) (manufactured by Asahi Kasei Chemicals Corporation), SEPTON (registered trademark) (manufactured by KURARAY CO.,LTD.), etc.
[0198] The block copolymer used in the second composition of the present invention is particularly preferably a composition containing the aforementioned block copolymers A to D, which are also used in the first composition of the present invention. By using a composition containing block copolymers A to D as the block copolymer, the second composition of the present invention can not only produce an elastomer with excellent color and low odor, and excellent ozone crack resistance, but also an elastomer with excellent formability, small film thickness variation, and low permanent elongation.
[0199] (wax)
[0200] The wax used in the second composition of the present invention contains both straight-chain hydrocarbons and branched-chain hydrocarbons. By containing a wax comprising both straight-chain and branched-chain hydrocarbons, the second composition of the present invention can yield an elastomer with excellent color and low odor, and excellent resistance to ozone cracking.
[0201] The wax used in the second composition of the present invention can be any wax that has been described in detail as the wax used in the first composition of the present invention.
[0202] The wax content in the second composition of the present invention is preferably 0.1 to 5 parts by weight, more preferably 0.3 to 3.5 parts by weight, and even more preferably 0.5 to 2 parts by weight, relative to 100 parts by weight of the block copolymer. If the wax content is too high, it may be difficult to obtain an elastomer with low permanent elongation; if the wax content is too low, it may be difficult to obtain an elastomer with excellent ozone resistance.
[0203] When obtaining the second composition of the present invention, the method for mixing the block copolymer and other components such as wax is not particularly limited. Examples include methods such as dissolving each component in a solvent, uniformly mixing them, and then removing the solvent by heating, or melt mixing each component using a screw extruder, kneader, or the like. Among these, melt mixing is preferred from the viewpoint of more efficient mixing. Furthermore, the temperature during melt mixing is not particularly limited, and is generally in the range of 100 to 250°C.
[0204] When melt-mixing block copolymers and other components such as waxes, it is preferable to pre-mix a portion of the block copolymer with the other components using a single-spindle extruder, a two-spindle extruder, a Banbury mixer, or the like to produce masterbatch granules in order to achieve a more uniform mixture between the other components and the block copolymer. Of the above, a two-spindle extruder is particularly preferred from the viewpoints of mixability, cleanliness, and cost.
[0205] When manufacturing elastomers, the aforementioned masterbatch particles are supplied simultaneously with the block copolymer and mixed uniformly, thereby obtaining an elastomer with good productivity and highly uniform dispersion of other components in the block copolymer.
[0206] The second composition of the present invention may further contain the above-mentioned polyolefin thermoplastic resin. Furthermore, the second composition of the present invention may, as needed, contain fatty acid amides, antioxidants, tackifying resins, softeners, antibacterial agents, light stabilizers, ultraviolet absorbers, dyes, lubricants, etc.
[0207] The first composition of the present invention can produce an elastomer with excellent formability, small film thickness variation, and low permanent elongation. Therefore, the first composition of the present invention is preferably used in elastomers, and particularly preferably in elastomers for sanitary materials. Furthermore, it is preferably used in the following applications.
[0208] The second composition of the present invention can produce an elastomer with excellent color and low odor, and excellent resistance to ozone cracking. Therefore, the second composition of the present invention is preferably used in elastomers, and particularly preferably in elastomers for sanitary materials. Furthermore, it is preferably used in the following applications.
[0209] The first and second compositions and the elastomer of the present invention can be used as molding materials for, for example, films, threads (elastic ropes), gloves, elastic bands, condoms, office automation equipment, various rolls for office use, shock absorbers, shock-absorbing rubber, shock-absorbing sheets, shock-absorbing films / sheets, residential shock absorbers, shock absorber materials, etc.; adhesives for adhesive tapes, adhesive sheets, adhesive labels, dust removal rollers, etc.; adhesives for hygiene products and binding; and elastic fibers for clothing, sporting goods, etc.
[0210] The first and second compositions and the elastomer of the present invention are preferably used in membranes, and particularly preferably in elastic membranes for sanitary materials. The elastomer and membrane of the present invention are obtained from the first and second compositions of the present invention, and are therefore strong and highly elastic, with minimal thickness variation and low permanent elongation. Furthermore, the first and second compositions and the elastomer of the present invention are also preferably used as threads (elastic ropes).
[0211] The thickness of the film of the present invention is not particularly limited and can be adjusted according to the application. When used as a film for hygiene products such as diapers and sanitary products, it is usually 0.01 to 5 mm, preferably 0.01 to 1 mm, and more preferably 0.02 to 0.2 mm.
[0212] The method for forming the first and second compositions of the present invention into a film is not particularly limited, and conventionally known film forming methods can be used. From the viewpoint of obtaining a smooth film with good productivity, extrusion molding is preferred, and extrusion molding using a T-die is particularly preferred.
[0213] As a specific example of extrusion molding using a T-die, the following method can be cited: A composition molten at 150–250°C is extruded from a T-die installed in a single-spindle or dual-spindle extruder, and then wound up while being cooled with traction rollers. The film can be stretched while being cooled with the traction rollers. Furthermore, when winding the film, it can be formed by coating the molten composition onto a substrate made of polyethylene terephthalate, polyethylene, polypropylene, nonwoven fabric, or release paper, or by clamping the molten composition between these substrates. The resulting film can be used integrally with the substrate or peeled off from the substrate.
[0214] The elastomer and membrane of the present invention exhibit excellent uniformity in film thickness.
[0215] The excellent uniformity of the film thickness of the elastomer and film of the present invention can be confirmed, for example, by cutting a 30 cm length of film as a sample along the melt flow direction during molding. At the center of the film, the film thickness is measured at 15 points every 2 cm along the melt flow direction using a digital thickness gauge (manufactured by Toyo Seiki Co., Ltd., measurement accuracy: 0.001 mm unit). The ratio of the standard deviation of the film thickness to the average value of the film thickness (standard deviation / average value) obtained from these measurements is usually 30% or less, preferably 20% or less.
[0216] The permanent elongation of the elastomer and membrane of the present invention is typically 5% or less, preferably 2% or less. The permanent elongation of the membrane can be determined by the method described in the examples.
[0217] The elastomer and membrane of the present invention can be used directly as a single layer or laminated with other components as a multilayer, depending on their intended use. Specific examples of using a single layer include: stretchable films for hygiene products such as diapers and sanitary products; protective films for protecting optical films; and heat-shrinkable films for shrink packaging of containers and heat-shrinkable labels. Specific examples of forming a multilayer include: after slitting the membrane of the present invention, applying a hot melt adhesive or the like to it to form a tape; and then bonding this tape to a nonwoven fabric, woven fabric, plastic film, or a laminate thereof in a shrunken state to reduce tape shrinkage, thereby forming a stretchable aggregated component. Furthermore, depending on other uses, it can be appropriately processed according to known methods and used as, for example, a stretchable wet dressing substrate, gloves, surgical gloves, finger cots, tourniquets, contraceptives, headbands, goggle straps, elastic bands, and other stretchable components.
[0218] Example
[0219] The present invention will now be specifically described with reference to examples and comparative examples. Unless otherwise specified, "parts" refers to weight. Furthermore, the tests and evaluations were conducted as follows.
[0220] [Weight-average molecular weight of each block copolymer]
[0221] High-performance liquid chromatography (HPLC) with tetrahydrofuran at a flow rate of 0.35 mL / min was used to determine the weight-average molecular weight of polystyrene. The apparatus was a TOSOH CORPORATION HLC 8320, and the column consisted of three Shodex KF-404HQ columns (40°C). Differential refractometers and ultraviolet detectors were used. Molecular weight calibration was performed using 12 points of standard styrene (5 million to 3 million) from TOSOH CORPORATION.
[0222] [Weight ratio of each block copolymer in the block copolymer mixture]
[0223] The peak area ratio corresponding to each block copolymer is determined based on the graph obtained by the above high performance liquid chromatography.
[0224] [Weight-average molecular weight of the styrene polymer blocks in each block copolymer]
[0225] The block copolymer was reacted with ozone and reduced with lithium aluminum hydride according to the method described in Rubber Chem. Technol., 45, 1295 (1972), thereby decomposing the isoprene polymer blocks of the block copolymer. Specifically, the following steps were performed: 300 mg of the sample was dissolved in a reaction vessel containing 100 ml of dichloromethane treated with molecular sieves. The reaction vessel was placed in a cooling bath at -25°C, and ozone generated by an ozone generator was introduced into the reaction vessel while oxygen was flowing in at a flow rate of 170 ml / min. After 30 minutes from the start of the reaction, the reaction was confirmed to be complete by introducing the gas flowing out of the reaction vessel into an aqueous solution of potassium iodide. Next, in another reaction vessel that had been nitrogen-replaced, 50 ml of diethyl ether and 470 mg of lithium aluminum hydride were added, and the reaction vessel was cooled with ice water while the solution that had reacted with ozone was slowly added dropwise. Then, the reaction vessel was placed in a water bath and the temperature was slowly increased, refluxed at 40°C for 30 minutes. Then, while stirring the solution, dilute hydrochloric acid was added dropwise to the reaction vessel in small amounts until hydrogen production was almost imperceptible. After the reaction, the solid product formed in the solution was filtered, and the solid product was extracted with 100 ml of diethyl ether for 10 minutes. The extract was combined with the filtrate from filtration, and the solvent was distilled off to obtain a solid sample. The weight-average molecular weight of the sample thus obtained was determined according to the above-described method for determining weight-average molecular weight, and this value was taken as the weight-average molecular weight of the styrene polymer block.
[0226] [Weight-average molecular weight of the isoprene polymer blocks in each block copolymer]
[0227] The weight-average molecular weight of the isoprene polymer block is calculated by subtracting the weight-average molecular weight of the corresponding styrene polymer block from the weight-average molecular weight of the block copolymer obtained in the manner described above.
[0228] [Vinyl bond content of isoprene polymer blocks in each block copolymer]
[0229] Determined based on HNMR measurements.
[0230] [Styrene unit content of each block copolymer]
[0231] The detection intensity ratio of the differential refractometer and the ultraviolet detector in the above-described high-performance liquid chromatography determination was determined. Additionally, copolymers with different styrene unit contents were prepared in advance, and standard curves were constructed using these copolymers.
[0232] [Film thickness uniformity (film thickness variation)]
[0233] A 30cm length of film was cut along the melt flow direction during molding. Using a digital thickness gauge (Toyo Seiki Co., Ltd., measurement accuracy: 0.001mm), the film thickness was measured at 15 points every 2cm along the melt flow direction at the center of the film. The average and standard deviation of these measurements were obtained. The ratio of the standard deviation of the film thickness to the average film thickness (standard deviation / average value) was calculated and evaluated using the following criteria. A smaller ratio indicates higher uniformity of film thickness, and consequently, better moldability of the composition used for molding.
[0234] 〇: 20% or less
[0235] △: More than 20% but less than 30%
[0236] ×: More than 30%
[0237] [Permanent elongation of the membrane]
[0238] The tests were performed according to ASTM 412 using a Tensilon RTC-1210 universal testing machine manufactured by ORIENTEC. Specifically, the sample shape was a Die A, with the mark spacing before stretching set to 40 mm and the film stretched to 200% elongation. After holding this state for 10 minutes, the film was suddenly contracted without springback. After resting for 10 minutes, the mark spacing was measured, and the permanent elongation was calculated based on the following formula.
[0239] Permanent elongation (%) = (L1 - L0) / L0 × 100
[0240] L0: Marking spacing before stretching (mm)
[0241] L1: Marking spacing (mm) after shrinking and leaving it for 10 minutes.
[0242] It should be noted that in this measurement, two films are used. One film is measured along the direction of melt flow during molding (MD), and the other film is measured along the direction perpendicular to the direction of melt flow during molding (CD). The following criteria are used for evaluation.
[0243] Permanent elongation in the melt flow direction (MD)
[0244] 〇: 2% or less
[0245] △: More than 2% but less than 5%
[0246] ×: More than 5%
[0247] Permanent elongation in the direction perpendicular to melt flow (CD)
[0248] 〇: 2% or less
[0249] △: More than 2% but less than 5%
[0250] ×: More than 5%
[0251] [Membrane resistance to ozone cracking]
[0252] The membrane was secured to a tension holder with a chuck spacing of 4.0 cm. The chuck spacing was then stretched to 5.0 cm, and the membrane was secured at 25% elongation. The secured membrane was placed in a thermostat at 30°C, 50% RH, and an ozone concentration of 5 pphm, and the time until cracks were visually identifiable was measured. Evaluation was performed using the following criteria.
[0253] 〇: No cracks appeared even after more than 2 hours.
[0254] ×: Cracks will appear within 2 hours.
[0255] [Film Color]
[0256] The Gardner colorimetry of the membrane was determined according to JIS K0071-2, and evaluated using the following criteria.
[0257] 〇: Gardner chromaticity less than 2
[0258] ×: Gardner color intensity is 2 or higher
[0259] [Membranous odor]
[0260] Sensory tests were conducted on the membrane according to the odor intensity display method in the odor measurement method published by the Japan Odor Countermeasures Research Association.
[0261] Specifically, firstly, a 100mm × 300mm membrane was placed in a 120mL heat-resistant container and covered with aluminum foil. Then, the heat-resistant container containing the membrane was placed in an oven and heated at 140℃ for 20 minutes to confirm the odor after heating. Odor confirmation was conducted by a six-member committee. In this experiment, to prevent olfactory fatigue, the six-member committee was divided into two groups of three, with one group smelling the odor at a time. Furthermore, the order in which the odor samples were smelled was randomized.
[0262] 0: Tasteless
[0263] 1: A barely discernible odor (detection threshold concentration)
[0264] 2: Identify a faint odor with a certain smell (identification threshold concentration).
[0265] 3: An easily detectable odor
[0266] 4: Strong odor
[0267] 5: Strong odor
[0268] In addition, the results of the sensory tests were obtained by removing the maximum and minimum values from the six-person committee's judgments and averaging the remaining four judgments, and were evaluated using the following criteria.
[0269] 〇: Sensory test score less than 3 points
[0270] ×: Sensory test score of 3 or above
[0271] [Manufacturing Example 1]
[0272] 23.3 kg of cyclohexane, 1.4 mmol of N,N,N',N'-tetramethylethylenediamine (TMEDA), and 1.04 kg of styrene were added to a pressure reactor. While stirring at 40°C, 92.9 mmol of n-butyllithium was added, and polymerization continued for 1 hour while the temperature was increased to 50°C. The polymerization conversion rate of styrene was 100%. Next, while maintaining the temperature at 50–60°C, 5.66 kg of isoprene was continuously added to the reactor over 1 hour. After the addition of isoprene, polymerization continued for another hour. The polymerization conversion rate of isoprene was 100%. Then, while continuing to maintain the temperature at 50–60°C, 1.04 kg of styrene was continuously added over 1 hour. After the addition of styrene, polymerization continued for another hour, forming triblock chains with active ends. The polymerization conversion rate of styrene was 100%. Next, 63.4 mmol of methanol was added as a polymerization terminator, and the mixture was stirred to deactivate some of the active ends of the triblock chains, forming a styrene-isoprene-styrene triblock copolymer B1. Then, while maintaining a temperature of 50–60°C, 0.98 kg of styrene was continuously added over 1 hour. After the addition of styrene was complete, polymerization continued for another hour to form triblock chains with active ends. The polymerization conversion rate of styrene was 100%. Finally, 63.4 mmol of methanol was added as a polymerization terminator, and the mixture was stirred to deactivate all the active ends of the triblock chains, forming a styrene-isoprene-styrene triblock copolymer A1. A portion of the resulting reaction solution was taken out, and the block copolymers were evaluated according to the above-described assay method. The results are shown in Table 2.
[0273] In 100 parts of the reaction solution obtained as described above (containing 30 parts of polymer components), 0.3 parts of 2,6-di-tert-butyl-p-cresol were added as an antioxidant and mixed. The mixture was then added dropwise in small amounts to warm water heated to 85–95°C to allow the solvent to evaporate, resulting in a precipitate. The precipitate was pulverized and dried with hot air at 85°C to recover the mixture containing block copolymer A1 and block copolymer B1.
[0274] The weight ratio of block copolymer A1 and block copolymer B1 in the above mixture (block copolymer A1 / block copolymer B1) is 40 / 60.
[0275] [Manufacturing Examples 2-4]
[0276] The amounts of raw materials such as styrene and isoprene were changed as shown in Table 1. Otherwise, the process was the same as in Manufacturing Example 1, and reaction solutions and mixtures were obtained. The evaluation results are shown in Table 2.
[0277] [Table 1]
[0278] Table 1
[0279]
[0280] [Table 2]
[0281] Table 2
[0282]
[0283] [Manufacturing Example 5]
[0284] 23.2 kg of cyclohexane, 1.5 mmol of N,N,N',N'-tetramethylethylenediamine (TMEDA), and 1.20 kg of styrene were added to a pressure reactor. While stirring at 40°C, 101.7 mmol of n-butyllithium was added, and polymerization continued for 1 hour while the temperature was increased to 50°C. The polymerization conversion rate of styrene was 100%. Next, while maintaining the temperature at 50–60°C, 6.53 kg of isoprene was continuously added to the reactor over 1 hour. After the addition of isoprene, polymerization continued for another hour to form diblock chains with active ends. The polymerization conversion rate of isoprene was 100%. Then, 25.4 mmol of dimethyldichlorosilane and 9.7 mmol of tetramethoxysilane were added as coupling agents, and a coupling reaction was carried out for 2 hours to form a styrene-isoprene coupling block copolymer C1. Then, 203 mmol of methanol was added as a polymerization terminator, and the mixture was stirred to deactivate all the active ends of the diblock chains, forming a styrene-isoprene diblock copolymer D1. A portion of the resulting reaction solution was taken out, and the block copolymer was evaluated according to the above-described assay method. The results are shown in Table 4.
[0285] Add 0.3 parts of 2,6-di-tert-butyl-p-cresol as an antioxidant to 100 parts of the reaction solution obtained as described above, mix, and add the mixture dropwise in small amounts to warm water heated to 85-95°C each time to allow the solvent to evaporate, obtaining a precipitate. Crush the precipitate and dry it with hot air at 85°C, thereby recovering the mixture containing block copolymer C1 and block copolymer D1.
[0286] The weight ratio of block copolymer C1 and block copolymer D1 in the above mixture (block copolymer C1 / block copolymer D1) is 90 / 10.
[0287] [Manufacturing Examples 6-7]
[0288] The amounts of raw materials such as styrene and isoprene were changed as shown in Table 3. Otherwise, the process was carried out in the same manner as in Manufacturing Example 4, and reaction solutions and mixtures were obtained. The evaluation results are shown in Table 4.
[0289] [Table 3]
[0290] Table 3
[0291]
[0292] [Table 4]
[0293] Table 4
[0294] Manufacturing Example 5 Manufacturing Example 6 Manufacturing Example 7 Block copolymer C C1 C2 C3 The proportion (by weight) of branches with n=2 56 100 100 The proportion (by weight) of branches with n=3 22 0 0 The proportion (by weight) of branches with n=4 22 0 0 <![CDATA[Weight-average molecular weight (×10 3 )]]> 250 190 158 <![CDATA[Ar c Weight-average molecular weight (×10) 3 )]]> 9 16 15 <![CDATA[D c Vinyl bond content (mol%) 7 7 7 <![CDATA[D c Weight-average molecular weight (×10) 3 )]]> 105 80 64 Styrene unit content (wt%) 14 24 25 Block copolymer D D1 D2 D3 <![CDATA[Weight-average molecular weight (×10 3 )]]> 112 95 79 <![CDATA[Ar d Weight-average molecular weight (×10) 3 )]]> 9 16 15 <![CDATA[D a Vinyl bond content (mol%) 7 7 7 <![CDATA[D d Weight-average molecular weight (×10) 3 )]]> 105 80 64 Styrene unit content (wt%) 14 24 25 weight ratio C / D 90 / 10 32 / 68 82 / 18
[0295] [Example 1]
[0296] The mixture obtained in Manufacturing Example 1 and the mixture obtained in Manufacturing Example 5 were mixed in the weight ratios of the block copolymers listed in Table 5 to prepare a composition. The resulting composition was fed into a biaxial extruder equipped with a T-die. Then, within the biaxial extruder, the mixture was heated and melted at 200°C, kneaded, and extruded into a PET release film for 20 consecutive minutes, thereby forming a film with an average thickness of 0.05 mm. The film thickness variation and permanent elongation of the film of Example 1 thus obtained were measured. The results are shown in Table 5. Details of the film forming conditions are described below.
[0297] (Membrane forming conditions)
[0298] Complex processing rate: 5 kg / hour
[0299] Membrane traction speed: 4 m / min
[0300] Extruder temperature: Adjust to 100℃ at the feed inlet and 200℃ at the T-die.
[0301] Screw: Full flight
[0302] Extruder L / D: 30
[0303] T-die head: 200mm wide, 0.5mm die lip
[0304] [Examples 2-3, Comparative Examples 1-4]
[0305] The weight ratios of the block copolymers were changed to those shown in Table 5, and the process was otherwise identical to that in Example 1 to obtain the compositions and films, which were then evaluated in the same manner. The results are shown in Table 5.
[0306] [Table 5]
[0307] Table 5
[0308]
[0309] As shown in Table 5, by using three block copolymers with different structures in combination and by appropriately adjusting the weight-average molecular weight of each block and the content of aromatic vinyl monomer units in each block copolymer, a composition with excellent formability can be obtained, and a film with small film thickness variation and low permanent elongation can be obtained (Examples 1-3).
[0310] On the other hand, even when three block copolymers with different structures are used in combination, when the block copolymer contains too much aromatic vinyl monomer unit, the moldability of the composition is not sufficient, the film thickness of the resulting film varies greatly, and the permanent elongation is also large (Comparative Examples 1-4).
[0311] [Example 4]
[0312] 100 parts of the composition prepared in Example 1 and 3 parts of the additives added as described in Table 7 were fed into a biaxial extruder equipped with a T-die. Then, within the biaxial extruder, they were heated and melted at 200°C, kneaded, and extruded into a PET release film for 20 consecutive minutes, thereby forming a film with an average thickness of 0.05 mm. The film thickness variation and permanent elongation of the film thus obtained in Example 4 were measured. The results are shown in Table 8. Details of the film forming conditions are described below. Furthermore, the weight ratios (normal / irregular) and melting points of the additives shown in Table 7 are shown in Table 6.
[0313] (Membrane forming conditions)
[0314] Additive processing speed: 5 kg / hour
[0315] Membrane traction speed: 4 m / min
[0316] Extruder temperature: Adjust to 100℃ at the feed inlet and 200℃ at the T-die.
[0317] Screw: Full range
[0318] Extruder L / D: 30
[0319] T-die head: 200mm wide, 0.5mm die lip
[0320] [Examples 5-14]
[0321] The types and amounts of additives were changed as shown in Table 8, but otherwise the procedure was the same as in Example 4, and the resulting membrane was evaluated in the same manner. The results are shown in Table 8.
[0322] [Refer to Examples 5-11]
[0323] The types and amounts of additives were changed as shown in Table 9, but otherwise the procedure was the same as in Example 4, and the resulting membrane was evaluated in the same manner. The results are shown in Table 9.
[0324] [Table 6]
[0325] Table 6
[0326]
[0327] [Table 7]
[0328]
[0329] [Table 8]
[0330]
[0331] [Table 9]
[0332] Table 9
[0333]
[0334] As shown in Table 8, when a wax containing linear hydrocarbons and branched hydrocarbons with a low melting point is added to the block copolymer in a specific weight ratio, a composition with excellent color and low odor can be obtained, and an elastomer with excellent ozone crack resistance can be obtained (Examples 4-14).
[0335] On the other hand, as shown in Table 9, when a wax with a high melting point is added, an elastomer with excellent ozone crack resistance cannot be obtained (see Example 5).
[0336] Furthermore, as shown in Table 9, even when using waxes with high melting points and without containing straight-chain and branched hydrocarbons in appropriate weight ratios, elastomers with excellent ozone crack resistance could not be obtained (see Examples 6-8).
[0337] Furthermore, as shown in Table 9, an elastomer with excellent ozone crack resistance could not be obtained when using waxes that did not contain straight-chain hydrocarbons and branched-chain hydrocarbons in an appropriate weight ratio (see Example 11).
[0338] Furthermore, as shown in Table 9, when additives other than wax were used, the resulting compositions had poor color and a strong odor (see Examples 9-10).
Claims
1. A composition comprising: a block copolymer having at least one aromatic vinyl polymer block and at least one conjugated diene polymer block, and a wax, The content of aromatic vinyl monomer units in the block copolymer is 5-55% by mass. The wax contains straight-chain hydrocarbons and branched-chain hydrocarbons, and the weight ratio of straight-chain hydrocarbons to branched-chain hydrocarbons is 50 / 50 to 99 / 1. The combined amount of the straight-chain hydrocarbons and the branched-chain hydrocarbons in the wax is 50% or more by mass. The melting point of the wax is less than 80°C. The wax content in the composition is 0.1 to 5 parts by weight relative to 100 parts by weight of the block copolymer.
2. The composition according to claim 1, wherein, The vinyl bond content of the conjugated diene polymer block is in the range of 1 to 20 mol%.
3. The composition according to claim 1 or 2, wherein, The block copolymer has a weight-average molecular weight of 40,000 to 500,000.
4. The composition according to claim 1 or 2, wherein, In the case where Ar represents an aromatic vinyl polymer block, D represents a conjugated diene polymer block, X represents a residual group of the coupling agent, and n represents an integer greater than 2,... The block copolymer is selected from aromatic vinyl-conjugated diene block copolymers represented as Ar-D and aromatic vinyl-conjugated diene-aromatic vinyl block copolymers represented as Ar-D-Ar or (Ar-D)nX, and mixtures thereof.
5. The composition according to claim 4, wherein, The block copolymer comprises an aromatic vinyl-conjugated diene-aromatic vinyl block copolymer represented as Ar-D-Ar or (Ar-D)nX.
6. The composition according to claim 5, wherein, The block copolymer also includes an aromatic vinyl-conjugated diene block copolymer denoted as Ar-D.
7. An elastomer obtained from the composition of any one of claims 1 to 6.
8. The elastomer according to claim 7, wherein it is an elastomer for sanitary materials.
9. The elastomer according to claim 7 or 8, wherein it is a film or a thread.
Citation Information
Patent Citations
Block copolymer composition and film
JP2016069565A
Block copolymer composition
JP2005139326A