Bonding structures and methods of forming the same and MEMS sensors, wearable devices

By employing a misaligned design of the aluminum-germanium bonding structure and a low-temperature eutectic process, the flow and uniformity issues of aluminum-germanium eutectic bonding were resolved, enabling the application of highly integrated and high-performance piezoelectric MEMS sensors suitable for wearable devices.

CN116469837BActive Publication Date: 2026-11-24PEKING UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310246317.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-07
Publication Date
2026-11-24
Estimated Expiration
2043-03-07

AI Technical Summary

Technical Problem

Existing aluminum-germanium eutectic bonding in piezoelectric MEMS wearable ultrasonic microsystems suffers from eutectic flow and extension phenomena, making it difficult to control the bonding process window and uniformity, and the bonding precision is insufficient, which makes it difficult to meet the requirements of high integration and high performance.

Method used

An aluminum-germanium bonding structure is adopted, which includes a misalignment structure and a bonding region. By forming protrusions on both sides of the aluminum bonding layer and trenches on both sides of the germanium bonding layer, combined with an oxide film and a monomolecular modification film, the eutectic flow range is restricted, and eutectic bonding is carried out under low temperature conditions.

Benefits of technology

It effectively controls eutectic flow and uneven heat transfer distribution, improves device performance sensitivity, possesses robustness and stability, and achieves bonding precision of 25µm and below, making it suitable for wearable devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116469837B_ABST
    Figure CN116469837B_ABST
Patent Text Reader

Abstract

This application belongs to the field of sensor technology, specifically relating to a bonding structure and its formation method, and related to MEMS sensors and wearable devices. The bonding structure in this application includes: a first wafer and a second wafer; at least one set of bonding regions and at least two sets of misalignment structures are provided between the first wafer and the second wafer, with the misalignment structures located on both sides of the bonding regions; the bonding regions include an aluminum bonding layer formed on the surface of the first wafer and a germanium bonding layer formed on the surface of the second wafer, with the germanium bonding layer in bonded contact with the aluminum bonding layer; the misalignment structures include protrusions located on both sides of the aluminum bonding layer and grooves located on both sides of the germanium bonding layer, with the protrusions extending into the grooves to form the misalignment structures. This solves the problems of existing sensors, especially piezoelectric MEMS sensors, where eutectic flow and extension phenomena in aluminum-germanium eutectic bonding lead to difficulties in controlling the bonding process window and uniformity, as well as insufficient precision and large size of aluminum-germanium bonding. Piezoelectric MEMS sensors incorporating this bonding structure have good application prospects in wearable devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of sensor technology, specifically relating to a bonding structure and its formation method, as well as MEMS sensors and wearable devices. Background Technology

[0002] One of the main bottlenecks currently facing the development of the piezoelectric MEMS wearable ultrasonic microsystem industry lies in the design and development of high-precision, low-temperature reliable wafer-level bonding technology that can endow it with multifunctional integration. Several wafer-level bonding technologies have been developed, such as surface-activated low-temperature bonding, anodic bonding, and eutectic bonding. However, wearable ultrasonic microsystem devices often require a uniform and controllable micron-gap electromechanical interface between the MEMS wafer and the CMOS substrate to be integrated, making it difficult for existing technologies to meet their technical requirements. For example, surface activation low-temperature bonding processes are time-consuming and inefficient, and due to surface treatment, they are difficult to meet the bonding requirements of wafers containing patterns and circuits. Anodic bonding is a widely used bonding technology, but its disadvantages are that it cannot directly bond two silicon wafers, and due to the presence of sodium ions, it is not compatible with MOS processes. The electrostatic force generated by the high voltage during the bonding process can cause device failure. Eutectic bonding technology is a low-temperature bonding method that is expected to overcome the defects of the aforementioned methods. Currently, common eutectic bonding materials include alloys such as gold (Au)-silicon (Si), gold (Au)-tin (Sn), aluminum (Al)-copper (Cu), aluminum (Al)-silicon (Si), and aluminum (Al)-germanium (Ge). In comparison, Al-Ge eutectic bonding has significant advantages in terms of compatibility with CMOS process technology, improved device performance and functionality, and reduced system power consumption, size and manufacturing costs. Therefore, it is expected to eventually realize the design and development of advanced piezoelectric MEMS wearable ultrasonic microsystems.

[0003] However, in response to the development needs of piezoelectric MEMS wearable ultrasonic microsystems with high integration, high patterning density, and high performance (the trend of miniaturization of bonding area / size), existing aluminum-germanium solutions are still hampered by the following bottlenecks: ① Eutectic flow and elongation phenomena make it difficult to control the bonding process window and uniformity; ② Insufficient bonding precision and large size of aluminum-germanium. Summary of the Invention

[0004] The technical objective of this application is to at least solve the problems in existing piezoelectric MEMS sensors, such as the difficulty in controlling the bonding process window and uniformity due to eutectic flow and extension phenomena in aluminum-germanium eutectic bonding, as well as the insufficient fineness and large size of aluminum-germanium bonding.

[0005] This objective is achieved through the following technical solutions:

[0006] In a first aspect, this application provides a bonding structure, the bonding structure comprising:

[0007] First wafer and second wafer;

[0008] At least one set of bonding regions and at least two sets of misalignment structures are provided between the first wafer and the second wafer, and the misalignment structures are located on both sides of the bonding regions;

[0009] The bonding region includes an aluminum bonding layer formed on the surface of the first wafer and a germanium bonding layer formed on the surface of the second wafer, wherein the germanium bonding layer is bonded to the aluminum bonding layer.

[0010] The misalignment structure includes protrusions on both sides of the aluminum bonding layer and trenches on both sides of the germanium bonding layer, with the protrusions extending into the trenches to form the misalignment structure. This bonding structure, comprising a bonding region and a misalignment structure, possesses good robustness and stability. The misalignment structures on both sides, by surrounding the bonding region, effectively limit the aluminum-germanium eutectic flow range and signal differences caused by uneven heat transfer distribution, ultimately facilitating the achievement of high integration, high patterning density, and high performance in the device.

[0011] In some embodiments of this application, the bonding structure further includes a first oxide film layer disposed between the first wafer and the aluminum bonding layer and / or a second oxide film layer disposed between the second wafer and the germanium bonding layer;

[0012] Wherein, a monomolecular modification film for reducing the surface energy of the oxide film is formed on the surface of the first oxide film layer and / or the second oxide film layer;

[0013] Preferably, the material of the first oxide film layer and the second oxide film layer includes any one or more of doped silicon dioxide, undoped silicon dioxide, or ethyl silicate, wherein the undoped silicon dioxide is USG, the doped silicon dioxide is any one of PSG and BPSG, and the ethyl silicate is PETEOS.

[0014] Preferably, the monomolecular modified film is a monomolecular layer formed by an oxide film layer and a surfactant, wherein the surfactant is an organosilane.

[0015] Because the oxide film has active groups on its surface, these active groups are conducive to the reaction to generate a monomolecular modified film. The surface energy of the monomolecular modified film is small, which is not conducive to the spread of aluminum-germanium liquid eutectic on its surface. Therefore, it helps to further strengthen the restriction of the flow range of aluminum-germanium liquid eutectic and is conducive to obtaining a clean bonding interface.

[0016] In some embodiments of this application, the area of ​​the bonding surface of the germanium bonding layer is smaller than the area of ​​the bonding surface of the aluminum bonding layer;

[0017] Preferably, the ratio of the area of ​​the bonding surface of the germanium bonding layer to the area of ​​the bonding surface of the aluminum bonding layer is 1:5 to 1:1.

[0018] The height of the germanium bonding layer is less than the height of the aluminum bonding layer;

[0019] Preferably, the ratio between the height of the germanium bonding layer and the height of the aluminum bonding layer is 0.2:1 to 0.8:1.

[0020] By controlling the area and height of the bonding surfaces of the germanium bonding layer and the aluminum bonding layer, it is beneficial to form a eutectic alloy and to ensure the high strength and airtightness of the eutectic alloy bonding.

[0021] In some embodiments of this application, a barrier layer is provided between the first oxide film layer and the aluminum bonding layer and / or a barrier layer is provided between the second oxide film layer and the germanium bonding layer;

[0022] Preferably, the barrier layer is made of titanium nitride and / or titanium.

[0023] Preferably, the thickness of the barrier layer is

[0024] This barrier layer effectively prevents aluminum-germanium metal from penetrating into the wafer during subsequent pressurization processes.

[0025] In some embodiments of this application, the second oxide film layer includes an oxide substrate and at least two sets of oxide pillars formed on the surface of the oxide substrate, the oxide pillars enclosing the trench.

[0026] In some embodiments of this application, the protrusion is a columnar protrusion, and preferably, the columnar protrusion is made of aluminum.

[0027] Secondly, this application provides a method for forming the bonding structure described in the first aspect, the method comprising:

[0028] Provide the first wafer and the second wafer;

[0029] At least one set of bonding regions and at least two sets of misalignment structures are formed between the first wafer and the second wafer, wherein the misalignment structures are located on both sides of the bonding regions;

[0030] An aluminum bonding layer is formed on the surface of the first wafer, and a germanium bonding layer is formed on the surface of the second wafer. The germanium bonding layer is bonded to the aluminum bonding layer and forms the bonding region.

[0031] Protrusions are formed on both sides of the aluminum bonding layer, and grooves are formed on both sides of the germanium bonding layer. The protrusions extend into the grooves to form the misalignment structure.

[0032] In some embodiments of this application, the method further includes forming a first oxide film layer between the first wafer and the aluminum bonding layer and / or forming a second oxide film layer between the second wafer and the germanium bonding layer;

[0033] The first oxide film layer and / or the second oxide film layer self-assemble to form a monomolecular modified film.

[0034] Thirdly, this application provides a MEMS sensor, the sensor comprising the bonding structure described in the first aspect or the bonding structure obtained by the method described in the second aspect.

[0035] In some embodiments of this application, the MEMS sensor is a piezoelectric MEMS sensor.

[0036] Fourthly, this application provides a wearable device that includes the sensor described in the third aspect.

[0037] The beneficial effects of the technical solution disclosed in this application are mainly reflected in the following:

[0038] 1. The aluminum-germanium eutectic bonding structure provided in this application can effectively reduce the device failure and signal interference caused by eutectic flow into other contact surfaces due to eutectic fluidity and elongation, or the device signal differences caused by uneven heat transfer distribution, which is beneficial to improving the sensitivity of device performance.

[0039] 2. The aluminum-germanium eutectic bonding structure provided in this application has good robustness, stability and bonding precision. If the bonding area is controlled to 25um or less, the piezoelectric MEMS sensor containing this bonding structure has good application prospects in wearable devices. Attached Figure Description

[0040] Various other advantages and benefits will become apparent to those skilled in the art upon reading the following detailed description of preferred embodiments. The accompanying drawings are for illustrative purposes only and are not intended to limit the scope of this application. Furthermore, the same reference numerals denote the same parts throughout the drawings. In the drawings:

[0041] Figure 1 A schematic diagram of a bonding structure according to an embodiment of this application is shown;

[0042] Figure 2 A schematic diagram of a bonding structure according to an embodiment of this application is shown;

[0043] Figure 3 A schematic diagram of a bonding structure according to an embodiment of this application is shown;

[0044] Figure 4 A schematic diagram of a bonding structure according to an embodiment of this application is shown;

[0045] Figure 5 A schematic diagram illustrating the process flow of the bonding structure according to an embodiment of this application is shown.

[0046] Figure 6 The accompanying drawing schematically illustrates a bonding structure in the bonding region according to an embodiment of this application; the reference numerals in the drawing are as follows:

[0047] 100, First wafer; 200, Second wafer; 300, Bonding region; 301, Aluminum bonding layer; 302, Germanium bonding layer; 400, Misalignment structure; 401, Protrusion; 402, Trench;

[0048] 500, First oxide film layer; 600, Second oxide film layer; 700, Monomolecular modified film; 800, Barrier layer.

[0049] Terminology Explanation and English Abbreviations:

[0050] MEMS: abbreviation for Micro-Electro Mechanical System, also known as micro-electromechanical system, refers to sensor devices with a size of a few millimeters or even smaller. Their internal structure is generally at the micrometer or even nanometer scale, and they are independent intelligent systems.

[0051] CMOS stands for Complementary Metal-Oxide-Semiconductor. It is a semiconductor made primarily of silicon and germanium, where N-type (negatively charged) and P-type (positively charged) semiconductors coexist. The current generated by these two complementary effects can be recorded and interpreted into images by the processing chip.

[0052] USG: Undoped silicon glass.

[0053] PSG: Phosphorus-doped silicon glass.

[0054] BPSG: Boron-phosphorus-doped silicon glass.

[0055] PETEOS: Plasma-enhanced tetraethyl orthosilicate.

[0056] BOE: Short for Buffered Oxide Etch, which is a buffered oxide etching solution, specifically made of hydrofluoric acid (49%) and water or ammonium fluoride and water.

[0057] OTS: Octadecyltrichlorosilane.

[0058] SAMs, short for self-assembly led monolayer, are a novel organic film-forming technology. They are ordered monolayers that spontaneously form at the interface through chemisorption between the head groups of surfactants and the substrate.

[0059] Lift-off is an integrated circuit process that involves peeling off or removing parts of an object. It can be used to omit the etching step.

[0060] DRIE: Deep reactive ion etching, is a standard etching process for MEMS. Detailed Implementation

[0061] In the design and development of piezoelectric MEMS wearable ultrasonic microsystems, existing technologies often employ eutectic bonding materials such as gold (Au)-silicon (Si), gold (Au)-tin (Sn), aluminum (Al)-copper (Cu), aluminum (Al)-silicon (Si), and aluminum (Al)-germanium (Ge) to meet the development requirements of high integration, high patterning density, and high performance. Among these, for aluminum (Al)-germanium (Ge) eutectic bonding materials, the limitations of wafer structure design and the stretching phenomenon caused by the flow of aluminum (Al)-germanium (Ge) eutectic bonding materials can easily generate bonding process windows. Furthermore, the uniformity of the eutectic is difficult to control, and the differences in heat transfer / distribution will inevitably interfere with the signal, leading to signal differences or device failure.

[0062] At the same time, the aluminum-germanium eutectic bonding in existing technologies is usually large in size, making it difficult to support the design and development of some advanced integrated devices.

[0063] To address the aforementioned technical problems, this application provides a bonding structure, its formation method, and related technologies for MEMS sensors and wearable devices. Firstly, this application employs low-temperature bonding technology to provide an aluminum-germanium bonding structure. The included misalignment structure and bonding region help restrict the extension and flow of the aluminum-germanium eutectic. Under the premise of obtaining a safe bonding process window, the eutectic exhibits good uniformity and relatively small differences in heat transfer / distribution. This avoids eutectic inflow into other electrical contact surfaces, preventing device failure and signal interference, and also reduces signal differences caused by uneven heat transfer distribution, thus improving device sensitivity. Simultaneously, this bonding structure itself possesses good robustness, stability, and bonding precision. If the bonding region is controlled to 25µm or less, piezoelectric MEMS sensors incorporating this bonding structure have promising application prospects in wearable devices.

[0064] Integrating this bonding structure design into MEMS sensors, such as piezoelectric MEMS sensors, has promising applications in wearable electronic devices, including AR / VR / MR headsets, smart audio glasses, Bluetooth headphones, wearable speakers, smartwatches / smart bracelets / smart rings, smart clothing / smart sneakers, and other fields.

[0065] To achieve the aforementioned technical effects, the first aspect of this application is to provide a bonding structure, which includes:

[0066] First wafer and second wafer;

[0067] At least one set of bonding regions and at least two sets of misalignment structures are provided between the first wafer and the second wafer, and the misalignment structures are located on both sides of the bonding regions;

[0068] The bonding region includes an aluminum bonding layer formed on the surface of the first wafer and a germanium bonding layer formed on the surface of the second wafer, wherein the germanium bonding layer is bonded to the aluminum bonding layer.

[0069] The misalignment structure includes protrusions on both sides of the aluminum bonding layer and grooves on both sides of the germanium bonding layer, with the protrusions extending into the grooves to form the misalignment structure.

[0070] In some embodiments, the first wafer includes a CMOS substrate or a MEMS substrate.

[0071] In some embodiments, the second wafer includes a MEMS substrate or a CMOS substrate.

[0072] In some embodiments, the first wafer is a CMOS substrate and the second wafer is a MEMS substrate.

[0073] In some embodiments, the bonding structure further includes a first oxide film layer disposed between the first wafer and the aluminum bonding layer, wherein the first oxide film layer is made of any one or more of doped silicon dioxide, undoped silicon dioxide, or tetraethyl orthosilicate. In some embodiments, the bonding structure further includes a second oxide film layer disposed between the second wafer and the germanium bonding layer, wherein the second oxide film layer is made of any one or more of doped silicon dioxide, undoped silicon dioxide, or tetraethyl orthosilicate. In some embodiments, the bonding structure further includes a first oxide film layer disposed between the first wafer and the aluminum bonding layer and a second oxide film layer disposed between the second wafer and the germanium bonding layer.

[0074] In some embodiments, the material of the second oxide film layer includes any one or more of doped silicon dioxide, undoped silicon dioxide, or ethyl silicate.

[0075] Wherein, the undoped silicon dioxide is USG, the doped silicon dioxide is either PSG or BPSG, and the ethyl silicate is PETEOS.

[0076] In some embodiments, a monomolecular modification film for reducing the surface energy of the oxide film is formed on the surface of the first oxide film layer.

[0077] In some embodiments, a monomolecular modification film for reducing the surface energy of the oxide film is formed on the surface of the second oxide film.

[0078] In some embodiments, a monomolecular modification film for reducing the surface energy of the oxide film is formed on the surface of the first oxide film and the surface of the second oxide film.

[0079] In some embodiments, the thicknesses of the monomolecular modified films formed on the surfaces of the first oxide film layer and / or the second oxide film layer are equal or unequal, wherein unequal thickness includes a relationship of large and small.

[0080] In some embodiments, the thickness of the monomolecular modified film is less than the thickness of the first oxide film layer and / or the second oxide film layer.

[0081] In some embodiments, the monomolecular modified film is an ordered monolayer spontaneously formed at the interface by the reaction of a surfactant with active groups such as hydroxyl groups in the oxide film layer. This monolayer has the characteristics of in-situ spontaneous formation, highly ordered bonding, few defects, strong binding force, and a "crystalline" state. The surfactant is an organosilane, such as octadecyltrichlorosilane.

[0082] In some embodiments, the area of ​​the bonding surface of the germanium bonding layer is smaller than the area of ​​the bonding surface of the aluminum bonding layer.

[0083] In some embodiments, the ratio between the area of ​​the bonding surface of the germanium bonding layer and the area of ​​the bonding surface of the aluminum bonding layer is 1:5 to 1:1.

[0084] For example, the ratio between the area of ​​the bonding surface of the germanium bonding layer and the area of ​​the bonding surface of the aluminum bonding layer is any one of 1:5, 1:4, 1:3, 1:2, 1:1 or any value that satisfies the above range.

[0085] In some embodiments, the ratio of the area of ​​the bonding surface of the germanium bonding layer to the area of ​​the bonding surface of the aluminum bonding layer is 1:3.

[0086] In some embodiments, the height of the germanium bonding layer is less than the height of the aluminum bonding layer.

[0087] In some embodiments, the ratio between the height of the germanium bonding layer and the height of the aluminum bonding layer is 0.2:1 to 0.8:1.

[0088] For example, the ratio between the height of the germanium bonding layer and the height of the aluminum bonding layer is any one of 0.2:1, 0.3:1, 0.4:1, 0.5:1, 0.6:1, 0.7:1, 0.8:1 or any value within the above range.

[0089] In some embodiments, the ratio between the height of the germanium bonding layer and the height of the aluminum bonding layer is 0.6:1.

[0090] This height was calculated under bonding temperature of 425℃ and bonding pressure of 1500N. The specific calculation process is as follows:

[0091] The ratio of the height of the germanium bonding layer to the height of the aluminum bonding layer satisfies the following mathematical relationship:

[0092]

[0093] In formula I, t Ge / t Al The metal layer thicknesses of germanium and aluminum, respectively, in at%. Ge / at% Al The percentages of metallic atoms in germanium and aluminum, respectively, ρ Ge / ρ Al The densities A and B are aluminum and germanium, respectively. Ge / A Al These are the atomic weights of germanium and aluminum, respectively. Calculations show that when the thickness ratio of germanium to aluminum is approximately 0.6:1, during aluminum-germanium eutectic bonding, the eutectic layer can just exhaust all the metallic germanium and aluminum, which is beneficial for forming a eutectic alloy and achieving high-strength, hermetic bonding.

[0094] In some embodiments, a barrier layer is provided between the first oxide film layer and the aluminum bonding layer.

[0095] In some embodiments, a barrier layer is provided between the second oxide film layer and the germanium bonding layer.

[0096] In some embodiments, a barrier layer is provided between the first oxide film layer and the aluminum bonding layer, and between the second oxide film layer and the germanium bonding layer.

[0097] The barrier layer is made of titanium nitride and / or titanium.

[0098] In some embodiments, the thickness of the barrier layer is

[0099] In some embodiments, the second oxide film layer comprises an oxide substrate and at least two sets of oxide pillars formed on the surface of the oxide substrate, the oxide pillars enclosing the trench.

[0100] In some embodiments, the groove can be a regular square groove, U-shaped groove, C-shaped groove, L-shaped groove, etc.

[0101] In some embodiments, the groove may also be an irregularly shaped groove.

[0102] In some embodiments, the second oxide film layer further includes oxide bonding regions located between the oxide pillars.

[0103] In some embodiments, the oxide bonding region is located beneath the germanium bonding layer.

[0104] In some embodiments, a monomolecular modification film for reducing the surface energy of the oxide film is formed on the surface of the oxide bonding region, and the monomolecular modification film satisfies the features listed above.

[0105] In some embodiments, a barrier layer is provided between the oxide bonding region and the germanium bonding layer, and the material of the barrier layer is the same as above, which will not be described in detail here.

[0106] In some embodiments, the protrusion is a columnar protrusion, and preferably, the columnar protrusion is made of aluminum.

[0107] In some embodiments, the columnar protrusion can be a regular cylinder, elliptical cylinder, prism, etc.

[0108] In some embodiments, the columnar protrusion may also be an irregular columnar protrusion of other shapes.

[0109] The columnar protrusion and the groove form a misaligned structure on the same horizontal plane. Any degree of misalignment is within the protection scope of this application. The columnar protrusion and the groove may or may not be in direct contact.

[0110] In some embodiments, the bonding structure further includes forming a trench or cavity on the surface of the second wafer away from the first wafer. The trench or cavity is constructed to form a representative MEMS structure, such as a sandwich structure, which is beneficial to improving the piezoelectric sensing performance of the device. Other MEMS devices or stacks can also be superimposed on it.

[0111] A second aspect of this application to achieve the above-mentioned technical effects is to provide a method for forming the bonding structure described in the first aspect, the method comprising:

[0112] Provide the first wafer and the second wafer;

[0113] At least one set of bonding regions and at least two sets of misalignment structures are formed between the first wafer and the second wafer, wherein the misalignment structures are located on both sides of the bonding regions;

[0114] An aluminum bonding layer is formed on the surface of the first wafer, and a germanium bonding layer is formed on the surface of the second wafer. The germanium bonding layer is bonded to the aluminum bonding layer and forms the bonding region.

[0115] Protrusions are formed on both sides of the aluminum bonding layer, and grooves are formed on both sides of the germanium bonding layer. The protrusions extend into the grooves to form the misalignment structure.

[0116] In some embodiments, the method further includes forming a first oxide film layer between the first wafer and the aluminum bonding layer.

[0117] In some embodiments, the method further includes forming a second oxide film layer between the second wafer and the germanium bonding layer.

[0118] In some embodiments, the method further includes forming a first oxide film layer between the first wafer and the aluminum bonding layer and forming a second oxide film layer between the second wafer and the germanium bonding layer.

[0119] In some embodiments, the first oxide film layer and / or the second oxide film layer are formed by patterned etching.

[0120] In some embodiments, the specific process of patterned etching includes main steps such as exposure, development, and etching. The etching process is the next step in the photolithography process, used to remove the bottom areas not covered by the photoresist, leaving only the desired pattern. This process aims to fix the mask pattern onto the photoresist-coated wafer and transfer the photoresist pattern back to the film layer beneath the photoresist. The patterned etching selected in this application is a conventional process, and this application does not impose specific or detailed limitations.

[0121] In some embodiments, the method further includes self-assembling a monomolecular modified film on the surface of the first oxide film layer.

[0122] In some embodiments, the method further includes self-assembling a monomolecular modified film on the surface of the second oxide film layer.

[0123] In some embodiments, the method further includes self-assembling a monomolecular modified film on the surfaces of the first oxide film layer and the second oxide film layer.

[0124] In some embodiments, the monomolecular modified film is formed by a self-assembly process.

[0125] In some embodiments, the specific process of the self-assembly process includes: introducing an appropriate amount of SAMs vapor into the air inlet of a vacuum-sealed cavity, such as an oven, maintaining the oven temperature at approximately 90°C, and processing for 150 minutes. At this point, the surface energy of the oxide film layer modified by the self-assembly process is approximately equal to 1.5 times the eutectic surface energy. It is generally considered that a modification effect ≤ 1.5 times the eutectic surface energy is the desired effect of this application. Typically, the SAMs vapor concentration, temperature, and time are controlled to adjust the surface energy of the oxide film layer modified by the self-assembly process. These adjustment methods are all conventional processes and are not specifically limited in detail in this application.

[0126] In some embodiments, the germanium bonding layer and the aluminum bonding layer are formed by eutectic bonding.

[0127] In some embodiments, the eutectic bonding process between the germanium bonding layer and the aluminum bonding layer includes: (1) a degassing process, (2) an activation process, and (3) a eutectic process.

[0128] The process will be described in detail below.

[0129] (1) Degassing process: Two silicon wafers sputtered with aluminum and glass wafers sputtered with germanium are cleaned before bonding to remove residual impurities on the surface. Then, they are immersed in HF BOE solution for a few seconds to remove surface oxides, and then placed in the bonding machine. The crosshairs of the two wafers are aligned, and the two wafers are fixed in place with wafer clamps. At this time, the bonding machine begins to pre-vacuum, and the temperature begins to rise. When it rises to about 200°C, the bonding machine begins to evacuate the vacuum until the vacuum degree reaches 10-5 Pa. The degassing process is then complete.

[0130] (2) Activation process: The temperature is further increased to approximately 350℃~400℃. At this time, N2 is introduced into the bonding machine as a purification gas. Due to process reasons, silicon and sputtered metal may contain residual impurity gases that are not removed during vacuuming in the gaps and pores. These impurity gases may affect the bonding quality during the bonding process. Therefore, during the activation process, heating and introducing nitrogen can effectively remove the residual impurity gases. The introduced N2 can contain a certain volume fraction of H2, such as 95% N2 and 5% H2. During this process, the two wafers are kept in close contact and aligned using silicon wafer clamps. After the N2 is charged to 1.25 atmospheres, vacuuming is performed again.

[0131] (3) Eutectic Process: The eutectic process officially begins after the two preceding processes are completed. Since the oxides and impurities on the aluminum surface have been removed in the preceding steps, the aluminum and germanium metals can be considered to be in direct contact. At this time, the temperature inside the bonding machine cavity is raised to 450°C, and a pressure of approximately 1500N is applied to both ends of the two silicon wafers and held for 15 minutes. During this process, the aluminum and germanium metals reach the eutectic temperature, and the contact portion of the aluminum and germanium metals becomes molten. The two metals diffuse and dissolve into each other, forming a eutectic layer, which becomes an aluminum-germanium liquid phase alloy layer. As time goes on, the diffusion depth of the liquid phase portion of aluminum and germanium increases. The liquid aluminum comes into contact with the germanium that has not yet entered the liquid phase, and the liquid germanium also comes into contact with the aluminum that has not yet entered the liquid phase, thus forming a new eutectic layer. Therefore, the liquid phase alloy layer continues to thicken, eventually consuming all the metals and forming a mechanically mixed alloy material. After the eutectic process is completed, cooling and venting are performed. At this time, the silicon wafer clamps are not loosened, and the position of the silicon wafers remains unchanged. Once the temperature of the bonding machine drops to room temperature and the gas pressure inside the wall returns to normal atmospheric pressure, the silicon wafer clamps can be loosened, the silicon wafers can be removed, and the eutectic process can be completed.

[0132] In some embodiments, the barrier layer is formed by sputtering or other methods.

[0133] In some embodiments, the method further includes etching a trench or cavity on the surface of the second wafer opposite to the first wafer.

[0134] In some embodiments, the specific method for forming the bonding structure is as described in the following examples.

[0135] A third aspect of this application to achieve the aforementioned technical effects is to provide a MEMS sensor. The MEMS sensor includes the bonding structure described in the first aspect or the bonding structure formed by the method described in the second aspect, and may further include stacked layers of other MEMS devices to improve the piezoelectric performance of the entire device. The MEMS sensor is a piezoelectric MEMS sensor.

[0136] A fourth aspect of this application to achieve the aforementioned technical effects is to provide a wearable device that includes the MEMS sensor described in the third aspect.

[0137] Exemplary embodiments of the present disclosure will now be described in more detail with reference to the accompanying drawings. While exemplary embodiments of the present disclosure are shown in the drawings, it should be understood that the present disclosure may be implemented in various forms and should not be limited to the embodiments set forth herein. Rather, these embodiments are provided so that this disclosure will be thorough and complete, and will fully convey the scope of the disclosure to those skilled in the art.

[0138] Example 1

[0139] A bonding structure is provided, which is as follows: Figure 1As shown, taking only a single bonding structure as an example, it actually contains several arrayed structures.

[0140] It includes a first wafer 100 and a second wafer 200. At least one set of bonding regions 300 and at least two sets of misalignment structures 400 are provided between the first wafer 100 and the second wafer 200, and the misalignment structures 400 are located on both sides of the bonding regions 300. The bonding regions 300 include an aluminum bonding layer 301 formed on the surface of the first wafer 100 and a germanium bonding layer 302 formed on the surface of the second wafer 200. The germanium bonding layer 302 is bonded to the aluminum bonding layer 301. The misalignment structures 400 include protrusions 401 located on both sides of the aluminum bonding layer 301 and trenches 402 located on both sides of the germanium bonding layer 302. The protrusions 401 extend into the trenches 402 to form the misalignment structures 400.

[0141] The bonding structure itself has good robustness and stability. The misalignment structure effectively restricts the flow range of aluminum-germanium eutectic by surrounding the bonding area in all directions.

[0142] Example 2

[0143] A bonding structure is provided, which is as follows: Figure 2 As shown, taking only a single bonding structure as an example, it actually contains several arrayed structures.

[0144] It is provided in Example 1 Figure 1 Based on the structure, it includes a first oxide film layer 500 arranged between the first wafer 100 and the aluminum bonding layer 301 and / or a second oxide film layer 600 arranged between the second wafer 200 and the germanium bonding layer 302; preferably, the first oxide film layer and the second oxide film layer are made of silicon dioxide.

[0145] It also includes forming a monomolecular modification film 700 on the surface of the first oxide film layer 500 and / or the second oxide film layer 600 to reduce the surface energy of the oxide film layer. Compared with the bonding interface, the monomolecular modification film 700 has a low surface energy, which is not conducive to the spread of aluminum-germanium eutectic on its surface. Therefore, it helps to further enhance the range of eutectic flow and is conducive to obtaining a clean bonding interface.

[0146] Meanwhile, the area of ​​the bonding surface of the germanium bonding layer 302 is smaller than the area of ​​the bonding surface of the aluminum bonding layer 301; preferably, the ratio between the area of ​​the bonding surface of the germanium bonding layer 302 and the area of ​​the bonding surface of the aluminum bonding layer 301 is 1:3; the height of the germanium bonding layer 302 is smaller than the height of the aluminum bonding layer 301; preferably, the ratio between the height of the germanium bonding layer 302 and the height of the aluminum bonding layer 301 is 0.6:1.

[0147] The germanium bonding layer and aluminum bonding layer with the required area-to-height ratio are conducive to the formation of a eutectic alloy during eutectic bonding, and help ensure the high strength and hermeticity of the eutectic alloy bonding.

[0148] Example 3

[0149] A bonding structure is provided, which is as follows: Figure 3 As shown, taking only a single bonding structure as an example, it actually contains several arrayed structures.

[0150] It is provided in Example 2 Figure 2 Based on the structure, a barrier layer 800 is provided between the first oxide film layer 500 and the aluminum bonding layer 301 and / or a barrier layer 800 is provided between the second oxide film layer 600 and the germanium bonding layer 302; preferably, the material of the barrier layer includes titanium nitride and / or titanium.

[0151] This barrier layer not only ensures adhesion between aluminum-germanium metal and the wafer, but also effectively prevents the metal from penetrating into the wafer during subsequent pressurization processes.

[0152] Example 4

[0153] A method was disclosed Figure 4 The structure shown includes a first wafer 100 and a second wafer 200. At least one set of bonding regions 300 and at least two sets of misalignment structures 400 are provided between the first wafer 100 and the second wafer 200, and the misalignment structures 400 are located on both sides of the bonding regions 300.

[0154] The bonding region 300 includes a first oxide film layer 500, a barrier layer 800, and an aluminum bonding layer 301 sequentially formed on the surface of the first wafer 100, and a second oxide film layer 600, a barrier layer 800, and a germanium bonding layer 302 sequentially formed on the surface of the second wafer 200, wherein the germanium bonding layer 302 is bonded to the aluminum bonding layer 301.

[0155] The misalignment structure 400 includes protrusions 401 on both sides of the aluminum bonding layer 301. The protrusions 401 are columnar protrusions, preferably aluminum column protrusions. Grooves 402 are formed on both sides of the germanium bonding layer 302. The grooves 402 are surrounded by oxide pillars. The protrusions 401 extend into the grooves 402 to form the misalignment structure 400.

[0156] Meanwhile, a monomolecular modification film 700 for reducing the surface energy of the oxide film is formed on the surface of the first oxide film layer 500 and / or the second oxide film layer 600.

[0157] Example 5

[0158] Provides a Figure 4The method for forming the bonded structure shown includes the following steps:

[0159] a) such as Figure 5 As shown in Figure a, oxide patterning etching is first performed on the second wafer. The oxide pillars are 5 μm high, and the cavity formed by the oxide pillars is also 5 μm deep. The oxide bonding region with a relatively low height is set between the oxide pillars. Its height is 4 μm, and its length × width is 30 μm × 30 μm.

[0160] b) Using the lift-off process Figure 5 b Deposition of a layer and a 0.6µm germanium metal layer; the pattern of the germanium metal layer is length × width = 25µm × 25µm;

[0161] c) such as Figure 5 As shown in c, the back of the MEMS is subjected to DRIE deep silicon etching and other processes to obtain a deep trench with length × width × height = 200um × 200um × 5um.

[0162] d) such as Figure 5 As shown in d, the surface energy of the oxide film surface after self-assembly process modification by performing OTS SAMs vapor phase fumigation on the MEMS wafer is approximately 1.5 times that of the eutectic surface energy.

[0163] e) such as Figure 5 As shown in e, sputtering is performed on the surface of the aforementioned CMOS wafer. A layer of 1µm aluminum metal film with uniform thickness, sputtered by magnetron sputtering;

[0164] f) Subsequently, photolithography is used to expose and develop the predetermined pattern to obtain the area to be etched. The aluminum is then etched using dry or wet methods, with titanium nitride as the etching stop layer. The photoresist is then removed using dry or wet methods. After cleaning, the aluminum layer pattern is obtained, resulting in a 6µm high protrusion (aluminum pillar). The oxide film layer contains a length × width of 70µm × 70µm. Then, OTS SAMs vapor phase fumigation treatment is performed, with the same treatment effect as step d).

[0165] g) The above wafer was subjected to aluminum-germanium bonding treatment (conditions: 425℃, 1500N, holding voltage for 30 minutes), which ultimately achieved a high-precision bonding interface, such as... Figure 6 The breakthrough bonding region is 25µm and below.

[0166] Comparative Example

[0167] The difference from Embodiment 5 of this application is that the misalignment structure shown in this application is not provided.

[0168] Figure 6Images of the bonding structure in the bonding region obtained in Embodiment 5 and the comparative example of this application are shown in conjunction with... Figure 6 It is evident that this application can achieve smaller bonding size and higher bonding accuracy.

[0169] In summary, the bonding structure provided in this application solves the problems of eutectic flow and extension phenomena in aluminum-germanium eutectic bonding in existing piezoelectric MEMS sensors, which lead to difficulties in controlling the bonding process window and uniformity, as well as insufficient bonding precision and large size. It provides a bonding structure with better robustness, stability, and bonding precision, such as controlling the bonding area to 25µm or less. Piezoelectric MEMS sensors incorporating this bonding structure have good application prospects in wearable devices.

[0170] It should be understood that the terminology used herein is for the purpose of describing particular exemplary embodiments only and is not intended to be limiting. Unless the context clearly indicates otherwise, the singular forms “a,” “an,” and “described” as used herein may also include the plural forms. The terms “comprising,” “including,” “containing,” and “having” are inclusive and therefore indicate the presence of the stated features, steps, operations, elements, and / or components, but do not exclude the presence or addition of one or more other features, steps, operations, elements, components, and / or combinations thereof. The method steps, processes, and operations described herein are not construed as requiring them to be performed in a particular order described or illustrated unless the order of performance is explicitly indicated. It should also be understood that additional or alternative steps may be used.

[0171] The above description is merely a preferred embodiment of this application, but the scope of protection of this application is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in this application should be included within the scope of protection of this application. Therefore, the scope of protection of this application should be determined by the scope of the claims.

Claims

1. A bonded structure, comprising: The bonding structure includes: First wafer and second wafer; At least one set of bonding regions and at least two sets of misalignment structures are provided between the first wafer and the second wafer, and the misalignment structures are located on both sides of the bonding regions; The bonding region includes an aluminum bonding layer formed on the surface of the first wafer and a germanium bonding layer formed on the surface of the second wafer, wherein the germanium bonding layer is bonded to the aluminum bonding layer. The misalignment structure includes protrusions on both sides of the aluminum bonding layer and grooves on both sides of the germanium bonding layer, wherein the protrusions extend into the grooves to form the misalignment structure; The bonding structure further includes a first oxide film layer disposed between the first wafer and the aluminum bonding layer and / or a second oxide film layer disposed between the second wafer and the germanium bonding layer; The second oxide film layer includes an oxide substrate and at least two sets of oxide pillars formed on the surface of the oxide substrate, the oxide pillars enclosing the trench; The protrusion is a columnar protrusion, and the columnar protrusion is made of aluminum; The surface of the first oxide film layer and / or the second oxide film layer is formed with a monomolecular modification film for reducing the surface energy of the oxide film layer; The first oxide film layer and the second oxide film layer are made of any one or more of doped silicon dioxide, undoped silicon dioxide, or ethyl silicate. The undoped silicon dioxide is USG, the doped silicon dioxide is any one of PSG or BPSG, and the ethyl silicate is PETEOS. The monomolecular modified film is a monomolecular layer formed by an oxide film layer and a surfactant, wherein the surfactant is an organosilane.

2. The bonded structure of claim 1, wherein, The area of ​​the bonding surface of the germanium bonding layer is smaller than the area of ​​the bonding surface of the aluminum bonding layer; The ratio of the area of ​​the bonding surface of the germanium bonding layer to the area of ​​the bonding surface of the aluminum bonding layer is 1:5 to 1:

1. Furthermore, the height of the germanium bonding layer is less than the height of the aluminum bonding layer; The ratio between the height of the germanium bonding layer and the height of the aluminum bonding layer is 0.2:1 to 0.8:

1.

3. The bonded structure of Claim 2, wherein, A barrier layer is provided between the first oxide film layer and the aluminum bonding layer and / or a barrier layer is provided between the second oxide film layer and the germanium bonding layer; The material of the barrier layer includes titanium nitride and / or titanium; The thickness of the barrier layer is 200 Å to 300 Å.

4. A method for forming the bonded structure according to any one of claims 1 to 3, characterized by, The method includes: Provide the first wafer and the second wafer; At least one set of bonding regions and at least two sets of misalignment structures are formed between the first wafer and the second wafer, wherein the misalignment structures are located on both sides of the bonding regions; An aluminum bonding layer is formed on the surface of the first wafer, and a germanium bonding layer is formed on the surface of the second wafer. The germanium bonding layer is bonded to the aluminum bonding layer and forms the bonding region. Protrusions are formed on both sides of the aluminum bonding layer, and grooves are formed on both sides of the germanium bonding layer. The protrusions extend into the grooves to form the misalignment structure.

5. The method of claim 4, wherein, The method further includes forming a first oxide film layer between the first wafer and the aluminum bonding layer and / or forming a second oxide film layer between the second wafer and the germanium bonding layer; The surfaces of the first oxide film layer and / or the second oxide film layer self-assemble to form a monomolecular modified film; The monomolecular modified film is a monomolecular layer formed by an oxide film layer and a surfactant, wherein the surfactant is an organosilane.

6. A MEMS sensor, characterized by The sensor comprises the bonding structure according to any one of claims 1 to 3 or the bonding structure prepared by the method according to any one of claims 4 to 5; The MEMS sensor is a piezoelectric MEMS sensor.

7. A wearable device, characterized in that, The device includes the sensor described in claim 6.

Citation Information

Patent Citations

  • Aluminum-germanium eutectic bonding method