A functional silicon nitride ceramic substrate based on transient liquid phase bonding and a preparation method thereof

By using silver-indium transient liquid phase bonding technology, bonding of silicon nitride ceramics to copper foil is achieved at low temperatures, solving the problems of high-temperature sintering and insufficient interfacial bonding strength in existing processes. This provides a highly reliable and low-cost silicon nitride copper-clad substrate suitable for high-power electronic devices.

CN116489883BActive Publication Date: 2026-11-24BEIJING INST OF TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310256305.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-16
Publication Date
2026-11-24
Estimated Expiration
2043-03-16

AI Technical Summary

Technical Problem

Existing copper-clad silicon nitride ceramic substrate processes suffer from problems such as high-temperature sintering, insufficient interfacial bonding strength, and high cost, making it difficult to meet the reliability and cost requirements of high-power electronic devices.

Method used

A transient liquid phase bonding process is employed, using a sandwich structure with alternating thin layers of low-melting-point and high-melting-point metals. The bonding of silicon nitride ceramics and copper foil is achieved at low temperatures through silver-indium transient liquid phase bonding technology, forming a void-free continuous bonding interface.

Benefits of technology

It achieves low-temperature bonding and high-temperature service, reduces equipment costs, improves interface bonding strength and reliability, and is suitable for the long-term reliability requirements of high-power electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116489883B_ABST
    Figure CN116489883B_ABST
Patent Text Reader

Abstract

This invention relates to the field of ceramic substrate technology, and more particularly to a functional silicon nitride ceramic substrate based on transient liquid phase bonding and its preparation method. The method includes sequentially preparing a titanium layer, a silver seed layer, an electroplated silver layer, and an indium plating layer on the surface of a silicon nitride substrate; preparing an electroplated silver layer on the surface of an oxygen-free copper foil; performing silver-indium transient liquid phase bonding between the silver-plated side of the oxygen-free copper foil and the indium-plated side of the silicon nitride substrate; and then etching the circuit pattern of the copper-clad substrate. The novel copper-clad silicon nitride substrate process provided by this invention can prepare highly reliable high-power electronic ceramic substrates, which are better suited for use in high-end power electronic products such as electric vehicle power control modules, high-power lasers, power transmission control modules, and wind turbine generators.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of ceramic substrate technology, and in particular to a functional silicon nitride ceramic substrate based on transient liquid phase bonding and its preparation method. Background Technology

[0002] In recent years, third-generation semiconductors, represented by silicon carbide (SiC), have advantages over silicon, such as a wider bandgap, higher critical breakdown field strength, and higher thermal conductivity. This allows power electronic devices based on SiC, such as high-power lasers, power control modules based on insulated-gate bipolar transistors (IGBTs), and high-voltage transmission modules, to withstand higher voltages and currents and operating temperatures exceeding 300°C, making them the core of a series of high-power devices. The upgrading of chips and changes in service environments have also placed higher demands on packaging substrates: traditional resin-based substrates can no longer withstand such high operating temperatures, currents, and voltages; furthermore, their copper plating is relatively thin (<100µm). Electronic ceramic substrates possess high thermal conductivity, heat resistance, high breakdown field strength, and excellent mechanical properties, and their coefficient of thermal expansion matches that of the chip material. They are currently the most suitable packaging substrates for high-power electronic devices. Currently, metallized ceramic substrates based on alumina (Al2O3), aluminum nitride (AlN), and silicon nitride (Si3N4) ceramics are widely used in power control and transportation, high-speed rail, electric vehicles, and aerospace. Alumina and aluminum nitride have been developed earlier and have formed relatively mature preparation and process flows, and have a long history of development in the fields of engineering and electronic devices. In recent years, with the gradual maturation of silicon nitride ceramic preparation technology, especially the breakthrough in the preparation technology of high thermal conductivity silicon nitride ceramic (>70W / (m·K)), silicon nitride ceramics have begun to surpass alumina and silicon nitride ceramics in all aspects of performance, and have become a key material for the further development of power devices.

[0003] In the field of high-power electronic devices, the most commonly used ceramic substrate materials are alumina (Al2O3) and aluminum nitride (AlN). Alumina has the lowest cost and good mechanical properties, and is currently the most widely used. The main problem is that alumina has a relatively low thermal conductivity (20-30 W / (m·K)), which cannot meet the heat dissipation requirements of higher-power power electronic devices. In contrast, aluminum nitride has a significantly improved thermal conductivity (140-260 W / (m·K)), which is 7-8 times that of alumina, and is used more in higher-end power electronics. However, its thermal cycling and functional cycle reliability is poor, making it unsuitable for applications with high reliability requirements for power devices and systems, and its manufacturing cost is high, ten times that of alumina. Silicon nitride has a more comprehensive performance than alumina and aluminum nitride ceramics, and has a qualitative improvement in key performance aspects: a higher thermal conductivity than alumina (80-170 W / (m·K)); ultra-high withstand voltage breakdown and bending strength; and stable reliability under high current loads and more than 5000 cycles. Silicon nitride possesses the best overall performance among numerous electronic ceramic materials, making it particularly suitable for applications requiring high reliability and long lifespan. The development of next-generation silicon nitride power electronic ceramic substrates has become a key area of ​​focus for electronic ceramic substrate manufacturers worldwide.

[0004] The primary function of power electronic ceramic substrates is to provide a working platform for chips, enabling reliable electrical connections and protection, while also dissipating the heat generated during power chip operation. They typically employ a structure where a ceramic sheet is double-sided covered with thick copper foil (200–300 μm). The main technological challenge is the heterogeneous bonding of metallic copper and ceramic materials. Early alumina copper-clad ceramic substrates used a direct copper plating (DBC) process, generating a layer of copper oxide on the copper foil surface. Bonding between the copper foil and alumina was achieved through a eutectic reaction between alumina and copper oxide at high temperatures. This method is simple and low-cost, but the resulting reaction layer affects thermal conductivity. Direct copper-clad alumina ceramic substrates have low reliability and are prone to cracking during long-term thermal cycling. When using aluminum nitride ceramics instead of alumina ceramics, pre-oxidation of the aluminum nitride surface is also required.

[0005] Currently, active metal brazing (AMB) is used in industry for copper cladding of aluminum nitride and silicon nitride ceramics. The principle involves using reactive solder containing small amounts of active metals, such as titanium and zirconium, to bond copper to the ceramic substrate. A commonly used brazing system is silver-copper-titanium solder paste, which contains (2%–5%) titanium. Titanium can react with elements such as N and Si in aluminum nitride (AlN) and silicon nitride (Si3N4) at around 900℃ to form compounds. While the AMB process is relatively simple, several issues limit its application: 1. Due to the easy oxidation of titanium, high requirements are placed on the solder and brazing equipment. The sintering process must be carried out under high vacuum. The organic components in the solder paste, such as diluents and binders, can affect the lifespan of the vacuum brazing furnace during long-term brazing. Furthermore, the venting process required during the low-temperature stage (150℃–400℃) of the solder sintering process can create bubbles or channels at the interface after gas escape, reducing the thermal conductivity of the substrate and lowering the interfacial bonding strength. 2. Solder composition significantly affects the microstructure of the sintered interface. Changes in solder composition, such as excessive titanium content, can lead to the formation of coarse compounds at the interface, resulting in decreased interfacial bonding strength. Conversely, insufficient titanium content prevents the formation of a continuous bonding interface. 3. The interfacial bonding strength of AMB-sintered copper-clad ceramic substrates is typically 15–25 MPa, which is insufficient for applications requiring high interfacial bonding strength and reliability. 4. The process temperature is relatively high, with typical brazing temperatures ranging from 850 to 900°C. 5. Activated solder is costly, typically priced at 20–30 RMB per gram. Therefore, there is an urgent need to develop novel copper-clad processes for silicon nitride substrates. Summary of the Invention

[0006] To address the aforementioned technical problems, this invention provides a functional silicon nitride ceramic substrate based on transient liquid phase bonding and its preparation method.

[0007] According to the present invention, the transient liquid phase bonding process uses a sandwich structure of alternating thin layers of low-melting-point metal and high-melting-point metal. This allows for the melting of the low-temperature metal at low temperatures and the rapid formation of corresponding intermetallic compounds and solid solutions with the high-melting-point metal. The resulting components can withstand much higher operating temperatures (>350°C), enabling low-temperature bonding and high-temperature operation. Commonly used transient liquid phase systems include Au-Sn, Au-In, Ag-In, Cu-In, and Cu-Sn, primarily using low-melting-point metals such as In and Sn in combination with commonly used metals in electronic packaging such as Au, Ag, and Cu. Among these, the Ag-In and Cu-In transient liquid phase systems have simple reactants, fast reaction rates, high joint strength and reliability, and good mechanical properties, enabling bonding of power electronic ceramic substrates to copper foil. In the international market, the unit price of raw materials for silver (~15 USD / oz.), copper, and indium (~5 USD / oz.) is much lower than that for gold, giving them a significant cost advantage over traditional Au-Sn and Au-Ga systems. Compared to AMB processes, transient liquid phase processes such as silver-indium and copper-indium bonding can lower the bonding temperature to around 200°C, effectively preventing substrate warping during bonding. This meets the low-temperature packaging requirements of many temperature-sensitive devices, including optoelectronic devices. Furthermore, the reaction does not need to be carried out under high vacuum; low vacuum is sufficient for bonding. In addition, the silver-indium transient liquid phase process does not involve the decomposition and venting of organic components during brazing, thus significantly reducing interfacial porosity and easily forming a void-free continuous bonding interface, enabling the production of highly reliable silicon nitride copper-clad ceramic substrates. Taking silver-indium transient liquid phase bonding technology as an example, the silver-indium system features fast reaction speed, a simple silver-indium reaction system, and no phase transition, meeting the long-term reliability requirements of power devices. The most important aspect of using silver-indium transient liquid phase bonding to connect thick copper foil to silicon nitride ceramic is the preparation of a silver / indium layer on the surface of both the silicon nitride ceramic and the copper foil. The thickness of the silver / indium layer used for transient liquid phase bonding is typically tens of micrometers, with the overall bonding layer thickness controlled below 50 μm. A silver / indium bilayer structure is fabricated on the surface of a silicon nitride substrate, and a layer of silver is also plated on the copper foil on the other side. After being assembled by a fixture, the copper foil is bonded to the surface of the silicon nitride substrate in a vacuum furnace.

[0008] In a first aspect, the present invention provides a method for preparing a functional silicon nitride ceramic substrate based on transient liquid-phase bonding, comprising:

[0009] 1) A titanium layer, a silver seed layer, an electroplated silver layer, and an indium plating layer are sequentially prepared on the surface of a silicon nitride substrate;

[0010] 2) Prepare an electroplated silver layer on the surface of oxygen-free copper foil;

[0011] 3) Perform silver-indium transient liquid phase bonding between the silver-plated side of the oxygen-free copper foil and the indium-plated side of the silicon nitride substrate;

[0012] 4) Perform copper-clad substrate circuit pattern etching.

[0013] Preferably, in step 1), a titanium layer of 40-60 nm is deposited by magnetron sputtering on the surface of the silicon nitride substrate, and then a silver seed layer of 0.5-1.5 μm is deposited by magnetron sputtering on the titanium layer. A first electroplated silver layer of 10-15 μm is electroplated on the surface of the silver seed layer, and an indium plating layer of 8-12 μm, preferably 10 ± 1 μm, is electroplated on the surface of the first electroplated silver layer.

[0014] Preferably, in step 1), an indium plating layer is prepared by low-temperature electroplating, and after indium plating, it is stored in a low-temperature freezer at a temperature preferably below -20°C; the thickness of the indium plating layer is preferably controlled at 10 μm.

[0015] Preferably, in step 1), during magnetron sputtering deposition, the deposition rate of titanium is 0.1–1.2 nm / s, the deposition rate of silver is 1–5 nm / s, the working pressure during titanium deposition is controlled at 1–2 Pa, and the working pressure during silver deposition is 0.2–0.4 Pa.

[0016] Preferably, the process also includes a step of fine polishing and cleaning the silicon nitride substrate and the oxygen-free copper foil.

[0017] Further preferred, the surface is finely polished to a roughness of <1µm; the silicon nitride substrate is cleaned with acetone, anhydrous ethanol and deionized water.

[0018] Further preferably, the titanium layer and the silver seed layer are made of titanium and silver targets with a purity of 99.99%, respectively; preferably, the basic vacuum of the deposition chamber is <3×10⁻⁶. -3 Pa; preferably, the electroplating silver solution is an environmentally friendly silver plating solution, the anode plate uses 99.99% silver foil, the cathode is a silicon nitride substrate, and the cathode current density is selected as 5-10 mA / cm². 2 .

[0019] Preferably, in step 2), a second silver plating layer of 8-12 μm is electroplated on the surface of the oxygen-free copper foil.

[0020] Further preferred, in step 2), the oxygen-free copper foil is flattened and its surface is cleaned using organic solvents, degreasing agents, and deionized water.

[0021] Preferably, in step 3), the silver-plated side of the oxygen-free copper foil is assembled with the indium-plated side of the silicon nitride substrate, and a pressure of 0.5 to 1.5 MPa is applied; the bonding process uses vacuum heating, the vacuum degree during the bonding process is <0.1 Pa, and the target bonding temperature is 190℃ to 220℃; the heating curve adopts a rapid heating and slow cooling method; preferably, the heating rate is >20℃ / min, and after reaching the target bonding temperature, it is held for 10 to 20 minutes, preferably 10 to 15 minutes, and then allowed to cool naturally.

[0022] Preferably, the method further includes laser drilling on the surface of a silicon nitride substrate to form a tapered hole with a sidewall angle, wherein the diameter of the tapered hole is 10–100 μm and the tapered hole angle is 4–6°.

[0023] As a preferred method, low-power laser drilling is used, and underwater laser drilling is even more preferred.

[0024] Preferably, in step 4), a wet etching method is used to pattern the circuit on the surface of the thick copper foil; preferably, the thick copper foil is etched first, and then the bonding layer material of the patterned area is removed. The etchant used for the thick copper foil is a PCB board etchant, preferably a spray etching solution; the etchant used for the bonding layer metal is a silver etchant, and the etching is preferably done in short, multiple passes.

[0025] Secondly, the present invention provides a functional silicon nitride ceramic substrate, which is prepared by the aforementioned method for preparing a functional silicon nitride ceramic substrate based on transient liquid phase bonding.

[0026] Thirdly, the present invention provides the application of functional silicon nitride ceramic substrates prepared by the method for preparing functional silicon nitride ceramic substrates based on transient liquid phase bonding in electric vehicle power control modules, high-power lasers, power transmission control modules, and wind turbine generator sets.

[0027] The functional silicon nitride ceramic substrate and its preparation method provided by this invention utilize transient liquid phase bonding to achieve copper cladding on silicon nitride ceramics. Through the metallization process of silicon nitride ceramics, bonding, and circuit patterning of the metallized ceramic substrate, this invention can prepare a high-reliability, high-power electronic ceramic substrate, which can be well used in high-end power electronic products such as electric vehicle power control modules, high-power lasers, power transportation control modules, and wind turbine generators. Attached Figure Description

[0028] To more clearly illustrate the embodiments of the present invention and the technical solutions in the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0029] Figure 1 A schematic diagram illustrating the preparation of a silicon nitride copper-clad ceramic substrate based on a transient liquid-phase bonding method according to an embodiment of the present invention;

[0030] Figure 2 The silver-indium phase diagram provided in the embodiments of the present invention;

[0031] Figure 3 A schematic diagram of a tapered hole formed on the surface of a silicon nitride substrate provided in an embodiment of the present invention;

[0032] Figure 4 This is a schematic diagram of the circuit pattern on the surface of a thick copper foil provided in an embodiment of the present invention. Detailed Implementation

[0033] To make the objectives, technical solutions, and advantages of the embodiments of the invention clearer, the technical solutions of the embodiments of the invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of the invention. All other embodiments obtained by those skilled in the art based on the embodiments of the invention without creative effort are within the scope of protection of the invention.

[0034] Unless otherwise stated, all raw materials and reagents used in the following examples are commercially available products or can be prepared by known methods. Where specific techniques or conditions are not specified in the examples, they are performed using conventional methods or in accordance with techniques or conditions described in the literature in this field, or according to the product instructions. Reagents and instruments whose manufacturers are not specified are all conventional products that can be purchased from legitimate channels.

[0035] In the description of the embodiments of the present invention, it should be noted that the terms "top," "bottom," "inner," "outer," "upper," and "lower," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing the embodiments of the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on the embodiments of the present invention. In addition, the terms "first," "second," and "third" are used for descriptive purposes only and should not be construed as indicating or implying relative importance.

[0036] In the description of the embodiments of the present invention, it should be noted that, unless otherwise explicitly specified and limited, the terms "connected" and "linked" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium. Those skilled in the art can understand the specific meaning of the above terms in the embodiments of the present invention based on the specific circumstances.

[0037] This invention provides a method for preparing a functional silicon nitride ceramic substrate based on transient liquid-phase bonding, as well as the functional silicon nitride ceramic substrate itself, according to some embodiments. The invention will be further described below with reference to embodiments and accompanying drawings.

[0038] In this embodiment of the invention, Figure 1 This paper illustrates the complete process and key technical points for preparing silicon nitride copper-clad ceramic substrates based on transient liquid-phase bonding. The silicon nitride substrate is pre-polished to reduce surface roughness (<1µm) to enhance the adhesion of subsequent metallization layers. Excessive roughness on the silicon nitride surface hinders the formation of a continuous and dense sputtered silver layer, affecting the thickening and bonding process of subsequent silver layers. Due to the relatively poor adhesion between the silicon nitride substrate and silver, a titanium layer of 40–60 nm (preferably 50 nm) is magnetron sputtered onto the silicon nitride substrate surface as an adhesion layer for the deposited silver. Then, a silver seed layer of 0.5–1.5 µm (preferably 1 µm) is magnetron sputtered onto the titanium layer as a seed layer for the subsequent first electroplated silver layer. The first electroplated silver layer is prepared using an environmentally friendly silver plating solution, with a thickness of 10–15 µm. Finally, an indium plating layer of 8–12 µm (preferably 10 µm) is electroplated onto the first electroplated silver layer. Both the titanium layer and the silver seed layer were deposited using magnetron sputtering with 99.99% pure titanium and silver targets. Before deposition, the silicon nitride substrate was cleaned with acetone, anhydrous ethanol, and deionized water. The surface cleanliness and smoothness of the silicon nitride ceramic are crucial for the quality of the metallization layer and subsequent bonding. The basic vacuum of the deposition chamber was <3×10⁻⁶. -3 Pa. Because titanium oxidizes readily in air, a dual-target or multi-target deposition system must be used. A high vacuum environment must be maintained throughout the deposition process, and the sample stage rotation system must be activated during deposition to ensure uniform thickness across different areas. A well-deposited silver seed layer is silvery-white, with no bubbles or protrusions on the surface and a good metallic luster. The sputtered silver film has fine grains, with surface particles at the nanometer or submicrometer level, consistent undulations, and a roughness similar to the initial roughness of the silicon nitride substrate surface. There are no obvious phenomena such as excessive grain growth, and its surface quality can be evaluated using scanning electron microscopy and atomic force microscopy. The silicon nitride substrate with a well-deposited silver seed layer can then be used for subsequent silver electroplating to thicken the silver layer. An environmentally friendly silver plating solution is used, with 99.99% silver foil as the anode plate and a silicon nitride substrate as the cathode. The cathode current density is selected as 5–10 mA / cm².2 Electroplating quality is ensured by using cathode movement, plating solution agitation, and continuous plating solution filtration. A profilometer is used to measure the thickness of the silver plating layer. The indium plating layer is prepared by electroplating. Because it is easily consumed prematurely at high temperatures due to diffusion reactions with silver, a low-temperature process is usually used. After indium plating, it should be stored in a low-temperature freezer (-15 to -25°C) to slow down silver-indium interdiffusion. This ensures sufficient liquid phase filling of the interface pores during subsequent transient liquid phase bonding, forming a continuous bonding interface. The thickness of the indium plating layer is controlled at around 10 μm, as its content affects the microstructure and distribution of the bonding interface. Maintaining a certain proportion of indium results in a more robust and reliable bonding joint. A second silver plating layer of 8–12 μm, preferably 10 μm, is electroplated onto the oxygen-free copper foil surface. Before metallization, oxygen-free copper foil also needs to undergo fine polishing and cleaning. Industrially produced oxygen-free copper foil is usually produced in roll form. After cutting, the surface is usually uneven. It needs to be flattened with a flattening machine to ensure good contact of the metal layers in the subsequent bonding process. Using organic solvents, degreasing agents and deionized water to clean the surface dust and rust inhibitors can ensure good adhesion of the second electroplated silver layer on the surface of oxygen-free copper foil and ensure its interface strength.

[0039] In a further preferred embodiment, when using magnetron sputtering for thin film preparation, the deposition rate must be controlled to maintain good film quality. The deposition rate is mainly determined by the instrument power; preferably, the deposition rate for titanium is 0.1–1.2 nm / s, more preferably 0.2–1 nm / s, while the deposition rate for silver is 1–5 nm / s. During deposition, argon gas is introduced to generate sputtered ions through glow discharge. The argon gas flow rate affects both the number of incident ions and the density of the deposited film. Studies have shown that at higher argon gas flow rates, the gas pressure increases, resulting in shorter molecular free paths for the incident ions, making them more prone to collisions and reduced kinetic energy during deposition. Appropriately reducing the argon gas flow rate, i.e., using the low argon gas flow rate employed in the art, yields a denser film. The working gas pressure for titanium deposition is controlled at 1–2 Pa, and the working gas pressure for silver deposition is 0.2–0.4 Pa, preferably 0.3 Pa. When depositing thick films, the prolonged bombardment of the substrate by incident ions leads to a continuous increase in substrate temperature. Studies have shown that when the substrate temperature is too high, the deposited film becomes more porous and prone to forming protrusions, resulting in poor film quality. Therefore, after a period of operation, the power supply can be interrupted to cool the substrate and target. Since the cooling rate is relatively slow under high vacuum conditions, when the magnetron sputtering time is long (>30 min), the cooling time should be extended to allow the substrate to cool down to below 60°C.

[0040] As a preferred embodiment, after the above deposition process is completed, such as Figure 1The process involves assembling an oxygen-free copper foil with a silver-plated side and an indium-plated side of a silicon nitride substrate, applying a pressure of 0.5–1.5 MPa (preferably 1 MPa) to maintain good contact at the silver-indium interface. A vacuum furnace is used for bonding, with a vacuum level <0.1 Pa to prevent indium oxidation. The heating profile employs a rapid heating and slow cooling method; the target bonding temperature is between 190°C and 220°C, with a heating rate >20°C / min. The heating rate is reduced as the temperature approaches the target temperature to prevent exceeding it. After reaching the target bonding temperature, the temperature is held for 10–20 minutes followed by natural cooling.

[0041] In the transient liquid-phase bonding process of silver and indium, the type of reactants at the bonding joint has a significant impact on the bonding effect. Intermetallic compounds between silver and indium include AgIn2, Ag2In, and silver-indium solid solutions. Due to the room-temperature diffusion reaction between silver and indium, when preparing an indium layer on the surface of an electroplated silver layer, silver diffuses into the indium through gaps and forms AgIn2. This leads to the consumption of In, and the reduction of the liquid phase during bonding is not conducive to the formation of a void-free interface. Therefore, a high preparation rate is required when preparing the indium layer to retain enough pure indium for the bonding reaction. During the heating process in bonding, the indium layer prepared on the silicon nitride substrate will first undergo solid-state interdiffusion and reaction with the silver layer on the copper foil surface. Since there is also an electroplated silver layer under the indium layer, the interface between the two silver and indium layers will see the growth of AgIn2 intermetallic compounds. Figure 2As shown in the silver-indium phase diagram, pure indium has a melting point of 156.6℃. When the temperature rises above 160℃, indium begins to melt in large quantities to form a liquid phase. The pressure applied by the bonding fixture allows the fluidity of the liquid phase to overcome the original roughness of the bonding layer surface, thus completely filling the voids and gaps at the bonding interface. This is the most significant advantage of transient liquid phase technology. During the solid-state diffusion reaction, AgIn2 will undergo peritectic decomposition, transforming into liquid indium and the intermetallic compound Ag2In at 166℃. The amount of liquid indium formed in this portion is very small and mixed with the Ag2In generated by the peritectic reaction, thus preventing the formation of a continuous wetting layer on the entire joint during the bonding process. Therefore, if excessive indium has already diffused with silver to form the AgIn2 intermetallic compound before the liquid phase forms, it is detrimental to the porosity-free bonding interface during the liquid phase reaction. However, a certain thickness of AgIn2 intermetallic compound layer can act as a barrier layer for silver-indium interdiffusion, thereby preventing excessive interdiffusion. When indium diffuses into silver, boundary diffusion is the preferred method. When liquid indium comes into direct contact with silver, the rapid diffusion along grain boundaries leads to a porous microstructure in the bonding joint, affecting the joint's strength and thermal conductivity, which is detrimental to the long-term reliability of high-power electronic ceramic substrates. Therefore, the volume ratio of the AgIn2 intermetallic compound layer and the pure silver layer is designed to achieve the best bonding effect. The thickness of the AgIn2 intermetallic compound layer can be controlled by a room-temperature aging process, with its thickness ratio to the pure indium layer controlled at 1:1 to 3, preferably 1:2, i.e., a 10µm thick pure indium layer. Before bonding, the thickness of the AgIn2 intermetallic compound layer is 2-4µm, preferably 3µm. This is achievable in previous studies; when 10µm thick indium is electroplated at room temperature, a 2-3µm thick AgIn2IMC layer can be grown after 3-4 hours at room temperature. In this invention, the sample before bonding is placed in a cryogenic freezer below -20°C to prevent excessive diffusion of silver and indium.

[0042] After the bonding temperature exceeds the indium liquidus line, a solid-liquid reaction occurs. Liquid indium continuously reacts with silver to form Ag₂In and a silver-indium solid solution. This process can be completed within tens of seconds to minutes, until all liquid phases are completely solidified, at which point the initial joint reaction is complete. A further holding period of 10–15 minutes is then applied to promote continued reaction and homogenization, until all peritectic reactions are complete. During the homogenization stage, the joint material recrystallizes, and the materials on both sides of the bonding interface grow together until they are completely fused, the initial interface disappears completely, and a reliable metallurgical bond is formed.

[0043] As a preferred embodiment, in power electronic ceramicized metal substrates, it is often necessary to drill holes in the ceramic substrate and metallize it to connect circuit wiring on both sides, or to create through holes for mounting vias. For example... Figure 3As shown, laser drilling is performed on the surface of a silicon nitride substrate to form tapered holes with sidewall angles. The diameter of the tapered holes varies from 10 to 100 μm, and the taper angle is 4 to 6°, preferably 5°. The purpose of setting the taper is to facilitate the subsequent metallization process. Metallization is performed using magnetron sputtering followed by electroplating. First, a 40-60 nm, preferably 50 nm, titanium layer is deposited on the silicon nitride surface as an adhesion layer, followed by electroplating of a silver or copper metallization layer. The tapered angle makes it easier for the titanium or other metallization layers to be deposited on the sidewalls. Since the adhesion of the titanium thin layer manufactured using thin-film technology is sensitive to the roughness and cleanliness of the hole wall, low power is used when drilling the silicon nitride substrate with a laser to avoid rapid material vaporization and the introduction of residues and oxidation. When the ceramic surface oxidizes, it will seriously affect the adhesion of the adhesion layer. Underwater laser drilling has become the preferred method for precision ceramic laser drilling because it avoids surface oxidation and ablation of materials. The method involves using a suitable aqueous solution as the medium, placing the ceramic part directly into the solution for drilling. The good cooling properties of the aqueous solution effectively remove the heat generated by the laser beam, preventing excessive ablation of the drilling area. Excessive ablation can lead to material vaporization and spatter, resulting in residue and surface oxidation. When fabricating holes with high aspect ratios, excessive ablation in the aperture direction must be avoided; therefore, underwater laser drilling is the preferred method.

[0044] In a preferred embodiment, the circuit patterning on the surface of the thick copper foil is processed using a wet etching method. For example... Figure 4As shown, the multilayer metal layers on the silicon nitride substrate are mainly thick copper foil, with a small amount of bonding layer materials such as titanium, silver, and indium at the interface. Wet etching etchants are generally specific, ensuring a high etching rate for one material without affecting other materials. In this invention, etching is performed in two steps: first, etching the thick copper foil; second, removing the bonding layer material from the patterned areas. The etching agent used for the thick copper is an environmentally friendly PCB etchant. Compared to traditional nitric acid or concentrated sulfuric acid etching, the environmentally friendly etchant has a faster etching rate, is pollution-free, and can etch sidewalls with high aspect ratios, which is beneficial for manufacturing fine-line-width circuit patterns. Before etching, the copper foil surface needs to be cleaned and finely polished to facilitate the adhesion of the masking layer material. Traditional PCB etching uses thermal transfer to create the masking layer material, transferring ink onto the copper-clad laminate via thermal transfer paper to act as the etching masking layer. Areas not covered by the masking layer are gradually etched by the etching solution during the etching process, forming the final circuit pattern. A masking layer is directly prepared on the surface of a copper-clad laminate using an inkjet printer. The inkjet printer shapes the masking layer material through inkjet printing, followed by photopolymerization for a strong adhesion. It is equipped with a corresponding cleaning solution, overcoming the drawback of traditional thermal transfer methods where ink is difficult to remove. In etching thick copper foils (200-300µm), the etching process requires a long time due to the large thickness. Wet etching is usually isotropic, which can lead to corrosion of the sidewalls of the circuit patterns. In areas with finer linewidths, this can result in excessive corrosion of the sidewalls of the interconnects. Spraying an etching solution can promote longitudinal corrosion of the copper foil and reduce sidewall corrosion. However, for power electronic ceramic substrates, due to the separate design of control and power circuits, the circuit patterns are usually simple, and the copper-clad laminate, which must withstand high currents, is not designed with very fine linewidths.

[0045] For the etching of the bonded metal layer, due to its thin thickness (<30µm) and composition mainly consisting of silver, its solid solution, and intermetallic compounds, a silver etchant is used. Etching should be performed in short, multiple passes to avoid over-etching.

[0046] According to embodiments of the present invention, the bonding joint prepared by silver-indium transient liquid-phase bonding exhibits excellent interfacial strength. After forming a void-free bonding interface, its shear strength can reach over 80 MPa, while the shear strength of traditional active metal brazing is <40 MPa. This high-strength bonding joint allows ceramic substrates to have higher reliability and lifespan during service. The bonding joint based on silver-indium transient liquid-phase bonding exhibits excellent high-temperature stability. Typical high-power electronic devices operate at temperatures exceeding 300°C. After the reaction, pure indium is completely consumed at the silver-indium interface, and the generated Ag₂In remains in a solid state at around 600°C. The silver-indium bonding joint is formed at around 180°C but can withstand temperatures above 350°C. The low bonding temperature and high service temperature protect the power chip from damage during bonding and allow it to withstand higher operating temperatures, which is highly advantageous for the operation of high-power devices. Ag₂In can withstand high and low temperature cycles and thermal shocks during power device operation without significant performance degradation.

[0047] Silver-indium bonding joints exhibit excellent chemical stability. Silver is easily corroded by sulfur vapors, hydrogen sulfide, sulfur dioxide, and other gases containing sulfur, and the resulting silver sulfide corrosion product is detrimental to the operation and long-term service of electronic devices. However, after forming Ag₂In and a silver-indium solid solution, the change in the valence electrons of silver gives it excellent chemical corrosion resistance. It can withstand long-term annealing in air without any oxidation or degradation.

[0048] For a long time, the electrochemical corrosion of silver has been a major factor limiting its application in electronic packaging. Silver has the highest electrochemical mobility among common electronic packaging metals, and it readily grows whiskers under the coupling effect of moisture and current. This can lead to severe current series connections, affecting the normal operation of current circuits. Research has found that silver-indium solid solutions have excellent resistance to electrochemical migration; a certain proportion of silver-indium solid solutions can completely resist electrochemical migration. Its unique chemical stability can ensure the normal operation of power circuits.

[0049] The mechanical properties of intermetallic compounds produced by transient liquid phase bonding processes significantly impact the bonding joints. Changes in joint composition often affect their mechanical properties. For silver-indium transient liquid phase bonding systems, by adjusting the volume ratio between silver and indium, a joint composition consisting of Ag₂In and a silver-indium solid solution can be obtained during the silver-indium transient liquid phase bonding process. This composition remains stable over a long period during operation, without undergoing phase transformation of the intermetallic compound, which is crucial for maintaining joint composition stability. Most intermetallic compounds are brittle due to their superlattice structure, which can lead to easy cracking at the bonding interface. Ag₂In, however, exhibits a certain degree of toughness. In standard micron indentation tests, Ag₂In demonstrates the characteristics of a tough material, exhibiting no cracks even under a maximum load of 1000 gf, while most intermetallic compounds, such as Cu₃Sn and Cu₆Sn₅, fracture under compressive stress. Therefore, the high mechanical toughness exhibited by Ag₂In enables it to maintain the stability and reliability of the mechanical connection during long-term service.

[0050] This invention discloses a silicon nitride ceramic copper-clad substrate process, encompassing the selection of the metal for the silicon nitride surface adhesion layer, the preparation method of the silver / indium bonding layer material, the control of the silver-indium transient liquid phase bonding process, and the etching of circuit patterns on the copper-clad substrate. It comprehensively covers the technical route for silicon nitride substrate copper clad substrates. This is expected to significantly reduce the process difficulty and equipment cost of silicon nitride substrate copper clad substrates. The silver-indium transient liquid phase bonding method employed can prepare highly reliable bonding interfaces, increasing the yield rate of product manufacturing. In terms of industrial applications, silicon nitride copper-clad substrates can be used in high-end power electronic products such as electric vehicle power control modules, high-power lasers, and wind turbine generators. Highly reliable and long-life silicon nitride copper-clad ceramic substrates can enable power electronic devices to better perform.

[0051] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a functional silicon nitride ceramic substrate based on transient liquid-phase bonding, characterized in that, include: 1) A titanium layer, a silver seed layer, an electroplated silver layer, and an indium plating layer are sequentially prepared on the surface of a silicon nitride substrate; 2) Prepare an electroplated silver layer on the surface of oxygen-free copper foil; 3) Perform silver-indium transient liquid phase bonding between the silver-plated side of the oxygen-free copper foil and the indium-plated side of the silicon nitride substrate; 4) Perform copper-clad substrate circuit pattern etching; In step 1), a titanium layer of 40-60 nm is deposited by magnetron sputtering on the surface of the silicon nitride substrate, and then a silver seed layer of 0.5-1.5 μm is deposited by magnetron sputtering on the titanium layer. A first electroplated silver layer of 10-15 μm is electroplated on the surface of the silver seed layer, and an indium plating layer of 8-12 μm is electroplated on the surface of the first electroplated silver layer. In step 2), a second silver plating layer of 8~12um is electroplated on the surface of the oxygen-free copper foil; In step 3), the silver-plated side of the oxygen-free copper foil is assembled with the indium-plated side of the silicon nitride substrate, and a pressure of 0.5~1.5 MPa is applied. Vacuum heating is used in the bonding process, with a vacuum degree of <0.1 Pa and a target bonding temperature of 190℃~220℃. The heating curve adopts a rapid heating and slow cooling method. The heating rate is >20℃ / min. After reaching the target bonding temperature, the temperature is held for 10~20 minutes and then allowed to cool naturally.

2. The method for preparing a functional silicon nitride ceramic substrate based on transient liquid-phase bonding according to claim 1, characterized in that, An indium plating layer of 10±1µm is electroplated on the surface of the first electroplated silver layer.

3. The method for preparing a functional silicon nitride ceramic substrate based on transient liquid-phase bonding according to claim 2, characterized in that, In step 1), an indium plating layer is prepared by low-temperature electroplating and stored at a temperature below -20°C after indium plating; the thickness of the indium plating layer is controlled at 10 μm.

4. The method for preparing a functional silicon nitride ceramic substrate based on transient liquid-phase bonding according to claim 3, characterized in that, In step 1), during magnetron sputtering deposition, the deposition rate of titanium is 0.1~1.2 nm / s, the deposition rate of silver is 1~5 nm / s, the working gas pressure during titanium deposition is controlled at 1~2 Pa, and the working gas pressure during silver deposition is 0.2~0.4 Pa.

5. The method for preparing a functional silicon nitride ceramic substrate based on transient liquid-phase bonding according to claim 1, characterized in that, After reaching the target bonding temperature, hold for 10-15 minutes and then allow to cool naturally.

6. The method for preparing a functional silicon nitride ceramic substrate based on transient liquid-phase bonding according to any one of claims 1-4, characterized in that, It also includes laser drilling on the surface of a silicon nitride substrate to form a tapered hole with a sidewall angle, the diameter of which is 10~100um and the angle of which is 4~6°.

7. The method for preparing a functional silicon nitride ceramic substrate based on transient liquid-phase bonding according to claim 1, characterized in that, In step 4), a wet etching process is used to pattern the circuit on the surface of the thick copper foil.

8. The method for preparing a functional silicon nitride ceramic substrate based on transient liquid-phase bonding according to claim 7, characterized in that, The wet etching method includes first etching a thick copper foil, and then removing the bonding layer material of the patterned area. The etchant used for the thick copper foil is a PCB board etchant, and the etching solution is sprayed. The etchant used for the bonding layer metal is a silver etchant, and the etching is performed in short, multiple passes.

9. A functional silicon nitride ceramic substrate, characterized in that, The substrate is prepared by the method for preparing a functional silicon nitride ceramic substrate based on transient liquid phase bonding as described in any one of claims 1-8.

10. The application of the functional silicon nitride ceramic substrate prepared by the method of transient liquid phase bonding according to any one of claims 1-8 in electric vehicle power control modules, high-power lasers, power transmission control modules, and wind turbine generator sets.

Citation Information

Patent Citations

  • Preparation method of aluminum-coated ceramic insulating lining plate

    CN113501725A

  • AlN ceramic copper-clad substrate with firmly combined copper layer and ceramic substrate and preparation method of AlN ceramic copper-clad substrate

    CN115557798A