Board level packaging method
By employing physical vapor deposition and slot coating processes in board-level packaging, the challenge of fabricating ultra-fine circuits on organic substrates has been solved, enabling finer circuit fabrication and lower production costs, making it suitable for high-density and miniaturized packaging needs.
Patent Information
- Application Number
- CN202310137908.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-20
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-02-20
AI Technical Summary
Existing board-level packaging methods cannot meet the requirements for fabricating ultra-fine circuits based on organic substrates, and they also have problems such as high chemical consumption and environmental pollution.
A physical vapor deposition process was used to form a metal seed layer. Combined with slot coating and conveyor immersion development, a redistribution layer was formed by photolithography and electroplating. Finally, a solder resist layer was formed and solder balls were implanted. This optimized the substrate preparation process and the preparation of the metal seed layer.
It enables more precise circuit fabrication, reduces the amount of chemicals used, lowers production costs, and improves production efficiency, making it suitable for high-density and miniaturized packaging needs.
Smart Images

Figure CN116469832B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor manufacturing technology, specifically to back-end packaging, and particularly to a board-level packaging method. Background Technology
[0002] With the application of heterogeneous integration technology in electronic packaging, high-end substrates are being driven towards miniaturization and integration, giving rise to a series of emerging technologies and products in the substrate field, such as embedded chip boards (eSiP), FC-BGA boards, POP packaging modules based on embedded chips, and PLP (Panel Level Package) modules based on embedded chips and RDL (Rewiring Layer). Currently, embedded chip boards have completed the development of related technologies and products and have entered the mass production stage. PLP modules based on embedded chips and RDL, which form a higher-density interconnect layer at the panel scale through RDL material layering on the basis of embedded chips, and complete surface packaging and dicing to form a fan-out heterogeneous integration module exceeding Moore's Law, have higher product added value.
[0003] To realize PLP modules based on embedded chips and RDLs, the fabrication of RDLs is essential. More importantly, PLP modules based on embedded chips and RDLs are assembled on a substrate, which requires high density and miniaturization. The technological capabilities of existing products, especially in the fabrication of ultra-fine lines, need further improvement. To reduce the cost of fan-out packaging and further expand its applications, the industry focuses on L / S (Line / Space) ratios between 1 / 1μm and 8 / 8μm for FOPLP (Fan-out Board-level Packaging). This represents a technological gap between upstream board manufacturers and downstream OSAT (Outer OSAT) manufacturers. Compared to silicon-based FOWLP (Fan-out Wafer-level Packaging) moving towards the board level, FOPLP based on organic substrates has a natural panel-level infrastructure and lower costs across the board, giving it a higher market prospect.
[0004] In the industry, the substrate for FOPLP (Follicular Unit Packaging) is generally made of materials such as the EMC molding layer for embedded chips, while the pattern transfer material used to fabricate fine circuits is a thin dry film. The manufacturing process is generally as follows: seed layer formation → vacuum lamination → exposure → development → electroplating → film removal → etching of the seed layer, thereby forming the desired circuitry. However, the inventors discovered through extensive experiments that when this process is applied to eSiP organic substrate packaging based on embedded chips, it is impossible to achieve ultra-fine circuitry due to the lack of very thin dry films (≤15μm) with performance sufficient to meet the requirements for fabricating fine circuitry below 8 / 8μm. This makes it difficult to meet the requirements for high-density and miniaturized packaging. Furthermore, existing board-level packaging methods also suffer from problems such as high chemical consumption and environmental pollution.
[0005] It should be noted that the above introduction to the technical background is only for the purpose of providing a clear and complete explanation of the technical solutions of this application and facilitating understanding by those skilled in the art. It should not be assumed that these technical solutions are known to those skilled in the art simply because they have been described in the background section of this application. Summary of the Invention
[0006] In view of the shortcomings of the prior art described above, the purpose of this invention is to provide a board-level packaging method to solve the problems of existing board-level packaging methods that can only meet the packaging requirements of FOPLP carrier boards based on materials such as embedded chip EMC molding layers, but cannot meet the requirements of ultra-fine circuit fabrication in board-level packaging based on organic carrier boards, as well as the problems of environmental pollution.
[0007] To achieve the above and other related objectives, the present invention provides a board-level packaging method, comprising the following steps:
[0008] S1: Prepare a substrate, in which a chip is embedded;
[0009] S2: A metal seed layer is formed on the substrate surface using physical vapor deposition, and then electrically connected to the chip through holes;
[0010] S3: A resist layer is coated on the metal seed layer using a slot coating process and then photolithography is performed.
[0011] S4: The photoresist layer after photolithography is developed using a conveyor-type immersion development process to define the redistribution layer pattern in the photoresist layer.
[0012] S5: A metal body layer is formed on a patterned resist layer using an electroplating process, wherein the metal body layer is electrically connected to the metal seed layer;
[0013] S6: Etch the metal seed layer according to the patterned resist layer to form a redistribution layer, and remove the residual resist layer;
[0014] S7: A solder mask layer is formed on the redistribution layer and solder balls electrically connected to the redistribution layer are implanted.
[0015] Optionally, the substrate includes an organic carrier plate, and the substrate preparation process includes the following steps: providing an organic carrier plate, forming a pattern on the organic carrier plate, laser cutting out a through groove for embedding the chip, applying adhesive tape to the bottom, embedding the chip, laminating molding material to fill the space around the chip, flipping the organic carrier plate and removing the adhesive tape, placing the active side of the chip facing upwards, coating or vacuum-pressing a dielectric layer, and forming a hole in the dielectric layer.
[0016] Alternatively, the molding material used is ABF material, the dielectric layer used is a photosensitive dielectric layer, and the method for forming holes in the dielectric layer is photolithography.
[0017] Optionally, the metal seed layer includes an adhesion layer located on the surface of the substrate and a metal seed layer located on the surface of the adhesion layer.
[0018] Alternatively, the adhesion layer includes a titanium layer and / or a titanium nitride layer, and the metal seed layer includes a copper layer; the thickness of the adhesion layer is 50nm-100nm, and the thickness of the copper layer is 100nm-500nm.
[0019] Optionally, the etching method in step S6 includes wet flash etching of the copper layer and wet flash etching or dry etching of the adhesion layer.
[0020] Alternatively, the wet flash etching method for the copper seed layer can be a method of etching with hydrogen peroxide and acid, the wet flash etching method for the titanium adhesion layer can be a method of etching with HF or NaOH+H2O2 and their alkaline mixtures, and the dry etching method for the titanium adhesion layer can be a method of etching with plasma or active ions including argon.
[0021] Optionally, the photolithography in step S3 is LDI photolithography using I-line.
[0022] Optionally, step S7 includes first preparing a solder resist layer using any one of the following methods: lamination, roller coating, and screen printing; then, after exposure, development, and post-curing, opening a window in the solder resist layer at the location where solder balls need to be implanted; and finally, implanting solder balls at the opening.
[0023] Optionally, the board-level packaging method includes repeating steps S2 to S6 several times to form two or more stacked and electrically connected rewiring layers.
[0024] As described above, the board-level packaging method of the present invention has the following beneficial effects: the improved process design of the present invention can produce finer circuitry and achieve thinner packages. It also helps to reduce the amount of chemicals used and wastewater generation. Furthermore, it helps to improve production efficiency and reduce packaging costs. Attached Figure Description
[0025] Figure 1 The flowchart shown is a board-level packaging method provided by the present invention.
[0026] Figure 2 The diagram shows the structure after photoforming a hole in the first dielectric layer on an organic substrate.
[0027] Figure 3 This diagram shows the grain size and surface roughness of the copper oxide layer.
[0028] Figure 4 This diagram shows the grain size and surface roughness of a metal seed layer deposited using a physical vapor deposition process.
[0029] Figure 5 The diagram shows the structure after physical vapor deposition.
[0030] Figure 6 The diagram shows the process of slot coating.
[0031] Figure 7 The diagram shows the structure after slit coating.
[0032] Figure 8 This is a schematic diagram showing the first layer of resist after it has been applied.
[0033] Figure 9 The diagram shows the structure after photolithography and development of the first resist layer.
[0034] Figure 10 The diagram shows the structure of the first redistribution layer formed after electroplating.
[0035] Figure 11 The diagram shows the structure after the first layer of resist has been removed.
[0036] Figure 12 The diagram shows the structure after the first metal seed layer has been removed.
[0037] Figure 13 This is a schematic diagram showing the structure after the formation of the second dielectric layer, the second metal seed layer, and the second redistribution layer.
[0038] Figure 14 The diagram shows the structure after the solder mask layer and solder balls are inserted. Detailed Implementation
[0039] The following specific examples illustrate the embodiments of the present invention. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and various details in this specification can be modified or changed based on different viewpoints and applications without departing from the spirit of the present invention. For ease of explanation, when detailing the embodiments of the present invention, the cross-sectional views showing the device structure are partially enlarged, not according to the general scale, and the schematic diagrams are merely examples and should not limit the scope of protection of the present invention. Furthermore, in actual manufacturing, the three-dimensional spatial dimensions of length, width, and depth should be included.
[0040] For ease of description, spatial relation terms such as “below,” “under,” “lower than,” “below,” “above,” and “upper” may be used herein to describe the relationship between one element or feature shown in the accompanying drawings and other elements or features. It will be understood that these spatial relation terms are intended to include directions other than those depicted in the drawings for devices in use or operation. Furthermore, when a layer is referred to as being “between” two layers, it may be the only layer between the two layers, or there may be one or more layers in between.
[0041] In the context of this application, the structure described above the first feature may include embodiments in which the first and second features are formed in direct contact, or embodiments in which additional features are formed between the first and second features, such that the first and second features may not be in direct contact.
[0042] It should be noted that the illustrations provided in this embodiment are only schematic representations of the basic concept of the present invention. Therefore, the drawings only show components related to the present invention and are not drawn according to the actual number, shape, and size of the components in the actual implementation. In the actual implementation, the form, quantity, and proportion of each component can be arbitrarily changed, and the layout of the components may also be more complex. To keep the illustrations as concise as possible, not all structures are shown in the figures.
[0043] Please see Figures 1 to 14 .
[0044] like Figure 1 As shown, the present invention provides a board-level packaging method, which includes the following steps:
[0045] S1: Prepare a substrate, in which a chip is embedded;
[0046] S2: A metal seed layer is formed on the substrate surface using physical vapor deposition, and then electrically connected to the chip through holes;
[0047] S3: A resist layer is coated on the metal seed layer using a slot coating process and then photolithography is performed.
[0048] S4: The photoresist layer after photolithography is developed using a conveyor-type immersion development process to define the redistribution layer pattern in the photoresist layer.
[0049] S5: A metal body layer is formed on a patterned resist layer using an electroplating process, wherein the metal body layer is electrically connected to the metal seed layer;
[0050] S6: Etch the metal seed layer according to the patterned resist layer to form a redistribution layer, and remove the residual resist layer;
[0051] S7: A solder mask layer is formed on the redistribution layer and solder balls electrically connected to the redistribution layer are implanted.
[0052] The board-level packaging method provided by the present invention will be further described below with reference to the accompanying drawings.
[0053] First, step S1 is performed to prepare substrate 2, in which chip 17 is embedded.
[0054] The packaging method provided by this invention is applicable to board-level packaging based on various substrate materials, including inorganic substrates. However, its advantages are more pronounced when used for board-level packaging based on organic substrates. Because of the advantages of inorganic substrates, such as good heat resistance and high dimensional stability, they are commonly used in the industry for board-level packaging requiring fine circuitry. However, there is not much precedent for fabricating fine circuitry based on organic substrates. Through extensive experimentation, the inventors discovered that when it is necessary to fabricate fine circuitry smaller than 8 / 8 μm on organic substrates, the existing traditional method of forming a seed layer → vacuum lamination → exposure → development → electroplating → film removal → etching the seed layer is insufficient. This is because existing dry film processes are difficult to achieve very thin films. Therefore, based on existing processes, the inventors proposed the improved solution of this application through extensive experimental research. In other words, the substrate 2 provided in this application can be an inorganic substrate or a composite substrate, but in a more preferred example, it is an organic substrate. Organic substrates have advantages such as low dielectric constant, making them more suitable for high-frequency signal transmission, easy processing, and light weight, which can better meet the current demand for high density and miniaturization of packaged devices. However, it is difficult to fabricate fine lines on organic substrates using traditional methods, while this application can solve this problem well.
[0055] When the substrate 2 used is an organic carrier board, the substrate preparation process includes, in sequence: providing an organic carrier board, i.e., a core board; fabricating patterns on the organic carrier board; laser-cutting through-holes for embedding the chip; applying adhesive tape to the bottom; embedding the chip 17; laminating molding compound 18 to fill the space around the chip 17; flipping the organic carrier board and removing the adhesive tape; placing the active side of the chip 17 upwards; coating or vacuum-laminating a dielectric layer 19; and forming holes in the dielectric layer 19, for example, drilling to form a plurality of holes 20. More specifically, for example, using laser drilling or photolithography to form holes, resulting in a structure as shown in the figure. Figure 2 As shown.
[0056] The core board, also called a copper-clad laminate, has an intermediate resin layer 15 made of materials such as polyimide resin, epoxy resin, polypropylene resin, polyethylene, polyetherketone resin, or bismaleimide-modified triazine resin. Metal circuitry 16 is fabricated on the surface of the core board; this metal circuitry 16 is typically copper foil, such as rolled copper foil or electrolytic copper foil. When attaching the chip 17, the active side of the chip 17 is closest to the adhesive tape. The active side of the chip typically has multiple metal pads exposed on the substrate surface for subsequent lead-out of the chip's electrical signals.
[0057] The dielectric layer 19, also called the insulating layer or dielectric layer, is the material that ultimately remains in the packaging substrate. In this embodiment, the dielectric layer 19 can be a dry film material layer or a wet film photoresist material layer, such as polyimide, phenolic resin, epoxy resin, etc. If a photoresist layer is used, the dielectric layer 19 is coated using slit coating; if a dry film is used, it is prepared by vacuum lamination. Laser drilling is preferred for dry film vias, and photolithography is preferred for photoresist vias. In a preferred example of this application, the dielectric layer 19 is a photosensitive dielectric layer, such as a photoresist layer, and photolithography is used to form vias in the dielectric layer 19. The molding material 18 is preferably ABF (Ajinomoto reinforced film). Vacuum lamination can also be used to form vias.
[0058] After the substrate is prepared, step S2 is performed: a metal seed layer 21 is formed on the substrate surface using a physical vapor deposition (PVD) process. The metal seed layer 21 will be electrically connected to the chip 17 through blind vias 31. The structure reference obtained after this step is... Figure 5 As shown.
[0059] In existing board-level packaging, the metal seed layer is commonly prepared using chemical copper plating (CCP). While CCP is more efficient, the thinnest copper layer produced is only 1 μm, thus limiting its fabrication to lines with a linewidth spacing greater than 8 / 8 μm. This application, however, selects physical vapor deposition (PVD), particularly sputtering deposition, which can produce a metal seed layer with smaller copper grain sizes, making it more suitable for fabricating lines with a linewidth spacing less than 8 / 8 μm. Furthermore, referencing... Figure 3 and 4 As shown, although the surface roughness 14 of the copper layer deposited by sputtering deposition is smaller than that of the copper layer 10 surface roughness 11, it is denser, which is beneficial to the subsequent electroplating of the copper layer as the metal host layer and the copper layer as the metal seed layer.
[0060] In a preferred embodiment, the fabricated metal seed layer 21 includes an adhesion layer 12 located on the surface of the substrate 9 and a metal seed layer 13 located on the surface of the adhesion layer 12. The adhesion layer 12 may include, but is not limited to, a titanium layer and / or a titanium nitride layer. The material of the metal seed layer 13 is preferably the same as that of the metal host layer, and may be, but is not limited to, a copper layer. For example, a titanium layer of 50 nm to 100 nm is first fabricated on the surface of the substrate 9, and then a copper layer of 100 nm to 500 nm is fabricated on the titanium layer. In a specific example, the titanium layer as the adhesion layer 12 is 100 nm, and the copper layer as the metal seed layer 13 is 300 nm.
[0061] In this process, the titanium layer acts as an adhesion layer, increasing the adhesion between the substrate 9 and the metal seed layer, while the copper layer adjusts the electroplating impedance, resulting in a more uniform copper surface on the substrate after electroplating. Current board-level packaging commonly uses chemical copper plating (CCP) to prepare the metal seed layer. However, CCP is a wet process, requiring wet desmearing to increase substrate surface roughness, making the process complex and generating significant wastewater and chemical consumption. Increased substrate surface roughness is detrimental to subsequent flash etching of fine circuitry. A rougher copper surface results in more etching at once, leading to greater side etching at the bottom of the circuit, thus hindering ultra-fine circuitry. In contrast, the physical vapor deposition (PVD) process used in this application to prepare the metal seed layer is not only environmentally friendly but also produces a smaller grain size and surface roughness, enabling finer line spacing.
[0062] In other examples, the metal seed layer may also be titanium, copper, titanium-tungsten alloy, or a combination thereof.
[0063] After the metal seed layer is fabricated, a prefabricated structure 2 is obtained. Step S3 is then performed, where a resist layer 8 is coated onto the metal seed layer using a slot coating process. After vacuum drying and hot plate pre-baking, photolithography is performed. Before coating, the surface of the prefabricated structure 2 can be cleaned with propylene glycol methyl ether acetate (PGMEA) cleaning solution to increase the surface adhesion between the photoresist layer 8 and the metal seed layer on the substrate. Slot coating using wet photoresist is a wet process, unlike the dry film lamination process. Compared to dry film fabrication, this wet-coated resist layer can be thinner and has better uniformity. Currently, the thinnest dry film thickness is 15 μm with a uniformity >10%, while the resist layer 8 fabricated using slot coating in this invention achieves a uniformity of less than 5% and a thickness ≤10 μm. The thinner and more uniform resist layer, combined with a high-precision photolithography machine, results in higher linewidth resolution during exposure.
[0064] Specifically, the principle and process of slot coating are explained in the reference section. Figure 6 and Figure 7 As shown. Figure 6 As shown, two photoresist tanks 5 and 7 are provided on both sides of the stage 1. The prefabricated structure 2 is fixed to the stage 1 by vacuum adsorption 3. Above the photoresist tanks are two slit nozzles 4 and 6 that can be drawn up by a vacuum pump. During coating, the nozzles 4 are kept at a certain distance from the prefabricated structure 2, i.e., from the substrate. One of the nozzles 4 automatically moves from one side to above the substrate 9, releasing the vacuum during the movement to spray out the photoresist. The nozzle moves to the other end and then returns to the initial position, thus completing the coating of the resist layer 8. The structure after coating can be seen from the following diagram. Figure 7 and 8 As shown. During mass production, nozzles 4 and 6 are used alternately to improve coating efficiency. After coating, the substrate is placed in a vacuum oven for vacuum drying. Vacuum drying removes air bubbles from the photoresist layer and the substrate surface, as well as dust around the substrate. If air bubbles remain in the photoresist layer, they will cause bulging and cracking during subsequent hot plate pre-baking, damaging the appearance and uniformity. After drying, the photoresist is cured. The curing process can be carried out on a heating platform, and parameters such as curing temperature and time can be set as needed. In a preferred example of this application, the curing temperature is 90°C and the time is 5 minutes. Curing can be carried out under vacuum or in an inert gas atmosphere, preferably the latter, i.e., an inert gas such as nitrogen or argon is introduced into the curing chamber during the curing process. Inert gas not only protects the substrate from contamination but also provides good thermal conductivity, improving heating uniformity.
[0065] It is important to note that the photoresist layer in this step is fundamentally different from the photoresist used as a dielectric layer in step S1, where it remains inside the substrate primarily to form vias 20, allowing the electrical signals of the internal chip to pass through the electroplated blind vias 31 to the redistribution layer 24. In contrast, the photoresist layer 22 used as the resist layer in this step is for fabricating the redistribution layer 24 and will ultimately be removed after exposure, development, and electroplating.
[0066] After the resist layer 22 has cured, patterning photolithography is performed. A suitable photolithography machine is selected based on the type of photoresist applied. Currently, photoresists typically require LDI (Laser Direct Imaging) or stepper lithography machines with mixed h-line (405nm), i-line (365nm), or ghi-line light sources for photolithography. The target linewidth produced by g-line lithography is generally greater than 10μm, while the target linewidth produced by h-line, i-line, or ghi-line light source photoresists is generally greater than 0.35μm. Considering only the photolithography effect, using photoresist with an i-line stepper lithography machine is a better choice. The inventors have experimentally discovered that using i-line LDI lithography in this embodiment can fully meet the linewidth requirements and significantly improve the photolithography efficiency, thus making it the preferred choice for this embodiment.
[0067] After photolithography is completed, step S4 is performed, using a transfer-type immersion developing process to develop the photolithographic resist layer 22 to define the redistribution layer pattern in the resist layer 22. The structure after development is as follows: Figure 9 As shown. Unlike dry film development, photoresist development typically uses a 2.38% tetramethylammonium hydroxide (TMAH) developer, or an inorganic developer including inorganic bases. Furthermore, unlike wafer-level development, this application pertains to board-level packaging products. Compared to wafer-level packaging, board-level packaging, due to its larger area and organic substrate, exhibits some warpage in practice. Therefore, the inventors chose horizontal conveyor immersion development instead of traditional jet development. This development method includes a passive shutter, accepting carrier boards with a warpage ≤10mm. During development, the carrier board is flattened, resulting in higher flatness and allowing for a more complete reaction between the developer and photoresist, which is more conducive to subsequent processes for fabricating ultra-fine circuitry.
[0068] Next, step S5 is performed: a metal body layer is formed on the patterned resist layer 23 using an electroplating process, for example, an electroplating process is used to form a main copper layer, and the metal body layer is electrically connected to the metal seed layer.
[0069] After the aforementioned development, the bottom metal seed layer 21 is exposed, and electroplating can then be performed. The structure after electroplating is shown in the reference diagram. Figure 10 As shown in the image, the aforementioned steps produce ultra-fine lines with small linewidths and spacing. This electroplating step typically uses high current density and low sulfur content (<9.6 ppm). After electroplating, an organic stripping solution is used to remove the photoresist in the protective metal seed layer area outside the lines. The structure after removing the first resist layer is shown in the image. Figure 11 As shown. Finally, baking removes any remaining moisture from the carrier plate.
[0070] Next, S6 is executed: the metal seed layer is etched according to the patterned resist layer 23 to form a redistribution layer, and the residual resist layer is removed.
[0071] After removing the first resist layer in step S6, the first metal seed layer 21 at the bottom of the line spacing needs to be removed. Generally, some copper on the lines of the metal body layer will be flashed at the same time. Therefore, appropriate compensation will be designed in the pattern design. In this embodiment, a compensation of about 1μm is performed.
[0072] In a preferred example, the etching process in this step is divided into two steps: first, wet etching is performed on the copper layer serving as the metal seed layer; then, dry etching using plasma, including argon, or wet flash etching is used to etch the titanium layer serving as the adhesion layer. Wet flash etching of the copper layer preferably uses hydrogen peroxide + acid, with the acid being sulfuric acid or a weak acid. Wet flash etching of the titanium layer requires HF (hydrofluoric acid) or NaOH + H2O2 and other alkaline mixtures. Dry etching has lower efficiency but higher etching quality and is pollution-free. Dry etching generally uses plasma or active ions, and nitrogen, argon, and other auxiliary gases can be introduced during the etching process, without limitation. At this point, the first ultra-fine circuit layer is completed. For the fan-out process of this embodiment, the inner layer linewidth spacing will be less than or equal to the outer layer linewidth spacing. After etching, the residual resist layer is removed to obtain the redistribution layer 24 of the desired structure, resulting in a structural reference. Figure 12 As shown.
[0073] The redistribution layer can be a single-layer structure, or it can be formed by repeating steps S2 to S6 several times as shown in this embodiment to create two or more stacked and electrically connected redistribution layers, for example... Figure 13 As shown, two redistribution layers are formed. For example, a second metal seed layer 32 is formed on the first redistribution layer 24 using a sputtering deposition process. Then, a second resist layer is formed using slot coating. The desired pattern is then formed through photolithography and transfer bath development. Metal is electroplated into the holes 26 formed in the resist layer, and then the second metal seed layer 32 is etched, thereby obtaining the second redistribution layer 28. A more detailed fabrication process can be found in the foregoing description, which is omitted for brevity. The materials and thicknesses of the first redistribution layer 24 and the second redistribution layer 28 can be the same or different, and this is not limited. In other examples, different redistribution layers can be interconnected through other interconnect structures, such as through an adapter board, or by bonding a redistribution layer prefabricated on another substrate to the structure prepared in this embodiment to achieve interconnection between different structures. Two or more redistribution layers stacked one on top of the other can meet the needs of different devices and higher-density device integration, but require higher circuit quality. The method provided in this embodiment effectively ensures interlayer interconnection and device performance.
[0074] After completing the fabrication of the redistribution layer, step S7 is performed to form a solder mask layer 29 on the redistribution layer and implant solder balls 30 that are electrically connected to the redistribution layer, resulting in a structural reference. Figure 14 As shown. At this point, the fabrication of ultra-fine circuitry for board-level packaging based on eSiP organic substrate is complete.
[0075] In one example, this step may specifically include first fabricating a solder resist layer 29 (also called green oil) using any of the following methods: lamination, roll coating, and screen printing, preferably using a wet coating method such as screen printing. Then, after exposure, development, and post-curing, a window is created in the solder resist layer 29 at the location where solder balls will be inserted. Finally, solder balls 30 are inserted at the window. The material of the solder balls may include, for example, copper, tin, nickel, silver, or several alloys. A protective coating may be formed on the surface of the solder balls. The shape of the solder balls may be ellipsoidal, cylindrical, or other suitable structures. In one example, grooves may be formed on the surface of the solder balls to prevent solder overflow and short circuits during subsequent soldering with other electrical connection structures. In other examples, solder balls electrically connected to the redistribution layer may be formed first using methods including but not limited to physical vapor deposition, followed by the formation of a solder resist layer in the area outside the solder balls. However, forming the solder resist layer first and then creating windows for ball insertion effectively confines the solder balls to a specific area, preventing short circuits.
[0076] After the solder balls are installed, a filler layer can be formed between them using methods including but not limited to capillary filling. This filler layer can be made of materials such as epoxy resin. The filler layer helps to secure the solder balls and prevents them from oxidizing, while also preventing moisture from penetrating into the encapsulated structure. Afterwards, protective frames and other structures can be further attached, followed by cutting.
[0077] The improved process design of this invention combines the advantages of physical vapor deposition (PVD) with its smaller grain size and surface roughness, thin and uniform resist layer in slot coating (resist layer thickness can be achieved from 0 to 15 μm, with uniformity controlled within 5%), high photoresist resolution, and high lithography precision. This enhances circuit precision and enables the fabrication of ultra-fine lines with a linewidth spacing ≤ 8 / 8 μm on an organic substrate structure for embedded chips. It should be noted that the above steps form an inseparable whole; they must work together to ultimately produce the desired ultra-fine lines.
[0078] To reduce the cost of fan-out packaging and expand its applications, the industry focuses on fan-out packaging with a line-to-span (L / S) ratio between 1 / 1μm and 8 / 8μm. This invention further bridges the technological gap between upstream board manufacturers and downstream OSAT (Optical System Assembly and Test) manufacturers. Compared to silicon-based FOWLP's move towards the board level, FOPLP based on organic substrates has a natural board-level infrastructure and lower costs in all aspects, giving it a higher market prospect.
[0079] Compared with the prior art, the advantages of the present invention are as follows:
[0080] 1) In terms of social benefits, the method of using fan-out packaging technology on the substrate with embedded chips provided by the present invention can produce fine circuits, which can achieve thinner packaging and can bridge the gap between the 1 / 1μm to 8 / 8μm circuits between upstream board manufacturers and downstream OSAT (outer packaging and testing) manufacturers, achieving high density and miniaturization while reducing the cost of fan-out packaging.
[0081] 2) From an economic perspective, the thickness of dry film is currently limited by filler properties, with a minimum thickness of only about 15μm. Furthermore, the resolution and adhesion of this thickness cannot meet the requirements for circuit fabrication below 8 / 8μm in subsequent electroplating processes. This invention abandons the traditional dry film application method and instead employs a wet slot coating method to create a thinner resist layer (≤10μm). Compared to spin coating in wafer-level packaging, this slot coating method can coat a larger area at once, thereby improving production efficiency and offering a capacity advantage. On the other hand, compared to the traditional wet chemical copper plating process, this invention uses a dry PVD method to create the metal seed layer for the redistribution layer, significantly reducing the use of chemicals and thus reducing industrial wastewater generation, making it more environmentally friendly. Moreover, only the substrate surface needs to be cleaned before the PVD process, while the traditional wet copper plating process requires a wet desmearing process on the dielectric layer surface, increasing the cost of chemicals and generating wastewater.
[0082] 3) In terms of technical benefits, the slit coating method of this invention can produce a thinner resist layer (≤10μm). The resolution and adhesion of this resist layer can fully meet the requirements of 8 / 8μm and below. Therefore, it is advantageous for the subsequent process of using electroplating to produce ultra-fine lines (≤8μm).
[0083] In traditional copper plating processes, a certain surface roughness of the dielectric layer is required to ensure that the copper plating layer and the dielectric layer achieve the peel strength required by the customer (typically requiring a peel strength > 4N). However, after the copper plating layer is formed (e.g., a copper plating layer thickness of 1μm), after the processes of coating a resist layer → exposure → development → electroplating → stripping, a flash etching process is still needed to remove the copper plating layer at the line spacing. At this point, the increased interface roughness between the dielectric layer and the dry film caused by the previous process of Desmearing makes it impossible to achieve a very small line spacing during subsequent flash etching. Moreover, the relatively thick copper plating layer, at 1μm, means that a larger amount of flash etching is required. Subsequently, in the additive method, a large amount of flash etching requires greater line compensation, i.e., a smaller spacing. However, the roughness of the copper plating layer and the dielectric layer at the spacing is relatively large, and flash etching can easily cause side etching at the bottom of the line, or even flying wires. These are the fundamental reasons why it is impossible to achieve more refined lines on the copper plating layer substrate. This invention utilizes PVD to fabricate a metal seed layer. Without increasing the roughness of the dielectric layer, it achieves a peel strength of >4N between the metal seed layer and the dielectric layer, with an adhesion strength far exceeding that between the copper plating layer and the dielectric layer. This is because PVD can form a very dense nanoscale metal seed layer, typically consisting of two layers. For example, the first layer, a titanium metal layer (with a thickness of 50-100 nm), exhibits high adhesion and conductivity, good thickness flatness, and a strong bond with the dielectric layer. A copper layer is then sputtered onto the titanium layer as the host metal layer for the redistribution layer. The copper layer thickness can be 100-500 nm, significantly reducing the required copper layer thickness compared to traditional copper plating layers. This results in shorter subsequent flash etching or dry etching times for the copper layer and less need for extensive compensation of the circuitry. This greatly improves production efficiency and reduces production costs.
[0084] This invention is not limited to board-level packaging based on organic carriers, but its advantages are particularly prominent when used in such packaging.
[0085] Therefore, this invention effectively overcomes the various shortcomings of the prior art and has high industrial application value.
[0086] The above embodiments are merely illustrative of the principles and effects of the present invention and are not intended to limit the invention. Any person skilled in the art can modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by those skilled in the art without departing from the spirit and technical concept disclosed in the present invention should still be covered by the claims of the present invention.
Claims
1. A board-level packaging method, characterized in that, Including the following steps: S1: Prepare a substrate, in which a chip is embedded; S2: A metal seed layer is formed on the substrate surface using physical vapor deposition, and then electrically connected to the chip through holes; S3: A resist layer is coated on the metal seed layer using a slot coating process and then photolithography is performed. S4: The photoresist layer after photolithography is developed using a conveyor-type immersion development process to define the redistribution layer pattern in the photoresist layer. S5: A metal body layer is formed on a patterned resist layer using an electroplating process, wherein the metal body layer is electrically connected to the metal seed layer; S6: Etch the metal seed layer according to the patterned resist layer to form a redistribution layer, and remove the residual resist layer; S7: A solder mask layer is formed on the redistribution layer and solder balls electrically connected to the redistribution layer are implanted.
2. The board-level packaging method according to claim 1, characterized in that, The substrate includes an organic carrier plate, and the substrate preparation process includes the following steps: providing an organic carrier plate, creating a pattern on the organic carrier plate, laser cutting out a through groove for embedding the chip, applying adhesive tape to the bottom, embedding the chip, laminating molding material to fill the space around the chip, flipping the organic carrier plate and removing the adhesive tape, placing the active side of the chip facing upwards, coating or vacuum-pressing a dielectric layer, and forming a hole in the dielectric layer.
3. The board-level packaging method according to claim 2, characterized in that, The molding material used is ABF material, the dielectric layer used is a photosensitive dielectric layer, and the method for forming holes in the dielectric layer is photolithography or vacuum lamination.
4. The board-level packaging method according to claim 1, characterized in that, The metal seed layer includes an adhesion layer located on the surface of the substrate and a metal seed layer located on the surface of the adhesion layer.
5. The board-level packaging method according to claim 4, characterized in that, The adhesion layer includes a titanium layer and / or a titanium nitride layer, and the metal seed layer includes a copper layer; the thickness of the adhesion layer is 50nm-100nm, and the thickness of the copper layer is 100nm-500nm.
6. The board-level packaging method according to claim 5, characterized in that, The etching method in step S6 includes wet flash etching of the copper layer and wet flash etching or dry etching of the adhesion layer.
7. The board-level packaging method according to claim 6, characterized in that, The wet flash etching method for the copper seed layer is to use hydrogen peroxide and acid for etching. The wet flash etching method for the titanium adhesion layer is to use HF or NaOH+H2O2 and their alkaline mixtures. The dry etching method for the titanium adhesion layer is to use plasma or active ions, including argon gas, for etching.
8. The board-level packaging method according to claim 1, characterized in that, The photolithography in step S3 is LDI photolithography using i-line.
9. The board-level packaging method according to claim 1, characterized in that, Step S7 includes first creating a solder resist layer using any one of the following methods: film application, roller coating, and screen printing; then, after exposure, development, and post-curing, creating a window in the solder resist layer at the location where solder balls need to be implanted; and finally, implanting solder balls at the window.
10. The board-level packaging method according to any one of claims 1 to 9, characterized in that, The board-level packaging method includes repeating steps S2 to S6 several times to form two or more stacked and electrically connected redistribution layers.
Citation Information
Patent Citations
Wafer level MMCM (microwave multichip module) packaging structure using photosensitive BCB (benzocyclobutene) as dielectric layer and method
CN102110673A
Method of manufacturing fine circuit capable of preventing lateral etching
CN110571157A