An In and Sb-enhanced Sn 24-x-y Bi 18 In x Sb y Low-temperature lead-free solder and its preparation method

CN116493805BActive Publication Date: 2026-11-24DALIAN UNIV OF TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310304555.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2026-11-24
Estimated Expiration
2043-03-27

AI Technical Summary

Technical Problem

[0005]本发明是要解决现有的SnBi共晶中Bi相粗大,时效下Bi偏析的性能问题,而设计开发了一种具有良好润湿性能和抗剪切性能的Sn24-x-yBi18InxSby多元焊料

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116493805B_ABST
    Figure CN116493805B_ABST
Patent Text Reader

Abstract

This invention provides an In and Sb-enhanced Sn 24‑x‑ y Bi 18 In x Sb y This invention relates to a low-temperature lead-free solder and its preparation method, belonging to the field of low-melting-point solders. The solder comprises Sn, Bi, In, and Sb elements, with As, S, Ni, Cd, Cr, Zn, and Pb as impurity elements. The alloy composition is derived from a cluster alloy composition design model. The mass percentage (wt.%) of the alloy composition is Bi: 57.0, In: 0.2-1.40, Sb: 0.21-1.50, and the total impurity content (As+S+Ni+Cd+Cr+Zn+Pb) ≤ 0.01, with Sn as the balance. The In / Sb mass percentage ratio is 1:1.06-1.6. This invention optimizes the pre-precipitated Sn-rich phase through alloy composition design by introducing Sb, while simultaneously refining the Bi phase, improving shear resistance, and enhancing wettability. The solder retains high shear resistance even after aging at 110℃ for 240 hours, making it suitable for low-temperature brazing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to an In and Sb-enhanced Sn 24-x-y Bi 18 In x Sb y Low-temperature lead-free solder and its preparation method belong to the fields of low-temperature brazing and electronic packaging. Background Technology

[0002] Sn-Pb solder has been widely used in the electronics industry in recent decades due to its good conductivity, wettability, and low cost. However, Pb is highly toxic, and the rapid pace of electronic device updates has led to an increase in electronic waste, causing significant environmental pollution. Since the beginning of the 21st century, various countries have successively issued restrictions or bans on the use of Pb-containing electronic products, such as the EU's WEEE Directive and RoHS Directive issued in 2003. To develop alternative lead-free solders, researchers have studied binary eutectic solders such as Sn-Ag, Sn-Cu, and Sn-Bi, as well as ternary or multi-component solders based on binary eutectic structures such as Sn-Ag-Cu and Sn-Zn-Cu.

[0003] Sn-Bi eutectic solder is commonly used as a lead-free solder in electronic packaging due to its advantages such as low melting point, low cost, good wettability, and high tensile strength. However, the brittleness of the Bi phase and the aging problem of the solder joint caused by Bi segregation at high temperatures limit its widespread application. Therefore, refining the Bi phase is the key to improving the performance of SnBi-based solder.

[0004] To address the above problems, this invention analyzes the compositional structure of SnBi eutectic solder using a cluster-connecting atom model, and designs a multi-element solder SnBi based on this model. 24-x-y Bi 18 In x Sb y . Summary of the Invention

[0005] This invention aims to address the performance issues of coarse Bi phase and Bi segregation under aging in existing SnBi eutectic materials, and to design and develop a SnBi eutectic material with good wetting and shear resistance. 24-x-y Bi 18 In x Sb y Multi-component solder.

[0006] To achieve the above objectives, the technical solution adopted by the present invention is as follows:

[0007] An In and Sb-enhanced Sn 24-x-y Bi 18 In x Sb yThe low-temperature lead-free solder, wherein the tin-bismuth based solder comprises Sn, Bi, In, and Sb elements, and As, S, Ni, Cd, Cr, Zn, and Pb are impurity elements. The mass percentage (wt.%) of its alloy composition is Bi: 57.0, In: 0.2-1.40, Sb: 0.21-1.50, the total impurities (As+S+Ni+Cd+Cr+Zn+Pb) ≤ 0.01, the balance being Sn, and the mass percentage ratio of In / Sb is 1:1.06-1.6.

[0008] The Sn 24-x-y Bi 18 In x Sb y Low-temperature lead-free solder has better wettability and shear resistance than SnBi eutectic solder, and can be used as the main material for low-temperature brazing and packaging.

[0009] An In and Sb-enhanced Sn 24-x-y Bi 18 In x Sb y The preparation method of low-temperature lead-free solder involves the following steps: First, the elements are proportioned according to their mass percentages, mixed, and placed in a quartz tube. The mixture is then vacuum-sealed and placed in a high-temperature muffle furnace at 650-750℃ for 5-6 hours of constant-temperature melting. During this process, the quartz tube is shaken every 0.5 hours to ensure thorough mixing of the liquid alloy. After melting, the quartz tube is rapidly cooled in cold water to obtain the pre-solder body. Second, the pre-solder body is polished, pressed into thin sheets, dipped in lead-free flux, and placed in a pure Ti crucible. Heating is then used to obtain solder balls. Finally, the solder balls are cooled, cleaned, and air-dried to obtain the final product.

[0010] Using the above technical solution, alloy composition design is implemented based on a cluster alloy design model, which provides the structural unit and corresponding composition formula of the SnBi eutectic. This invention analyzes the SnBi eutectic point composition using a SnBi binary phase diagram and eutectic point composition, determining that the SnBi eutectic point is composed of a Bi-rich Sn phase and a pure Bi phase. The structural unit of the eutectic point is analyzed using a cluster plus connecting atom model as: 2{[Sn-Sn... 10 ]Bi3Sn1}+[Bi-Bi6]Bi5=Sn 24 Bi 18 =Sn 57.1 Bi 42.9 (at.%) = Sn - 57Bi (wt.%). Sn is prepared by introducing strengthening elements In and Sb to slightly replace Sn. 24-x-y Bi 18 In x Sb y Lead-free solder.

[0011] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0012] (1) This invention is based on the cluster alloy design model developed by our team and is an In and Sb-strengthened Sn alloy. 24-x-y Bi 18 In x Sb y Low-temperature lead-free solder. Compared to SnBi eutectic solder, which has a coarse Bi phase structure and suffers from Bi segregation affecting solder joint reliability under high-temperature aging, this invention optimizes the composition by introducing In and Sb elements through a cluster alloy design model. This not only refines the Bi phase but also improves the alloy's wettability and shear resistance, thus mitigating solder joint failure caused by Bi segregation at high temperatures.

[0013] (2) An In and Sb-enhanced Sn provided by the present invention 24-x-y Bi 18 In x Sb y The low-temperature lead-free solder, by adding Sb, allows the Sb element, which is miscible with Bi at high temperatures, to preferentially and uniformly precipitate in the Sn-rich phase during the cooling process, refining the coarse Bi phase and improving the solder's wetting and shear resistance. In addition, the preferential and uniform precipitation of the Sn-rich phase containing a small amount of Sb significantly reduces Bi segregation on the solder surface, and it still exhibits excellent shear resistance after aging at 110℃ for 240 hours. Attached Figure Description

[0014] Figure 1 Example 1: Low-Temperature Lead-Free Solder Sn 23.6 Bi 18 In 0.2 Sb 0.2 Compared with Comparative Example 1, the eutectic solder Sn 24 Bi 18 DSC spectrum;

[0015] Figure 2 Example 1: Low-Temperature Lead-Free Solder Sn 23.6 Bi 18 In 0.2 Sb 0.2 Compared with Comparative Example 1, the eutectic solder Sn 24 Bi 18 Shear resistance diagrams before and after aging at 110℃ for 240 hours;

[0016] Figure 3 Example 1: Low-Temperature Lead-Free Solder Sn 23.6 Bi 18 In 0.2 Sb 0.2 Compared with Comparative Example 1, the eutectic solder Sn 24 Bi18 Backscattering plot; Figure 3 (a) is the solder Sn of Comparative Example 1 24 Bi 18 Backscattering plot; Figure 3 (b) is the solder Sn in Example 1 23.6 Bi 18 In 0.2 Sb 0.2 Backscattering diagram Detailed Implementation

[0017] The technical solution of the present invention will be described in detail below with reference to embodiments and accompanying drawings.

[0018] An In and Sb-enhanced Sn 24-x-y Bi 18 In x Sb y Low-temperature lead-free solder is applied using the following steps:

[0019] I. Sn 24-x-y Bi 18 In x Sb y Composition design and preparation of low-temperature lead-free solder: Based on the cluster alloy composition design model, the solder composition by mass percentage (wt.%) is determined to be Bi: 56.9-58.0, In: 0.2-1.40, Sb: 0.21-1.50, total impurities (As+S+Ni+Cd+Cr+Zn+Pb) ≤ 0.01, with the balance being Sn, and the In / Sb mass percentage ratio being 1:1.06-1.6. The elements are proportioned according to their mass percentages, mixed, and placed in a quartz tube. The mixture is then vacuum-sealed and placed in a high-temperature muffle furnace for constant-temperature melting at 650-750℃ for 5-6 hours. During this period, the quartz tube is shaken every 0.5 hours to ensure thorough mixing of the liquid alloy. After melting, the quartz tube is rapidly cooled in cold water to obtain the pre-solder.

[0020] II. Solder Ball Preparation: The solder before the body is sanded smooth to remove the surface oxide scale, and then pressed into a thin sheet of 0.2 mm using a micro-roller. The thinned solder sheet is cut into small pieces of a certain weight, dipped in a small amount of LR721H2 AlphaFlux lead-free flux, and placed in a pure Ti crucible. The Ti crucible is then placed on a heating table (pre-heated to 250℃), and the solder sheet will quickly melt into a solder ball with a diameter of about 1 mm. The solder ball is cooled in anhydrous ethanol and ultrasonically cleaned for 2 minutes to remove excess flux. Finally, it is rinsed with deionized water and air-dried to obtain the solder ball for later use.

[0021] III. Solder Wetting and Shear Resistance Tests: The prepared solder balls were soldered and wetted on a Cu substrate (TP2 phosphorus deoxidized copper). For the shear resistance test, three 40mg solder balls were used in a lap-welded reflow soldering process on a Cu substrate measuring 40mm × 10mm × 1mm. For the wettability test, one 10mg solder ball was used on a Cu substrate measuring 10mm × 10mm × 1mm. Tensile shear resistance tests were conducted at room temperature (25℃) at a tensile rate of 0.3mm / min. Three tensile shear resistance test pieces were prepared for each solder, and the shear strength σ was averaged: σ = P / S, where P is the maximum shear force and S is the effective solder area. Soldering and wettability tests were performed in a T200N+ nitrogen-filled lead-free reflow soldering machine at 165℃ for 90s. The shear resistance test pieces were aged in a forced-air drying oven at 110℃ for 240 hours. DSC testing was performed in an Ar atmosphere, with the temperature increased from 50°C to 200°C at a rate of 10°C / min. The microstructure of the solder was observed using an MPMA-1600 electron probe microanalyzer.

[0022] Example 1: An In and Sb-enhanced Sn 24-x-y Bi 18 In x Sb y Low-temperature lead-free solder, x=y=0.2, In / Sb mass percentage ratio is 1:1.06

[0023] Example 1 is a low-temperature Sn with good wetting and shear resistance properties. 23.6 Bi 18 In 0.2 Sb 0.2 Lead-free solder is applied using the following steps:

[0024] I. Composition Design and Preparation: Sn was obtained based on the cluster alloy composition design model. 24-x-y Bi 18 In x Sb y Low-temperature lead-free solder composition formula Sn 23.6 Bi 18 In 0.2 Sb 0.2 Convert the number of atoms of an element into a mass percentage Sn 42.28 Bi 57.0 In 0.35 Sb 0.37 The components (wt.%) were proportioned, mixed, and placed in a quartz tube. The mixture was then vacuum-sealed and placed in a high-temperature muffle furnace at 700°C for 5 hours of constant-temperature melting. During this period, the quartz tube was shaken every 0.5 hours to ensure thorough mixing of the molten alloy. After melting, the quartz tube was rapidly cooled in cold water to obtain the pre-soldering material.

[0025] II. Solder Ball Preparation: After smoothing the pre-body solder with sandpaper, press it into a 0.2mm thin sheet using a micro-roller. Cut the thinned solder sheet into small pieces of 40mg±0.2mg and 10mg±0.1mg. Dip each piece in a small amount of LR721H2 Alpha Flux lead-free flux and place it in a pure Ti crucible. Then place the Ti crucible on a heating stage (preheated to 250℃). The solder sheet will quickly melt into a solder ball with a diameter of approximately 1mm. Cool the solder ball in anhydrous ethanol and ultrasonically clean it for 2 minutes to remove excess flux. Finally, rinse with deionized water and air dry to obtain the solder ball.

[0026] III. Solder Wetting and Shear Resistance Test Components: A 10mg±0.1mg solder ball was dipped in a small amount of LR721H2 Alpha Flux lead-free flux and placed on a 10mm×10mm×1mm Cu substrate. It was then placed in a T200N+ nitrogen-based lead-free reflow soldering machine and reflowed at 165℃ for 90 seconds. After natural cooling, the wetting results were obtained, photographed, and the wetting area was calculated using Photoshop software. Three 40mg±0.1mg solder balls were dipped in a small amount of LR721H2 Alpha Flux lead-free flux and placed on a 40mm×10mm×1mm Cu substrate. A support wire with a diameter of approximately 0.5mm was inserted about 10mm from the end. After overlapping with another 40mm×10mm×1mm Cu substrate, the substrate was placed in a T200N+ nitrogen-based lead-free reflow soldering machine and reflowed at 165℃ for 90 seconds. After natural cooling, the shear resistance test components were obtained. Three shear resistance test specimens were placed in a forced-air drying oven at 110℃ for 240 hours to obtain the aged shear resistance test specimens.

[0027] Figure 1 The low-temperature lead-free solder Sn prepared in Example 1 23.6 Bi 18 In 0.2 Sb 0.2 Compared with Comparative Example 1, the eutectic solder Sn 24 Bi 18 The DSC spectrum of Sn is shown in the figure. 23.6 Bi 18 In 0.2 Sb 0.2 eutectic solder Sn 24 Bi 18 It has a low melting point. Furthermore, the wetting area of ​​the solders prepared in Example 1 and Comparative Example 1 on the Cu substrate was calculated using Photoshop software, and the wetting areas were 4.411 mm², respectively. 2 and 4.325mm 2 It can be seen that the solder Sn in Example 1 23.6 Bi18 In 0.2 Sb 0.2 Comparison with eutectic solder Sn in Example 1 24 Bi 18 It has superior wetting properties.

[0028] Example 2: An In and Sb-enhanced Sn 24-x-y Bi 18 In x Sb y Low-temperature lead-free solder, x = 0.2, y = 0.3, In / Sb mass percentage ratio is 1:1.6

[0029] Example 2 is a low-temperature Sn with good wetting and shear resistance properties. 23.6 Bi 18 In 0.2 Sb 0.3 Lead-free solder is applied using the following steps:

[0030] I. Composition design and preparation of high-strength and high-toughness titanium alloys for high-temperature applications at 600℃: Sn was obtained based on the composition design model of cluster alloys. 24-x-y Bi 18 In x Sb y Low-temperature lead-free solder composition formula Sn 23.6 Bi 18 In 0.2 Sb 0.3 Convert the number of atoms of an element into a mass percentage Sn 42.10 Bi 57.0 In 0.35 Sb 0.55 The components (wt.%) were proportioned, mixed, and placed in a quartz tube. The mixture was then vacuum-sealed and placed in a high-temperature muffle furnace at 700°C for 5 hours of constant-temperature melting. During this period, the quartz tube was shaken every 0.5 hours to ensure thorough mixing of the molten alloy. After melting, the quartz tube was rapidly cooled in cold water to obtain the pre-soldering material.

[0031] II. Solder Ball Preparation: After smoothing the pre-body solder with sandpaper, press it into a 0.2mm thin sheet using a micro-roller. Cut the thinned solder sheet into small pieces of 40mg±0.2mg and 10mg±0.1mg. Dip each piece in a small amount of LR721H2 Alpha Flux lead-free flux and place it in a pure Ti crucible. Then place the Ti crucible on a heating stage (preheated to 250℃). The solder sheet will quickly melt into a solder ball with a diameter of approximately 1mm. Cool the solder ball in anhydrous ethanol and ultrasonically clean it for 2 minutes to remove excess flux. Finally, rinse with deionized water and air dry to obtain the solder ball.

[0032] III. Solder Wetting and Shear Resistance Test Components: Solder balls (10 mg ± 0.1 mg) were dipped in a small amount of LR721H2 Alpha Flux lead-free flux and placed on a 10 mm × 10 mm × 1 mm Cu substrate. The substrate was then placed in a T200N+ nitrogen-based lead-free reflow soldering machine and reflowed at 165°C for 90 seconds. After natural cooling, the wetting results were obtained, photographed, and the wetting area was calculated using Photoshop software. Three solder balls (40 mg ± 0.1 mg) were dipped in a small amount of LR721H2 Alpha Flux lead-free flux and placed on a 40 mm × 10 mm × 1 mm Cu substrate. A support wire with a diameter of approximately 0.5 mm was inserted about 10 mm from the end of each ball. After overlapping with another 40 mm × 10 mm × 1 mm Cu substrate, the substrate was placed in a T200N+ nitrogen-based lead-free reflow soldering machine and reflowed at 165°C for 90 seconds. After natural cooling, the shear resistance test components were obtained. Three shear resistance test specimens were placed in a forced-air drying oven at 110℃ for 240 hours to obtain the aged shear resistance test specimens.

[0033] Comparative Example 1: SnBi eutectic solder obtained from cluster model analysis 24 Bi 18

[0034] This embodiment is a comparative experiment. The difference from Embodiment 1 is that in step one: a Sn model is designed based on the cluster alloy composition. 24 Bi 18 The mass percentage of the eutectic point composition Sn was obtained. 43.0 Bi 57.0 The ingredients were proportioned (wt.%). Everything else was the same as in Example 1.

[0035] Comparative Example 2: Analytical Design of Multi-element Solder Sn Using Cluster Model 23.6 Bi 18 In 0.6 Sb 0.6

[0036] This embodiment is a comparative experiment. The difference from Embodiment 1 is that in step one: the multi-element solder Sn is designed based on the cluster alloy composition. 24-x-y Bi 18 In x Sb y x = y = 0.6, converted to the mass percentage of the component Sn 40.84 Bi 57.0 In 1.05 Sb 1.11 The ingredients were proportioned (wt.%). Other aspects were the same as in Example 1.

[0037] Comparative Example 3: Analytical Design of Multi-element Solder Sn Using Cluster Model 23.6 Bi 18 In1.0 Sb 1.0

[0038] This embodiment is a comparative experiment. The difference from Embodiment 1 is that in step one: the multi-element solder Sn is designed based on the cluster alloy composition. 24-x-y Bi 18 In x Sb y x = y = 1.0, converted to component mass percentage Sn 39.40 Bi 57.0 In 1.75 Sb 1.85 The ingredients were proportioned (wt.%). Other aspects were the same as in Example 1.

[0039] Figure 1 Sn prepared in Example 1 23.6 Bi 18 In 0.2 Sb 0.2 Solder and the eutectic solder Sn prepared in Comparative Example 1 24 Bi 18 The DSC spectrum shows that the melting point of the multi-element solder is higher than that of the eutectic solder Sn. 24 Bi 18 Low melting point, melting range similar to eutectic Sn 24 Bi 18 The melting ranges are similar. Its wetting area on the Cu substrate is 4.411 mm². 2 And the eutectic solder Sn prepared in Comparative Example 1 is superior. 24 Bi 18 The wetting area on the Cu substrate is 4.325 mm². 2 It exhibits superior performance.

[0040] The shear resistance of the solder was tested at room temperature before and after aging at 110℃ for 240 hours. The shear resistance of the solder was obtained as follows: Figure 2 As shown, blank areas represent before aging, and shaded stripes represent after aging. The left side shows Sn prepared in Example 1. 23.6 Bi 18 In 0.2 Sb 0.2 Solder, the one on the right represents the eutectic solder Sn prepared in Comparative Example 1. 24 Bi 18 .pass Figure 2 It can be seen that Comparative Example 1 prepared eutectic solder Sn 24 Bi 18 The shear strength was 45.83 MPa, and the shear strength after aging at 110℃ for 240 h was 40.6 MPa; the Sn prepared in Example 1 23.6 Bi 18 In 0.2Sb 0.2 The shear strength of the solder was 48.04 MPa, and the shear strength after aging at 110℃ for 240 h was 48.51 MPa. This is compared to the eutectic solder Sn prepared in Comparative Example 1. 24 Bi 18 In Example 1, the Sn preparation had an In / Sb mass percentage ratio of 1:1.06. 23.6 Bi 18 In 0.2 Sb 0.2 The shear strength of the solder increased by 2.21 MPa, and the shear strength after high-temperature aging increased by 7.91 MPa.

[0041] Additionally from Figure 3 Sn prepared in Example 1 shown 23.6 Bi 18 In 0.2 Sb 0.2 Solder and the eutectic solder Sn prepared in Comparative Example 1 24 Bi 18 The backscattered image shows that the Bi phase is refined, and small amounts of βSn(SbBi) and InSb phases exist in the matrix. The Sb content in the βSn(SbBi) phase is 45-55 wt.%. In the molten state, Sb and Bi are miscible, which allows the Sn-rich βSn(Bi) phase to precipitate first, forming a new peritectic structure βSn(SbBi). This also refines the Bi phase in the eutectic structure, thereby enhancing the solder performance and reducing Bi segregation.

[0042] Sn prepared in Example 2 23.6 Bi 18 In 0.2 Sb 0.3 The lead-free solder wets a surface area of ​​4.385 mm² on the Cu substrate. 2 The shear strength at room temperature is 47.86 MPa, and the shear strength after aging at 110℃ for 240 h is 47.24 MPa, which is also superior to the eutectic solder Sn prepared in Comparative Example 1. 24 Bi 18 It can be seen that Sn prepared with a small amount of In and Sb is enhanced. 24-x-y Bi 18 In x Sb y Low-temperature lead-free solder has good shear resistance, and its shear resistance does not change significantly after aging.

[0043] Furthermore, the multi-element solder Sn prepared in Comparative Examples 2 and 3 23.6 Bi 18 In 0.6 Sb 0.6 and Sn23.6 Bi 18 In 1.0 Sb 1.0 The wetting area on the Cu substrate is 4.25 mm. 2 and 3.72mm 2 Comparison with eutectic solder Sn in Example 1 24 Bi 18 The wettability of the multi-element solders in Examples 1 and 2 is poor. Meanwhile, their shear strengths under room temperature tension are 41.96 MPa and 35.47 MPa, respectively, and their shear strengths after aging at 110°C for 240 h are 41.88 MPa and 36.38 MPa, respectively. This is in contrast to the eutectic solder Sn prepared in Comparative Example 1. 24 Bi 18 The problem is that as the amount of In and Sb increases, once the saturation of Sb and In in the Sn matrix is ​​reached, a brittle InSb phase will precipitate in the matrix, which will reduce the wettability and shear resistance of the solder.

[0044] The embodiments described above are merely illustrative of the implementation methods of the present invention, but should not be construed as limiting the scope of the present invention. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these modifications and improvements all fall within the protection scope of the present invention.

Claims

1. An In and Sb-enhanced Sn 24-x-y Bi 18 In x Sb y Low-temperature lead-free solder, characterized in that, Tin-bismuth based solder contains Sn, Bi, In, and Sb elements, while As, S, Ni, Cd, Cr, Zn, and Pb are impurity elements. The mass percentage (wt.%) of its alloy composition is Bi: 57.0, In: 0.2-1.40, Sb: 0.21-1.50, the total impurity (As+S+Ni+Cd+Cr+Zn+Pb) ≤ 0.01, and the balance is Sn. The mass percentage ratio of In / Sb is 1:1.06-1.

6. The alloy composition was designed based on the cluster alloy design model, which provides the structural unit and corresponding composition formula of the SnBi eutectic. Through the SnBi binary phase diagram and eutectic point composition, it was analyzed that the SnBi eutectic point is composed of a Bi-rich Sn phase and a pure Bi phase. Using a cluster plus connecting atom model, the structural unit of its eutectic point is analyzed as: 2{[Sn-Sn 10 ]Bi3Sn1}+[Bi-Bi6]Bi5=Sn 24 Bi 18 =Sn 57.1 Bi 42.9 (at.%) = Sn-57Bi(wt.%); Sn is prepared by introducing strengthening elements In and Sb to replace Sn. 24-x-y Bi 18 In x Sb y Lead-free solder.

2. The In and Sb reinforced Sn according to claim 1 24-x-y Bi 18 In x Sb y Low-temperature lead-free solder, characterized in that, The Sn 24-x-y Bi 18 In x Sb y Low-temperature lead-free solder has better wettability and shear resistance than SnBi eutectic solder, and can be used as the main material for low-temperature brazing and packaging.

3. An In and Sb-reinforced Sn as described in claim 1 or 2 24-x-y Bi 18 In x Sb y A method for preparing low-temperature lead-free solder, characterized in that, First, the elements are mixed according to the mass percentage ratio and placed in a quartz tube. After vacuum sealing, the tube is placed in a high-temperature muffle furnace and melted at a constant temperature of 650-750℃ for 5-6 hours. During this period, the quartz tube is shaken every 0.5 hours to ensure that the alloy in the liquid state is fully mixed. After melting, the quartz tube is rapidly cooled in cold water to obtain the pre-body solder. Second, the pre-body solder is polished and pressed into a thin sheet. After being dipped in lead-free flux, it is placed in a pure Ti crucible and heated to obtain solder balls. Finally, the solder balls are cooled, cleaned, and air-dried to obtain the product.

Citation Information

Patent Citations

  • SnBiSb-series low-temperature lead-free solder and preparation method thereof

    CN106216872A

  • Lead-free low-temperature solder alloy containing Bi and In and preparation process of lead-free low-temperature solder alloy

    CN115595466A