A process for the preparation of polyether polyols from isocyanuric acid triglycidyl ester by-products

Polyether polyols were prepared by hydrolyzing and desolventizing TGIC byproducts, which solved the problem of underutilization of TGIC byproducts and achieved efficient and environmentally friendly resource utilization, producing high-quality polyether polyols.

CN116478394BActive Publication Date: 2026-11-24JIANGSU YANGNONG CHEMICAL GROUP CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310409209.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-17
Publication Date
2026-11-24
Estimated Expiration
2043-04-17

AI Technical Summary

Technical Problem

In the existing technology, the byproducts of triglycidyl isocyanate (TGIC) are not fully utilized, resulting in an environmentally unfriendly production process and an increase in the amount of byproducts. Finding a clean and efficient utilization method is an urgent problem to be solved.

Method used

The intermediate product is generated by hydrolyzing triglycidyl isocyanurate byproduct with propylene oxide and alkali under catalysis. The intermediate product is then obtained by solvent removal treatment, including steps such as negative pressure solvent removal, centrifugation, neutralization and filtration.

Benefits of technology

This method enables the resource utilization of TGIC byproducts to produce high-value-added polyether polyols. The process is simple, environmentally friendly, and the products are non-toxic, have low volatility, and have a wide range of applications, showing promising commercial prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure QLYQS_2
    Figure QLYQS_2
  • Figure QLYQS_3
    Figure QLYQS_3
Patent Text Reader

Abstract

This invention provides a method for preparing polyether polyols from triglycidyl isocyanurate byproducts. The method includes: S1, mixing the triglycidyl isocyanurate byproduct with propylene oxide and an alkali, and performing a hydrolysis reaction to obtain an intermediate product; wherein the triglycidyl isocyanurate byproduct is a byproduct of the reaction of isocyanuric acid with epichlorohydrin to produce triglycidyl isocyanurate; S2, subjecting the intermediate product to solvent removal and separation treatment to obtain the polyether polyol. This invention enables the full resource utilization of triglycidyl isocyanurate byproducts in the prior art and solves the environmentally unfriendly problems of the production process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of resource utilization technology of chemical production by-products, and more specifically, to a method for preparing polyether polyols from isocyanuric acid triglycidyl ester by-products. Background Technology

[0002] Polyether polyols are important intermediates in the production of polyurethane. In recent years, with the continuous improvement of polyurethane performance requirements, research on polyether polyols has become increasingly in-depth in order to further improve production efficiency and reduce production costs. Polyether polyols are generally polymerized by reacting low-molecular-weight alcohols or amines, which contain active hydrogen, with epoxide compounds such as ethylene oxide and propylene oxide under the action of a catalyst. Among them, modified polyether polyols are more widely studied, generally including graft-modified polyether polyols, polymerized polyols, and polyurea polyols.

[0003] During the production of triglycidyl isocyanurate (TGIC), byproducts such as incomplete chlorohydrin ring-closing, epoxy ring-opening byproducts on TGIC under alkaline conditions, and byproducts from the incomplete reaction of cyanuric acid and epichlorohydrin remain in the recrystallization mother liquor of TGIC. The comprehensive utilization of byproducts in TGIC production and ensuring the cleanliness of the production process have always been key concerns for production enterprises and environmental protection departments.

[0004] The resource utilization of byproducts from TGIC production has been extensively studied at the laboratory level. For example, Ye Weide et al. used TGIC byproducts to replace liquid epoxy resin in the production of UV-curable resins. They added propylene in an amount equal to the epoxy value of the system to the TGIC byproducts, along with a catalyst and polymerization inhibitor. After the reaction reached the predetermined acid and epoxy values, a diluent was added to prepare a UV-curable resin with UV photoactivity. CN103382376A uses a small amount of urea to react with TGIC byproducts to generate a novel formaldehyde-free adhesive with a chemical structure containing hydroxyl and amino groups consistent with the functional groups of urea-formaldehyde resin. However, current methods for utilizing TGIC byproducts are still limited. With the increasing demand for TGIC, the output of byproducts is also increasing. Finding clean and efficient ways to utilize TGIC byproducts to manufacture high-value-added products and turn waste into treasure is an urgent problem to be solved.

[0005] In view of this, the present invention is proposed. Summary of the Invention

[0006] The main objective of this invention is to provide a method for preparing polyether polyols from triglycidyl isocyanurate byproducts, in order to solve the problems of insufficient resource utilization of triglycidyl isocyanurate byproducts and environmentally unfriendly production processes in the prior art.

[0007] To achieve the above objectives, according to one aspect of the present invention, a method for preparing polyether polyols from triglycidyl isocyanurate byproducts is provided, comprising: S1, mixing the triglycidyl isocyanurate byproducts with propylene oxide and an alkali, and performing a hydrolysis reaction to obtain an intermediate product; wherein the triglycidyl isocyanurate byproducts are byproducts of the reaction of isocyanuric acid with epichlorohydrin to produce triglycidyl isocyanurate; S2, subjecting the intermediate product to solvent removal treatment and separation treatment to obtain polyether polyols.

[0008] Further, in step S1, the weight of the base is 0.1 to 10% of the triglycidyl isocyanurate byproduct.

[0009] Furthermore, the weight ratio of the triglycidyl isocyanurate byproduct to propylene oxide is (2-6):1.

[0010] Furthermore, the triglycidyl isocyanurate byproduct, propylene oxide, and base are mixed simultaneously; or, the triglycidyl isocyanurate byproduct is first mixed with the first part of the base for the first step reaction, and then propylene oxide and the second part of the base are added for the second step reaction, wherein the weight ratio of the first part of the base to the second part of the base is 1:1 to 5.

[0011] Furthermore, when the triglycidyl isocyanurate byproduct, propylene oxide, and alkali are mixed simultaneously, the hydrolysis reaction temperature is 40–100°C and the time is 2–12 h; or, when the alkali is added in two steps, the hydrolysis reaction includes: mixing the triglycidyl isocyanurate byproduct and the first part of the alkali, and carrying out the first step reaction at 40–100°C to obtain the first step reaction product; then adding propylene oxide and the second part of the alkali, and carrying out the second step reaction at 50–80°C, with the reaction time of the second step reaction being 2–10 h.

[0012] Furthermore, the hydrolysis reaction is carried out under the protection of an inert gas; preferably, the inert gas is nitrogen and / or argon.

[0013] Furthermore, the triglycidyl isocyanurate byproducts include solvents and one or more of compounds a, b, and c;

[0014]

[0015] In compounds a, b, and c, the R groups are each independently... One or more of the following: In the triglycidyl isocyanurate by-product, the weight content of triglycidyl isocyanurate is ≤10%, the weight content of by-products with a boiling point above 110℃ is 10-50%, and the weight content of solvent is 40-90%; preferably, the solvent is one or more of methanol, ethanol, diethyl ether, and ethyl acetate; more preferably, the mother liquor after the reaction of isocyanuric acid and epichlorohydrin is heated and distilled at 60-110℃, and the fraction is used as a recycled solvent, and the remaining liquid is the triglycidyl isocyanurate by-product.

[0016] Furthermore, the base is one or more of sodium hydroxide, potassium hydroxide, hexadecyltrimethylammonium chloride, tetramethylammonium chloride, and hexadecyltrimethylammonium bromide.

[0017] Furthermore, the solvent removal process is performed under negative pressure; preferably, the vacuum degree of the negative pressure solvent removal is -0.08 to -0.1 MPa, the temperature is 60 to 100°C, and the time is 10 to 60 min; after solvent removal, a residue is obtained, and more preferably, the solvent weight content in the residue is 10 to 30%.

[0018] Furthermore, the separation process includes centrifugation, neutralization, adsorption, and filtration performed sequentially.

[0019] By applying the technical solution of this invention, polyether polyols were prepared using triglycidyl isocyanate (TGIC) byproducts. This invention achieves resource utilization of byproducts from TGIC production, yielding high-value-added products. Furthermore, the process is simple, environmentally friendly, and has promising prospects for commercialization. In addition, the polyether polyols prepared by the method of this invention possess some of the corresponding structures of isocyanates, exhibit low volatility, are non-toxic, and have a wide range of applications, which is beneficial for their use in the preparation of downstream products. Detailed Implementation

[0020] It should be noted that, unless otherwise specified, the embodiments and features described in this application can be combined with each other. The present invention will now be described in detail with reference to the embodiments.

[0021] To address the aforementioned problems in the prior art, according to one aspect of the present invention, a method for preparing polyether polyols from triglycidyl isocyanurate byproducts is provided, comprising: S1, mixing the triglycidyl isocyanurate byproducts with propylene oxide and an alkali, and performing a hydrolysis reaction to obtain an intermediate product; wherein the triglycidyl isocyanurate byproduct is a byproduct of the reaction of triglycidyl isocyanurate with epichlorohydrin to produce triglycidyl isocyanurate; S2, subjecting the intermediate product to solvent removal treatment and separation treatment to obtain polyether polyols.

[0022] This invention utilizes triglycidyl isocyanate (TGIC) byproducts to prepare polyether polyols. This invention achieves resource utilization of byproducts from TGIC production, yielding high-value-added products. Furthermore, the process is simple, environmentally friendly, and has promising commercial application prospects. In addition, the polyether polyols prepared by this method possess some of the corresponding isocyanate structures, exhibit low volatility, are non-toxic, and have a wide range of applications, which is beneficial for their use in the preparation of downstream products.

[0023] Specifically, in the method of the present invention, the reaction includes, under the catalysis of an alkali, opening the ring of the incompletely cyclically closed isocyanate byproducts in the TGIC byproducts to generate hydroxyl groups, and further polymerizing the hydroxyl groups with propylene oxide to generate polyether polyols.

[0024] In a preferred embodiment, in step S1, the weight of the alkali is 0.1-10% of the triglycidyl isocyanurate byproduct. The above-mentioned amount of alkali is preferred as it is more conducive to the catalytic reaction and improves product quality.

[0025] For the purpose of further promoting the polymerization reaction, in a preferred embodiment, the weight ratio of the triglycidyl isocyanurate byproduct to propylene oxide is (2-6):1.

[0026] In a preferred embodiment, the triglycidyl isocyanate byproduct, propylene oxide, and alkali are mixed simultaneously; alternatively, the triglycidyl isocyanate byproduct is first mixed with the first portion of alkali for a first-step reaction, followed by the addition of propylene oxide and the second portion of alkali for a second-step reaction, wherein the weight ratio of the first portion of alkali to the second portion of alkali is 1:1-5. Those skilled in the art can choose to add the alkali in one or two steps depending on the actual production situation. When adding the alkali in two steps, the TGIC byproduct is first hydrolyzed and ring-opened by the first portion of alkali before the polymerization reaction, resulting in a polyether polyol with a higher molecular weight and better quality.

[0027] In a preferred embodiment, when the triglycidyl isocyanurate byproduct, propylene oxide, and alkali are mixed simultaneously, the hydrolysis reaction temperature is 40–100°C, and the time is 2–12 hours. Alternatively, when the alkali is added in two steps, the hydrolysis reaction includes: mixing the triglycidyl isocyanurate byproduct and a first portion of the alkali, and carrying out a first-step reaction at 40–100°C to obtain the first-step reaction product; then adding propylene oxide and a second portion of the alkali, and carrying out a second-step reaction at 50–80°C for 2–10 hours. The preferred reaction conditions are more conducive to promoting the occurrence of reactions in each process flow.

[0028] To better protect the reactants from interference, in a preferred embodiment, the hydrolysis reaction is carried out under an inert gas atmosphere; preferably, the inert gas is nitrogen and / or argon.

[0029] In a preferred embodiment, the triglycidyl isocyanurate byproduct includes a solvent and one or more of compounds a, b, and c;

[0030]

[0031]

[0032] In compounds a, b, and c, the R groups are each independently... The method involves one or more of the following: In the triglycidyl isocyanurate byproduct, the weight content of triglycidyl isocyanurate is ≤10%, and the weight content of byproducts with a boiling point above 110℃ is 10-50%; the weight content of the solvent is 40-90%; preferably, the solvent is one or more of methanol, ethanol, diethyl ether, and ethyl acetate; more preferably, the mother liquor after the reaction of isocyanuric acid and epichlorohydrin is heated and distilled at 60-110℃, and the fraction is used as a recycled solvent, with the remaining liquid being the triglycidyl isocyanurate byproduct. The TGIC byproduct utilized in this invention may or may not contain TGIC; when TGIC is present, it can also react directly with a base to obtain a polyether polyol.

[0033] Among the aforementioned byproducts, a is an incomplete chlorohydrin ring-closing byproduct, b is an epoxy ring-opening byproduct on triglycidyl isocyanurate under alkaline conditions, and c is an incomplete reaction of cyanuric acid with epichlorohydrin.

[0034] Among the aforementioned byproducts, those with a boiling point higher than 110℃ are generally referred to as high-boiling-point byproducts.

[0035] In a preferred embodiment, the base is one or more selected from sodium hydroxide, potassium hydroxide, hexadecyltrimethylammonium chloride, tetramethylammonium chloride, and hexadecyltrimethylammonium bromide. The aforementioned strong bases are preferred as they are more conducive to the catalytic effect.

[0036] In a preferred embodiment, the solvent removal process is a negative pressure solvent removal process; preferably, the vacuum degree of the negative pressure solvent removal process is -0.08 to -0.1 MPa, the temperature is 60 to 100°C, and the time is 10 to 60 min; after solvent removal, a residue is obtained, and more preferably, the solvent weight content in the residue is 10 to 30%. The above-mentioned solvent removal process conditions are more conducive to the purification of the synthesized product.

[0037] In a preferred embodiment, the separation process includes sequential centrifugation, neutralization, adsorption, and filtration. Further purification methods are well known to those skilled in the art and will not be described in detail here.

[0038] The present application will be further described in detail below with reference to specific embodiments, which should not be construed as limiting the scope of protection claimed in the present application.

[0039] Example 1

[0040] At room temperature, 1000g of a byproduct solution containing 5% TGIC, 45% high-boiling-point byproducts, and 50% ethyl acetate and methanol as solvents, generated during the production of TGIC, was placed in a 2L round-bottom flask. The mixture was stirred and heated to 90℃, and the distillate was collected. The temperature was lowered to 20℃, and the residue was collected. The residue was placed in a round-bottom flask, and 2g of potassium hydroxide was added. Nitrogen gas was introduced for protection, and the temperature was raised to 80℃. Then, 3g of potassium hydroxide and 80g of propylene oxide were added, and the mixture was refluxed at 80℃ for 8 hours. After the reflux was completed, the solvent was removed under a vacuum of less than -0.09MPa until the temperature of the residue in the flask reached 70℃. The solution was held for 30 minutes. The residue after solvent removal was centrifuged while hot, neutralized, adsorbed, and filtered to obtain the target product, polyether polyol.

[0041] Example 2

[0042] At room temperature, 1000g of a byproduct solution containing 2% TGIC, 38% high-boiling-point byproducts, and 60% methanol as solvent, generated during the production of TGIC, was placed in a 2L round-bottom flask. The mixture was stirred and heated to 100℃, and the distillate was collected. The mixture was then cooled and the residue was collected. The residue was placed in a round-bottom flask, and 2g of sodium hydroxide was added. The mixture was heated to 90℃, and 4g of sodium hydroxide and 70g of propylene oxide were added. The mixture was then refluxed and kept at this temperature for 6 hours. After the reflux was completed, the solvent was removed under a vacuum of less than -0.1MPa until the temperature of the residue in the flask reached 70℃. The solution was kept at this temperature for 25 minutes. The residue was then centrifuged while hot, neutralized, adsorbed, and filtered to obtain the target product, polyether polyol.

[0043] Example 3

[0044] At room temperature, 1000g of a byproduct solution containing 48% high-boiling-point byproducts and 62% ethanol as solvent, generated during the production of TGIC, was placed in a 2L round-bottom flask. The mixture was stirred and heated to 100℃, and the distillate was collected. The mixture was then cooled and the residue was collected. The residue was placed in a round-bottom flask, and 3g of hexadecyltrimethylammonium chloride was added. The mixture was heated to 85℃, and then 3g of hexadecyltrimethylammonium chloride and 100g of propylene oxide were added. The mixture was refluxed and kept at this temperature for 4 hours. After the reaction was completed, the solvent was removed under a vacuum of less than -0.085MPa until the temperature of the reactor reached 80℃. The solution was kept at this temperature for 60 minutes. The residue was then centrifuged while hot, neutralized, adsorbed, and filtered to obtain the target product, polyether polyol.

[0045] Example 4

[0046] At room temperature, 1000g of a byproduct solution containing 40% high-boiling-point byproducts and 60% methanol as solvent during TGIC production was placed in a 2L round-bottom flask. The mixture was stirred and heated to 100℃, and the distillate was collected. The mixture was then cooled and the residue was collected. The residue was placed in a round-bottom flask, and 4g of tetramethylammonium chloride was added. The mixture was heated to 80℃, and then 4g of tetramethylammonium chloride and 60g of propylene oxide were added. The mixture was refluxed and kept at this temperature for 5 hours. After the reaction was completed, the solvent was removed under a vacuum of less than -0.09MPa until the temperature of the reactor reached 90℃. The solution was kept at this temperature for 20 minutes. The residue was then centrifuged while hot, neutralized, adsorbed, and filtered to obtain the target product, polyether polyol.

[0047] Example 5

[0048] At room temperature, 1000g of a byproduct solution containing 5% TGIC, 45% high-boiling-point byproducts, and 50% methanol as solvent during TGIC production was placed in a 2L round-bottom flask. The mixture was stirred and heated to 90°C, and the distillate was collected. The mixture was then cooled and the residue was collected. The residue was placed in a round-bottom flask, and 5g of cetyltrimethylammonium bromide was added. The mixture was heated to 70°C, and cetyltrimethylammonium bromide and 60g of propylene oxide were added. The mixture was refluxed and kept at this temperature for 4 hours. After the reaction was completed, the solvent was removed under a vacuum of -0.084MPa until the temperature in the reactor reached 80°C. The solution was kept at this temperature for 35 minutes. The residue was then centrifuged while hot, neutralized, adsorbed, and filtered to obtain the target product, polyether polyol.

[0049] Example 6

[0050] The difference from Example 1 is that 5g of potassium hydroxide and 80g of propylene oxide were added simultaneously. The hydrolysis reaction conditions were as follows: 5g of potassium hydroxide was added to a round-bottom flask, nitrogen gas was introduced for protection, the temperature was raised to 80°C, and reflux was maintained for 8 hours. After the reflux was completed, the solvent was removed under a vacuum of less than -0.09MPa until the reactor temperature reached 70°C, and the temperature was maintained for 30 minutes. The residue after solvent removal was centrifuged while hot, neutralized, adsorbed, and filtered to obtain the target product, polyether polyol.

[0051] The concentrations and weight-average molecular weights of the polyether polyols obtained in Examples 1-6 are shown in Table 1.

[0052] Table 1

[0053] serial number Conversion rate (%) Hydroxyl value (mgKOH / g) weight average molecular weight Example 1 99.96 634 673 Example 2 99.71 483 724 Example 3 99.25 510 590 Example 4 99.69 469 1035 Example 5 99.37 550 845 Example 6 99.18 475 749

[0054] As can be seen from the above description, the embodiments of the present invention achieve the following technical effects:

[0055] This invention achieves the effective resource utilization of TGIC byproducts, and the method is simple, green, and environmentally friendly. The resulting polyether polyol has excellent product quality and good market prospects.

[0056] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for preparing polyether polyols from triglycidyl isocyanate byproducts, characterized in that, include: S1, the triglycidyl isocyanurate byproduct is mixed with propylene oxide and alkali, and subjected to hydrolysis reaction to obtain intermediate product; wherein, the triglycidyl isocyanurate byproduct is a byproduct of the reaction of isocyanuric acid and epichlorohydrin to produce triglycidyl isocyanurate. S2, the intermediate product is subjected to solvent removal treatment and separation treatment to obtain the polyether polyol; The weight ratio of the triglycidyl isocyanurate byproduct to the propylene oxide is (2~6):1; The triglycidyl isocyanurate byproduct includes a solvent and one or more of compounds a, b, and c; 、 、 In compounds a, b, and c, the R groups are each independently... , , One or more of the following combinations; In the triglycidyl isocyanurate byproduct, the weight content of triglycidyl isocyanurate is ≤10%, the weight content of byproducts with a boiling point higher than 110℃ is 10~50%, and the weight content of the solvent is 40~90%.

2. The method for preparing polyether polyols from triglycidyl isocyanate byproducts according to claim 1, characterized in that, In step S1, the weight of the alkali is 0.1-10% of the triglycidyl isocyanurate byproduct.

3. The method for preparing polyether polyols from triglycidyl isocyanate byproducts according to claim 1, characterized in that, The triglycidyl isocyanurate byproduct, the propylene oxide, and the base are mixed simultaneously; or, the triglycidyl isocyanurate byproduct is first mixed with the base in the first part for a first step reaction, and then the propylene oxide and the base in the second part are added for a second step reaction, wherein the weight ratio of the base in the first part to the base in the second part is 1:1 to 5.

4. The method for preparing polyether polyols from triglycidyl isocyanate byproducts according to claim 3, characterized in that, When the triglycidyl isocyanurate byproduct, the propylene oxide, and the alkali are mixed simultaneously, the hydrolysis reaction is carried out at a temperature of 40-100°C for 2-12 hours; or... When the alkali is added in two steps, the hydrolysis reaction includes: The triglycidyl isocyanurate byproduct and the base in the first part are mixed and the first step reaction is carried out at 40~100℃ to obtain the first step reaction product; then the propylene oxide and the base in the second part are added and the second step reaction is carried out at 50~80℃ for 2~10h.

5. The method for preparing polyether polyols from triglycidyl isocyanate byproducts according to claim 4, characterized in that, The hydrolysis reaction is carried out under the protection of an inert gas, which is nitrogen and / or argon.

6. The method for preparing polyether polyols from triglycidyl isocyanate byproducts according to claim 1, characterized in that, The solvent is one or more of methanol, ethanol, diethyl ether, and ethyl acetate.

7. The method for preparing polyether polyols from triglycidyl isocyanate byproducts according to claim 4, characterized in that, The mother liquor after the reaction of isocyanuric acid and epichlorohydrin is heated and distilled at 60-110°C, and the fraction is used as a recycled solvent. The remaining liquid is the isocyanuric acid triglycidyl ester byproduct.

8. The method for preparing polyether polyols from triglycidyl isocyanate byproducts according to claim 3, characterized in that, The alkali is one or more of sodium hydroxide, potassium hydroxide, hexadecyltrimethylammonium chloride, tetramethylammonium chloride, and hexadecyltrimethylammonium bromide.

9. The method for preparing polyether polyols from triglycidyl isocyanate byproducts according to claim 1, characterized in that, The solvent removal process is a negative pressure solvent removal process; the vacuum degree of the negative pressure solvent removal is -0.08 to -0.1 MPa, the temperature is 60 to 100°C, and the time is 10 to 60 min; after solvent removal, a residual liquid is obtained, and the solvent weight content in the residual liquid is 10 to 30%.

10. The method for preparing polyether polyols from the triglycidyl isocyanate byproduct according to any one of claims 1 to 9, characterized in that, The separation process includes centrifugation, neutralization, adsorption, and filtration performed sequentially.

Citation Information

Patent Citations

  • Treatment method of TGIC by-product and utilization method for obtaining adhesion agent by utilizing same

    CN103382376A

  • High activityhydroxyl-terminated polyepichlorohydrin polyatomic alcohol and preparation thereof

    CN101497691A

  • Heat-resisting flame-retardant isocyanurate-ring-containing polyether polyol with controllable hard segment / soft segment ratio and preparation method thereof

    CN103834004A