A sulfonic acid functionalized porous organic polymer material and its preparation method and application

CN116478374BActive Publication Date: 2024-10-11HEBEI LONGHAI BIOENERGY TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310245505.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-15
Publication Date
2024-10-11
Estimated Expiration
2043-03-15

Smart Images

  • Figure CN116478374B_ABST
    Figure CN116478374B_ABST
Patent Text Reader

Abstract

The present invention provides a sulfonic acid functional porous organic polymer material, which is generated by the reaction and polymerization of raw materials 1,4-dibromomethylbenzene, a polymer connecting chain, a substituted phenol and 1,3-propanesulfonyl lactone. An application of the sulfonic acid functional porous organic polymer material, the sulfonic acid functional porous organic polymer material is applied to the reaction of preparing biodiesel from waste oil and methanol. The present invention selects organic molecules such as substituted phenol and bromomethyl substituted benzene as raw materials of the porous organic polymer material, realizes the synthesis of the sulfonic acid functional porous organic polymer material through a simple catalytic reaction, uses bromomethyl substituted benzene as a polymer connecting group, and adjusts the polymer material to have amphiphilicity due to the different chain lengths of alkyl substituents in the substituted phenol molecules, and has the properties of being lipophilic to fats and methanol, and can efficiently realize the conversion of fats and methanol systems to produce biodiesel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of organic polymer material preparation, and specifically relates to a sulfonic acid functionalized porous organic polymer material and a preparation method and application thereof. Background Art

[0002] Biodiesel is considered an important alternative energy source to fossil resources, which can greatly reduce carbon emissions and pollutant sulfur dioxide emissions. In the production process of biodiesel, non-edible oils such as woody plant oils, animal fats and waste oils are mainly used as raw materials, which can control production costs based on the cost of raw materials; however, the biggest problem faced by the use of non-edible oils is the high acid value, which requires highly active, highly stable, and acid-resistant catalytic materials. Therefore, the development of environmentally friendly, non-corrosive, and highly efficient porous organic polymer heterogeneous catalytic materials has shown a broader application prospect in biodiesel production. Summary of the invention

[0003] The purpose of the present invention is to solve the shortcomings of the prior art. The present invention provides an organic polymer material that can efficiently realize the conversion of oil and methanol system to produce biodiesel.

[0004] The technical solution adopted by the present invention is: a sulfonic acid functionalized porous organic polymer material, the molecular structure of the organic polymer material is as follows:

[0005]

[0006] The molecular structure of the polymer connecting chain is:

[0007] One of;

[0008] Wherein R is a substituted alkyl group, which is one of methyl, ethyl, butyl, tert-butyl, octyl, dodecyl, bisphenol A, pentadecyl or hexadecyl.

[0009] Furthermore, the raw material 1,4-dibromomethylbenzene is used as a polymer linking chain, substituted phenol reacts, and 1,3-propanesulfonyl lactone is functionalized and polymerized.

[0010] A method for preparing a sulfonic acid functionalized porous organic polymer material comprises the following steps:

[0011] 1,4-dibromomethylbenzene is used as a polymer link chain and polymerized with substituted phenol under catalyst conditions to generate a hydroxyl functional group substituted organic polymer material; the hydroxyl functional group substituted organic polymer material reacts with 1,3-propanesulfonyl lactone under alkaline conditions to obtain a sodium sulfonate substituted organic polymer material; the sodium sulfonate substituted organic polymer material undergoes proton exchange under acidic conditions to finally obtain a sulfonic acid functionalized porous organic polymer material.

[0012] Furthermore, the substituted phenol is one of the following molecular structures:

[0013]

[0014] Furthermore, the catalyst is FeCl3.

[0015] Furthermore, the molar ratio of the 1,4-dibromomethylbenzene to the substituted phenol is 2:1.

[0016] The invention discloses an application of a sulfonic acid functionalized porous organic polymer material. The sulfonic acid functionalized porous organic polymer material is applied to the reaction of preparing biodiesel from waste cooking oil and methanol.

[0017] The beneficial effects obtained by the present invention are as follows: the present invention selects organic molecules such as substituted phenol and bromomethyl substituted benzene as raw materials for porous organic polymer materials, realizes the synthesis of sulfonic acid functionalized porous organic polymer materials through a simple catalytic reaction, utilizes bromomethyl substituted benzene as a polymer linking group, and adjusts the polymer materials to have amphiphilicity and fat and methanol affinity by using different chain lengths of alkyl substituents in the substituted phenol molecules, thereby efficiently realizing the conversion of fat and methanol systems to produce biodiesel.

[0018] In the present invention: 1) phenols with different carbon chain lengths, including methyl, ethyl, butyl, tert-butyl, octyl, dodecyl, pentadecyl or hexadecyl, and bromomethyl substituted benzenes, including 1,4-dibromomethylbenzene, 1,3,5-tribromomethylbenzene, 4,4'-dibromomethylbiphenyl, tri-4'-bromomethylbenzene, are polymerized under the action of ferric chloride as a catalyst to synthesize hydroxyl functionalized organic polymer materials with different carbon chain lengths, and then react with 1,3-propanesulfonyl lactone, and then undergo ion exchange to finally obtain sulfonic acid functionalized organic polymer materials; 2) bromomethyl substituted benzenes and phenols with different carbon chain lengths are used to regulate the microstructure of the polymer material, including specific surface area, pore structure, sulfonic acid center distribution and strength; 3) the catalytic material is applied to the transesterification of oils and fats with short-chain alcohols, and the reaction of higher fatty acids with short-chain alcohols to prepare biodiesel. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 The synthetic route of the sulfonic acid functionalized porous organic polymer material of the present invention is as follows;

[0020] Figure 2 FT-IR graph of the polymer material E precursor of the present invention;

[0021] Figure 3 FT-IR graph of polymer material E of the present invention;

[0022] Figure 4 is the XPS full element diagram of the polymer material E of the present invention;

[0023] Figure 5 is the C1s XPS graph of the polymer material E of the present invention;

[0024] Figure 6 is the O1s XPS graph of the polymer material E of the present invention;

[0025] Figure 7 is the S2p XPS graph of the polymer material E of the present invention;

[0026] Figure 8 The polymer material E of the present invention 13 C-NMR spectrum;

[0027] Fig. 9 This is the SEM image (1 μm) of the polymer material E precursor of the present invention;

[0028] Fig.10 This is the SEM image (10 μm) of the polymer material E precursor of the present invention;

[0029] Fig.11 is a SEM image (1 μm) of the polymer material E of the present invention;

[0030] Fig.12 This is a SEM image (10 μm) of the polymer material E of the present invention. DETAILED DESCRIPTION

[0031] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0032] The present invention uses dibromomethyl substituted benzene (tribromomethylphenylbenzene) as a polymer material connecting skeleton, and undergoes electrophilic substitution reaction with alkyl substituted phenols of different carbon chain lengths through Friedel-Crafts alkylation reaction under catalytic conditions to obtain a hydroxyl functionalized organic polymer material whose polarity is adjusted by the alkyl group, and then transforms the hydroxyl group into a catalytic active site through a post-modification method to synthesize a sulfonic acid functionalized porous organic polymer material. The synthetic route is as follows: Figure 1 The synthesized polymer material is used as a catalyst for the preparation of biodiesel.

[0033] When implementing:

[0034] Substituted phenols can be of the following molecular structures:

[0035]

[0036] The specific synthesis steps are as follows:

[0037] Synthesis of Material A: 1,4-bromomethylbenzene (8mmol, 2.112g), p-tert-butylphenol (4mmol, 0.6g), and FeCl3 (12mmol, 1.96g) were added to a 250mL three-necked flask. After adding 90mL of dichloroethane to the three-necked flask, a condenser was added, and the mixture was reacted under reflux for 24h. After the reaction was completed, it was cooled to room temperature, and the mixture was transferred to a sand core funnel, filtered, washed with methanol, and vacuum dried to obtain 1.56g of brown solid. 1g of brown solid was dispersed in 20mL of anhydrous ethanol, and 100mg of NaOH and 1mL of 1,3-propanesulfonyl lactone were added in sequence. The mixture was reacted under reflux for 24h, filtered, washed, and dried. The solid was dispersed in 20mL of 3mol / L ethanol-hydrochloric acid solution, and after replacement at room temperature for 24h, it was filtered and dried to obtain a sulfonic acid functionalized porous organic polymer material, and 1.12g of brown solid was obtained.

[0038] Synthesis of Material B: 1,4-bromomethylbenzene (8mmol, 2.112g), p-butylphenol (4mmol, 0.6g), and FeCl3 (12mmol, 1.96g) were added to a 250mL three-necked flask. After adding 90mL of dichloroethane to the three-necked flask, a condenser was added, and the mixture was reacted under reflux for 24h. After the reaction was completed, it was cooled to room temperature, and the mixture was transferred to a sand core funnel, filtered, washed with methanol, and vacuum dried to obtain 1.42g of brown solid. 1g of brown solid was dispersed in 20mL of anhydrous ethanol, and 100mg of NaOH and 1mL of 1,3-propanesulfonyl lactone were added in sequence. The mixture was reacted under reflux for 24h, filtered, washed, and dried. The solid was dispersed in 20mL of 3mol / L ethanol-hydrochloric acid solution, and after replacement at room temperature for 24h, it was filtered and dried to obtain a sulfonic acid functionalized porous organic polymer material, and 1.10g of brown solid was obtained.

[0039] Synthesis of Material C: 1,4-bromomethylbenzene (8mmol, 2.112g), p-octylphenol (4mmol, 0.84g), and FeCl3 (12mmol, 1.96g) were added to a 250mL three-necked flask. After adding 90mL of dichloroethane to the three-necked flask, a condenser was added, and the mixture was reacted under reflux for 24h. After the reaction was completed, it was cooled to room temperature, and the mixture was transferred to a sand core funnel, filtered, washed with methanol, and vacuum dried to obtain 1.67g of brown solid. 1g of brown solid was dispersed in 20mL of anhydrous ethanol, and 100mg of NaOH and 1mL of 1,3-propanesulfonyl lactone were added in sequence. The mixture was reacted under reflux for 24h, filtered, washed, and dried. The solid was dispersed in 20mL of 3mol / L ethanol-hydrochloric acid solution, and after replacement at room temperature for 24h, it was filtered and dried to obtain a sulfonic acid functionalized porous organic polymer material, and 1.09g of brown solid was obtained.

[0040] Synthesis of Material D: 1,4-bromomethylbenzene (8mmol, 2.112g), p-dodecylphenol (4mmol, 1.05g), and FeCl3 (12mmol, 1.96g) were added to a 250mL three-necked flask. After adding 90mL of dichloroethane to the three-necked flask, a condenser was added, and the mixture was reacted under reflux for 24h. After the reaction was completed, it was cooled to room temperature, and the mixture was transferred to a sand core funnel, filtered, washed with methanol, and vacuum dried to obtain 1.72g of brown solid. 1g of brown solid was dispersed in 20mL of anhydrous ethanol, and 100mg of NaOH and 1mL of 1,3-propanesulfonyl lactone were added in sequence. The mixture was reacted under reflux for 24h, filtered, washed, and dried. The solid was dispersed in 20mL of 3mol / L ethanol-hydrochloric acid solution, and after replacement at room temperature for 24h, it was filtered and dried to obtain a sulfonic acid functionalized porous organic polymer material, and 1.07g of brown solid was obtained.

[0041] Synthesis of Material E: 1,4-bromomethylbenzene (8mmol, 2.112g), m-pentadecylphenol (4mmol, 1.22g), and FeCl3 (12mmol, 1.96g) were added to a 250mL three-necked flask. After adding 90mL of dichloroethane to the three-necked flask, a condenser was added and the mixture was reacted under reflux for 24h. After the reaction was completed, it was cooled to room temperature, the mixture was transferred to a sand core funnel, filtered, washed with methanol, and vacuum dried to obtain 1.82g of brown solid. 1g of brown solid was dispersed in 20mL of anhydrous ethanol, 100mg of NaOH and 1mL of 1,3-propanesulfonyl lactone were added in sequence, the mixture was reacted under reflux for 24h, filtered, washed, and dried. The solid was dispersed in 20mL of 3mol / L ethanol-hydrochloric acid solution, and after replacement at room temperature for 24h, it was filtered and dried to obtain a sulfonic acid functionalized porous organic polymer material, and 1.05g of brown solid was obtained.

[0042] Synthesis of Material F: 1,4-bromomethylbenzene (8mmol, 2.112g), bisphenol A (2mmol, 0.46g), and FeCl3 (12mmol, 1.96g) were added to a 250mL three-necked flask. After adding 90mL of dichloroethane to the three-necked flask, a condenser was added, and the mixture was reacted under reflux for 24h. After the reaction was completed, it was cooled to room temperature, and the mixture was transferred to a sand core funnel, filtered, washed with methanol, and vacuum dried to obtain 1.27g of brown solid. 1g of brown solid was dispersed in 20mL of anhydrous ethanol, and 100mg of NaOH and 1mL of 1,3-propanesulfonyl lactone were added in sequence. The mixture was reacted under reflux for 24h, filtered, washed, and dried. The solid was dispersed in 20mL of 3mol / L ethanol-hydrochloric acid solution, and after replacement at room temperature for 24h, it was filtered and dried to obtain a sulfonic acid functionalized porous organic polymer material, and 1.12g of brown solid was obtained.

[0043] The obtained porous organic polymer materials functionalized with different sulfonic acids were applied to the reaction of waste oil and methanol to prepare biodiesel. The specific reaction data are shown in Table 1:

[0044] Table 1. Effect of polymer structure on reactivity

[0045] sequence catalyst Waste oil conversion rate (%) 1 A 40.8 2 B 21.6 3 C 24.3 4 D 23.5 5 E 45.6 6 F 23.7 7 none 0

[0046] Waste oil: 10 mmol, methanol: 1.17 mL, reaction time: 6 h, temperature: 65 ° C, catalyst dosage 2 wt%.

[0047] It can be seen from the table that the sulfonic acid functionalized porous organic polymer material E has the highest reaction activity. Taking material E as an example, the amount of catalyst, reaction temperature and reaction time are tested. The experimental data are shown in Table 2-4 below.

[0048] Table 2. Effect of catalyst dosage on reaction activity

[0049] sequence Catalyst dosage (wt%) Waste oil conversion rate (%) 1 1 30.7 2 2 45.6 3 4 56.6 4 6 67.8 5 10 75.6

[0050] Waste oil: 10 mmol, methanol: 1.17 mL, reaction time: 6 h, temperature: 65 °C, catalyst E.

[0051] Table 3. Effect of reaction temperature on reaction activity

[0052] sequence Reaction temperature (℃) Waste oil conversion rate (%) 1 55 48.1 2 60 57.2 3 65 67.8 4 70 78.6 5 75 87.3 6 80 94.5

[0053] Waste oil: 10 mmol, methanol: 1.17 mL, reaction time: 6 h, catalyst E, dosage: 6 wt%.

[0054] Table 4. Effect of reaction time on reaction activity

[0055] sequence Reaction time (h) Waste oil conversion rate (%) 1 2 53.1 2 4 77.9 3 6 94.5 4 8 95.6 5 10 96.3

[0056] Waste oil: 10 mmol, methanol: 1.17 mL, reaction time: 6 h, temperature: 80°C, catalyst E, dosage: 6 wt%.

[0057] In summary: sulfonic acid functionalized porous organic polymer material E is the best catalyst, and in the reaction of waste oil and methanol, when the amount of catalyst E is 10wt%, the reaction time is 10h, and the reaction temperature is 80°C, the esterification conversion rate of waste oil is the highest.

[0058] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A sulfonic acid functionalized porous organic polymer material, characterized in that: The molecular structure of the organic polymer material is as follows: The molecular structure of the polymer linking chain is: One of; wherein R is a substituted alkyl group, which is one of methyl, ethyl, butyl, tert-butyl, octyl, dodecyl, pentadecyl or hexadecyl; The raw material 1,4-dibromomethylbenzene is used as a polymer linker to react with substituted phenol, and 1,3-propanesulfonyl lactone is functionalized and polymerized to generate the product.

2. The method for preparing a sulfonic acid functionalized porous organic polymer material according to claim 1, characterized in that: The following steps are involved: 1,4-dibromomethylbenzene is used as a polymer link chain and polymerized with substituted phenol under catalyst conditions to generate a hydroxyl functional group substituted organic polymer material; the hydroxyl functional group substituted organic polymer material reacts with 1,3-propanesulfonyl lactone under alkaline conditions to obtain a sodium sulfonate substituted organic polymer material; the sodium sulfonate substituted organic polymer material undergoes proton exchange under acidic conditions to finally obtain a sulfonic acid functionalized porous organic polymer material.

3. The method for preparing a sulfonic acid functionalized porous organic polymer material according to claim 2, characterized in that: The substituted phenol is one of the following molecular structures:

4. The method for preparing a sulfonic acid functionalized porous organic polymer material according to claim 2, characterized in that: The catalyst is FeCl3.

5. The method for preparing a sulfonic acid functionalized porous organic polymer material according to claim 2, characterized in that: The molar ratio of the 1,4-dibromomethylbenzene to the substituted phenol is 2:

1.