Preparation method of sub-micron manganese ferrite electrode material and supercapacitor
The preparation of compact submicron manganese ferrite electrode materials by a solvothermal method solves the problems of poor safety and environmental protection in the preparation of existing manganese ferrite materials, and achieves high specific capacitance and good cycle characteristics of supercapacitors, making it suitable for large-scale production.
Patent Information
- Application Number
- CN202310473145.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-27
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-04-27
AI Technical Summary
Existing manganese ferrite material preparation processes suffer from poor safety and environmental performance due to high-temperature calcination and the use of acid and alkali solutions. Furthermore, manganese ferrite is primarily used as a positive electrode material, while activated carbon is used as a negative electrode material, resulting in high process costs, which necessitates further optimization.
A loosely structured spherical precursor for manganese ferrite electrode material was prepared by a solvothermal method using ethylene glycol, ferric chloride, manganese acetate, and acetate. The voids were then filled by further reaction to obtain a compact submicron manganese ferrite electrode material, which was then used as the positive and negative electrode material for supercapacitors. Neutral materials were used to avoid high-temperature calcination.
The prepared submicron manganese ferrite electrode material has high stability, and the supercapacitor has good specific capacitance and cycle characteristics. The production process is safe and environmentally friendly, with low cost, and is suitable for large-scale production.
Smart Images

Figure CN116525313B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a submicron manganese ferrite electrode material and a method for preparing a supercapacitor, belonging to the field of supercapacitor electrode material preparation technology. Background Technology
[0002] Supercapacitors (also known as electric double-layer capacitors) are a new type of highly efficient energy storage device, primarily storing electrical charge. They fall between traditional capacitors and batteries, possessing unique advantages unmatched by traditional batteries, and complementing the charging and discharging functions of conventional batteries. Supercapacitors are widely used in various fields due to their long cycle life, high power output, simple principles and manufacturing methods, inexpensive raw materials, and ability to be combined with secondary batteries for hybrid applications. These applications include portable and flexible electronic products such as electronic newspapers, roll-up displays, and wearable devices, as well as power supply equipment for hybrid electric vehicles.
[0003] Electrode materials are the core components of supercapacitors, and they mainly include carbon materials, transition metal oxides, and organic polymers. Currently, achieving high specific capacitance through the synthesis of bimetallic manganese ferrite materials has become a research trend. Manganese ferrite (MnFe2O4) is a soft magnetic material with a spinel structure, also known as manganese spinel or manganese ferrite. It features high saturation magnetization, high initial permeability, and low coercivity, and is widely used in electronic devices such as electronics, communications, navigation, radar, and telemetry.
[0004] The main reported methods for preparing manganese ferrite are as follows: Preparation Method 1: Alcohol-soluble manganese and iron salts are dissolved in anhydrous ethanol. The solution is ignited and combusted. After combustion, the solution is calcined in a programmable temperature-controlled furnace at 250–800°C to obtain spherical magnetic manganese ferrite nanosheets. This technique uses high-temperature calcination, resulting in high process costs. Furthermore, the use of acid during preparation significantly reduces safety. The prepared manganese ferrite structure is in the form of spherical nanosheets, primarily intended for use in the biomedical field, not as electrode materials.
[0005] Preparation Method Two: Manganese and iron salts are added to water, followed by the addition of organic acid and direct heating, and then high-temperature calcination in a tube furnace to obtain nano-iron oxide composite electrode materials for supercapacitors. This method uses nano-manganese-iron materials to prepare the positive electrode and activated carbon to prepare the negative electrode. This approach, using high-temperature calcination and activated carbon as the negative electrode, not only results in high processing costs but also significantly reduces safety due to the use of acid during preparation.
[0006] Preparation Method 3: A water / solvothermal method is used to prepare manganese iron oxide / carbon composite materials. This method involves adding manganese salts, iron salts, and surfactants to water, then adding an alkaline solution dropwise for synthesis. The composite material (MnO-MnFe2O4 / c) is then obtained by high-temperature calcination under an inert gas atmosphere. However, this method yields samples with irregular shapes, and the use of an alkaline solution significantly reduces the safety of the preparation process.
[0007] In summary, most existing methods for preparing manganese ferrite materials using solvothermal methods and then further preparing supercapacitors involve alkaline or acidic solutions. Safer and more environmentally friendly preparation processes need to be explored. Furthermore, existing technologies for preparing supercapacitors using manganese iron oxides all use the prepared manganese iron oxides as the positive electrode material and activated carbon as the negative electrode material, which indicates that the preparation process of supercapacitors also needs further exploration. Summary of the Invention
[0008] To address the aforementioned problems in existing technologies, this invention provides a method for preparing submicron manganese ferrite electrode materials and supercapacitors. First, this invention prepares a loosely structured spherical precursor for manganese ferrite electrode materials by reacting ethylene glycol, ferric chloride, manganese acetate, and acetate using a solvothermal method. Then, based on the above spherical precursor, ethylene glycol, ferric chloride, manganese acetate, and acetate are added again, and the reaction is carried out again using a solvothermal method to further fill the voids in the spherical precursor, thereby obtaining a compact submicron manganese ferrite electrode material with a near-spherical particle structure (see [link to invention]). Figure 2 The electrode material prepared by the above method has high stability and can be further processed into electrodes (positive and negative electrodes) for supercapacitors, thereby producing supercapacitors with good specific capacitance, good cycle characteristics, and high cycle capacity retention. The raw materials used in this invention are all neutral substances, and the preparation process does not require calcination, making the process safer, environmentally friendly, and cost-effective for large-scale production.
[0009] The first objective of this invention is to provide a method for preparing submicron manganese ferrite electrode materials. The method is characterized by using ethylene glycol as a solvent, and reacting ferric chloride, manganese acetate, and acetate at 150-200 °C using a solvothermal method to first prepare a loosely structured spherical precursor for the manganese ferrite electrode material. Then, based on the above spherical precursor, ethylene glycol, ferric chloride, manganese acetate, and acetate are further added, and the reaction is carried out at 200-300 °C using a solvothermal method to further fill the voids in the spherical precursor, thereby obtaining a compact submicron manganese ferrite electrode material with an approximately spherical particle structure.
[0010] Furthermore, the aforementioned spherical precursor is a small particle with a particle size of less than 300 nm selected by screening (those that do not meet the requirements are screened out), and the aforementioned submicron manganese ferrite electrode material with a compact, approximately spherical particle structure is a small particle with a particle size of 100-300 nm selected by screening (those that do not meet the requirements are screened out).
[0011] The above preparation method specifically includes the following steps: 1) Add ferric chloride and manganese acetate to ethylene glycol solvent and stir continuously at room temperature until the solid powder is completely dissolved; 2) Add neutral acetate and stir continuously until a homogeneous suspension is formed; 3) Then transfer the suspension prepared in step 2) into a polytetrafluoroethylene stainless steel high-pressure reactor, place the reactor in a forced-air drying oven, heat at 150-200 ℃ for 5-20 hours, and then cool the reactor to room temperature to obtain a solid product; 4) The obtained solid product is washed, centrifuged, collected, dried and then screened to remove small particles with a particle size of less than 300nm (loose spherical precursor structure). 5) Add ferric chloride, manganese acetate and the small particles obtained in step 4) to ethylene glycol solvent and stir continuously at room temperature until a homogeneous suspension is formed; 6) Add neutral acetate and stir continuously until a homogeneous suspension is formed; 7) Then transfer the suspension prepared in step 6) into a polytetrafluoroethylene stainless steel high-pressure reactor, place the reactor in a forced-air drying oven, heat at 200-300 ℃ for 8-20 hours, and then cool the reactor to room temperature to obtain a solid product. 8) The obtained solid product is washed, centrifuged, collected, dried and then screened to obtain small particles with a particle size of 100-300nm, resulting in submicron-sized manganese ferrite electrode material (compact, approximately spherical particles).
[0012] Furthermore, in steps 1) and 5) above, the molar ratio of manganese acetate to ferric chloride is 1:1.8-2.2, preferably 1:2. In the embodiments of the present invention, ferric chloride hexahydrate is used; and manganese acetate tetrahydrate is used.
[0013] Furthermore, the neutral acetate in steps 2) and 6) can be any one of ammonium acetate, sodium acetate, and potassium acetate, with ammonium acetate being preferred. The molar ratio of the neutral acetate to ferric chloride is 0.75-1.0:1, preferably 0.8:1.
[0014] Furthermore, the drying process in steps 4) and 8) is as follows: the collected solid product is placed in an oven and dried at 40-80 ℃ for 6-10 hours, followed by natural cooling.
[0015] Furthermore, the washing in steps 4) and 8) is performed by washing with distilled water and ethanol respectively, 3-10 times, preferably 5 times with distilled water first and then 5 times with ethanol.
[0016] It should be noted that compared to the particles prepared in step 4), the particles actually prepared in step 8) have a larger particle size and a more compact structure. In order to meet the final requirements, particles that are too large (above 300 nm) were screened out.
[0017] The submicron manganese ferrite electrode material prepared by the above method is characterized by its approximately spherical particle structure (compact structure) and particle size range of 100-300 nm. (See [link to documentation]). Figure 2 .
[0018] The second objective of this invention is to prepare electrodes for supercapacitors using the prepared submicron-sized manganese ferrite electrode material. The method involves using the prepared submicron-sized manganese ferrite material as the active material, acetylene black as the conductive agent, and polytetrafluoroethylene (PTFE) as the binder. These three materials are mixed evenly, and an appropriate amount of methylpyrrolidone (NMP) is added and ground to obtain a uniformly mixed slurry. The slurry is then evenly coated onto nickel foam, dried, and subsequently cut into small circular pieces to prepare electrodes for supercapacitors.
[0019] Furthermore, the mass ratio of the aforementioned submicron-sized manganese ferrite material, acetylene black, and polytetrafluoroethylene is 15-17:2.5-3.5:1, with a preferred mass ratio of 16:3:1.
[0020] Furthermore, the mass ratio of the above-mentioned isopropanol to the solids (total mass of submicron-sized manganese ferrite material, acetylene black and polytetrafluoroethylene) is 0.8-1.2:1, preferably 1:1.
[0021] Furthermore, the above drying process involves vacuum drying at 100-130℃ for 6-12 hours.
[0022] A third objective of this invention is to provide a supercapacitor characterized by using electrodes made of submicron-sized manganese ferrite material as the positive and negative electrodes of the supercapacitor.
[0023] In steps 1) to 4) of the preparation process of this invention, ethylene glycol is used as a solvent, and ferric chloride, manganese acetate, and acetate are reacted using a solvothermal method at 150-200 °C. This reaction process mainly yields two different types of structures: the majority are spherical structures, approximately spherical nanoaggregates (possibly precursors to spherical structures, with a relatively loose structure); the other type is a nanowire structure with a relatively large particle size. Small particles with a uniform particle size of less than 300 nm (more than 85% of the total) are screened using a particle sieving mechanism to obtain spherical precursors. Then, in steps 5) to 8) based on the above spherical precursors, ethylene glycol, ferric chloride, manganese acetate, and acetate are added and reacted using a solvothermal method at 200-300 °C to further fill the voids in the spherical precursors, thereby obtaining a compact, approximately spherical submicron manganese ferrite electrode material. Small particles with a uniform particle size of 100-300 nm are screened using a particle sieving mechanism. That is, through the reactions in steps 5) to 8), the spherical aggregates or spherical structures are further stabilized.
[0024] The technical effects of this invention are: 1. This invention first prepares a loosely structured spherical precursor of manganese ferrite electrode material by reacting ethylene glycol, ferric chloride, manganese acetate, and acetate using a solvothermal method. Then, based on the above spherical precursor, ethylene glycol, ferric chloride, manganese acetate, and acetate are added again and reacted by a solvothermal method to further fill the voids in the spherical precursor, thereby obtaining a submicron manganese ferrite electrode material with a compact, approximately spherical particle structure. The electrode material prepared in the above method has high stability. 2. The supercapacitor prepared by this invention using submicron-sized manganese ferrite material as the active material exhibits good specific capacitance, excellent cycling characteristics, and high cycle retention. Experiments have shown that the supercapacitor prepared using this method has a specific capacitance of over 100.92 F / g at 0.01 A / g and over 98.34 F / g at 0.02 A / g. After 6000 charge-discharge cycles at a current density of 0.2 A / g, the cycle capacity retention is over 92%, indicating that the sample maintains a high cycle capacity retention even after 6000 charge-discharge cycles. 3. The specific surface area of the manganese ferrite material prepared by this invention has an average value of 30-60 m². 2 / g, which indicates that the manganese ferrite assembled by the nanocrystals of the present invention has a better specific surface area; 4. Compared with the existing technology of preparing manganese ferrite electrode materials through acidic or alkaline solutions, the present invention adds neutral additives such as ammonium acetate during the preparation process, making the preparation process safer and environmentally friendly. 5. Compared with the high-temperature calcination method used in the prior art, the present invention can control the solvothermal reaction at 150-300 ℃, which results in low production cost and is easy to mass-produce. 6. In this invention, an appropriate amount of polytetrafluoroethylene (PTFE) and methylpyrrolidone solvent (NMP) are added to the process for preparing supercapacitor electrodes, and the slurry is uniformly coated onto nickel foam to prepare the positive and negative electrodes of the supercapacitor. The purpose of this is to simplify the capacitor manufacturing process. Attached Figure Description
[0025] Figure 1 This is a process flow diagram for the preparation of the submicron manganese ferrite electrode material of the present invention; Figure 2 This is a scanning electron microscope image of the submicron-scale manganese ferrite electrode material (sample 1) of the present invention; Figure 3 This is a charge-discharge curve of the supercapacitor prepared using submicron-sized manganese ferrite electrode material (sample 1) according to the present invention. Detailed Implementation
[0026] The effects are illustrated below with reference to embodiments and accompanying drawings. It should be noted that the following detailed description is illustrative and intended to provide further explanation of the invention. Unless otherwise specified, all technical and scientific terms used in this invention have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains.
[0027] To enable those skilled in the art to better understand the technical solution of this application, the technical solution of this application will be described in detail below with reference to specific embodiments and comparative examples.
[0028] The test materials used in the following examples are all conventional test materials in the art and can be purchased through commercial channels.
[0029] like Figure 1 As shown, the process flow of a submicron manganese ferrite electrode material of the present invention is as follows: 1) Add ferric chloride and manganese acetate to ethylene glycol and dissolve them to obtain a colored solution A; 2) Add acetate to the colored solution A and stir to obtain a homogeneous suspension B; 3) Transfer suspension B to a polytetrafluoroethylene stainless steel high-pressure reactor, place the reactor in a forced-air drying oven, and heat at 150-200 ℃ for 5-20 hours; then cool the reactor to room temperature to obtain solid product C; 4) Wash and dry solid product C, and screen out small particles with a particle size of less than 300 nm to obtain solid product D; 5) Add ferric chloride, manganese acetate and the solid product D from step 4) to ethylene glycol and stir until a homogeneous suspension E is formed; 6) Add acetate to suspension E and stir to obtain a homogeneous suspension F; 7) Transfer the suspension F to a polytetrafluoroethylene stainless steel high-pressure reactor, place the reactor in a forced-air drying oven, and heat at 200-300 ℃ for 8-20 hours; then cool the reactor to room temperature to obtain solid product G; 8) The obtained solid product G is washed, dried, and small particles with a particle size of 100-300nm are screened out to obtain solid product H.
[0030] Example 1: The following samples illustrate the preparation method of submicron-sized manganese ferrite electrode materials, as well as the fabrication process of supercapacitor electrodes and supercapacitors.
[0031] The preparation steps for sample 1 are as follows: 1) Add 10 mmol of ferric chloride hexahydrate and 5 mmol of manganese acetate tetrahydrate to 35 ml of ethylene glycol solvent. Dissolve at room temperature with magnetic stirring to obtain a colored solution A. 2) Add 8 mmol of ammonium acetate to the colored solution A and stir on a magnetic stirrer for 2 hours to obtain a homogeneous suspension B; 3) Then transfer the above suspension B to a polytetrafluoroethylene stainless steel high-pressure reactor, place the reactor in a forced-air drying oven, heat at 180 °C for 7 hours, and then cool the reactor to room temperature to obtain solid product C; 4) The obtained solid product C was washed 5 times each with distilled water and ethanol, centrifuged, and then placed in an oven to dry at 60 ℃ for 10 hours. Finally, solid product D was collected. Small particles with a uniform particle size of less than 300 nm were then screened using a particle sieving device (mainly removing relatively large nanowire structures). 5) Add 10 mmol of ferric chloride hexahydrate, 5 mmol of manganese acetate tetrahydrate and the small particles obtained in step 4) to 55 ml of ethylene glycol solvent, and stir continuously at room temperature until a homogeneous suspension E is formed. 6) Add 8 mmol of ammonium acetate to the suspension E from step 5) and stir on a magnetic stirrer for 1 hour to obtain a homogeneous suspension F. 7) Then transfer the suspension F prepared in step 6) into a polytetrafluoroethylene stainless steel high-pressure reactor, place the reactor in a forced-air drying oven, and heat at 200 °C for 8 hours; then cool the reactor to room temperature to obtain solid product G; 8) The obtained solid product G is washed (washed 5 times each with distilled water and ethanol), centrifuged, and the solid product is collected and dried (placed in an oven and dried at 60 ℃ for 10 hours). Then, small particles with uniform particle size of 100-300 nm are screened out through a particle screening mechanism to obtain submicron-sized manganese ferrite electrode material (sample 1). The manganese ferrite material screened out in the above two screenings accounts for about 20.5% of the total amount, which can be recycled and reused in a suitable way.
[0032] The scanning electron microscope image of the submicron-sized manganese ferrite electrode material (sample 1) prepared by this invention is shown below. Figure 2 As shown, Figure 2 This indicates that the obtained manganese ferrite material can achieve an approximately spherical particle structure with a compact structure. This structure results in good material stability and a larger specific surface area, which allows for better electrochemical reactions.
[0033] Sample 2 preparation steps (adjusting the reaction temperature for the second time): 1) Add 10 mmol of ferric chloride hexahydrate and 5 mmol of manganese acetate tetrahydrate to 35 ml of ethylene glycol solvent. Dissolve at room temperature with magnetic stirring to obtain a colored solution A. 2) Add 8 mmol of ammonium acetate to the colored solution A and stir on a magnetic stirrer for 2 hours to obtain a homogeneous suspension B; 3) Then transfer the above suspension B to a polytetrafluoroethylene stainless steel high-pressure reactor, place the reactor in a forced-air drying oven, heat at 180 °C for 7 hours, and then cool the reactor to room temperature to obtain solid product C; 4) The obtained solid product C was washed 5 times each with distilled water and ethanol, centrifuged, and then placed in an oven and dried at 60 °C for 10 hours. Finally, solid product D was collected and then screened by a particle screening device to obtain small particles with a uniform particle size of less than 300 nm. 5) Add 10 mmol of ferric chloride hexahydrate, 5 mmol of manganese acetate tetrahydrate and the small particles obtained in step 4) to 55 ml of ethylene glycol solvent, and stir continuously at room temperature until a homogeneous suspension E is formed. 6) Add 8 mmol of ammonium acetate to the suspension E from step 5) and stir on a magnetic stirrer for 1 hour to obtain a homogeneous suspension F. 7) Then transfer the suspension F prepared in step 6) into a polytetrafluoroethylene stainless steel high-pressure reactor, place the reactor in a forced-air drying oven, and heat at 250 °C for 8 hours; then cool the reactor to room temperature to obtain solid product G; 8) The obtained solid product G is washed, centrifuged, collected, and dried. Then, it is screened through a particle screening mechanism to remove small particles with a uniform particle size of 100-300 nm, thus obtaining submicron-sized manganese ferrite electrode material (sample 2). The manganese ferrite material rejected in the above two screenings accounts for approximately 21.2% of the total amount, which can be recycled and reused in a suitable manner.
[0034] Sample 3 preparation steps (adjusting the molar ratio of hydrated ferric chloride and manganese acetate tetrahydrate in the two reactions): 1) Add 9 mmol of ferric chloride hexahydrate and 6 mmol of manganese acetate tetrahydrate to 35 ml of ethylene glycol solvent. Dissolve them at room temperature with magnetic stirring to obtain a colored solution A. 2) Add 8 mmol of ammonium acetate to the colored solution A and stir on a magnetic stirrer for 2 hours to obtain a homogeneous suspension B; 3) Then transfer the above suspension B to a polytetrafluoroethylene stainless steel high-pressure reactor, place the reactor in a forced-air drying oven, heat at 180 °C for 7 hours, and then cool the reactor to room temperature to obtain solid product C; 4) The obtained solid product C was washed 5 times each with distilled water and ethanol, centrifuged, and then placed in an oven and dried at 60 °C for 10 hours. Finally, solid product D was collected and then screened by a particle screening device to obtain small particles with a uniform particle size of less than 300 nm. 5) Add 9 mmol of ferric chloride hexahydrate, 6 mmol of manganese acetate tetrahydrate and the small particles obtained in step 4) to 55 ml of ethylene glycol solvent, and stir continuously at room temperature until a homogeneous suspension E is formed. 6) Add 8 mmol of ammonium acetate to the suspension E from step 5) and stir on a magnetic stirrer for 1 hour to obtain a homogeneous suspension F. 7) Then transfer the suspension F prepared in step 6) into a polytetrafluoroethylene stainless steel high-pressure reactor, place the reactor in a forced-air drying oven, and heat at 200 °C for 8 hours; then cool the reactor to room temperature to obtain solid product G; 8) The obtained solid product G is washed, centrifuged, collected, dried, and then screened through a particle screening mechanism to remove small particles with uniform particle size, namely submicron-sized manganese ferrite electrode material with a particle size of 100-300 nm (sample 3). The manganese ferrite material rejected in the above two screenings accounts for about 22.5% of the total amount, which can be recycled and reused in a suitable manner.
[0035] Sample 4 preparation steps (adjusting the amount of acetate added): 1) Add 10 mmol of ferric chloride hexahydrate and 5 mmol of manganese acetate tetrahydrate to 35 ml of ethylene glycol solvent. Dissolve them at room temperature with magnetic stirring to obtain a colored solution A. 2) Add 10 mmol of ammonium acetate to the colored solution A and stir on a magnetic stirrer for 2 hours to obtain a homogeneous suspension B. 3) Then transfer the above suspension B to a polytetrafluoroethylene stainless steel high-pressure reactor, place the reactor in a forced-air drying oven, heat at 180 °C for 7 hours, and then cool the reactor to room temperature to obtain solid product C; 4) The obtained solid product C was washed 5 times each with distilled water and ethanol, centrifuged, and then placed in an oven and dried at 60 ℃ for 10 hours. Finally, solid product D was collected; then small particles with a uniform particle size of less than 300 nm were screened out by a particle screening device. 5) Dissolve 10 mmol of ferric chloride hexahydrate, 5 mmol of manganese acetate tetrahydrate and the small particles obtained in step 4) in 55 ml of ethylene glycol solvent, and stir continuously at room temperature until a homogeneous suspension E is formed. 6) Add 8 mmol of ammonium acetate to the suspension E from step 5), and stir on a magnetic stirrer for 1 hour to obtain a homogeneous suspension F. 7) Then transfer the suspension F prepared in step 6) into a polytetrafluoroethylene stainless steel high-pressure reactor, place the reactor in a forced-air drying oven, and heat at 200 °C for 8 hours; then cool the reactor to room temperature to obtain solid product G; 8) The obtained solid product is washed, centrifuged, collected, dried, and then screened through a particle screening mechanism to remove small particles with uniform particle size, namely submicron-sized manganese ferrite electrode material with a particle size of 100-300 nm (sample 4). The manganese ferrite material rejected in the above two screenings accounts for about 22.1% of the total amount, which can be recycled and reused in a suitable manner.
[0036] Sample 5 preparation steps (adjustment of added materials): By replacing ammonium acetate with an equal molar amount of sodium acetate, and following the same preparation method as Sample 1, submicron-sized manganese ferrite electrode materials (Sample 5) with a particle size of 100-300 nm were obtained. The manganese ferrite material rejected in the above two screenings accounts for approximately 20.2% of the total amount, which can be recycled and reused using appropriate methods.
[0037] Preparation steps for comparison sample 1: 1) Add 10 mmol of ferric chloride hexahydrate and 5 mmol of manganese acetate tetrahydrate to 35 ml of dimethylformamide solvent. Dissolve at room temperature with magnetic stirring to obtain a colored solution A. 2) Add 8 mmol of ammonium acetate to the colored solution A and stir on a magnetic stirrer for 2 hours to obtain a homogeneous suspension B; 3) Then transfer the above suspension B to a polytetrafluoroethylene stainless steel high-pressure reactor, place the reactor in a forced-air drying oven, heat at 180 °C for 7 hours, and then cool the reactor to room temperature to obtain solid product C; 4) The obtained solid product C was washed 5 times each with distilled water and ethanol, centrifuged, and then placed in an oven to dry at 60 °C for 10 hours. Finally, solid product D (without particle screening) was collected. 5) Add 10 mmol of ferric chloride hexahydrate, 5 mmol of manganese acetate tetrahydrate and the particles obtained in step 4) to 55 ml of dimethylformamide solvent, and stir continuously at room temperature until a homogeneous suspension E is formed. 6) Add 8 mmol of ammonium acetate to the suspension E from step 5), and stir on a magnetic stirrer for 1 hour to obtain a homogeneous suspension F. 7) Then transfer the suspension F prepared in step 6) into a polytetrafluoroethylene stainless steel high-pressure reactor, place the reactor in a forced-air drying oven, and heat at 200 °C for 8 hours; then cool the reactor to room temperature to obtain the solid product G; 8) Wash solid product G (wash 5 times each with distilled water and ethanol), centrifuge, collect solid product and dry (dry at 60 ℃ for 10 hours) to obtain a comparison sample (without particle screening), with an average particle size range of 400-900 nm, thus obtaining manganese ferrite electrode material (comparison sample 1).
[0038] Preparation steps for comparison sample 2: 1) Add 10 mmol of ferric chloride hexahydrate and 5 mmol of manganese acetate tetrahydrate to 35 ml of ethylene glycolamine solvent. Dissolve at room temperature with magnetic stirring to obtain a colored solution A. 2) Add 8 mmol of phenylammonium to the colored solution A and stir on a magnetic stirrer for 2 hours to obtain a homogeneous suspension B; 3) Then transfer the above suspension B to a polytetrafluoroethylene stainless steel high-pressure reactor, place the reactor in a forced-air drying oven, heat at 180 °C for 7 hours, and then cool the reactor to room temperature to obtain solid product C; 4) The obtained solid product C was washed 5 times each with distilled water and ethanol, centrifuged, and then placed in an oven to dry at 60 °C for 10 hours. Finally, solid product D (without particle screening) was collected. 5) Add 10 mmol of ferric chloride hexahydrate, 5 mmol of manganese acetate tetrahydrate and the particles obtained in step 4) to 55 ml of ethylene glycolamine solvent, and stir continuously at room temperature until a homogeneous suspension E is formed. 6) Add 8 mmol of phenylammonium to the suspension E in step 5) and stir on a magnetic stirrer for 1 hour to obtain a homogeneous suspension F; 7) Then transfer the suspension F prepared in step 6) into a polytetrafluoroethylene stainless steel high-pressure reactor, place the reactor in a forced-air drying oven, and heat at 200 °C for 8 hours; then cool the reactor to room temperature to obtain solid product G; 8) The obtained solid product G was washed (washed 5 times each with distilled water and ethanol), centrifuged, and the solid product was collected and dried (dried at 60 ℃ for 10 hours) to obtain the comparison sample (without particle screening), with an average particle size range of 600-1000 nm, which is the manganese ferrite electrode material (comparison sample 2).
[0039] The preparation steps of the manganese ferrite supercapacitor are as follows: All the obtained submicron-sized manganese ferrite samples are used to prepare the electrodes of the supercapacitor. Submicron-sized manganese ferrite materials prepared from samples 1-5 and control samples 1-2 are used as active materials, acetylene black as a conductive agent, and polytetrafluoroethylene (PTFE) as a binder. These three materials are uniformly mixed at a mass ratio of 16:3:1, and methylpyrrolidone (NMP) solvent (solvent to solid mass ratio 1:1) is added and ground to obtain a uniformly mixed slurry. The slurry is uniformly coated onto nickel foam and vacuum dried at 100-130℃ for 6-12 h. The foam is then cut into small circular pieces to prepare the electrodes (positive and negative electrodes) of the supercapacitor. The supercapacitor is then assembled according to standard procedures and allowed to stand for approximately 4 h before electrochemical testing.
[0040] Electrochemical performance testing of supercapacitors: At room temperature, a symmetrical two-electrode supercapacitor was assembled by separating the two electrodes using a porous membrane. The electrochemical performance of the symmetrical two-electrode supercapacitor was tested and characterized using an electrochemical workstation. The obtained cyclic voltammetry curves were all symmetrical and rectangular in shape, indicating that the assembled supercapacitor has good capacitance characteristics. The test temperature was room temperature. The cyclic voltammetry curves are not rectangular but rather rectangular in shape, mainly due to the influence of the assembly structure, assembly process, and nanocrystal surface characteristics. They are also affected by various additives used in the experiment, as well as the process temperature, test environment, and test temperature.
[0041] All samples were assembled into supercapacitors, and their performance, including charge / discharge capacity, discharge voltage, and cycle retention, was tested. The charge / discharge curves of the supercapacitor in sample 1 are shown below. Figure 3As shown in the figure, the test results of charge-discharge capacity and cycle retention rate of samples 1-5 and control samples 1-2 are shown in Table 1. The charge-discharge test voltage for each sample in Table 1 is 0–1V. The charge-discharge curve of the supercapacitor in sample 1 is shown in the figure. Figure 3 As shown in Table 1, the specific capacitance of samples 1-5 at 0.01 A / g is above 100.92 F / g, and the specific capacitance at 0.02 A / g is above 98.34 F / g. After 6000 charge-discharge cycles at a current density of 0.2 A / g, the cycle capacity retention rate is above 92%, indicating that the cycle capacity retention rate of the samples is still relatively high after 6000 charge-discharge cycles.
[0042] Table 1. Comparison of specific capacity and cycle retention between samples 1-5 and control sample 1-2
[0043] As shown in Table 1 above, the supercapacitors using submicron-sized manganese ferrite materials as active materials in samples 1-5 exhibit better specific capacitance, better cycling characteristics, and higher cycle retention, significantly exceeding the performance of the supercapacitors in comparative samples 1-2. This is because the assembled particle size of the aforementioned manganese ferrite materials is submicron-sized, and the particle diameter is significantly smaller than that of comparative samples 1-2, greatly increasing the contact surface area. Furthermore, the specific capacitance at low current density can be regained after high current density charge-discharge cycles, indicating that the electrode material prepared by this method has high reversibility. The manganese ferrite prepared by this method possesses good structural stability, cycling stability, and good charge-discharge performance.
[0044] Furthermore, the submicron-scale manganese ferrite material prepared in this invention uses neutral materials, which have almost zero harm to the human body and no other impact on the surrounding environment. The prepared manganese ferrite material has good cycle stability and is a very promising electrode material for supercapacitors.
[0045] Meanwhile, the specific surface area of the product was characterized using a specific surface area analyzer at liquid nitrogen (77K). The average specific surface area of the prepared manganese ferrite material (sample 1) was 48.7 m², as measured by the specific surface area analyzer. 2 / g indicates that the manganese ferrite assembled from nanocrystals of the present invention has a better specific surface area.
[0046] In summary, this invention provides a manganese ferrite electrode material, an electrode, and a supercapacitor prepared by a solvothermal method. This method enables the preparation of submicron-sized manganese ferrite electrode materials, broadening the possibilities for manganese ferrite electrode material preparation. It provides a framework for the development of subsequent submicron-sized manganese ferrite electrode materials, and the manganese ferrite electrode material prepared by this method is low-cost and easy to mass-produce.
[0047] This invention assembles the electrodes (positive and negative electrodes) of a supercapacitor from submicron-sized manganese ferrite supercapacitor electrode material, and then further assembles the supercapacitor into a single unit. Because this submicron-sized manganese ferrite supercapacitor electrode material not only possesses excellent electrical conductivity but also exhibits a robust structure and good electrochemical performance, the supercapacitor demonstrates relatively stable performance, good conductivity, and a relatively stable structure during operation.
[0048] This invention presents a supercapacitor based on a submicron-sized manganese ferrite supercapacitor electrode material. The electrode made from the submicron-sized manganese ferrite supercapacitor electrode material endows the supercapacitor with excellent discharge specific capacity and good electrochemical cycling characteristics. Furthermore, the supercapacitor exhibits stable electrochemical performance, good capacity, and long lifespan during charge-discharge cycles.
Claims
1. A method for preparing a submicron manganese ferrite electrode material, characterized in that, Using ethylene glycol as a solvent, ferric chloride, manganese acetate, and acetate were reacted at 150-200 °C using a solvothermal method to first prepare a loosely structured spherical precursor for manganese ferrite electrode material. Then, based on the above spherical precursor, ethylene glycol, ferric chloride, manganese acetate, and acetate were added and reacted at 200-300 °C using a solvothermal method to obtain a compact submicron manganese ferrite electrode material with an approximately spherical particle structure.
2. The preparation method according to claim 1, characterized in that, The spherical precursor is a small particle with a particle size of less than 300 nm selected from screening.
3. The preparation method according to claim 1, characterized in that, The compact, near-spherical particle structure of the submicron manganese ferrite electrode material is composed of small particles with a particle size of 100-300 nm selected from screening.
4. The preparation method according to any one of claims 1-3, characterized in that, Specifically, the following steps are included: 1) Add ferric chloride and manganese acetate to ethylene glycol solvent and stir continuously until the solid powder is completely dissolved; 2) Add neutral acetate and stir continuously until a homogeneous suspension is formed; 3) Then transfer the suspension prepared in step 2) into a high-pressure reactor, place the high-pressure reactor in a forced-air drying oven, heat at 150-200 ℃ for 5-20 hours, and then cool the high-pressure reactor to room temperature to obtain a solid product; 4) The obtained solid product is washed, centrifuged, collected, dried and then screened to remove small particles with a particle size of less than 300nm. 5) Add ferric chloride, manganese acetate and the small particles obtained in step 4) to ethylene glycol solvent and stir continuously until a homogeneous suspension is formed; 6) Add neutral acetate and stir continuously until a homogeneous suspension is formed; 7) Then transfer the suspension prepared in step 6) to a high-pressure reactor, place the high-pressure reactor in a forced-air drying oven, heat at 200-300 ℃ for 8-20 hours, and then cool the high-pressure reactor to room temperature to obtain a solid product; 8) The obtained solid product is washed, centrifuged, collected, dried and then screened to remove small particles with a particle size of 100-300nm to obtain submicron-sized manganese ferrite electrode material.
5. The preparation method according to claim 4, characterized in that, The neutral acetate in steps 2) and 6) is any one of ammonium acetate, sodium acetate, or potassium acetate.
6. The preparation method according to claim 4, characterized in that, The molar ratio of the neutral acetate to ferric chloride is 0.75-1.0:
1.
7. The preparation method according to claim 4, characterized in that, The drying process in steps 4) and 8) is as follows: place the collected solid product in an oven and dry it at 40-80 ℃ for 6-10 hours, then allow it to cool naturally.
8. The submicron manganese ferrite electrode material prepared by the method of claim 4, characterized in that, It has an approximately spherical particle structure with a particle size range of 100-300 nm.
9. A method for preparing electrodes for a supercapacitor, characterized in that, Using the submicron-sized manganese ferrite material of claim 8 as the active material, acetylene black as the conductive agent, and polytetrafluoroethylene as the binder, the three are mixed evenly, and N-methylpyrrolidone is added and ground to obtain a uniformly mixed slurry. The slurry is evenly coated on nickel foam, dried, and then the sheet is cut into small circular pieces to prepare the electrode of the supercapacitor.
10. A supercapacitor, characterized in that, The electrodes prepared according to claim 9 are used as the positive and negative electrodes of a supercapacitor.