Interlayer filler fiber material and method of making same
By using a sandwich structure and hot-melt bonding technology for low-melting-point polyester fibers, the problems of bedding filling materials being difficult to restore their fluffiness after vacuum compression and the poor stability of pearl cotton materials have been solved, resulting in a sandwich filling fiber material with high stability and high resilience.
Patent Information
- Application Number
- CN202310467342.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-27
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-04-27
AI Technical Summary
Existing bedding filling materials are difficult to restore to their fluffy state after vacuum compression, and pearl cotton material has poor stability and is prone to movement.
The sandwich structure is adopted, and the fiber flakes and fiber clusters are thermally bonded together by low melting point polyester fibers to form a sandwich filling fiber material with high stability and high resilience.
It improves the stability and resilience of bedding filling materials, solves the problem of materials being difficult to restore their fluffiness after vacuum compression, and prevents the movement of pearl cotton materials.
Abstract
Description
Technical Field
[0001] This invention relates to the field of new materials, specifically to filling materials for bedding. Background Technology
[0002] Most bedding products use multi-layered wadding as filling material. Products made with this material have the problem of low fluffiness and resilience, especially after vacuum compression packaging, it is difficult to restore the fluffiness. Some products also use pearl cotton as filling material. Products made with this material have good resilience but poor stability and are prone to movement. In addition, the pearl cotton balls clumping together affects the use of the product. Summary of the Invention
[0003] The purpose of this invention is to provide a sandwich-filled fiber material to solve the above-mentioned problems.
[0004] Another objective of this invention is to provide a method for preparing sandwich-filled fiber materials.
[0005] The technical problem solved by this invention can be achieved by the following technical solutions:
[0006] A sandwich-filled fiber material, characterized in that it comprises at least two layers of sheet-like fiber flakes stacked one on top of the other, with spherical fiber clusters laid between adjacent layers of fiber flakes;
[0007] Both the fiber flakes and the fiber clusters contain low-melting-point polyester fibers, and the fiber flakes and the fiber clusters are bonded together by thermal fusion bonding of the low-melting-point polyester fibers.
[0008] First, this invention combines fiber flakes and fiber clusters, giving the product the high stability of fiber flake filling materials and the high resilience of pearl cotton materials. Second, this invention creatively introduces low-melting-point polyester fibers, using the melting of these fibers to connect the fiber flakes and fiber clusters. Compared to sewing methods, this method is easier to manufacture, more efficient, and allows for more and more uniform connection points. This further improves the stability and resilience of the product.
[0009] The method for preparing sandwich-filled fiber materials is characterized by,
[0010] Step 1: Prepare fiber flakes and fiber clusters, both of which contain low-melting-point polyester fibers.
[0011] Step 2: Lay out fiber flakes and fiber clusters alternately in layers to form a sandwich structure;
[0012] Step 3: Heat the sandwich structure to melt the low-melting-point polyester fibers in the fiber flakes and fiber clusters.
[0013] Step 4: After cooling the sandwich structure, a sandwich filling fiber material is obtained, in which fiber flakes and fiber clusters are bonded together by thermal fusion of low-melting-point polyester fibers.
[0014] The preparation method is simple, easy to manufacture, and highly efficient. Detailed Implementation
[0015] To make the technical means, creative features, objectives and effects of this invention easier to understand, the invention will be further described below.
[0016] The interlayer filling fiber material comprises at least two layers of sheet-like fiber wadding stacked one on top of the other, with spherical fiber clusters laid between adjacent layers of fiber wadding. Both the fiber wadding and the fiber clusters contain low-melting-point polyester fibers, which are thermally bonded together by the low-melting-point polyester fibers.
[0017] Regarding fiber flocs
[0018] Preferably, the fiber wadding is composed of composite fibers and low-melting-point polyester fibers. The composite fibers are one or more of the following: polyester fiber, soybean fiber, polylactic acid fiber, and cellulose fiber. The composite fibers have a fineness of 1D-15D and a length of 20mm-70mm. The low-melting-point polyester fibers have a melting point of 110℃-180℃. The mass percentage of low-melting-point polyester fibers in the fiber wadding is 5%-15%.
[0019] Regarding fiber clusters
[0020] The fiber cluster is composed of low-melting-point polyester fibers, functional fibers, and microfibers. The functional fibers preferably contain three-dimensional hollow synthetic fibers, including at least one of PET, PTT, and PP fibers; the three-dimensional hollow synthetic fibers have a fineness of 2D-15D, a length of 20mm-64mm, and a content of 30%-70%. The low-melting-point polyester fibers have a melting point of 110℃-180℃. The mass percentage of low-melting-point polyester fibers in the fiber cluster is 5%-15%. The diameter of the fiber cluster is 5mm-18mm.
[0021] A method for preparing sandwich-filled fiber material includes the following steps: Step 1: Preparing fiber flakes and fiber clusters, both of which contain low-melting-point polyester fibers; Step 2: Alternatingly layering the fiber flakes and fiber clusters to form a sandwich structure; Step 3: Heating the sandwich structure to melt the low-melting-point polyester fibers in the fiber flakes and fiber clusters; Step 4: After cooling the sandwich structure, obtaining a sandwich-filled fiber material in which the fiber flakes and fiber clusters are bonded together by the thermal fusion of low-melting-point polyester fibers. Specific Implementation Example 1
[0023] First, select the raw materials for the fiber clusters: low-melting-point polyester fiber (melting point 110-130℃, content 5%); functional fiber (3D hollow synthetic fiber, fineness 3D, length 32mm, content 60%); and ultrafine fiber (0.7D ultrafine polyester fiber, length 32mm, content 35%). Feed the low-melting-point polyester fiber, 3D hollow synthetic fiber, and ultrafine polyester fiber into a mixer according to the above mass percentages and mix evenly. Then, convey the mixture to an opening machine to fully open the fibers. The opened fibers are then fed into a pearl cotton ball machine to form fiber clusters. Inside the pearl cotton ball machine, the fibers are squeezed, rubbed, and rotated to form balls. By adjusting the counterweight at the machine outlet, the size and tightness of the clusters are adjusted to achieve a fiber cluster diameter of 5-12mm.
[0024] Secondly, the raw materials for the fiber wadding are selected: low-melting-point polyester fiber (melting point 110-130℃, content 10%); and composite fiber, which consists of 30% three-dimensional 3D polyester fiber (length 64mm, fineness 3D) and 60% three-dimensional 7D polyester fiber (length 64mm, fineness 7D). The low-melting-point polyester fiber and composite fiber are fed into a mixer according to the above mass percentages and mixed evenly, then conveyed to an opening machine to fully open the fibers. The opened fibers are then fed into a carding machine, and after carding, they are evenly spread into fiber wadding of a certain thickness and width by a web-laying machine.
[0025] Then, after cutting the fiber wadding according to the product design specifications, it is laid on the bottom layer of the pillow core mold. Fiber clusters are then laid on the bottom layer of fiber wadding, and another piece of fiber wadding is laid on top of the fiber clusters to form a sandwich structure.
[0026] Finally, the pillow core mold with the sandwich structure is sent into the hot melt equipment for hot melt shaping. The hot melt temperature is 180℃. After cooling, a sandwich filling fiber material is obtained in which fiber flakes and fiber clusters are bonded together by hot melt bonding with low melting point polyester fibers. Specific Implementation Example 2
[0028] First, select the raw materials for the fiber clusters: low-melting-point polyester fiber (melting point 110-130℃, content 5%); functional fiber (3D hollow synthetic fiber, 64mm length, content 50%); and ultrafine fiber (far-infrared modified polyester fiber, 0.9D fineness, 38mm length, content 45%). Feed the low-melting-point polyester fiber, 3D hollow synthetic fiber, and far-infrared modified polyester fiber into a mixer according to the above mass percentages, mix them evenly, and then convey them to an opening machine to fully open the fibers. The opened fibers are then fed into a pearl cotton ball machine to form fiber clusters. Inside the pearl cotton ball machine, the fibers are squeezed, rubbed, and rotated to form balls. By adjusting the counterweight at the machine outlet, the size and tightness of the clusters are adjusted to achieve a fiber cluster diameter of 5-12mm.
[0029] Secondly, the raw materials for the fiber wadding are selected: low-melting-point polyester fiber, melting point 110-130℃, content 15%; the composite fiber consists of 30% soybean fiber (length 51mm, fineness 1.56D), 45% three-dimensional hollow silicone virgin polyester (length 64mm, fineness 3D), and 10% two-dimensional 7D ten-pore silicone recycled polyester fiber (length 64mm, fineness 7D). The low-melting-point polyester fiber and composite fiber are fed into a mixer according to the above mass percentages and mixed evenly, then conveyed to an opening machine to fully open the fibers. The opened fibers are then fed into a carding machine, and after carding, they are evenly spread into fiber wadding of a certain thickness and width by a web-laying machine.
[0030] Then, after cutting the fiber wadding according to the product design specifications, it is laid on the bottom layer of the pillow core mold. Fiber clusters are then laid on the bottom layer of fiber wadding, and another piece of fiber wadding is laid on top of the fiber clusters to form a sandwich structure.
[0031] Finally, the pillow core mold with the sandwich structure is sent into the hot melt equipment for hot melt shaping. The hot melt temperature is 180℃. After cooling, a sandwich filling fiber material is obtained in which fiber flakes and fiber clusters are bonded together by hot melt bonding with low melting point polyester fibers. Specific Implementation Example 3
[0033] First, select the raw materials for the fiber clusters: low-melting-point polyester fiber (melting point 110-130℃, content 10%); functional fibers consisting of 35% three-dimensional hollow silicone virgin polyester fiber (length 64mm, fineness 7D) and 30% antibacterial modified polyester fiber (length 64mm, fineness 3D); and ultrafine fiber consisting of 25% ultrafine polyester fiber (fineness 0.9D, length 38mm). The low-melting-point polyester fiber, three-dimensional hollow silicone virgin polyester fiber, antibacterial modified polyester fiber, and ultrafine polyester fiber are fed into a mixer according to the above mass percentages and mixed evenly. The mixture is then conveyed to an opening machine to fully open the fibers. The opened fibers are then fed into a pearl cotton ball machine to form fiber clusters. Inside the pearl cotton ball machine, the fibers are squeezed, rubbed, and rotated to form balls. By adjusting the counterweight at the machine outlet, the size and tightness of the clusters are adjusted to achieve a fiber cluster diameter of 8-15mm.
[0034] Secondly, the raw materials for the fiber wadding are selected: low-melting-point polyester fiber, with a melting point of 110-130℃, and a content of 15%; the composite fiber consists of 40% antibacterial three-dimensional hollow polyester fiber (64mm in length, 3D fineness) and 45% three-dimensional hollow polyester fiber (64mm in length, 7D fineness). The low-melting-point polyester fiber and composite fiber are fed into a mixer according to the above mass percentages and mixed evenly, then conveyed to an opening machine to fully open the fibers. The opened fibers are then fed into a carding machine, and after carding, they are evenly spread into fiber wadding of a certain thickness and width by a web-laying machine.
[0035] Then, after cutting the fiber wadding according to the product design specifications, it is laid on the bottom layer of the pillow core mold. Fiber clusters are then laid on the bottom layer of fiber wadding, and another piece of fiber wadding is laid on top of the fiber clusters to form a sandwich structure.
[0036] Finally, the pillow core mold with the sandwich structure is sent into the hot melt equipment for hot melt shaping. The hot melt temperature is 180℃. After cooling, a sandwich filling fiber material is obtained in which fiber flakes and fiber clusters are bonded together by hot melt bonding with low melting point polyester fibers. Specific Implementation Example 4
[0038] First, the raw materials for fiber clusters and fiber flakes are selected: low-melting-point polyester fiber with a melting point of 110-130℃ and a content of 10%; functional fibers are 45% three-dimensional hollow silicone virgin polyester fiber (64mm in length and 7D in fineness) and 25% antibacterial modified polyester fiber (64mm in length and 3D in fineness); ultrafine fiber is ultrafine polyester fiber with a fineness of 0.9D, a length of 38mm, and a content of 20%.
[0039] Low-melting-point polyester fiber, three-dimensional hollow silicon-containing virgin polyester fiber, antibacterial modified polyester fiber, and ultrafine polyester fiber are fed into the mixer according to the above mass percentages and mixed evenly. The mixture is then conveyed to the opening machine to fully open the fibers.
[0040] Secondly, the opened fiber portion is fed into the pearl cotton ball machine to form fiber clusters. The fibers are squeezed, rubbed, and rotated inside the pearl cotton ball machine to form balls. By adjusting the counterweight at the machine outlet, the size and tightness of the clusters are adjusted so that the diameter of the fiber clusters is 8-15mm.
[0041] The opened fiber portion is fed into a carding machine, and after carding, it is evenly spread into fiber flakes of a certain thickness and width by a web-laying machine.
[0042] Then, after cutting the fiber wadding according to the product design specifications, it is laid on the bottom layer of the pillow core mold. Fiber clusters are then laid on the bottom layer of fiber wadding, and another piece of fiber wadding is laid on top of the fiber clusters to form a sandwich structure.
[0043] Finally, the pillow core mold with the sandwich structure is sent into the hot melt equipment for hot melt shaping. The hot melt temperature is 180℃. After cooling, a sandwich filling fiber material is obtained in which fiber flakes and fiber clusters are bonded together by hot melt bonding with low melting point polyester fibers.
[0044] Product Performance Comparison
[0045] Example 1 Example 2 Example 3 Example 4 Production cost lowest lower Highest higher Antibacterial none none most better stability high high higher Highest Resilience good most better better
[0046] The comparison in the table above shows that the solution in specific embodiment 4 has the best overall performance and is the preferred solution.
[0047] In the above specific embodiments, besides heating the sandwich structure by heating the pillow core mold, the following scheme can also be adopted: Scheme 1: The sandwich structure passes through the gap between two hot rollers, and the initial connection is completed by the heat transmission and pressing effect of the hot rollers. Then it passes through a high-temperature space for a secondary connection. The temperature in the high-temperature space is not lower than the melting point of the low-melting-point polyester fiber. This structure preferably includes a first rotating roller, a second rotating roller, a first hot roller, a second hot roller, and a traction roller. The first rotating roller is wound with a fiber wadding as the bottom layer, and the second rotating roller is wound with a fiber wadding as the upper layer. There is a gap between the first hot roller and the second hot roller. The fiber wadding wound on the first rotating roller and the fiber wadding wound on the second rotating roller pass through the gap under the traction of the traction roller. Before reaching the first hot roller, the fiber clusters are laid on the fiber wadding as the bottom layer. To prevent the fiber clusters from rolling on the fiber wadding, it is preferable that the fiber clusters are wetted before being placed on the fiber wadding as the bottom layer, or the fiber wadding is made into a mesh (the mesh size of the fiber wadding is smaller than the diameter of the fiber clusters). The traction roller is located behind the high-temperature space, while the first and second hot rollers are located at the entrance, inside, or in front of the high-temperature space. When the first and second hot rollers are located inside the high-temperature space, they can be made of heat-conducting materials instead of heating elements, utilizing the thermal conductivity of these materials to achieve a high temperature. The outer walls of the first and second hot rollers have inward-facing recesses to accommodate spherical fiber clusters. This prevents the fiber clusters from being flattened during the heat-fusion bonding process with the fiber flakes, which would cause them to be pulled by the low-melting-point polyester fibers after cooling, affecting their resilience. The recesses on the first and second hot rollers are aligned one-to-one.
[0048] In the above specific embodiments, low-melting-point polyester fibers can also be laid between two adjacent layers of fiber wadding. Preferably, the low-melting-point polyester fibers are laid along the edges of the fiber wadding. On the one hand, the low-melting-point polyester fibers laid along the edges of the fiber wadding can restrict the movement of the fiber clusters, preventing displacement of the fiber clusters during the production process, especially before hot-melt bonding. On the other hand, the low-melting-point polyester fibers laid along the edges of the fiber wadding can improve the thickness uniformity of the sandwich structure's edges, making the final product relatively uniform in thickness throughout. This avoids the situation where the fiber wadding at the edges is supported by the fiber clusters without connection, and also prevents the sandwich structure from collapsing at the edges after hot-melt bonding.
[0049] To ensure more uniform bonding of the interlayer filling fiber material, the pillow core mold rotates within the hot-melt mold. This allows for more diverse flow directions of the molten low-melting-point polyester fibers, and the force generated during rotation further enhances the flow force of the molten low-melting-point polyester fibers, ultimately resulting in more uniform dispersion. Preferably, the hot-melt mold rotates along the central axis of the interlayer filling fiber material. An inclined track can be installed within the hot-melt equipment, and support legs matching the track can be provided on the hot-melt mold. After the hot-melt mold is placed inside the hot-melt equipment, it rolls from a higher position to a lower position on the track under the influence of gravity, thus achieving the rolling of the hot-melt mold.
[0050] The foregoing has shown and described the basic principles, main features, and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The embodiments and descriptions in the specification are merely illustrative of the principles of the invention. Various changes and modifications can be made to the invention without departing from its spirit and scope, and all such changes and modifications fall within the scope of the present invention as claimed. The scope of protection of this invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a sandwich-filled fiber material, characterized in that, Step 1: Prepare fiber flakes and fiber clusters, both of which contain low-melting-point polyester fibers. Step 2: The fiber flakes and fiber clusters are laid alternately in layers to form a sandwich structure. The fiber flakes as the bottom layer are wound on the first rotating roller, and the fiber flakes as the top layer are wound on the second rotating roller. There is a gap between the first hot roller and the second hot roller. The fiber flakes wound on the first rotating roller and the fiber flakes wound on the second rotating roller pass through the gap under the traction of the traction roller. Before reaching the first hot roller, the fiber clusters are laid on the fiber flakes as the bottom layer. Step 3: Heat the sandwich structure to melt the low-melting-point polyester fibers in the fiber flakes and fiber clusters. The sandwich structure passes through the gap between the two hot rollers and completes the initial connection by using the heat transmission and pressing effect of the hot rollers. Then it passes through the high-temperature space and is connected a second time in the high-temperature space. The temperature in the high-temperature space is not lower than the melting point of the low-melting-point polyester fibers. The traction roller is located behind the high-temperature space. The first hot roller and the second hot roller are located at the entrance of the high-temperature space, inside the high-temperature space, or in front of the high-temperature space. The outer walls of the first hot roller and the second hot roller have inward recesses, and the recesses on the first hot roller and the second hot roller are aligned one to one. Step 4: After cooling the sandwich structure, a sandwich filling fiber material is obtained, in which fiber flakes and fiber clusters are bonded together by thermal fusion of low-melting-point polyester fibers.
2. The method of making a sandwiched fibrous filler material according to claim 1, characterized in that, The fiber clusters are wetted and then placed on the fiber wadding as the bottom layer, or the fiber wadding is made into a mesh shape, with the mesh size of the fiber wadding being smaller than the diameter of the fiber clusters.
3. The method of making a sandwiched fibrous filler material according to claim 1, wherein, The raw materials for fiber clusters and fiber flakes are: low-melting-point polyester fiber with a melting point of 110-130℃ and a content of 10%; three-dimensional hollow silicon-containing virgin polyester fiber with a length of 64mm, a fineness of 7D, and a content of 45%; antibacterial modified polyester fiber with a length of 64mm, a fineness of 3D, and a content of 25%; and ultrafine fiber, ultrafine polyester fiber with a fineness of 0.9D, a length of 38mm, and a content of 20%.
Citation Information
Patent Citations
Heat preservation flocculus material, preparing method of heat preservation flocculus material and heat preservation product
CN105463697A