Semiconductor thin film and method for growing the same

By employing a multilayer semiconductor thin film growth method in surface acoustic wave filters, and utilizing the oxygen-rich region and air gap design of aluminum nitride thin films, the dislocation problem of polycrystalline thin film materials was solved, thereby improving the performance of the device.

CN116470874BActive Publication Date: 2026-11-24CEC COMPOUND SEMICON CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202310093400.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-18
Publication Date
2026-11-24
Estimated Expiration
2043-01-18

AI Technical Summary

Technical Problem

In the prior art, the polycrystalline thin film materials used in surface acoustic wave filters have an amorphous transition region, which leads to a decrease in the device's quality factor, increases acoustic wave transmission loss, and limits device performance.

Method used

A multilayer semiconductor thin film growth method is employed, comprising a substrate, a buffer layer, bumps, and multiple semiconductor layers. By controlling the molar ratio of nitrogen to aluminum and annealing, oxygen-rich regions and gas gaps are formed, dislocations are terminated or bent, thereby improving the quality of aluminum nitride thin films.

Benefits of technology

Low dislocation density and high quality aluminum nitride thin films have been achieved, improving the performance of acoustic wave devices, especially in acoustic filters.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116470874B_ABST
    Figure CN116470874B_ABST
Patent Text Reader

Abstract

This invention provides a semiconductor thin film and its growth method. The semiconductor thin film includes at least: a substrate; a first buffer layer located on the surface of the substrate; a second buffer layer located on the surface of the first buffer layer; a plurality of protrusions located on the surface of the second buffer layer; a first semiconductor layer located on the surfaces of the second buffer layer and the protrusions; a second semiconductor layer located on the surface of the first semiconductor layer; and a third semiconductor layer located on the surface of the second semiconductor layer. The semiconductor thin film and its growth method provided by this invention can effectively improve the quality of the thin film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of acoustic device materials technology, specifically to a semiconductor thin film and its growth method. Background Technology

[0002] Surface Acoustic Wave (SAW) filters are frequency-selective devices fabricated using the surface acoustic wave effect and resonance characteristics. SAW filters utilize semiconductor materials with a hexagonal zinc-piston structure, which possess advantages such as high longitudinal acoustic velocity, high thermal conductivity, good dielectric properties, and a low coefficient of thermal expansion. Semiconductor materials oriented along the c-axis exhibit excellent piezoelectricity and high-speed SAW propagation performance, making them superior piezoelectric materials for SAW devices.

[0003] However, the semiconductor materials used in surface acoustic wave (SAW) filters are mainly obtained through magnetron sputtering and are polycrystalline thin film materials. Polycrystalline thin films typically have an amorphous transition region of a certain thickness, which reduces the device's quality factor (Q value), increases acoustic wave transmission loss, and is detrimental to acoustic wave transmission, thus limiting the device's performance. Summary of the Invention

[0004] This invention proposes a semiconductor thin film and its growth method, which can obtain aluminum nitride thin films with low dislocation density and high quality, thereby improving the performance of devices.

[0005] To solve the above-mentioned technical problems, the present invention is achieved through the following technical solution:

[0006] This invention proposes a semiconductor thin film comprising at least:

[0007] Substrate;

[0008] A first buffer layer is located on the surface of the substrate;

[0009] A second buffer layer is located on the surface of the first buffer layer;

[0010] Multiple protrusions, the multiple protrusions being located on the surface of the second buffer layer;

[0011] A first semiconductor layer is located between the second buffer layer and the protruding surface;

[0012] A second semiconductor layer, the second semiconductor layer being located on the surface of the first semiconductor layer; and

[0013] A third semiconductor layer is located on the surface of the second semiconductor layer.

[0014] In one embodiment of the present invention, the protrusion is made of aluminum nitride.

[0015] In one embodiment of the present invention, the protrusion is a semi-ellipsoidal sphere, and the major axis of the protrusion is 50-600nm, the minor axis is 20-400nm, and the height is 10-500nm.

[0016] In one embodiment of the present invention, the surface roughness of the third semiconductor layer is 0.68 nm.

[0017] The present invention also proposes a method for growing semiconductor thin films, comprising at least the following steps:

[0018] Provide a substrate;

[0019] A first buffer layer is formed on the surface of the substrate;

[0020] A second buffer layer is formed on the surface of the first buffer layer;

[0021] The second buffer layer is patterned to form multiple protrusions on its surface;

[0022] A first semiconductor layer is formed in the second buffer layer and the protruding surface;

[0023] A second semiconductor layer is formed on the surface of the first semiconductor layer; and

[0024] A third semiconductor layer is formed on the surface of the second semiconductor layer.

[0025] In one embodiment of the present invention, the step of forming the second buffer layer includes:

[0026] The first buffer layer is subjected to a first annealing treatment to form a first oxygen-rich zone within the first buffer layer;

[0027] A second buffer layer is formed on the surface of the first buffer layer after annealing; and

[0028] The second buffer layer is subjected to a second annealing process to form a second oxygen-rich zone within the second buffer layer.

[0029] In one embodiment of the present invention, the step of forming a plurality of protrusions on the surface of the second buffer layer includes:

[0030] A photoresist layer is formed on the surface of the second buffer layer;

[0031] The photoresist layer is exposed and developed to form a patterned photoresist layer, in which multiple openings are formed;

[0032] Aluminum nitride material is deposited within the opening to form a thin film; and

[0033] The thin film is etched to form protrusions.

[0034] In one embodiment of the present invention, the molar ratio of nitrogen to aluminum in the step of forming the first semiconductor layer is (100-5000):1.

[0035] In one embodiment of the present invention, in the step of forming the second semiconductor layer, the molar ratio of nitrogen to aluminum is (100-1000):1.

[0036] In one embodiment of the present invention, in the step of forming the third semiconductor layer, the molar ratio of nitrogen to aluminum is (500-1000):1, and the reaction temperature is 1200-1400℃.

[0037] This invention proposes a semiconductor thin film and its growth method, which can alleviate the crystal mismatch between the aluminum nitride thin film and the substrate, and can effectively reduce or stop dislocations during the growth process of the aluminum nitride thin film, thereby improving the growth quality of the aluminum nitride thin film and improving the performance of the device. Attached Figure Description

[0038] Figure 1 This is a flowchart of a semiconductor thin film growth method according to the present invention.

[0039] Figure 2 This is a schematic diagram of the structure of the first buffer layer in this invention.

[0040] Figure 3 This is a schematic diagram of the structure of the first oxygen-enriched region in this invention.

[0041] Figure 4 This is a schematic diagram of the structure of the second buffer layer in this invention.

[0042] Figure 5 This is a schematic diagram of the patterned photoresist layer in this invention.

[0043] Figure 6 This is a schematic diagram of the protrusion structure in this invention.

[0044] Figure 7 This is a top view of the protrusion in this invention.

[0045] Figure 8 This is a schematic diagram of the structure of the first semiconductor layer in this invention.

[0046] Figure 9 This is a schematic diagram of the structure of the second semiconductor layer in this invention.

[0047] Figure 10 This is a schematic diagram of the structure of the third semiconductor layer in this invention.

[0048] Figure 11 This is an atomic force microscope image of the third semiconductor layer in this invention.

[0049] 100, Substrate; 200, First buffer layer; 210, First oxygen-rich region; 300, Second buffer layer; 310, Second oxygen-rich region; 400, Patterned photoresist layer; 401, Opening; 500, Protrusion; 600, First semiconductor layer; 601, Air gap; 700, Second semiconductor layer; 800, Third semiconductor layer. Detailed Implementation

[0050] The following specific examples illustrate the implementation of the present invention. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and various details in this specification can also be modified or changed based on different viewpoints and applications without departing from the spirit of the present invention.

[0051] It should be noted that the illustrations provided in this embodiment are only schematic representations of the basic concept of the present invention. Therefore, the drawings only show the components related to the present invention and are not drawn according to the actual number, shape and size of the components in the actual implementation. In the actual implementation, the form, quantity and proportion of each component can be arbitrarily changed, and the layout of the components may also be more complex.

[0052] The technical solution of the present invention will be further described in detail below with reference to several embodiments and accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0053] Acoustic filters, characterized by high performance, small size, high operating frequency, and industrial-scale manufacturing capabilities, are widely used in base stations, radar, navigation, mobile communications, and digital electronics, especially in the rapidly developing 5G field. This invention proposes a semiconductor thin film and its growth method, which can obtain low dislocation density and high-quality aluminum nitride thin films, enabling their use in acoustic filtering devices and improving device performance.

[0054] Please see Figure 1 As shown, the present invention proposes a semiconductor thin film and its growth method, including but not limited to the following steps S100-S700.

[0055] S100, providing a substrate.

[0056] S200, A first semiconductor layer is formed on the substrate surface.

[0057] S300, A second buffer layer is formed on the surface of the first buffer layer.

[0058] S400: The second buffer layer is patterned to form multiple protrusions on the surface of the second buffer layer.

[0059] S500, a first semiconductor layer is formed on the second buffer layer and the raised surface.

[0060] S600, a second semiconductor layer is formed on the surface of the first semiconductor layer.

[0061] S700, a third semiconductor layer is formed on the surface of the second semiconductor layer.

[0062] Please see Figure 1 and Figure 2 As shown, in one embodiment of the present invention, in step S100, the substrate 100 is selected, for example, from sapphire, silicon carbide substrate, or silicon substrate. In this embodiment, the substrate 100 is selected, for example, from a sapphire substrate.

[0063] Please see Figure 1 and Figure 2 As shown, in one embodiment of the present invention, in step S200, a first buffer layer 200 is deposited on the substrate 100 using, for example, a physical vapor deposition (PVD) process. Specifically, the substrate 100 is placed on a magnetron sputtering machine for magnetron sputtering, and a low content of oxygen is introduced during sputtering, with an oxygen flow rate of, for example, 0.01-0.2 L / min, to deposit the first buffer layer 200 on the surface of the substrate 100, and the thickness of the first buffer layer 200 is, for example, 100-550 nm.

[0064] Please see Figures 1 to 3 As shown, in one embodiment of the present invention, in step S200, after depositing the first buffer layer 200 on the substrate 100, the substrate 100 can be subjected to a first annealing treatment, for example. Specifically, the substrate 100 is placed in a high-temperature annealing furnace, nitrogen (N2) is introduced into the furnace tube, and annealing is performed at a temperature of 1650-1750°C for 0.5-1.5 hours. After the first annealing treatment, the substrate 100 and the first buffer layer 200 form a sapphire-AlN composite substrate, on which an AlN thin film is grown. The lattice is rearranged, which can better alleviate the problem of lattice mismatch. Furthermore, after the first annealing treatment, a first oxygen-rich region 210 is formed in the first buffer layer 200, and the first oxygen-rich region 210 is located in the middle region of the first buffer layer 200. The oxygen-rich region contains a high concentration of aluminum oxide compounds, which causes AlN to undergo polarity reversal in the oxygen-rich region and grow towards the Al polar face. This is more conducive to the subsequent growth of AlN materials, and at the same time, it will cause the dislocations formed by the AlN film deposited by the PVD process to terminate or redirect.

[0065] Please see Figures 1 to 4As shown, in one embodiment of the present invention, in step S300, after the first buffer layer 200 is formed, a second buffer layer 300 is formed on the surface of the first buffer layer 200, and the second buffer layer 300 is deposited on the first buffer layer 200, for example, using a physical vapor deposition process. Specifically, the substrate 100 is placed on a magnetron sputtering machine for magnetron sputtering, and a low content of oxygen is introduced during sputtering, with an oxygen flow rate of, for example, 0.01-0.2 L / min. The second buffer layer 300 is deposited on the surface of the first buffer layer 200, and the thickness of the second buffer layer 300 is, for example, 50-500 nm.

[0066] Please see Figures 1 to 4 As shown, in one embodiment of the present invention, in step S300, after depositing the second buffer layer 300 on the surface of the first buffer layer 200, the substrate 100 can be subjected to a second annealing treatment, for example. Specifically, the substrate 100 is placed in a high-temperature annealing furnace, nitrogen gas is introduced into the furnace tube, and annealing is performed at a temperature of 1650-1750°C for 0.5-1.5 hours. After the second annealing treatment, the lattice is rearranged, further alleviating the lattice mismatch problem. Furthermore, after the second annealing treatment, a second oxygen-rich region 310 is formed in the second buffer layer 300, located in the middle region of the second buffer layer 300. The oxygen-rich region contains a high concentration of aluminum oxide compounds, causing AlN to undergo polarity reversal in the oxygen-rich region, turning towards the Al polar face for growth. This is more conducive to the subsequent growth of AlN materials, and also causes the dislocations formed by the AlN thin film deposited by the PVD process to terminate or redirect.

[0067] Please see Figure 1 , Figure 5 , Figure 6 and Figure 7As shown, in one embodiment of the present invention, in step S400, the second buffer layer 300 is patterned using processes such as masking, exposure, development, and photolithography. Specifically, for example, a photoresist layer is deposited on the surface of the second buffer layer 300 using a spin coating process. After exposure and development, a patterned photoresist layer 400 is formed, and multiple openings 401 are formed in the patterned photoresist layer 400, exposing the second buffer layer 300. Then, for example, aluminum nitride material is deposited in the openings 401 using a low-temperature deposition technique to form a thin film. Using the patterned photoresist layer 400 as a mask, the thin film is etched to form protrusions 500. The protrusions 500 are made of the same material as the subsequently deposited semiconductor layer, and homoepitaxial growth is beneficial for better growth of the subsequent semiconductor layer. After the protrusions 500 are formed, the patterned photoresist layer 400 is removed. Specifically, for example, dry etching is used to etch towards the substrate 100 to form bumps 500, and the etching gas includes, for example, one or a mixture of several of chlorine (Cl2), trifluoromethane (CHF3), difluoromethane (CH2F2), nitrogen trifluoride (NF3), sulfur hexafluoride (SF6), hydrogen bromide (HBr), or nitrogen (N2). After forming bumps 500, the substrate 100 is cleaned, for example, with a mixed solution of concentrated sulfuric acid (H2SO4) and hydrogen peroxide (H2O2) to remove the patterned photoresist layer 400. In one embodiment of the present invention, the concentration of H2SO4 is, for example, 90%-98%, the concentration of H2O2 is, for example, 30%-40%, and the volume ratio of H2SO4 to H2O2 is, for example, 2:1-4:1.

[0068] Please see Figure 1 , Figure 5 , Figure 6 and Figure 7 As shown, in one embodiment of the present invention, the protrusion 500 is, for example, conical, hemispherical, semi-ellipsoidal, or columnar. In this embodiment, the protrusion 500 is, for example, a semi-ellipsoidal shape, with a major axis L of, for example, 50-600 nm, a minor axis D of, for example, 20-400 nm, a height H of, for example, 10-500 nm, a long period X1 (i.e., the interval between two adjacent columns of protrusions) of, for example, 0-1000 nm, and a short period X2 (i.e., the interval between two adjacent rows of protrusions) of, for example, 0-500 nm.

[0069] Please see Figure 1 and Figure 8As shown, in one embodiment of the present invention, in step S500, after the protrusion 500 is formed, a first semiconductor layer 600 is deposited on the surface of the second buffer layer 300 and the protrusion 500, for example, using a metal-organic chemical vapor deposition (MOCVD) process. Specifically, the substrate 100 is placed in a furnace tube, using trimethylaluminum (TMAl) as the Al source and ammonia (NH3) as the N source, and a mixed gas of TMAl, NH3, and high-purity hydrogen (H2) is introduced into the furnace tube, wherein hydrogen is used as the carrier gas, and the molar ratio of N to Al (i.e., V / V molar ratio) is, for example, (100-5000):1. The growth pressure is set to, for example, 10-100 mbar, and the reaction temperature is set to, for example, 1000-1200 °C. Under these reaction conditions, the growth rate of AlN is less than Furthermore, the thickness of the first semiconductor layer 600 is, for example, 50-500 nm. During the deposition of the first semiconductor layer 600, the AlN lateral growth rate is relatively slow, which helps to reduce the generation of dislocations, especially screw dislocations. Also, due to the presence of the protrusions 500, small and dense air gaps 601 are formed in the first semiconductor layer 600. Further, the air gaps 601 are, for example, elliptical. The presence of the air gaps 601 can reduce dislocations generated during subsequent AlN growth or cause dislocations to bend or annihilate.

[0070] Please see Figure 1 and Figure 9 As shown, in one embodiment of the present invention, in step S600, after the formation of the first semiconductor layer 600, a second semiconductor layer 700 is formed on the surface of the first semiconductor layer 600 using MOCVD technology, and the reaction conditions are changed. Specifically, trimethylaluminum (TMAl) is used as the Al source, ammonia (NH3) is used as the N source, and a mixed gas of TMAl, NH3, and high-purity hydrogen (H2) is continuously introduced into the furnace tube. The molar ratio of N to Al is, for example, (100-1000):1, the growth pressure is set to, for example, 10-100 mbar, and the reaction temperature is set to, for example, 1200-1400 °C. Under these reaction conditions, the growth rate of AlN is greater than... Furthermore, the thickness of the second semiconductor layer 700 is, for example, 200-3000 nm. During this process, the rapid growth of AlN allows dislocations to bend, thereby preventing them from continuing to extend upwards.

[0071] Please see Figure 1 , Figures 8 to 11As shown, in one embodiment of the present invention, in step S700, after the formation of the second semiconductor layer 700, a third semiconductor layer 800 is formed on the surface of the second semiconductor layer 700 using MOCVD technology, and the reaction conditions are changed again. Specifically, trimethylaluminum (TMAl) is used as the Al source, ammonia (NH3) is used as the N source, and a mixed gas of TMAl, NH3, and high-purity hydrogen (H2) is continuously introduced into the furnace tube. The molar ratio of N to Al is, for example, (500-1000):1, the growth pressure is set to, for example, 10-100 mbar, and the reaction temperature is set to, for example, 1200-1400 °C. Under these reaction conditions, the growth rate of AlN is... Furthermore, the thickness of the third semiconductor layer 800 is, for example, 50-500 nm. Due to the presence of the air gap 601, the small and dense air gaps converge and coalesce within a very thin thickness, thereby causing dislocation termination or bending, thus reducing the dislocation density. Moreover, during the deposition of the third semiconductor layer 800, the molar ratio of N to Al is greater than 500, which improves the surface morphology of the third semiconductor layer 800, thereby improving its surface roughness. Atomic force microscopy (AFM) images of the third semiconductor layer 800 show that its surface is smooth and crack-free, with reduced defect density, and a surface roughness of, for example, 0.68 nm.

[0072] The aluminum nitride thin film prepared by the above-mentioned growth method in this invention has the advantages of low dislocation density and high quality, and can be used to make semiconductor devices such as acoustic filters. Moreover, this semiconductor device has very good piezoelectricity and high-speed propagation performance of surface acoustic waves, and can be applied to base stations, radar, navigation, mobile communication and digital electronics, especially in the 5G field.

[0073] In summary, this invention proposes a semiconductor thin film and its growth method. First, one or more aluminum nitride layers are deposited on a substrate surface using a PVD process and then subjected to high-temperature annealing to alleviate lattice mismatch between the subsequent aluminum nitride thin film and the substrate. An oxygen-rich region is formed within this aluminum nitride layer, causing dislocations formed during the PVD deposition to terminate or redirect, which is beneficial for the subsequent growth of aluminum nitride materials. By forming protrusions within this aluminum nitride layer, and then depositing an aluminum nitride thin film on these protrusions using an MOCVD process, small and dense air gaps are formed. These air gaps converge and coalesce within a very thin thickness, causing dislocation termination or bending, thereby reducing dislocation density. Further deposition of an aluminum nitride thin film on this aluminum nitride layer containing air gaps, by controlling the molar ratio of N to Al to be greater than 500, can improve the surface roughness of the final aluminum nitride thin film, thereby improving the deposition quality of the aluminum nitride thin film and ultimately enhancing device performance.

[0074] The above description is merely a preferred embodiment of this application and an explanation of the technical principles used. Those skilled in the art should understand that the scope of the invention involved in this application is not limited to the technical solutions formed by a specific combination of the above-mentioned technical features, but should also cover other technical solutions formed by any combination of the above-mentioned technical features or their equivalent features without departing from the inventive concept. For example, technical solutions formed by replacing the above-mentioned features with technical features with similar functions disclosed in this application (but not limited to) each other.

[0075] Apart from the technical features described in the specification, the other technical features are known to those skilled in the art. To highlight the innovative features of this invention, the other technical features will not be described in detail here.

Claims

1. A method for growing a semiconductor thin film, characterized in that, At least the following steps are included: Provide a substrate; A first buffer layer is formed on the surface of the substrate; Forming a second buffer layer on the surface of the first buffer layer includes: performing a first annealing treatment on the first buffer layer to form a first oxygen-rich region within the first buffer layer; forming a second buffer layer on the surface of the annealed first buffer layer; and performing a second annealing treatment on the second buffer layer to form a second oxygen-rich region within the second buffer layer. The second buffer layer is patterned to form multiple protrusions on its surface; A first semiconductor layer is formed in the second buffer layer and the protruding surface; wherein the molar ratio of nitrogen to aluminum is (100-5000):1, and the growth rate of AlN is less than 1 Å / s; A second semiconductor layer is formed on the surface of the first semiconductor layer; wherein the molar ratio of nitrogen to aluminum is (100-1000):1, and the growth rate of AlN is greater than 2 Å / s; and A third semiconductor layer is formed on the surface of the second semiconductor layer; wherein the molar ratio of nitrogen to aluminum is (500-1000):1, and the growth rate of AlN is 1-2 Å / s.

2. The method for growing a semiconductor thin film according to claim 1, characterized in that, The step of forming multiple protrusions on the surface of the second buffer layer includes: A photoresist layer is formed on the surface of the second buffer layer; The photoresist layer is exposed and developed to form a patterned photoresist layer, in which multiple openings are formed; Aluminum nitride material is deposited within the opening to form a thin film; and The thin film is etched to form protrusions.

3. The method for growing a semiconductor thin film according to claim 1, characterized in that, In the step of forming the third semiconductor layer, the reaction temperature is 1200-1400°C.

4. A semiconductor thin film produced by the growth method of a semiconductor thin film according to any one of claims 1-3, characterized in that, At least including: Substrate; A first buffer layer is located on the surface of the substrate; A second buffer layer is located on the surface of the first buffer layer; Multiple protrusions, the multiple protrusions being located on the surface of the second buffer layer; A first semiconductor layer is located between the second buffer layer and the protruding surface; A second semiconductor layer, the second semiconductor layer being located on the surface of the first semiconductor layer; and A third semiconductor layer is located on the surface of the second semiconductor layer.

5. A semiconductor thin film according to claim 4, characterized in that, The protrusion is made of aluminum nitride.

6. A semiconductor thin film according to claim 4, characterized in that, The protrusion is a semi-ellipsoid, with a major axis of 50-600 nm, a minor axis of 20-400 nm, and a height of 10-500 nm.

7. A semiconductor thin film according to claim 4, characterized in that, The surface roughness of the third semiconductor layer is 0.68 nm.

Citation Information

Patent Citations

  • Growth method of GaN light emitting diode LED (Light-Emitting Diode) epitaxial wafer

    CN110504340A