Method for manufacturing an optical material

By using a variety of optical material monomers and polymerization catalysts for prepolymerization and curing processes, the problems of ripples and lengthy manufacturing times in optical material manufacturing have been solved, achieving efficient and smooth manufacturing of optical materials.

CN116529048BActive Publication Date: 2026-11-24MITSUI CHEMICALS INC
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202180078034.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-07-29
Filing Date
2021-11-22
Publication Date
2026-11-24
Estimated Expiration
2041-11-22

AI Technical Summary

Technical Problem

In existing optical material manufacturing methods, the polymerization reaction time is long, which leads to insufficient curing of optical materials or the formation of ripples, affecting quality and making the manufacturing process lengthy.

Method used

Using a total of 100 parts by weight of two or more different monomers for optical materials and 0.010 to 2.0 parts by weight of a polymerization catalyst, through a prepolymerization process and a curing process, including prepolymerization, manufacturing of a polymeric composition for optical materials and curing, viscosity and temperature are controlled to shorten manufacturing time.

Benefits of technology

It effectively suppresses ridges in optical materials, improves the smoothness of optical materials, shortens manufacturing time, and enhances the quality of optical materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116529048B_ABST
    Figure CN116529048B_ABST
Patent Text Reader

Abstract

A method for manufacturing optical materials, comprising using a total of 100 parts by mass of two or more different optical material monomers and 0.010 to 2.0 parts by mass of a polymerization catalyst as raw materials, the method comprising the following steps: a preparation step, preparing a total of 100 parts by mass of two or more different optical material monomers and 0.010 to 2.0 parts by mass of a polymerization catalyst; and a prepolymerization step, mixing a portion of the two or more different optical material monomers and at least a portion of the polymerization catalyst, and polymerizing at least a portion of the portion of the two or more different optical material monomers to obtain a prepolymer, thereby obtaining a mixture containing the prepolymer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to methods for manufacturing optical materials, polymeric compositions for optical materials, optical material manufacturing systems, methods for manufacturing optical components, films for manufacturing optical components, molds for manufacturing optical components, and cured products. Background Technology

[0002] As a method for manufacturing resins that can be used in optical materials for plastic lenses, examples include casting polymerization, which involves injecting a polymeric composition containing monomers into a mold (casting) and then heating and curing it.

[0003] In the casting polymerization method, after preparing and degassing the polymerizable composition, the polymerizable composition is injected into a mold (casting mold), heated and cured (polymerization reaction), the product is removed from the mold (demolding), and annealed to obtain optical materials (e.g., lenses, semi-finished blanks, etc.).

[0004] In heat curing, to improve the quality of optical materials, polymerization is typically carried out over several hours to tens of hours by slowly increasing the temperature; specifically, it usually takes about 20 to 48 hours. Furthermore, it is known that a significant portion of the total manufacturing process time (e.g., 90% of the total time) is spent on polymerization.

[0005] In an embodiment of Patent Document 1, it is described that the mold into which the polymerizable composition is injected is slowly heated from 10°C to 120°C, and polymerization is carried out for 20 hours to obtain a molded body.

[0006] In addition, in an embodiment of Patent Document 2, it is described that the mold into which the polymeric composition is injected is slowly heated from 25°C to 120°C over 16 hours, and then heated at 120°C for 4 hours to obtain the molded body.

[0007] Patent Document 1: International Publication No. 2014 / 027427 Patent Document 2: International Publication No. 2014 / 133111 Summary of the Invention

[0008] The problem that the invention aims to solve As mentioned above, in the past, during the manufacturing of optical materials, the polymerization reaction was usually carried out by slowly heating the material while the temperature was gradually increased for several hours to tens of hours (e.g., about 20 to 48 hours).

[0009] On the other hand, it is believed that when optical materials are manufactured using conventional methods, insufficient polymerization occurs when the heating polymerization time is shortened, resulting in the optical materials not curing or, even if they do cure, causing defects such as ripples in the optical materials, thus reducing the quality of the optical materials.

[0010] Based on the above, it is required to suppress the ripples in the optical materials obtained during the manufacturing process and to shorten the manufacturing time of the optical materials.

[0011] The problem to be solved by one embodiment of the first embodiment of this disclosure is to provide a method for manufacturing an optical material that can suppress ripples in the obtained optical material and shorten the manufacturing time of the optical material, and a polymeric composition for the optical material used in the above-described method for manufacturing an optical material.

[0012] The problem to be solved by one embodiment of the second embodiment of this disclosure is to provide a method for manufacturing an optical material and an optical material manufacturing system capable of suppressing U-shaped ridges in the obtained optical material.

[0013] The problem to be solved by one embodiment of the third embodiment of this disclosure is to provide a method for manufacturing an optical component capable of producing an optical component with a smooth outer peripheral surface, a film for manufacturing an optical component, a mold for manufacturing an optical component, and a cured product.

[0014] The problem to be solved by one embodiment of the fourth embodiment of this disclosure is to provide a method for manufacturing an optical component capable of producing an optical component with a smooth outer peripheral surface, a film for manufacturing an optical component, a mold for manufacturing an optical component, and a cured product.

[0015] Methods for solving problems The specific means used to solve the aforementioned problems include the following methods.

[0016] <1> A method for manufacturing optical materials, comprising using two or more different optical material monomers totaling 100 parts by mass and 0.010 to 2.0 parts by mass of a polymerization catalyst as raw materials, the method comprising the following steps: The preparation process involves preparing a total of 100 parts by mass of the aforementioned two or more different monomers for optical materials, and 0.010 to 2.0 parts by mass of the aforementioned polymerization catalyst; and The prepolymerization process involves mixing a portion of the monomers of the aforementioned two or more different optical materials with at least a portion of the aforementioned polymerization catalyst, and polymerizing at least a portion of the monomers of the aforementioned two or more different optical materials to obtain a prepolymer, thereby obtaining a mixture containing the aforementioned prepolymer.

[0017] <2> like <1> The method for manufacturing the optical material further includes the following steps: A manufacturing process for a polymeric composition for optical materials involves adding the remainder of at least two different monomers for optical materials to a mixture comprising the aforementioned prepolymer, thereby obtaining a polymeric composition for optical materials containing the aforementioned two or more different monomers for optical materials, the aforementioned prepolymer, and the aforementioned polymerization catalyst; and The curing process involves curing two or more different optical material monomers in the aforementioned polymeric composition for optical materials, thereby obtaining an optical material as a cured product of the aforementioned polymeric composition for optical materials.

[0018] <3> like <2> The method for manufacturing the optical material, wherein the aforementioned prepolymerization step comprises the following steps: mixing a portion of the aforementioned two or more different optical material monomers and all of the aforementioned polymerization catalyst, and polymerizing at least a portion of the aforementioned two or more different optical material monomers to obtain a prepolymer, thereby obtaining a mixture containing the aforementioned prepolymer.

[0019] <4> like <3> The method for manufacturing the optical material, wherein a portion of the aforementioned two or more different optical material monomers is composed of all of one of the aforementioned two or more different optical material monomers and a portion of the other optical material monomers besides the aforementioned one optical material monomer.

[0020] <5> like <2> The method for manufacturing the optical material, wherein the aforementioned prepolymerization step comprises the following steps: mixing a portion of the aforementioned two or more different optical material monomers and a portion of the aforementioned polymerization catalyst, and polymerizing at least a portion of the aforementioned two or more different optical material monomers to obtain a prepolymer, thereby obtaining a mixture containing the aforementioned prepolymer; The manufacturing process of the aforementioned polymeric composition for optical materials is as follows: adding at least the remaining portions of the aforementioned two or more different monomers for optical materials and the remaining portions of the aforementioned polymerization catalyst to a mixture containing the aforementioned two or more different monomers for optical materials, the aforementioned prepolymer, and the aforementioned polymerization catalyst, thereby obtaining a polymeric composition for optical materials containing the aforementioned two or more different monomers for optical materials, the aforementioned prepolymer, and the aforementioned polymerization catalyst.

[0021] <6> like <5> The method for manufacturing the optical material, wherein the monomers of the aforementioned two or more different optical materials include isocyanate compound (A). A portion of the aforementioned two or more different optical material monomers contains a portion of isocyanate compound (A), and the remaining portion of the aforementioned two or more different optical material monomers contains the remaining portion of isocyanate compound (A).

[0022] <7> like <5> or <6> In the method for manufacturing the optical material, a portion of the aforementioned polymerization catalyst is 5 to 80 parts by mass out of 100 parts by mass of the aforementioned polymerization catalyst.

[0023] <8> like <2> ~ <7> The method for manufacturing an optical material according to any one of the above-mentioned methods, wherein a portion of the aforementioned two or more different optical material monomers is 5 to 95 parts by mass out of 100 parts by mass of the aforementioned two or more different optical material monomers.

[0024] <9> like <2> ~ <8> The method for manufacturing an optical material according to any one of the above-mentioned methods further includes, after the aforementioned prepolymerization step and before the aforementioned optical material manufacturing step using a polymeric composition, a viscosity adjustment step of adjusting the viscosity of the mixture containing the aforementioned prepolymer, measured using a type B viscometer at 25°C and 60 rpm, to 30 mPa·s to 2000 mPa·s.

[0025] <10> like <1> The method for manufacturing the optical material further includes the following steps: In the second prepolymerization step, the remaining portions of the monomers of the two or more different optical materials mentioned above and the remaining portions of the polymerization catalyst mentioned above are mixed, and at least a portion of the remaining portions of the monomers of the two or more different optical materials mentioned above are polymerized to obtain the second prepolymer, thereby obtaining a mixture containing the aforementioned second prepolymer. A manufacturing process for a polymerizable composition for optical materials involves adding a mixture containing the aforementioned second prepolymer to a mixture containing the aforementioned prepolymer, thereby obtaining a polymerizable composition for optical materials containing the aforementioned prepolymer, the aforementioned second prepolymer, and the aforementioned polymerization catalyst; and The curing process cures the aforementioned prepolymer and the aforementioned second prepolymer in the aforementioned polymeric composition for optical materials, thereby obtaining an optical material as a cured product of the aforementioned polymeric composition for optical materials.

[0026] <11> like <2> ~ <10> The method for manufacturing an optical material according to any one of the above methods, wherein, after the aforementioned manufacturing step of the polymeric composition for the optical material and before the aforementioned curing step, a liquid feeding step is further included, which involves feeding the aforementioned polymeric composition for the optical material into a casting mold. The aforementioned liquid delivery process involves mixing the aforementioned optical material with a polymeric composition in a static mixer while simultaneously delivering the liquid to a casting mold.

[0027] <12> like <2> ~ <11> The method for manufacturing an optical material according to any one of the above methods, wherein the curing step includes a step of curing the optical material with a polymeric composition by allowing the optical material to stand in a polymeric composition.

[0028] <13> like <2> ~ <12> The method for manufacturing an optical material according to any one of the above methods, wherein the curing step includes a step of curing the optical material with a polymeric composition by placing the optical material in a closed space and allowing it to stand.

[0029] <14> like <2> ~ <13> The method for manufacturing an optical material according to any one of the above methods, wherein the curing step includes a step of curing the optical material with a polymeric composition by allowing the optical material to stand without external heating.

[0030] <15> like <2> ~ <14> The method for manufacturing an optical material according to any one of the above methods, wherein the curing step includes a step of curing the optical material with a polymeric composition by allowing the optical material to stand for 2 to 10 hours.

[0031] <16> like <1> ~ <15> The method for manufacturing an optical material according to any one of the above-mentioned two or more different optical material monomers comprises an isocyanate compound (A) and an active hydrogen compound (B), wherein the active hydrogen compound (B) is at least one selected from the group consisting of a polythiol compound having two or more thiol groups, a hydroxythiol compound having one or more thiol groups and one or more hydroxyl groups, a polyol compound having two or more hydroxyl groups, and an amine compound.

[0032] <17> like <16> The method for manufacturing the optical material, wherein the aforementioned isocyanate compound (A) comprises at least one of an alicyclic isocyanate compound and an aromatic isocyanate compound.

[0033] <18> like <1> ~ <17> The method for manufacturing an optical material according to any one of the following methods, wherein the aforementioned polymerization catalyst comprises at least one selected from the group consisting of an alkaline catalyst with a pKa value of 4 to 8 and an organometallic catalyst.

[0034] <19> like <1> ~ <18> The method for manufacturing an optical material according to any one of the above methods, wherein the aforementioned polymerization catalyst comprises at least one selected from the group consisting of amine catalysts and organotin catalysts.

[0035] <20> like <1> ~ <19> The method for manufacturing an optical material according to any one of the following, wherein the aforementioned polymerization catalyst comprises at least one selected from the group consisting of 3,5-dimethylpyridine, 2,4,6-trimethylpyridine, triethylenediamine, N,N-dimethylethanolamine, triethylamine, N-ethylmorpholine, dibutyltin dichloride, dimethyltin dichloride, dibutyltin dilaurate, and dibutyltin diacetate.

[0036] <21> Polymer compositions for optical materials, comprising: Two or more different optical materials using monomers, Polymerization catalysts, and A prepolymer obtained by polymerizing at least two of the aforementioned two or more different optical materials using monomers. The content of the polymerization catalyst is 0.010 to 2.0 parts by mass relative to a total of 100 parts by mass of the aforementioned two or more different optical material monomers and the aforementioned prepolymers.

[0037] <22> like <21> The polymeric composition for optical materials described herein has a viscosity of 70 mPa·s to 1000 mPa·s, measured using a type B viscometer at 25°C and 60 rpm.

[0038] <23> like <1> ~ <20> The method for manufacturing the optical material according to any one of the following methods is a method for manufacturing the optical material using a polymerizable composition for optical materials containing two or more different monomers for optical materials and a polymerization catalyst, the manufacturing method comprising the following steps: The raw material composition preparation process includes preparing the first raw material composition and the second raw material composition; The shearing process applies shear force to the aforementioned first raw material composition and the aforementioned second raw material composition to manufacture the aforementioned polymeric composition for optical materials; The stirring process involves applying a stirring force to the aforementioned polymeric composition for optical materials; The casting process involves casting the aforementioned optical material into a mold using a polymeric composition after the aforementioned mixing process; and The curing process involves polymerizing the aforementioned optical material in the aforementioned mold with monomers from two or more different optical materials in the polymeric composition, thereby curing the aforementioned optical material with the polymeric composition. At least one of the aforementioned first raw material composition and the aforementioned second raw material composition contains a mixture comprising the aforementioned prepolymer.

[0039] <24> like <23> In the method for manufacturing the optical material, the absolute value V of the difference between the viscosity Va of the first raw material composition measured by a type B viscometer at 25°C and 60 rpm and the viscosity Vb of the second raw material composition measured by a type B viscometer at 25°C and 60 rpm is in the range of 20 mPa·s to 1500 mPa·s.

[0040] <25> like <24> The method for manufacturing the optical material, wherein the aforementioned viscosity Va is in the range of 10 mPa·s to 2000 mPa·s.

[0041] <26> like <23> ~ <25> The method for manufacturing an optical material according to any one of the following, wherein the aforementioned first raw material composition comprises at least one compound selected from the group consisting of polyisocyanate compounds, epoxy compounds and cyclic sulfur compounds.

[0042] <27> like <23> ~ <26> The method for manufacturing an optical material according to any one of the following, wherein the aforementioned second raw material composition comprises at least one active hydrogen compound selected from the group consisting of a polythiol compound having two or more thiol groups, a hydroxythiol compound containing one or more thiol groups and one or more hydroxyl groups, a polyol compound containing two or more hydroxyl groups, and an amine compound.

[0043] <28> like <23> ~ <27> The method for manufacturing an optical material according to any one of the above-mentioned methods, wherein the viscosity of the aforementioned optical material polymeric composition in the aforementioned casting process, measured using a type B viscometer at 25°C and 60 rpm, is 10 mPa·s to 1000 mPa·s.

[0044] <29> like <23> ~ <28> The method for manufacturing the optical material according to any one of the above methods, wherein the aforementioned polymerization catalyst satisfies the following condition 1.

[0045] [Condition 1] -Ea / R is above -7100 and below -2900.

[0046] (Ea is the activation energy calculated from the Arrhenius curve of the reaction rate constants of the aforementioned two or more different optical materials at two or more different temperatures using monomers; R is the gas constant (8.314 J / mol / K).) <30> like <23> ~ <29> The method for manufacturing an optical material according to any one of the following, wherein the aforementioned polymerization catalyst comprises at least one selected from the group consisting of an alkaline catalyst with a pKa value of 4 to 8 and an organometallic catalyst.

[0047] <31> An optical material manufacturing system is a system for manufacturing optical materials using a polymerizable composition containing two or more different optical material monomers and a polymerization catalyst, the optical material manufacturing system comprising: A shearing section applies shear force to the first raw material composition and the second raw material composition to manufacture the aforementioned polymeric composition for optical materials; The stirring section applies a stirring force to the aforementioned polymeric composition for optical materials; The casting section casts the aforementioned optical material into a mold using a polymeric composition; The curing section polymerizes two or more different optical materials in the polymeric composition of the aforementioned optical material in the aforementioned mold using monomers, thereby curing the aforementioned optical material in the polymeric composition; and Quantitative liquid delivery part.

[0048] <32> like <31> The optical material manufacturing system further includes a viscosity control unit, which controls the viscosity of the aforementioned optical material polymeric composition in the aforementioned stirring unit, as measured by a type B viscometer at 25°C and 60 rpm, based on at least one of the following conditions: the shear force of the aforementioned shearing unit, the temperature of the aforementioned polymeric composition for optical materials in the aforementioned stirring unit, the optical quality of the cured product obtained by curing the aforementioned polymeric composition for optical materials in the aforementioned curing unit, and a characteristic quantity associated with the viscosity of the aforementioned polymeric composition for optical materials measured by a type B viscometer at 25°C and 60 rpm.

[0049] <33> like <31> or <32> The optical material manufacturing system further includes a temperature control unit that controls the temperature in the stirring unit based on at least one of the following conditions: the shear force of the shearing unit, the temperature of the polymeric composition for optical materials in the stirring unit, the optical quality of the cured product obtained by curing the polymeric composition for optical materials in the curing unit, and a characteristic quantity related to the viscosity of the polymeric composition for optical materials measured using a type B viscometer at 25°C and 60 rpm.

[0050] <34> A method for manufacturing an optical component includes the following steps: a space forming step, in which a film is attached to the outer peripheral surface of two mold substrates arranged at a predetermined interval to form a space surrounded by the two mold substrates and the film; an injection step, in which a polymeric composition is injected into the space; and a curing step, in which the polymeric composition injected into the space is cured to obtain a cured product, wherein the film is a film that is completely peeled off from the glass after being attached to glass and subjected to a heat resistance index test at 85°C, and the heat distortion temperature of the film is 70°C or higher.

[0051] <35> like <34> The method for manufacturing the optical component, wherein the aforementioned polymeric composition exhibits a viscosity-increasing curve (y=ae) at 25°C. bx The slope of ) is above 0.4.

[0052] <36> like <34> or <35> The method for manufacturing the optical component, wherein the curing time in the aforementioned curing process is less than 10 hours.

[0053] <37> like <34> ~ <36> The manufacturing method of the optical component according to any one of the above-mentioned methods, wherein, for the aforementioned film, when a glass ball adhesion test is performed at 80°C, the movement distance of the glass ball is less than 200 mm.

[0054] <38> like <34> ~ <37> The method for manufacturing an optical component according to any one of the above-mentioned methods, wherein, during the curing step, as the polymeric composition is cured, at least one of the two mold substrates moves on the contact surface with the film, and the gap between the mold substrates becomes smaller than the gap between the mold substrates in the space forming step.

[0055] <39> like <34> ~ <38> The method for manufacturing an optical component according to any one of the following, wherein the aforementioned polymeric composition comprises two or more different monomers for optical materials and a polymerization catalyst, wherein the content of the aforementioned polymerization catalyst is 0.010 parts by mass to 2.0 parts by mass relative to a total of 100 parts by mass of the aforementioned two or more different monomers for optical materials, and the viscosity measured using a type B viscometer at 25°C and 60 rpm is 10 mPa·s to 1000 mPa·s.

[0056] <40> like <34> ~ <39> The method for manufacturing an optical component according to any one of the following methods, wherein the aforementioned polymeric composition comprises two or more different monomers for optical materials, a polymerization catalyst, and a prepolymer containing polymeric functional groups, wherein the prepolymer is a polymer of the aforementioned two or more different monomers for optical materials.

[0057] <41> like <39> or <40> The method for manufacturing the optical component, wherein the monomers for the aforementioned two or more different optical materials include at least one active hydrogen compound selected from the group consisting of a polythiol compound containing two or more thiol groups, a hydroxythiol compound containing one or more thiol groups and one or more hydroxyl groups, a polyol compound containing two or more hydroxyl groups, and an amine compound.

[0058] <42> like <39> ~ <41> The method for manufacturing an optical component according to any one of the following methods, wherein the aforementioned polymerization catalyst satisfies the following condition 1.

[0059] [Condition 1] -Ea / R is above -7100 and below -2900.

[0060] (Ea is the activation energy calculated from the Arrhenius curve of the reaction rate constants of the aforementioned two or more different optical materials at two or more different temperatures using monomers; R is the gas constant (8.314 J / mol / K).) <43> like <39> ~ <42> The method for manufacturing an optical component according to any one of the following, wherein the aforementioned polymerization catalyst comprises at least one selected from the group consisting of amine catalysts and organotin catalysts.

[0061] <44> An optical component manufacturing film is used to manufacture optical components through the following process: attaching a film to the outer peripheral surfaces of two mold substrates arranged opposite each other at a predetermined interval to form a space surrounded by the two mold substrates and the film; placing a polymerizable composition in the space; and curing the polymerizable composition for 10 hours or less to obtain a cured product. The film for manufacturing optical components includes at least a substrate layer and an adhesive layer, and after being attached to glass and subjected to a heat resistance index test at 85°C, it completely peels off from the glass.

[0062] <45> An optical component manufacturing mold is used to manufacture optical components through the following process: attaching a film to the outer peripheral surfaces of two mold substrates arranged opposite each other at a predetermined interval to form a space surrounded by the two mold substrates and the film; placing a polymerizable composition in the space; and curing the polymerizable composition to obtain a cured product. The approximate diameter of the main surface of the aforementioned mold is 60cm to 80cm.

[0063] <46> The cured material, which is a cured material of two or more different optical monomers, does not have ripples longer than 1.0 mm within a radius of 15 mm from the center of the aforementioned cured material. The outer peripheral surface of the aforementioned solidified material is mirror-like, and the shape between the intersection of one main surface and the outer peripheral surface, and the intersection of another main surface and the outer peripheral surface, is approximately a straight line.

[0064] <47> like <46> The solidified material includes protrusions that are substantially parallel to the aforementioned outer peripheral surface at the intersection of one of the aforementioned main surfaces and the outer peripheral surface, and at the intersection of the other of the aforementioned main surfaces and the outer peripheral surface.

[0065] <48> like <46> or <47> The solidified product, wherein the amine content, as determined by gas chromatography-mass spectrometry, is 0.03% by mass or more and 2.5% by mass or less.

[0066] <49> like <46> ~ <48> The cured product according to any one of the following methods comprises a thiourethane resin.

[0067] <50> A method for manufacturing an optical component includes the following steps: a space forming step, in which a film is attached to the outer peripheral surface of two mold substrates arranged at a predetermined interval to form a space surrounded by the two mold substrates and the film; an injection step, in which a polymeric composition is injected into the space; and a curing step, in which the polymeric composition injected into the space is cured to obtain a cured product, wherein the film, when attached to glass and subjected to a heat resistance index test at 85°C, has a heat resistance index of 1 mm or more (excluding cases where it completely peels off from the glass), and the heat distortion temperature of the film is 120°C or less.

[0068] <51> like <50> The method for manufacturing the optical component, wherein the slope of the viscosity-enhancing curve of the aforementioned polymeric composition at 25°C (y=ae) bx The value is above 0.4.

[0069] <52> like <50> or <51> The method for manufacturing the optical component, wherein the curing time in the aforementioned curing process is less than 10 hours.

[0070] <53> like <50> ~ <52> The manufacturing method of the optical component according to any one of the above-mentioned methods, wherein, for the aforementioned film, when a glass ball adhesion test is performed at 80°C, the movement distance of the glass ball is less than 200 mm.

[0071] <54> like <50> ~ <53> The method for manufacturing an optical component according to any one of the above methods, wherein, in the curing step, the polymeric composition is cured by allowing the polymeric composition injected into the aforementioned space to stand in a closed space.

[0072] <55> like <50> ~ <54> The method for manufacturing an optical component according to any one of the following, wherein the aforementioned polymeric composition comprises two or more different monomers for optical materials and a polymerization catalyst, wherein the content of the aforementioned polymerization catalyst is 0.010 parts by mass to 2.0 parts by mass relative to a total of 100 parts by mass of the aforementioned two or more different monomers for optical materials, and the viscosity measured using a type B viscometer at 25°C and 60 rpm is 10 mPa·s to 1000 mPa·s.

[0073] <56> like <50> ~ <55> The method for manufacturing an optical component according to any one of the following methods, wherein the aforementioned polymeric composition comprises two or more different monomers for optical materials, a polymerization catalyst, and a prepolymer containing polymeric functional groups, wherein the prepolymer is a polymer of the aforementioned two or more different monomers for optical materials.

[0074] <57> like <55> or <56> The method for manufacturing the optical component, wherein the monomers for the aforementioned two or more different optical materials include at least one active hydrogen compound selected from the group consisting of a polythiol compound containing two or more thiol groups, a hydroxythiol compound containing one or more thiol groups and one or more hydroxyl groups, a polyol compound containing two or more hydroxyl groups, and an amine compound.

[0075] <58> like <55> ~ <57> The method for manufacturing an optical component according to any one of the following methods, wherein the aforementioned polymerization catalyst satisfies the following condition 1.

[0076] [Condition 1] -Ea / R is above -7100 and below -2900.

[0077] (Ea is the activation energy calculated from the Arrhenius curve of the reaction rate constants of the aforementioned two or more different optical materials at two or more different temperatures using monomers; R is the gas constant (8.314 J / mol / K).) <59> like <55> ~ <58> The method for manufacturing an optical component according to any one of the following, wherein the aforementioned polymerization catalyst comprises at least one selected from the group consisting of amine catalysts and organotin catalysts.

[0078] <60> An optical component manufacturing film is used to manufacture optical components through the following process: attaching a film to the outer peripheral surfaces of two mold substrates arranged opposite each other at a predetermined interval to form a space surrounded by the two mold substrates and the film; placing a polymerizable composition in the space; and curing the polymerizable composition for 10 hours or less to obtain a cured product. The film for manufacturing optical components includes at least a substrate layer and an adhesive layer, and when it is attached to glass and subjected to a heat resistance index test at 85°C, the heat resistance index is 1 mm or more (excluding cases where it is completely peeled off from the aforementioned glass).

[0079] <61> An optical component manufacturing mold is used to manufacture optical components through the following process: attaching a film to the outer peripheral surfaces of two mold substrates arranged opposite each other at a predetermined interval to form a space surrounded by the two mold substrates and the film; placing a polymerizable composition in the space; and curing the polymerizable composition to obtain a cured product. The approximate diameter of the main surface of the aforementioned mold is 60cm to 80cm.

[0080] <62> The cured material, which is a cured material of two or more different optical monomers, does not have ripples longer than 1.0 mm within a radius of 15 mm from the center of the aforementioned cured material. The outer peripheral surface of the aforementioned cured material is mirror-like, and the shape between the intersection of one main surface and the outer peripheral surface, and the intersection of another main surface and the outer peripheral surface, is a concave curve.

[0081] <63> like <62> The solidified material includes protrusions that are substantially parallel to the aforementioned outer peripheral surface at the intersection of one of the aforementioned main surfaces and the outer peripheral surface, and at the intersection of the other of the aforementioned main surfaces and the outer peripheral surface.

[0082] <64> like <62> or <63> The solidified product, wherein the amine content, as determined by gas chromatography-mass spectrometry, is 0.03% by mass or more and 2.5% by mass or less.

[0083] <65> like <62> ~ <64> The cured product according to any one of the following methods comprises a thiourethane resin.

[0084] Invention Effects According to one embodiment of the first embodiment of this disclosure, a method for manufacturing an optical material that can suppress ripples in the obtained optical material and shorten the manufacturing time of the optical material, and a polymeric composition for the optical material used in the above-described method for manufacturing the optical material can be provided.

[0085] According to one embodiment of the second embodiment of this disclosure, a method for manufacturing an optical material and an optical material manufacturing system capable of suppressing U-shaped ridges in the obtained optical material can be provided.

[0086] According to one embodiment of the third embodiment of this disclosure, a method for manufacturing an optical component capable of producing an optical component with a smooth outer peripheral surface, a film for manufacturing an optical component, a mold for manufacturing an optical component, and a cured product can be provided.

[0087] According to one embodiment of the fourth embodiment of this disclosure, a method for manufacturing an optical component capable of producing an optical component with a smooth outer peripheral surface, a film for manufacturing an optical component, a mold for manufacturing an optical component, and a cured product can be provided. Attached Figure Description

[0088] [ Figure 1 This is a flowchart illustrating an example of a control routine when shear force information is obtained using a viscosity control unit and a temperature control unit.

[0089] [ Figure 2 This is a flowchart illustrating an example of a control routine in which temperature information of a polymeric composition for optical materials in a stirring section is obtained using a viscosity control unit and a temperature control unit.

[0090] [ Figure 3This is a flowchart illustrating an example of a control routine in which information related to the viscosity of a polymeric composition for optical materials is obtained using a viscosity control unit and a temperature control unit.

[0091] [ Figure 4 This is a flowchart illustrating an example of a control routine when optical quality information of a cured product is obtained using a viscosity control unit and a temperature control unit.

[0092] [ Figure 5 This is a schematic diagram illustrating an example of an optical material manufacturing system.

[0093] [ Figure 6 This diagram illustrates an example of the configuration of a computer that implements the viscosity control unit and the temperature control unit.

[0094] [ Figure 7 [This is a schematic diagram used to illustrate the space-forming process.]

[0095] [ Figure 8 [This is a schematic diagram used to illustrate the injection process.]

[0096] [ Figure 9 This is a schematic diagram illustrating the movement of the mold substrate during the curing process.

[0097] [ Figure 10 This is a schematic diagram used to illustrate the shape changes of the film during the curing process. Detailed Implementation

[0098] In this public document, the range of values ​​indicated by “~” refers to the range of values ​​recorded before and after “~” as the lower and upper limits.

[0099] In this disclosure, when a composition contains multiple substances belonging to each component, unless otherwise specified, the amount of each component in the composition refers to the total amount of the multiple substances present in the composition.

[0100] In the numerical ranges described in stages in this disclosure, the upper or lower limit of one numerical range can be replaced with the upper or lower limit of other numerical ranges described in stages. Furthermore, the upper or lower limit of a numerical range described in this disclosure can be replaced with the values ​​shown in the embodiments.

[0101] In this disclosure, the term "process" refers not only to an independent process, but also to any process that can be clearly distinguished from other processes, as long as it achieves the desired purpose of that process.

[0102] This disclosure includes the following first to fourth embodiments. Each embodiment is described in detail.

[0103] [First Implementation] Manufacturing Methods of Optical Materials The method for manufacturing the optical material according to the first embodiment is a method for manufacturing the optical material using two or more different optical material monomers totaling 100 parts by mass and 0.010 to 2.0 parts by mass of a polymerization catalyst as raw materials. The method includes the following steps: a preparation step, in which two or more different optical material monomers totaling 100 parts by mass and 0.010 to 2.0 parts by mass of a polymerization catalyst are prepared; and a prepolymerization step, in which a portion of the aforementioned two or more different optical material monomers and at least a portion of the aforementioned polymerization catalyst are mixed, and at least a portion of the aforementioned two or more different optical material monomers are polymerized to obtain a prepolymer, thereby obtaining a mixture containing the aforementioned prepolymer.

[0104] The optical material manufacturing method of the first embodiment includes a preparation step and a prepolymerization step, thereby suppressing ripples in the obtained optical material and shortening the manufacturing time of the optical material.

[0105] It should be noted that, in the first embodiment, a ridge refers to a condition where the refractive index of a specific portion differs from the surrounding normal refractive index. Rifts in optical materials are one of the main factors that degrade quality.

[0106] The preferred method for manufacturing the optical material according to the first embodiment includes, in addition to the preparation and prepolymerization processes described above, the following processes: A manufacturing process for a polymeric composition for optical materials involves adding the remainder of at least two different monomers for optical materials to a mixture comprising the aforementioned prepolymer, thereby obtaining a polymeric composition for optical materials containing the aforementioned two or more different monomers for optical materials, the aforementioned prepolymer, and the aforementioned polymerization catalyst; and The curing process involves curing two or more different optical material monomers in the aforementioned polymeric composition for optical materials, thereby obtaining an optical material as a cured product of the aforementioned polymeric composition for optical materials.

[0107] The optical material manufacturing method of the first embodiment includes, in addition to the preparation step and the prepolymerization step, a manufacturing step of a polymeric composition for optical materials and a curing step. As a result, the ripples in the obtained optical material can be suppressed better, and the manufacturing time of the optical material can be shortened more effectively.

[0108] In the preparation step of the first embodiment, the content of the polymerization catalyst in the polymeric composition for optical materials prepared is 0.010 to 2.0 parts by mass relative to a total of 100 parts by mass of two or more different optical material monomers. This content of the polymerization catalyst is much higher than that in conventional optical material manufacturing methods.

[0109] Therefore, when the monomers of the optical material in the polymeric composition for optical materials are polymerized in the curing process, the heat of reaction of the polymeric composition for optical materials (i.e., heat generated due to self-heating) can be generated in a short time.

[0110] The aforementioned heat of reaction can be used to promote the polymerization reaction of the monomers for optical materials in the polymeric composition for optical materials. Therefore, high-quality optical materials in which ripples can be suppressed can be obtained in a shorter time than before.

[0111] Conventionally, during polymerization, the polymeric composition for optical materials is heated to induce polymerization. However, in the method for manufacturing optical materials according to the first embodiment, it is not necessary to heat the polymeric composition for optical materials.

[0112] Furthermore, the optical material manufacturing method of the first embodiment includes a preparation step, a prepolymerization step, a manufacturing step of a polymerizable composition for optical materials, and a curing step, thereby suppressing convection within the mold where the polymerization reaction takes place and suppressing the generation of ripples in the obtained cured product.

[0113] Furthermore, the prepolymer in the optical material manufacturing method of the first embodiment can maintain good storage stability. For example, even when the prepolymer is stored for a certain period of time, curing of the prepolymer can be suppressed. That is, a long service life can be ensured.

[0114] <Preparation Process> The method for manufacturing optical materials according to the first embodiment includes a preparation step of preparing two or more different monomers for optical materials totaling 100 parts by mass and 0.010 to 2.0 parts by mass of a polymerization catalyst.

[0115] The number of monomers used in two or more different optical materials can be, for example, up to five or up to three.

[0116] (Single for optical materials) A portion of the monomers of two or more different optical materials in the preparation process is used to obtain the prepolymer in the prepolymerization process described later.

[0117] In addition, the remaining portions of two or more different optical material monomers are included in the optical material polymeric composition manufactured in the manufacturing process of the optical material polymeric composition described later.

[0118] Examples of monomers used in optical materials include isocyanate compounds, polythiols having two or more thiol groups, hydroxythiols having one or more thiol groups and one or more hydroxyl groups, polyols having two or more hydroxyl groups, and amine compounds.

[0119] The monomers for two or more different optical materials preferably include an isocyanate compound (A) and an active hydrogen compound (B), wherein the active hydrogen compound (B) is at least one selected from the group consisting of a polythiol compound having two or more thiol groups, a hydroxythiol compound having one or more thiol groups and one or more hydroxyl groups, a polyol compound having two or more hydroxyl groups, and an amine compound.

[0120] [Isocyanate compound (A)] Examples of isocyanate compounds (A) include aliphatic isocyanate compounds, alicyclic isocyanate compounds, aromatic isocyanate compounds, heterocyclic isocyanate compounds, etc., and one or more types may be used. These isocyanate compounds may include dimers, trimers, and prepolymers. Examples of these isocyanate compounds include those illustrated in International Publication No. 2011 / 055540.

[0121] It should be noted that, in the first embodiment, alicyclic isocyanate compounds refer to isocyanate compounds that contain alicyclic structures and may contain heterocyclic structures or other structures other than alicyclic structures.

[0122] Aromatic isocyanate compounds refer to isocyanate compounds that contain an aromatic structure and may contain any one or a combination of aliphatic, alicyclic, and heterocyclic structures.

[0123] Heterocyclic isocyanate compounds are isocyanate compounds that contain heterocyclic structures but do not contain alicyclic or aromatic structures.

[0124] Aliphatic isocyanate compounds refer to isocyanate compounds that do not contain aromatic, alicyclic, or heterocyclic structures.

[0125] As isocyanate compound (A), it preferably includes at least one selected from aliphatic isocyanate compounds, alicyclic isocyanate compounds, aromatic isocyanate compounds and heterocyclic isocyanate compounds, and more preferably includes at least one of alicyclic isocyanate compounds and aromatic isocyanate compounds.

[0126] In the first embodiment, from the viewpoint of suppressing ripples in optical materials and shortening the manufacturing time of optical materials, the isocyanate compound (A) preferably comprises at least one selected from 2,5-bis(isocyanate-methyl)bicyclo-[2.2.1]-heptane, 2,6-bis(isocyanate-methyl)bicyclo-[2.2.1]-heptane, m-phenylene diisocyanate, 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, dicyclohexylmethane diisocyanate, 1,3-bis(isocyanate-methyl)cyclohexane, 1,4-bis(isocyanate-methyl)cyclohexane, isophorone diisocyanate, 1,6-hexanediisocyanate, and 1,5-pentanediisocyanate. More preferably, it comprises at least one selected from 2,5-bis(isocyanate-methyl)bicyclo-[2.2.1]-heptane, 2,6-bis(isocyanate-methyl)bicyclo-[2.2.1]-heptane, m-phenylene diisocyanate, dicyclohexylmethane diisocyanate, and 1,3-bis(isocyanate-methyl)cyclohexane. Further preferably, it includes at least one selected from isophthalene diisocyanate, 2,5-bis(isocyanate-methyl)bicyclo-[2.2.1]-heptane, and 2,6-bis(isocyanate-methyl)bicyclo-[2.2.1]-heptane.

[0127] [Active hydrogen compounds] Examples of active hydrogen compounds include polythiols with two or more thiol groups, hydroxythiols with one or more thiol groups and one or more hydroxyl groups, polyols with two or more hydroxyl groups, and amine compounds.

[0128] As active hydrogen compounds, oligomers of the above-mentioned active hydrogen compounds and halogen-substituted derivatives of the above-mentioned active hydrogen compounds (e.g., chlorine-substituted derivatives, bromine-substituted derivatives, etc.) may also be used.

[0129] In addition, active hydrogen compounds can be used alone or in combination of two or more.

[0130] (Polythiol compounds with two or more thiol groups) Polythiol compounds are compounds having two or more thiol groups, and examples of such compounds can be found in International Publication No. 2016 / 125736.

[0131] In the first embodiment, from the viewpoint of suppressing ripples in optical materials and shortening the manufacturing time of optical materials, the polythiol compound preferably comprises a compound selected from 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane, 5,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,8-dimercaptomethyl-1,11-dimercapto- At least one of the following: 3,6,9-trithiaundecane, pentaerythritol tetra(3-mercaptopropionate), bis(mercaptoethyl) sulfide, pentaerythritol tetra(2-mercaptoacetate), 2,5-bis(mercaptomethyl)-1,4-dithiacyclohexane, 1,1,3,3-tetra(mercaptomethylthio)propane, 4,6-bis(mercaptomethylthio)-1,3-dithiacyclohexane, and 2-(2,2-bis(mercaptomethylthio)ethyl)-1,3-dithiacyclobutane. More preferably, it comprises at least one selected from 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane, 5,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,8-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, pentaerythritol tetrakis(3-mercaptopropionate), pentaerythritol tetrakis(2-mercaptoacetate), and 2,5-bis(mercaptomethyl)-1,4-dithiacyclohexane. Further preferably, it comprises at least one selected from 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane, 5,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,8-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, and pentaerythritol tetra(3-mercaptopropionate).

[0132] (Hydroxythiol compounds having one or more thiol groups and one or more hydroxyl groups) Examples of thiol compounds having a hydroxyl group include, for example, 2-mercaptoethanol, 3-mercapto-1,2-propanediol, glycerol bis(mercaptoacetate), 4-mercaptophenol, 2,3-dimercapto-1-propanol, pentaerythritol tris(3-mercaptopropionate), pentaerythritol tris(mercaptoacetate), etc., but are not limited to these exemplary compounds.

[0133] (Polyol compounds with two or more hydroxyl groups) As polyol compounds, one or more aliphatic or alicyclic alcohols can be mentioned. Specifically, examples include straight-chain or branched aliphatic alcohols, alicyclic alcohols, and alcohols obtained by adding at least one alcohol selected from the group consisting of ethylene oxide, propylene oxide, and ε-caprolactone to these alcohols. More specifically, the compounds illustrated in International Publication No. 2016 / 125736 can be mentioned.

[0134] The polyol compound is preferably selected from at least one of ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, 1,3-propanediol, 1,2-cyclopentanediol, 1,3-cyclopentanediol, 1,2-cyclohexanediol, 1,3-cyclohexanediol, and 1,4-cyclohexanediol.

[0135] (Amine compounds) Examples of amine compounds include: ethylenediamine, 1,2- or 1,3-diaminopropane, 1,2-, 1,3- or 1,4-diaminobutane, 1,5-diaminopentane, 1,6-diaminohexane, 1,7-diaminoheptane, 1,8-diaminooctane, 1,10-diaminodecane, 1,2-, 1,3- or 1,4-diaminocyclohexane, o-, m- or p-diaminobenzene, 3,4- or 4,4'-diaminobenzophenone, 3,4- or 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane, and 4,4'-diaminodiphenylmethane. Primary polyamine compounds including diphenyl sulfide, 3,3' or 4,4'-diaminodiphenyl sulfone, 2,7-diaminofluorene, 1,5-, 1,8- or 2,3-diaminonaphthalene, 2,3-, 2,6- or 3,4-diaminopyridine, 2,4- or 2,6-diaminotoluene, meta- or p-phenylenediamine, isophorone diamine, diaminomethylbicycloheptane, 1,3- or 1,4-diaminomethylcyclohexane, 2- or 4-aminopiperidine, 2- or 4-aminomethylpiperidine, 2- or 4-aminoethylpiperidine, N-aminoethylmorpholine, N-aminopropylmorpholine, etc. Diethylamine, dipropylamine, di-n-butylamine, di-sec-butylamine, diisobutylamine, di-n-pentylamine, di-3-pentylamine, dihexylamine, dioctylamine, di(2-ethylhexyl)amine, methylhexylamine, diallylamine, N-methylallylamine, piperidine, pyrrolidine, diphenylamine, N-methylamine, N-ethylamine, dibenzylamine, N-methylbenzylamine, N-ethylbenzylamine, dicyclohexylamine, N-methylaniline, N-ethylaniline, dinaphthylamine, 1-methylpiperazine, morpholine, and other monofunctional secondary amine compounds; N,N'-Dimethylethylenediamine, N,N'-Dimethyl-1,2-diaminopropane, N,N'-Dimethyl-1,3-diaminopropane, N,N'-Dimethyl-1,2-diaminobutane, N,N'-Dimethyl-1,3-diaminobutane, N,N'-Dimethyl-1,4-diaminobutane, N,N'-Dimethyl-1,5-diaminopentane, N,N'-Dimethyl-1,6-diaminohexane, N,N'-Dimethyl-1,7-diaminoheptane, N,N'-Diethylethylenediamine, N,N'-Diethyl-1,2-diaminopropane, N,N'-Diethyl-1,3-diaminopropane, N,N' -Diethyl-1,2-diaminobutane, N,N'-diethyl-1,3-diaminobutane, N,N'-diethyl-1,4-diaminobutane, N,N'-diethyl-1,5-diaminopentane, N,N'-diethyl-1,6-diaminohexane, N,N'-diethyl-1,7-diaminoheptane, piperazine, 2-methylpiperazine, 2,5-dimethylpiperazine, 2,6-dimethylpiperazine, high-piperazine, 1,1-di(4-piperidinyl)methane, 1,2-di(4-piperidinyl)ethane, 1,3-di(4-piperidinyl)propane, 1,4-di(4-piperidinyl)butane, tetramethylguanidine, and other secondary polyamine compounds; etc.

[0136] Of the above, the active hydrogen compound (B) preferably includes a polythiol compound having two or more thiol groups.

[0137] The content of polythiol compounds having two or more thiol groups is preferably 60% by mass or more, more preferably 70% by mass or more, and even more preferably 80% by mass or more, relative to the total mass of the active hydrogen compound (B).

[0138] Furthermore, as the active hydrogen compound (B) in the first embodiment, the total content of 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane and pentaerythritol tetra(3-mercaptopropionate) is preferably 60% by mass or more, more preferably 70% by mass or more, and even more preferably 80% by mass or more, relative to the total mass of the active hydrogen compound (B).

[0139] In the composition, the molar ratio (NCO group / (OH group + SH group)) of the total number of hydroxyl (OH group) and mercapto (SH group) groups in the active hydrogen compound relative to the isocyanate group (NCO group) in the isocyanate compound (A) is preferably 0.8 to 1.2, more preferably 0.85 to 1.15, and even more preferably 0.9 to 1.1.

[0140] <Polymerization Catalyst> At least a portion of the polymerization catalyst in the preparation step is used to obtain the prepolymer in the prepolymerization step described later.

[0141] There are no particular limitations on the polymerization catalysts used; for example, basic catalysts, organometallic catalysts, zinc carbamates, ammonium salts, sulfonic acids, etc., can be used.

[0142] The polymerization catalysts mentioned above can be used in combination of one type or two or more types.

[0143] (Alkaline catalyst) Examples of alkaline catalysts include amine catalysts and imidazole catalysts.

[0144] Specifically, examples include tertiary amine catalysts such as triethylenediamine, N,N-dimethylethanolamine, triethylamine, and N-ethylmorpholine; and catalysts such as 2-methylpyrazine, pyridine, α-methylpyridine, β-methylpyridine, γ-methylpyridine, 2,6-dimethylpyridine, 3,5-dimethylpyridine, 2,4,6-trimethylpyridine, 3-chloropyridine, N,N-diethylaniline, N,N-dimethylaniline, hexamethylenetetramine, quinoline, isoquinoline, N,N-dimethyl-p-toluidine, N,N-dimethylpiperazine, quinalidine, 4-methylmorpholine, triallylamine, trioctylamine, 1,2-dimethylimidazole, and 1-benzyl-2-methylimidazole.

[0145] Of the above, the amine-based catalyst described above is preferred as the alkaline catalyst.

[0146] Examples of amine catalysts include tertiary amine catalysts such as 3,5-dimethylpyridine, 2,4,6-trimethylpyridine, triethylenediamine, N,N-dimethylethanolamine, triethylamine, and N-ethylmorpholine.

[0147] The amine catalyst preferably contains at least one selected from 3,5-dimethylpyridine, 2,4,6-trimethylpyridine, triethylenediamine, N,N-dimethylethanolamine, triethylamine, and N-ethylmorpholine.

[0148] The alkaline catalyst also preferably contains compounds represented by the following general formula (2) and / or compounds represented by the following general formula (3).

[0149] [Chemical Formula 1] In general formula (2), R1 represents a straight-chain alkyl group with 1 to 20 carbon atoms, a branched alkyl group with 3 to 20 carbon atoms, a cycloalkyl group with 3 to 20 carbon atoms, or a halogen atom. There may be multiple R1s, which may be the same or different. Q represents a carbon atom or a nitrogen atom. m represents an integer from 0 to 5.

[0150] [Chemical Formula 2] In general formula (3), R2, R3 and R4 each independently represent a straight-chain alkyl group with 1 to 20 carbon atoms, a branched alkyl group with 3 to 20 carbon atoms, a cycloalkyl group with 3 to 20 carbon atoms, or an allyl group.

[0151] As an alkaline catalyst, the pKa value is preferably 1 to 9, more preferably 3 to 8, and even more preferably 4 to 8.

[0152] The pKa value (acid dissociation index) can be determined by methods such as (a) The Journal of Physical Chemistry vol.68, number 6, page 1560 (1964), (b) using an automatic potentiometric titration apparatus (AT-610 (trade name) etc.) manufactured by Kyoto Electronics Industry Co., Ltd., or by using the acid dissociation index described in (c) Chemical Handbook compiled by the Chemical Society of Japan (revised 3rd edition, published by Maruzen Co., Ltd. on June 25, 1959).

[0153] (Organometallic catalysts) Examples of organometallic catalysts include organotin catalysts; organic acid salts such as iron, nickel, and zinc; acetylacetone complexes; catalyst compositions formed by carboxylic acid metal compounds and quaternary ammonium salt compounds; catalyst compositions formed by bicyclic tertiary amine compounds and quaternary ammonium salt compounds; metal catalysts composed of alkoxy and carboxyl groups coordinated to titanium or aluminum; and so on.

[0154] Of the above, organometallic catalysts are preferably organotin catalysts.

[0155] Examples of organotin catalysts include dibutyltin dichloride (DBC), dimethyltin dichloride (DMC), dibutyltin dilaurate (DBTDL), and dibutyltin diacetate.

[0156] The organotin catalyst preferably contains at least one selected from dibutyltin dichloride, dimethyltin dichloride, dibutyltin dilaurate, and dibutyltin diacetate.

[0157] As a polymerization catalyst, it is preferred to include at least one of the group consisting of a basic catalyst selected from the group consisting of a pKa value of 4 to 8 and an organometallic catalyst.

[0158] As a polymerization catalyst, it is also preferred to include at least one selected from amine catalysts and organotin catalysts.

[0159] As a polymerization catalyst, it is also preferred to include at least one selected from the group consisting of 3,5-dimethylpyridine, 2,4,6-trimethylpyridine, triethylenediamine, N,N-dimethylethanolamine, triethylamine, N-ethylmorpholine, dibutyltin dichloride, dimethyltin dichloride, dibutyltin dilaurate, and dibutyltin diacetate.

[0160] In the preparation process, a total of 100 parts by mass of two or more different monomers for optical materials and 0.010 to 2.0 parts by mass of polymerization catalyst are prepared.

[0161] That is, the method for manufacturing optical materials in the first embodiment uses a polymerization catalyst in an amount of 0.010 to 2.0 parts by mass relative to a total of 100 parts by mass of two or more different optical material monomers.

[0162] As described above, the amount of polymerization catalyst used in the first embodiment is much larger than that used in conventional optical material manufacturing methods.

[0163] Therefore, when the monomers for optical materials in the polymerizable composition for optical materials are polymerized during the curing process, the heat of reaction of the polymerizable composition for optical materials can be generated in a short time. By further using this heat of reaction for polymerization, the polymerization reaction can be effectively promoted, and high-quality optical materials with suppressed ripples can be obtained in a shorter time than before.

[0164] By using a polymerization catalyst containing 0.010 or more parts by mass relative to 100 parts by mass of monomers used in two or more different optical materials, the polymerization reaction can be effectively promoted, thus enabling the production of high-quality optical materials with suppressed ripples in a short time. Furthermore, by effectively promoting the polymerization reaction, the demolding properties when removing the cured material from the mold can be improved.

[0165] From the above perspective, relative to 100 parts by mass of monomers for two or more different optical materials, it is preferable to use 0.015 parts by mass or more of polymerization catalyst, more preferably 0.038 parts by mass or more of polymerization catalyst, even more preferably 0.10 parts by mass or more of polymerization catalyst, and particularly preferably 0.17 parts by mass or more of polymerization catalyst.

[0166] The range of the above-mentioned polymerization catalyst content can be appropriately changed according to the type of monomer used in optical materials and the type of polymerization catalyst.

[0167] For example, when the monomers for optical materials contain 2,5(6)-bis(isocyanate methyl)-bicyclo-[2.2.1]-heptane, pentaerythritol tetra(3-mercaptopropionate), and 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane, and the polymerization catalyst contains 3,5-dimethylpyridine, it is preferable to use 0.10 parts by mass or more of the polymerization catalyst, and more preferably 0.17 parts by mass or more of the polymerization catalyst, relative to 100 parts by mass of two or more different monomers for optical materials.

[0168] For example, when the monomers for optical materials include isophthalene diisocyanate, 5,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, and 4,8-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, and the polymerization catalyst includes 3,5-dimethylpyridine, it is preferable to use 0.015 parts by mass or more of the polymerization catalyst, and more preferably 0.020 parts by mass or more of the polymerization catalyst, relative to 100 parts by mass of two or more different monomers for optical materials.

[0169] For example, when the monomers for optical materials include isophthalene diisocyanate and 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane, and the polymerization catalyst includes 3,5-dimethylpyridine, it is preferable to use 0.010 parts by mass or more of the polymerization catalyst, and more preferably 0.015 parts by mass or more of the polymerization catalyst, relative to 100 parts by mass of two or more different monomers for optical materials.

[0170] For example, when the monomer for optical materials comprises dicyclohexylmethane diisocyanate, and a mixture of 5,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, and 4,8-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, and the polymerization catalyst comprises 3,5-dimethylpyridine, it is preferable to use 1.0 part by mass or more of the polymerization catalyst, and more preferably 1.5 part by mass or more of the polymerization catalyst, relative to 100 parts by mass of two or more different monomers for optical materials.

[0171] For example, when the monomers for optical materials contain 1,3-bis(isocyanate methyl)cyclohexane, pentaerythritol tetra(2-mercaptoacetate), and 2,5-bis(mercaptomethyl)-1,4-dithiacyclohexane, and the polymerization catalyst contains 3,5-dimethylpyridine, it is preferable to use 0.03 parts by mass or more of the polymerization catalyst, and more preferably 0.07 parts by mass or more of the polymerization catalyst, relative to 100 parts by mass of two or more different monomers for optical materials.

[0172] By using a polymerization catalyst that is 2.0 parts by mass or less relative to 100 parts by mass of monomers for two or more different optical materials, it is possible to improve, for example, the operability when injecting a polymeric composition of optical materials into a mold.

[0173] From the above perspective, it is preferable to use a polymerization catalyst of 1.5 parts by mass or less, relative to 100 parts by mass of monomers for two or more different optical materials.

[0174] In addition, depending on the type of monomer and polymerization catalyst used in optical materials, for 100 parts by mass of two or more different monomers used in optical materials, a polymerization catalyst of less than 1.0 parts by mass, less than 0.3 parts by mass, or less than 0.15 parts by mass can be used.

[0175] It should be noted that the amount of the polymerization catalyst can be appropriately set according to the type of polymerization catalyst, the type and amount of monomers used (isocyanate compounds, active hydrogen compounds, other components, etc.), and the desired shape of the molded body.

[0176] <Prepolymerization Process> The method for manufacturing an optical material according to the first embodiment includes: a prepolymerization step in which two or more different optical materials are mixed with a portion of a monomer and at least a portion of a polymerization catalyst, and the two or more different optical materials are polymerized with at least a portion of the monomer to obtain a prepolymer, thereby obtaining a mixture containing the prepolymer.

[0177] The inventors of this application believe that convection occurs due to uneven temperature distribution within the mold where the polymerization reaction takes place, which is one of the reasons for the formation of ripples in the resulting cured product.

[0178] Therefore, the inventors of this application have focused on manufacturing a prepolymer by prepolymerizing a portion of the monomers used in optical materials, and then including the prepolymer in the polymeric composition for optical materials to increase the viscosity of the polymeric composition for optical materials. This allows for the suppression of convection within the mold.

[0179] Furthermore, regarding the method for manufacturing optical materials according to the first embodiment, by preventing the self-heating from dissipating to the outside, it is possible to prevent the temperature difference between the inside and the outside of the mold from being generated.

[0180] Based on the above points, it can be inferred that the manufacturing method of the optical material in the first embodiment can suppress the ripples of the obtained cured material.

[0181] In the method for manufacturing optical materials according to the first embodiment, by including all of one of two or more different optical material monomers, a portion of other optical material monomers besides the aforementioned one, and all or a portion of the polymerization catalyst in the prepolymerization process, a prepolymer with excellent service life can be obtained.

[0182] There are no particular restrictions on the way it is used as "part of two or more different optical material monomers".

[0183] For example, "a portion of two or more different optical material monomers" can be a portion of each of two or more different optical material monomers.

[0184] In addition, "part of two or more different optical material monomers" can also refer to all of one or more optical material monomers among two or more different optical material monomers.

[0185] In the prepolymerization process, the polymerization catalyst can be used in part or all of its components.

[0186] When used as a part of a polymerization catalyst, there are no particular restrictions on the manner of using "part of a monomer for two or more different optical materials".

[0187] For example, "a portion of the polymerization catalyst" can be a portion of the amount of the polymerization catalyst.

[0188] When used as a part of the polymerization catalyst, from the viewpoint of ensuring a long service life, the part of the polymerization catalyst is preferably 5 to 80 parts by mass of 100 parts by mass of the polymerization catalyst, more preferably 10 to 60 parts by mass, and even more preferably 15 to 50 parts by mass.

[0189] From the viewpoint of ensuring a long service life, the portion of the monomers for two or more different optical materials is preferably 5 to 95 parts by mass out of 100 parts by mass of the monomers for two or more different optical materials, more preferably 20 to 80 parts by mass, and even more preferably 30 to 70 parts by mass.

[0190] The following are examples of specific methods of the prepolymerization process, but the prepolymerization process in the first embodiment is not limited to the following methods.

[0191] (Method a) The prepolymerization process of method a is as follows: mixing two or more different optical materials with a portion of the monomer and all of the polymerization catalyst, and polymerizing the two or more different optical materials with at least a portion of the monomer to obtain a prepolymer, thereby obtaining a mixture containing the prepolymer.

[0192] In method a, a portion of two or more different optical material monomers preferably consists of all of one of the two or more different optical material monomers and a portion of the other optical material monomers besides the one optical material monomer.

[0193] (Method b) The prepolymerization process of method b is as follows: mixing two or more different optical materials with a portion of monomer and a portion of polymerization catalyst, and polymerizing the two or more different optical materials with at least a portion of the monomer to obtain a prepolymer, thereby obtaining a mixture containing the prepolymer.

[0194] In the case that the method for manufacturing optical materials according to the first embodiment includes the prepolymerization step of method b, the manufacturing step of the polymeric composition for optical materials described later is the following step: adding at least two different monomers for optical materials and the remaining portion of the polymerization catalyst to a mixture containing the prepolymer, thereby obtaining a polymeric composition for optical materials containing two or more different monomers for optical materials, prepolymers, and polymerization catalysts.

[0195] In method b, preferably, two or more different optical material monomers contain isocyanate compound (A), a portion of the two or more different optical material monomers contains a portion of isocyanate compound (A), and the remaining portion of the two or more different optical material monomers contains the remaining portion of isocyanate compound (A).

[0196] <Viscosity Adjustment Process> For the manufacturing method of the optical material according to the first embodiment, it is preferable to include a viscosity adjustment step after the prepolymerization step and before the manufacturing step of the optical material with a polymeric composition, wherein the viscosity (hereinafter also referred to as viscosity) of the mixture containing the prepolymer, measured by a type B viscometer at 25°C and 60 rpm, is adjusted to 30 mPa·s to 2000 mPa·s.

[0197] By ensuring that the viscosity of the mixture containing the prepolymer is within the aforementioned range, from the viewpoint of suppressing ripples in the obtained optical material, it is possible to ensure that the viscosity of the polymeric composition for optical materials manufactured in the manufacturing process of the polymeric composition for optical materials is within an appropriate range. As a result, ripples in the obtained optical material can be suppressed.

[0198] From the above perspective, the viscosity of the mixture containing the prepolymer is preferably 40 mPa·s to 2000 mPa·s, more preferably 50 mPa·s to 1800 mPa·s.

[0199] It should be noted that the viscosity was measured using a type B viscometer at 25°C and 60 rpm (revolutions per minute).

[0200] There are no particular limitations on the method of adjusting the viscosity of mixtures containing prepolymers.

[0201] For example, the viscosity of a mixture containing prepolymers can be adjusted by methods such as heating or stirring.

[0202] The temperature used to prepare the mixture containing the prepolymer is not particularly limited, as long as it is a temperature at which the prepolymer can be obtained through the polymerization reaction. For example, it can be 20℃~50℃ or 25℃~45℃.

[0203] The stirring time used when preparing a mixture containing a prepolymer is not particularly limited, as long as it allows the prepolymer to be obtained through a polymerization reaction. For example, it can be 30 minutes to 5 hours, or 1 hour to 5 hours.

[0204] As a method for preparing a mixture containing a prepolymer, specifically, the following method can be used: the mixture containing a prepolymer is prepared by stirring at 40°C for 3 hours, thereby adjusting the viscosity.

[0205] <Manufacturing Process of Polymer Compositions for Optical Materials> The method for manufacturing an optical material according to the first embodiment includes a manufacturing step of a polymeric composition for optical materials, wherein at least two different monomers for optical materials are added to a mixture containing a prepolymer, thereby obtaining a polymeric composition for optical materials containing two or more different monomers for optical materials, a prepolymer, and a polymerization catalyst.

[0206] The manufacturing process of the polymeric composition for optical materials is as follows: adding the remainder of at least two different monomers for optical materials to a mixture containing a prepolymer, thereby obtaining a polymeric composition for optical materials containing two or more different monomers for optical materials, a prepolymer, and a polymerization catalyst.

[0207] Therefore, before mixing the mixture containing the prepolymer with the remaining portions of the two or more different optical material monomers, polymerization of the prepolymer with the remaining portions of the two or more different optical material monomers can be prevented.

[0208] Therefore, by performing the manufacturing process of the polymeric composition for optical materials at the appropriate time, it is possible to improve, for example, the operability when injecting the polymeric composition for optical materials into a mold.

[0209] In the manufacturing process of polymeric compositions for optical materials, when adding the remaining portions of at least two different monomers for optical materials to a mixture containing a prepolymer, the remaining portions of the two or more different monomers for optical materials may be mixed once or in multiple batches.

[0210] There are no particular limitations on the temperature at which the above-mentioned components are mixed, but it is preferably below 30°C, and more preferably below room temperature (25°C).

[0211] The temperature at which the components are mixed is sometimes preferably set to be lower than 25°C. However, if the additives such as internal release agents do not dissolve well in the components, the components may be preheated to dissolve the additives in the components.

[0212] Specific methods for manufacturing polymeric compositions for optical materials include, for example, the following.

[0213] First, an additive (such as an internal release agent) is added to the mixture containing the prepolymer to prepare a mixture. The mixture is stirred at 25°C for 1 hour to ensure that all components are completely dissolved, and then degassed to obtain the first mixture.

[0214] In addition, the remaining portion of the monomer for optical materials and the remaining portion of the desired polymerization catalyst are stirred at 25°C for 30 minutes to completely dissolve them, thus obtaining the second mixture.

[0215] Then, the first mixture and the second mixture are mixed, stirred, and degassed to obtain a polymeric composition for optical materials as a homogeneous solution.

[0216] <Liquid feeding process> In the method for manufacturing optical materials according to the first embodiment, after the manufacturing step of the polymeric composition for optical materials and before the curing step, a liquid feeding step of feeding the polymeric composition for optical materials into a casting mold may be included.

[0217] The liquid delivery process can be a process in which optical materials are mixed in a static mixer while being delivered to a casting mold.

[0218] The liquid delivery process can also be a process in which optical materials are mixed with a polymeric composition using a dynamic mixer while being delivered to a casting mold.

[0219] Therefore, it is possible to eliminate the non-uniformity of the distribution of the polymeric composition of optical material during the process of feeding the polymeric composition of optical material into the mold, thereby suppressing the ripples of the resulting cured product.

[0220] Polymer compositions for optical materials The polymeric composition for optical materials according to the first embodiment comprises two or more different optical material monomers, a polymerization catalyst, and a prepolymer obtained by polymerizing at least two of the two or more different optical material monomers. The content of the polymerization catalyst is 0.010 parts by mass to 2.0 parts by mass relative to a total of 100 parts by mass of the two or more different optical material monomers and the prepolymer.

[0221] Therefore, when the monomers of optical materials in the polymerizable composition for optical materials are polymerized, the heat of reaction of the polymerizable composition for optical materials (i.e., the heat generated due to self-heating) can be increased.

[0222] The above-mentioned reaction heating can be used to promote the polymerization reaction of the monomers for optical materials in the polymeric composition for optical materials, and high-quality optical materials in which ripples can be suppressed can be obtained in a shorter time than before.

[0223] Furthermore, the polymerizable composition for optical materials of the first embodiment, by having the above-described structure, is able to suppress convection within the mold in which the polymerization reaction takes place, and is able to suppress the generation of ripples in the resulting cured product.

[0224] In the polymeric composition for optical materials according to the first embodiment, the content of the polymerization catalyst is preferably 0.015 parts by mass or more, more preferably 0.038 parts by mass or more, further preferably 0.10 parts by mass or more, and particularly preferably 0.17 parts by mass or more, relative to a total of 100 parts by mass of two or more different optical material monomers and prepolymers.

[0225] In the polymeric composition for optical materials of the first embodiment, the content of the polymerization catalyst is preferably 1.5 parts by mass or less, more preferably 1.0 parts by mass or less, relative to a total of 100 parts by mass of two or more different optical material monomers and prepolymers.

[0226] For the polymeric composition for optical materials according to the first embodiment, from the viewpoint of suppressing ripples, the viscosity (hereinafter referred to as viscosity) measured by a type B viscometer at 25°C and 60 rpm is preferably 70 mPa·s or more, more preferably 80 mPa·s or more, further preferably 100 mPa·s or more, and particularly preferably 120 mPa·s or more.

[0227] For the polymeric composition for optical materials of the first embodiment, from the viewpoint of maintaining operability when molding the optical material into the desired shape, the viscosity is preferably 1000 mPa·s or less, more preferably 700 mPa·s or less, and even more preferably 400 mPa·s or less.

[0228] It should be noted that the viscosity measurement method is as described above.

[0229] (Other additives) The polymeric composition for optical materials according to the first embodiment may contain any additives.

[0230] Examples of any additive include photochromic compounds, internal mold release agents, bluing agents, and ultraviolet absorbers.

[0231] (Photochromic compounds) Photochromic compounds are compounds whose molecular structure changes reversibly when exposed to light of a specific wavelength, and whose light absorption properties (absorption spectra) change accordingly.

[0232] Examples of photochromic compounds used in the first embodiment include compounds whose absorption characteristics (absorption spectra) change with respect to a specific wavelength of light.

[0233] In the first embodiment, there are no particular limitations on the photochromic compound, and any photochromic compound can be suitably selected from conventionally known compounds that can be used in photochromic lenses. For example, one or more of spiropyran compounds, spiroxazine compounds, fumonisin anhydride compounds, naphthopyran compounds, and diimidazole compounds can be used depending on the desired coloring.

[0234] Examples of photochromic compounds in the first embodiment include Vivimed's Reversacol Humber Blue (polydimethylsiloxane chain, naphthopyran chromophore), Reversacol Calder Blue (polydimethylsiloxane chain, naphthopyran chromophore), Reversacol Trent Blue (polydimethylsiloxane chain, naphthopyran chromophore), Reversacol Pennine Green (polydimethylsiloxane chain, naphthopyran chromophore), Reversacol Heath Green (polyoxyalkylene chain, naphthopyran chromophore), Reversacol Chilli Red (polydimethylsiloxane chain, naphthopyran chromophore), Reversacol Wembley Grey (polyoxyalkylene chain, naphthopyran chromophore), Reversacol Cayenne Red (polyoxyalkylene chain, naphthopyran chromophore), Peacock Blue (polyoxyalkylene chain, naphthopyran chromophore), and Jalapeno. Red (polyoxyalkylene chain, naphthopyran chromophore), etc., can be used in one or in combination of two or more.

[0235] Acidic phosphate esters can be used as internal mold release agents. Examples of acidic phosphate esters include monophosphate esters and diphosphate esters, and two or more can be used individually or in combination.

[0236] It should be noted that when using highly polymerizable optical material monomers, it is preferable to use an internal mold release agent with relatively low mold release properties. Examples of highly polymerizable optical material monomers include isocyanate compounds with aromatic rings and trifunctional polythiol compounds (specifically, 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane, etc.). These highly polymerizable optical material monomers are prone to peeling off from the mold earlier than intended (e.g., during the polymerization of optical material monomers) (also known as early release). Therefore, when using highly polymerizable optical material monomers, the occurrence of such early release can be suppressed by using an internal mold release agent with relatively low mold release properties.

[0237] As an internal release agent with relatively low release properties, an acidic phosphate ester with relatively low release properties is preferred, and more particularly, JP-506H (manufactured by Jōhoku Chemical Industry Co., Ltd.) is preferred.

[0238] In addition, from the viewpoint of suppressing premature release, it is also preferable to reduce the release properties of the monomers used in optical materials by adjusting the amount of internal release agent added.

[0239] Specifically, from the viewpoint of suppressing premature release, the content of the internal release agent is preferably below 1000 ppm by mass.

[0240] Furthermore, there is no particular limitation on the timing of adding the internal release agent to mixtures containing prepolymers, polymeric compositions for optical materials, etc.

[0241] The internal release agent can be added during the prepolymerization process, or it can be added to the mixture containing the prepolymer after the prepolymerization process, or it can be added to the remaining portion of two or more different optical material monomers added to the mixture containing the prepolymer.

[0242] When using internal release agents such as acidic phosphate esters that may form salts with the polymerization catalyst, the catalytic activity of the polymerization catalyst may decrease and the reaction time may become longer due to the formation of such salts.

[0243] Therefore, from the viewpoint of suppressing the prolongation of polymerization reaction time in the prepolymerization process, it is preferable not to add an internal release agent during the polymerization reaction stage in the prepolymerization process.

[0244] From the viewpoint of shortening the polymerization reaction time in the prepolymerization process, the internal release agent is preferably added to the mixture containing the prepolymer in a stable state after the polymerization reaction has proceeded to a certain extent, or to the remaining portion of two or more different monomers for optical materials.

[0245] Furthermore, from the viewpoint of improving the stability of the prepolymer (e.g., increasing its pot life), in order to suppress the activity of the polymerization catalyst in the mixture containing the prepolymer, the internal release agent is preferably added to the mixture containing the prepolymer when the polymerization reaction in the prepolymerization process is stable to a certain extent or at a time when it is desired to stabilize it.

[0246] Examples of bluing agents include substances that have absorption bands in the orange to yellow wavelength region of the visible light spectrum and that function to adjust the hue of optical materials formed from resins. More specifically, bluing agents include substances that exhibit a blue to violet hue.

[0247] Examples of usable ultraviolet absorbers include benzophenone-based ultraviolet absorbers such as 2,2'-dihydroxy-4-methoxybenzophenone, 2-hydroxy-4-acryloyloxybenzophenone, 2-hydroxy-4-acryloyloxy-5-tert-butylbenzophenone, and 2-hydroxy-4-acryloyloxy-2',4'-dichlorobenzophenone. 2-[4-[(2-hydroxy-3-dodecyloxypropyl)oxy]-2-hydroxyphenyl]4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-[4-(2-hydroxy-3-tetrazyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-[4-[(2-hydroxy-3-(2'-ethyl)hexyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-[4-[(2-hydroxy-3-(2'-ethyl)hexyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine]-2-hydroxyphenyl]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine]-2-[4-[(2-hydroxy-3-(2'-ethyl)hexyl)oxy]-2-hydroxyphenyl ... Triazine-based ultraviolet absorbers include [2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2,4-bis(2-hydroxy-4-butyloxyphenyl)-6-(2,4-bis-butyloxyphenyl)-1,3,5-triazine, and 2-(2-hydroxy-4-[1-octyloxycarbonylethoxy]phenyl)-4,6-bis(4-phenylphenyl)-1,3,5-triazine. 2-(2H-benzotriazol-2-yl)-4-methylphenol, 2-(2H-benzotriazol-2-yl)-4-tert-octylphenol, 2-(2H-benzotriazol-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol, 2-(2H-benzotriazol-2-yl)-4,6-di-tert-pentylphenol, 2-(5-chloro-2H-benzotriazol-2-yl)-4-methyl-6-tert-butylphenol, 2-(5-chloro-2H- Benzotriazole-based ultraviolet absorbers include benzotriazole-2-yl)-2,4-tert-butylphenol and 2,2'-methylenebis[6-(2H-benzotriazole-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol], with preferred examples being benzotriazole-based ultraviolet absorbers such as 2-(2H-benzotriazole-2-yl)-4-tert-octylphenol and 2-(5-chloro-2H-benzotriazole-2-yl)-4-methyl-6-tert-butylphenol. These ultraviolet absorbers can be used alone or in combination of two or more.

[0248] <Curing Process> The method for manufacturing an optical material according to the first embodiment includes a curing step in which two or more different optical material monomers in a polymeric composition for optical materials are cured to obtain an optical material as a cured product of the polymeric composition for optical materials.

[0249] The method for manufacturing an optical material according to the first embodiment includes a curing step, thereby enabling the optical material to be polymerized with a polymeric composition to obtain a cured product, which can be used as an optical material.

[0250] Conventionally, during polymerization, the polymerizable composition for optical materials is heated to induce polymerization. However, for the polymerizable composition for optical materials in the first embodiment, the polymerization reaction of the monomers for optical materials in the polymerizable composition for optical materials can be promoted by increasing the heat of reaction associated with the polymerization reaction (i.e., heat generated due to self-heating).

[0251] In the method for manufacturing optical materials according to the first embodiment, the polymeric composition for optical materials can be heated, but from the above viewpoint, it is also possible not to heat the polymeric composition for optical materials.

[0252] That is, in the curing process of the first embodiment, the polymeric composition for optical materials can be left to stand, thereby allowing the polymeric composition for optical materials to be cured by polymerization.

[0253] As described above, the curing process may include a process of curing the optical material with the polymeric composition by allowing the optical material to stand in a polymeric composition.

[0254] In addition, from the viewpoint of curing, the optical material can be placed in a closed space or in an open space during the curing process, but it is preferred to place it in a closed space.

[0255] An enclosed space is an environment that retains heat internally and inhibits heat conduction between the interior and exterior. An environment that inhibits heat conduction between the interior and exterior is one where, when an optical material polymeric composition is placed statically within an enclosed space, the heat conduction between the interior and exterior of the enclosed space is sufficient to allow the optical material polymeric composition to cure.

[0256] As an enclosed space, an example is an insulated environment.

[0257] Open space refers to the space outside of enclosed spaces.

[0258] The curing process preferably includes a process of curing the optical material with the polymeric composition by placing the optical material in a closed space.

[0259] By placing the polymeric composition of the optical material in a closed space, heat generated by the self-heating of the polymeric composition can be prevented from being released to the outside. This allows the heat generated by self-heating to be retained within the closed space, thus promoting the polymerization reaction more efficiently and enabling the manufacture of optical materials in a shorter time.

[0260] In the "heat insulation" or "heat insulation environment" of the first embodiment, it is preferable to perform heating to make the heat insulation reaction tank a constant temperature state (constant temperature reaction tank) within a range that does not hinder the polymerization reaction based on the heat of reaction of the polymeric composition for optical materials, or excessively promote the polymerization reaction of the polymeric composition for optical materials due to external heating.

[0261] Therefore, based on the heating state formed by the self-heating of the monomers through optical materials, the ambient temperature in the reaction tank (constant temperature reaction tank) where the mold is placed can be kept at a constant temperature or a heat-preserving state, thus promoting the polymerization reaction more effectively.

[0262] As an insulated environment, an insulated reaction tank or a constant temperature reaction tank, such as the one described above, can be used.

[0263] For example, when a mold containing monomers is placed in a vacuum container that serves as an insulated reaction tank, insulated polymerization in an insulated environment using an insulated reaction tank (constant temperature reaction tank) can be carried out through the following steps.

[0264] The inner surface of the vacuum container is covered with heat-insulating or heat-preserving components such as polyurethane foam and cork, and the mold containing monomers is wrapped with components such as cloth as needed. Then, the mold containing monomers is placed in the vacuum container to stand.

[0265] The curing process may include a process of curing the optical material with the polymeric composition by allowing the optical material to stand without external heating (i.e., a non-heating process).

[0266] As described above, in the method for manufacturing optical materials according to the first embodiment, the polymeric composition of the optical material may be heated, but it is not necessary to heat the polymeric composition of the optical material.

[0267] In order to heat from the outside, a device is sometimes used, which sometimes increases the economic burden. If it is the optical material manufacturing method of the first embodiment, the optical material can be manufactured in a simple way, thus reducing the economic burden.

[0268] The curing process preferably includes a process of curing the optical material with the polymeric composition by letting the optical material stand for 2 to 10 hours.

[0269] According to conventional methods, polymerization typically occurs by slowly heating the material while the temperature is gradually increased over several hours to tens of hours (e.g., about 20 to 48 hours).

[0270] If the polymerization reaction time is short, the polymeric composition for optical materials will not be completely cured, and therefore, optical materials cannot be obtained, or the quality of the optical materials will be reduced.

[0271] However, the method for manufacturing optical materials according to the first embodiment can suppress ripples in the obtained optical material and manufacture the optical material in a short time. Specifically, the optical material can be manufactured by letting the optical material stand with a polymeric composition for 10 hours or less.

[0272] From the above perspective, in the curing process, it is more preferable to let the optical material be left to stand for 8 hours or less with the polymeric composition.

[0273] Furthermore, from the viewpoint of obtaining well-cured optical materials through polymerization, it is preferable to let the optical materials stand for 2 hours or more with the polymeric composition.

[0274] In the curing process, a microwave irradiation process can also be set up to irradiate the polymeric composition of the optical material with microwaves for a specified time, as needed.

[0275] As a method of curing process, examples include the following steps a and b.

[0276] Process a: Inject (cast) the optical material into the mold (mold cavity) using a polymeric composition.

[0277] Step b: The mold containing the polymeric composition for optical materials is left to stand for a specified time to allow it to cure.

[0278] (Process a) First, a polymeric composition is injected into a molding die (mold) held in place by a gasket or tape. Then, depending on the required properties of the resulting optical material, degassing under reduced pressure, filtration under increased pressure, or filtration under reduced pressure are preferably performed as needed.

[0279] (Process b) As described above, in step b, the mold containing the polymerizable composition of the optical material can be polymerized by standing in an open space for a specified time, or it can be polymerized by standing in a closed space under heat insulation.

[0280] There are no limitations on the polymerization conditions, but they are preferably adjusted appropriately according to the composition of the polymerizable composition for optical materials, the type and amount of catalyst used, the shape of the mold, etc.

[0281] Alternatively, the mold containing the polymeric composition of the optical material can be left to stand in an insulated environment for 2 to 4 hours to carry out polymerization.

[0282] In step b, if necessary, a heating step can be added after the heat-insulated polymerization process in which the mold containing the polymeric composition of optical material is placed in a heat-insulated environment for a certain period of time.

[0283] In step b, as needed, the mold containing the polymeric composition for optical materials may be heated continuously or intermittently at a temperature not exceeding the self-heating temperature emitted by the polymeric composition for optical materials during the heat insulation polymerization process, in parallel with the step of placing the mold containing the polymeric composition for optical materials in a heat-insulated environment (heat insulation polymerization). Alternatively, the heat insulation reaction tank may be heated to maintain the ambient temperature within the heat insulation reaction tank.

[0284] The curing process may include the process of heating an optical material with a polymeric composition to cure it (i.e., the heating process).

[0285] As described above, in the method for manufacturing optical materials according to the first embodiment, it is not necessary to heat the optical material with the polymeric composition, but the curing process may include the heating process described above.

[0286] That is, the curing process in the first embodiment can combine a non-heating process with a heating process.

[0287] When the curing process includes a heating process, the heating process is preferably carried out for 1% to 40% of the total curing period, and more preferably for 1% to 35% of the total curing period.

[0288] <Second Prepolymerization Process> The method for manufacturing the optical material according to the first embodiment may include the following steps in addition to the preparation and prepolymerization steps described above: In the second prepolymerization step, the remaining portions of the monomers of the two or more different optical materials mentioned above and the remaining portions of the polymerization catalyst mentioned above are mixed, and at least a portion of the remaining portions of the monomers of the two or more different optical materials mentioned above are polymerized to obtain the second prepolymer, thereby obtaining a mixture containing the aforementioned second prepolymer. A manufacturing process for a polymerizable composition for optical materials involves adding a mixture containing the aforementioned second prepolymer to a mixture containing the aforementioned prepolymer, thereby obtaining a polymerizable composition for optical materials containing the aforementioned prepolymer, the aforementioned second prepolymer, and the aforementioned polymerization catalyst; and The curing process cures the aforementioned prepolymer and the aforementioned second prepolymer in the aforementioned polymeric composition for optical materials, thereby obtaining an optical material as a cured product of the aforementioned polymeric composition for optical materials.

[0289] The optical material manufacturing method of the first embodiment, by including the above-described structure, is able to obtain a mixture containing a prepolymer obtained by the prepolymerization process and a mixture containing a second prepolymer obtained by the second prepolymerization process.

[0290] Therefore, the viscosity of the mixture containing the prepolymer can be made similar to that of the mixture containing the second prepolymer, thus making it easier to mix the two.

[0291] In the second prepolymerization process, the monomers, polymerization catalysts, specific methods, and preferred methods used for two or more different optical materials are the same as those used for two or more different optical materials in the prepolymerization process.

[0292] In the case where the optical material manufacturing method of the first embodiment includes a second prepolymerization step, the manufacturing step of the polymeric composition for optical materials is as follows: adding a mixture containing the aforementioned second prepolymer to a mixture containing the aforementioned prepolymer, thereby obtaining a polymeric composition for optical materials containing the aforementioned prepolymer, the aforementioned second prepolymer, and the aforementioned polymerization catalyst.

[0293] The manufacturing process of the polymeric composition for optical materials described above includes the same mixture of prepolymers, specific methods, preferred methods, etc. as those in the above-mentioned <Manufacturing Process of Polymeric Composition for Optical Materials>.

[0294] In the case where the optical material manufacturing method of the first embodiment includes a second prepolymerization step, the curing step is as follows: the aforementioned prepolymer and the aforementioned second prepolymer in the aforementioned polymeric composition for optical materials are cured to obtain an optical material as a cured product of the aforementioned polymeric composition for optical materials.

[0295] In the above curing process, the prepolymer, specific method, preferred method, etc. are the same as those in the above-mentioned curing process.

[0296] Annealing process As needed, the method for manufacturing the optical material according to the first embodiment may include an annealing step of annealing the cured optical material with a polymeric composition.

[0297] The annealing temperature is typically between 50 and 150°C, but preferably between 90 and 140°C, and more preferably between 100 and 130°C.

[0298] <Optical Materials> The optical material in the first embodiment is a cured product of a polymeric composition for optical materials.

[0299] The optical material in the first embodiment is a high-quality optical material that suppresses ridges.

[0300] Generally, the thicker the optical material, the more likely it is to produce ridges.

[0301] The optical material manufactured using the optical material manufacturing method of the first embodiment can effectively suppress ripples even when it is relatively thick.

[0302] For example, the thickness of the optical material in the first embodiment can be 1 mm to 20 mm, or 4 mm to 16 mm.

[0303] Applications of Optical Materials The optical material in the first embodiment can be used in plastic lenses, prisms, optical fibers, information recording substrates, filters, light-emitting diodes, etc.

[0304] Of the above, the optical material in the first embodiment can be suitably used for plastic lenses, and is more suitable for plastic lenses for eyeglasses.

[0305] [Second Implementation] Manufacturing Methods of Optical Materials The method for manufacturing an optical material according to the second embodiment is a method for manufacturing an optical material using a polymeric composition for optical materials containing two or more different optical material monomers and a polymerization catalyst. The method includes the following steps: a raw material composition preparation step, preparing a first raw material composition and a second raw material composition; a shearing step, applying shear force to the first raw material composition and the second raw material composition to manufacture the aforementioned polymeric composition for optical materials; a stirring step, applying a stirring force to the aforementioned polymeric composition for optical materials; a casting step, casting the aforementioned polymeric composition for optical materials into a mold after the stirring step; and a curing step, polymerizing the two or more different optical material monomers in the aforementioned polymeric composition for optical materials in the mold, thereby curing the aforementioned polymeric composition for optical materials.

[0306] The term "applying shear force to the first raw material composition and the second raw material composition" means that while the first raw material composition and the second raw material composition are flowing, a force is applied to the first raw material composition and the second raw material composition mainly in a direction intersecting with the flow direction.

[0307] The term "applying a stirring force to the polymeric composition for optical materials" means: while allowing the polymeric composition for optical materials to flow, applying a force to the polymeric composition for optical materials in a generally parallel and opposite direction to the flow direction (i.e., the direction from the inlet to the outlet on the virtual line connecting the part of the aforementioned composition entering the process of applying the stirring force (inlet) and the part exiting (outlet); or stopping the flow and stirring the aforementioned polymeric composition for optical materials.

[0308] The method for manufacturing optical materials according to the second embodiment includes the steps described above, thereby suppressing U-shaped ridges in the obtained optical materials.

[0309] U-shaped corrugations are easily formed after a certain period of time following the casting of optical materials into a mold using a polymeric composition.

[0310] The inventors of this application, from the viewpoint of suppressing U-shaped ripples, focused on the process of shearing and stirring the first raw material composition and the second raw material composition.

[0311] Furthermore, the methods and order of shearing and stirring were further studied, and it was found that by making the optical material manufacturing method of the second embodiment include the above-described shearing process and the above-described stirring process, the U-shaped ridges in the obtained optical material can be suppressed.

[0312] The reason can be inferred as follows.

[0313] It is believed that by simultaneously flowing the first and second raw material compositions and applying force to them in a direction intersecting the flow direction, the first and second raw material compositions are sheared and oriented. By simultaneously flowing the obtained polymeric composition for optical materials and applying force to it in a direction substantially parallel and opposite to the flow direction, it is possible to homogenize the concentration unevenness before and after the flow direction, and to mitigate or homogenize the aforementioned orientation. As a result, it is believed that U-shaped ripples can be suppressed.

[0314] The polymeric composition for optical materials in the second embodiment contains two or more different monomers for optical materials and a polymerization catalyst.

[0315] In addition, the polymeric composition for optical materials is manufactured by applying shear force to the first raw material composition and the second raw material composition.

[0316] Therefore, the first raw material composition and the second raw material composition, as a whole combining the first raw material composition and the second raw material composition, contain two or more different monomers for optical materials and polymerization catalysts.

[0317] For example, the first raw material composition and the second raw material composition may each contain different types of monomers for optical materials, and at least one of the first raw material composition and the second raw material composition may contain the form of a polymerization catalyst (see, for example, the Example Items).

[0318] In the second embodiment, preferably at least one of the aforementioned first raw material composition and the aforementioned second raw material composition contains the mixture containing the prepolymer in the first embodiment.

[0319] More specifically, the method for manufacturing the optical material according to the second embodiment is preferably a method for manufacturing the optical material using a polymerizable composition for optical materials containing two or more different monomers for optical materials and a polymerization catalyst, which includes the following steps: The raw material composition preparation process includes preparing the first raw material composition and the second raw material composition; The shearing process applies shear force to the aforementioned first raw material composition and the aforementioned second raw material composition to manufacture the aforementioned polymeric composition for optical materials; The stirring process involves applying a stirring force to the aforementioned polymeric composition for optical materials; The casting process involves casting the aforementioned optical material into a mold using a polymeric composition after the aforementioned mixing process; and The curing process involves polymerizing the aforementioned optical material in the aforementioned mold with monomers from two or more different optical materials in the polymeric composition, thereby curing the aforementioned optical material with the polymeric composition. At least one of the aforementioned first raw material composition and the aforementioned second raw material composition contains the mixture containing the prepolymer in the first embodiment.

[0320] <Preparation Process of Raw Material Composition> The raw material composition preparation process is the process of preparing the first raw material composition and the second raw material composition.

[0321] In the raw material composition preparation process, the first raw material composition and the second raw material composition can be used as a whole to contain two or more different monomers for optical materials and polymerization catalysts, without any particular restrictions.

[0322] The first and second raw material compositions can each be ready-made products, or they can be prepared by mixing optical materials with monomers and polymerization catalysts.

[0323] There are no particular restrictions on the above-mentioned hybrid methods; any known methods can be used.

[0324] There are no particular limitations on the temperature at which the above-mentioned components are mixed, but it is preferably below 30°C, and more preferably below room temperature (25°C).

[0325] From the viewpoint of the pot life of the prepared polymeric composition for optical materials, it is sometimes preferable to set a temperature lower than 25°C. However, in cases where additives such as internal release agents have poor solubility with the aforementioned components, the aforementioned components may be preheated to dissolve the additives in the aforementioned components.

[0326] When mixing the above components, it is preferable to do so under a dry, inactive gas to prevent moisture from being introduced into the polymeric composition for optical materials.

[0327] In the raw material composition preparation process, after the polymerization catalyst is mixed in a portion of two or more different optical material monomers, the remaining portions of the two or more different optical material monomers can be mixed once or in multiple batches.

[0328] Specific methods for preparing the raw material composition can be exemplified by the following.

[0329] First, a portion of the monomer for optical materials and an additive (such as an internal release agent) are added to prepare a mixture. The mixture is stirred at 25°C for 1 hour to ensure complete dissolution of all components. Then, a portion of the remaining monomer for optical materials is added, and the mixture is stirred to form a homogeneous solution. The solution is then degassed to obtain the first raw material composition.

[0330] Then, the remaining portion of the monomer for the optical material and the catalyst were stirred at 25°C for 30 minutes to completely dissolve them, forming a homogeneous solution. The solution was then degassed to obtain the second raw material composition.

[0331] <Cutting Process> The shearing process is a process of manufacturing a polymeric composition for optical materials by applying shear force to the first raw material composition and the second raw material composition.

[0332] In the second embodiment, the force applied along the direction intersecting the flow direction is also referred to as shear force.

[0333] In the second embodiment, the force is also applied mainly along the direction intersecting the flow direction, which is referred to as "shear".

[0334] The term "to make...flow" can refer to, for example, the flow of a composition by performing actions such as feeding the composition from a tank to a power mixer or feeding the composition from a power mixer to a mixing tank.

[0335] From the viewpoint of suppressing the increase in viscosity of the polymeric composition for optical materials and improving productivity during shearing, the flow rates of the first raw material composition and the second raw material composition are preferably 3 g / s or more, more preferably 6 g / s or more, and even more preferably 9 g / s or more.

[0336] When shearing, from the viewpoint of suppressing U-shaped ripples in the polymeric composition for optical materials, the flow rates of the first raw material composition and the second raw material composition are preferably 50 g / s or less, more preferably 45 g / s or less, and even more preferably 40 g / s or less.

[0337] There are no particular limitations on the method of applying force to the first and second raw material compositions in a direction intersecting the flow direction. For example, a method using a powered mixer can be cited as an example of the above method.

[0338] The rotational speed in the shearing process is preferably 200 rpm or more, more preferably 400 rpm or more, and even more preferably 500 rpm or more.

[0339] The rotational speed in the shearing process is preferably 3000 rpm or less, more preferably 2500 rpm or less, and even more preferably 2000 rpm or less.

[0340] Polymer compositions for optical materials The polymeric composition for optical materials is manufactured by applying shear force to a first raw material composition and a second raw material composition.

[0341] The polymeric composition for optical materials contains two or more different monomers for optical materials and a polymerization catalyst.

[0342] (Single for optical materials) The details of specific examples, preferred methods, preferred contents, etc. of the optical material monomer in the second embodiment are the same as those of the specific examples, preferred methods, preferred contents, etc. of the optical material monomer in the first embodiment.

[0343] [Isocyanate compound (A)] The details of specific examples, preferred methods, preferred content, definitions, etc. of the isocyanate compound (A) in the second embodiment are the same as those of the specific examples, preferred methods, preferred content, definitions, etc. of the isocyanate compound (A) in the first embodiment.

[0344] [Active hydrogen compounds] The details of specific examples, preferred methods, preferred contents, etc. of the active hydrogen compound in the second embodiment are the same as those of the specific examples, preferred methods, preferred contents, etc. of the active hydrogen compound in the first embodiment.

[0345] (Polythiol compounds with two or more thiol groups) The details of specific examples, preferred methods, preferred contents, etc. of the polythiol compounds having two or more thiol groups in the second embodiment are the same as those of the polythiol compounds having two or more thiol groups in the first embodiment.

[0346] (Hydroxythiol compounds having one or more thiol groups and one or more hydroxyl groups) The details of specific examples, preferred methods, preferred contents, etc. of the hydroxythiol compound having one or more thiol groups and one or more hydroxyl groups in the second embodiment are the same as those of the specific examples, preferred methods, preferred contents, etc. of the hydroxythiol compound having one or more thiol groups and one or more hydroxyl groups in the first embodiment.

[0347] (Polyol compounds with two or more hydroxyl groups) The details of specific examples, preferred methods, preferred contents, etc. of the polyol compounds having two or more hydroxyl groups in the second embodiment are the same as those of the specific examples, preferred methods, preferred contents, etc. of the polyol compounds having two or more hydroxyl groups in the first embodiment.

[0348] (Amine compounds) The details of specific examples, preferred methods, preferred content, (NCO group / (OH group + SH group)), viscosity Va, viscosity difference V, etc. of the amine compound in the second embodiment are the same as those of the specific examples, preferred methods, preferred content, (NCO group / (OH group + SH group)), viscosity Va, viscosity difference V, etc. of the amine compound in the first embodiment.

[0349] <Polymerization Catalyst> The details of the specific examples, preferred methods, preferred contents, etc. of the polymerization catalyst in the second embodiment are the same as those of the specific examples, preferred methods, preferred contents, etc. of the polymerization catalyst in the first embodiment.

[0350] (Alkaline catalyst) The details of specific examples, preferred methods, preferred pKa, etc. of the alkaline catalyst in the second embodiment are the same as those of the specific examples, preferred methods, preferred pKa, etc. of the alkaline catalyst in the first embodiment.

[0351] (Organometallic catalysts) The details of specific examples and preferred embodiments of the organometallic catalyst in the second embodiment are the same as those of the specific examples and preferred embodiments of the organometallic catalyst in the first embodiment.

[0352] The polymerization catalyst preferably satisfies the following condition 1.

[0353] [Condition 1] -Ea / R is above -7100 and below -2900.

[0354] (Ea is the activation energy calculated from the Arrhenius curve of the reaction rate constants of the aforementioned two or more different optical materials at two or more different temperatures using monomers; R is the gas constant (8.314 J / mol / K).) By ensuring that the polymerization catalyst meets condition 1, deviations in the polymerization rate can be suppressed during the polymerization and curing process of the polymerizable composition. As a result, optical strain and the generation of ridges are suppressed, and optical materials with excellent appearance can be obtained.

[0355] The value of Ea is calculated using the following method.

[0356] The value of Ea can be calculated by performing the following steps: In the property acquisition process, a composition 1 containing a polymerization reactive compound and a specified amount of polymerization catalyst is heated to obtain property values ​​1a of the functional groups of the polymerization reactive compound before heating and property values ​​1b of the residual functional groups after heating for a specified time, under conditions of holding at various temperatures. The residual functional group ratio calculation process calculates the residual functional group ratio 1 at various temperatures mentioned above from the physical property value 1a and physical property value 1b. The reaction rate constant calculation process involves calculating the reaction rate constant 1 at various aforementioned temperatures based on the residual functional group ratio 1 and the reaction rate formula; and The fitting process involves calculating the activation energy Ea1 and the frequency factor A1 from the reaction rate constant 1 at various aforementioned temperatures using an Arrhenius curve.

[0357] Use the calculated Ea to determine whether the polymerization catalyst satisfies condition 1.

[0358] The specific methods for calculating the value of Ea and for determining whether the polymerization catalyst meets condition 1 are the same as those described in International Publication No. 2020 / 256057.

[0359] <Mixing Process> The stirring process is the process of applying a stirring force to the aforementioned polymeric composition for optical materials.

[0360] In the second embodiment, the force applied in a direction that is approximately parallel to and opposite to the flow direction is also referred to as the stirring force.

[0361] When a force is applied in a direction that is substantially parallel to and opposite to the flow direction, the preferred range of the flow rate of the polymeric composition for optical materials is the same as the preferred range of the flow rate of the polymeric composition for optical materials in the above-described <shearing process>.

[0362] There are no particular limitations on the method of applying force to the polymeric composition of the optical material in a direction that is generally parallel to and opposite to the flow direction. For example, a method using a stirred tank containing a stir bar can be cited as an example of the above method.

[0363] The rotation speed in the stirring process is preferably 50 rpm or more, more preferably 100 rpm or more, and even more preferably 200 rpm or more.

[0364] The rotation speed during the stirring process is preferably 800 rpm or less, more preferably 700 rpm or less, and even more preferably 600 rpm or less.

[0365] The method for manufacturing optical materials according to the second embodiment includes a shearing process and a stirring process, thereby enabling the continuous production of a uniform polymeric composition for optical materials from the viewpoint of suppressing U-shaped ripples in the obtained optical materials.

[0366] From the viewpoint of suppressing U-shaped ridges in the obtained optical material, the manufacturing method of the optical material in the second embodiment preferably includes a shearing step and a stirring step in sequence.

[0367] That is, the method for manufacturing the optical material according to the second embodiment is preferably a method for manufacturing the optical material using a polymerizable composition for optical materials containing two or more different optical material monomers and a polymerization catalyst, which sequentially includes the following steps: a raw material composition preparation step, preparing a first raw material composition and a second raw material composition; a shearing step, applying shear force to the first raw material composition and the second raw material composition to manufacture the aforementioned polymerizable composition for optical materials; a stirring step, applying a stirring force to the aforementioned polymerizable composition for optical materials; a casting step, casting the aforementioned polymerizable composition for optical materials into a mold after the aforementioned stirring step; and a curing step, polymerizing the aforementioned two or more different optical material monomers in the aforementioned polymerizable composition for optical materials in the aforementioned mold, thereby curing the aforementioned polymerizable composition for optical materials.

[0368] <Filtration Process> The method for manufacturing optical materials according to the second embodiment may include a filtration step of further filtering the optical material with a polymeric composition.

[0369] The filtration process can be performed using a filter.

[0370] As a filter, a capsule filter, for example, can be used.

[0371] The preferred filtration accuracy for a filter is 1.0 μm to 4.5 μm.

[0372] <Second mixing process> The method for manufacturing optical materials according to the second embodiment may include, in addition to the steps described above, a second stirring step in which the polymeric composition of the optical material is further stirred.

[0373] The second stirring step is a step other than the shearing and stirring steps described above, used to further stir the polymeric composition for optical materials.

[0374] When a second mixing step is performed, the mixing step described in the above-mentioned <mixing step> is also called the first mixing step.

[0375] In the second stirring step, as a method for stirring the polymeric composition for optical materials, one example is using a static mixer.

[0376] When using a static mixer, the inner diameter of the static mixer Preferably, it is 5 to 8, and more preferably 6 to 8.

[0377] When using a static mixer, the number of elements in the static mixer is preferably 16 to 48, more preferably 24 to 48.

[0378] <Casting Process> The casting process is the process of casting the aforementioned optical material into a mold using a polymeric composition after the first or second mixing process.

[0379] The viscosity of the aforementioned polymeric composition for optical materials used in the casting process, measured by a Type B viscometer at 25°C and 60 rpm, is preferably 10 mPa·s to 1000 mPa·s.

[0380] The preferred casting process is to adjust the viscosity of the aforementioned polymeric composition for optical materials, measured using a type B viscometer at 25°C and 60 rpm, to 10 mPa·s to 1000 mPa·s and then cast it into a mold.

[0381] By adjusting the viscosity of the polymeric composition for optical materials to the above-mentioned range and then casting it, the viscosity of the polymeric composition for optical materials can be kept within an appropriate range, thereby suppressing ripples in the resulting optical material.

[0382] From the above perspective, the viscosity of the polymeric composition for optical materials in the casting process is preferably 10 mPa·s or more, more preferably 40 mPa·s or more, even more preferably 70 mPa·s or more, particularly preferably 80 mPa·s or more, even more preferably 100 mPa·s or more, and even more preferably 120 mPa·s or more.

[0383] From the viewpoint of maintaining operability when molding optical materials into the desired shape, the viscosity of the polymeric composition for optical materials in the casting process is preferably 1000 mPa·s or less, more preferably 700 mPa·s or less, and even more preferably 400 mPa·s or less.

[0384] There are no particular limitations on the method for adjusting the viscosity of polymeric compositions used in optical materials.

[0385] For example, the viscosity of polymeric compositions for optical materials can be adjusted by adding high-viscosity compounds, heating, stirring, etc.

[0386] The casting process can also be a process of casting optical materials into a mold using a multi-axis method with a polymeric composition. Alternatively, it can be a process of casting optical materials into a mold using a pre-casting mixing method with a polymeric composition.

[0387] In the casting process, the casting method can be manual casting or mechanical automatic casting.

[0388] Automatic casting methods can be either nitrogen-based pressure delivery or pump-based liquid delivery (diaphragm pumps, gear pumps, etc.).

[0389] In the casting process, it is preferable to use nitrogen or the like to apply pressure (e.g., back pressure) to the polymeric composition for optical materials, thereby casting the polymeric composition for optical materials into a mold.

[0390] Therefore, it is even more preferable to use a multi-axis method to cast optical materials into a mold using a polymeric composition.

[0391] <Curing Process> The curing process is as follows: the aforementioned optical material in the aforementioned mold is polymerized with monomers of two or more different optical materials in the aforementioned polymeric composition, thereby curing the aforementioned optical material with the polymeric composition.

[0392] The method for manufacturing the optical material according to the second embodiment includes a curing step, thereby enabling the aforementioned optical material to be polymerized with a polymeric composition and thus enabling the manufacture of the optical material.

[0393] There are no particular restrictions on the polymerization method; any method that uses known methods to heat the material to cause the polymerization reaction to occur can be used.

[0394] For example, the following method can be used: injecting a polymeric composition into a molding die (mold) held by a gasket or tape, and slowly increasing the temperature while heating to promote the polymerization reaction. At this time, depending on the required physical properties of the obtained optical material, degassing under reduced pressure, filtration under pressure, or filtration under reduced pressure are preferably performed as needed.

[0395] As a polymerization method, it is also possible to carry out the polymerization reaction without heating.

[0396] That is, in the curing process of the second embodiment, the polymeric composition for optical materials can be left to stand, thereby allowing the polymeric composition for optical materials to be cured by polymerization.

[0397] There are no particular restrictions on the environment in which the curing process is carried out, and the mold can also be cured by heating it from the outside. However, from the viewpoint of improving the optical quality such as the corrugations and polymerizing in a short time, it is preferable to cure the aforementioned optical material with the polymeric composition by placing it in a closed space.

[0398] By placing the polymeric composition of the optical material in a closed space, heat generated by the self-heating of the polymeric composition can be prevented from being released to the outside. This allows the heat generated by self-heating to be retained within the closed space, thus promoting the polymerization reaction more efficiently and enabling the manufacture of optical materials in a shorter time.

[0399] As an enclosed space, an example is an insulated environment.

[0400] A thermally insulated environment refers to an environment that retains heat internally and inhibits heat conduction between the interior and exterior. An environment that inhibits heat conduction between the interior and exterior is one in which the heat conduction between the interior and exterior of the optical material polymeric composition is such that the polymeric composition cures.

[0401] Thermal insulation environments can be created, for example, using thermal insulation materials.

[0402] That is, optical materials can be placed in a polymeric composition within an insulated container formed of insulating material, thereby retaining heat inside the insulated container and inhibiting heat conduction between the inside and outside.

[0403] The thermal conductivity of the insulation material is preferably below 0.50 W / mK, more preferably below 0.10 W / mK, and even more preferably below 0.05 W / mK.

[0404] The density of the thermal insulation material is preferably 10 kg / m³. 3 The above, preferably 15 kg / m 3 The above is further optimized to 20 kg / m 3 above.

[0405] In the "heat insulation" or "heat insulation environment" of the second embodiment, it is preferable to perform heating to make the heat insulation reaction tank a constant temperature state (constant temperature reaction tank) within a range that does not hinder the polymerization reaction based on the heat of reaction of the polymeric composition for optical materials, or excessively promote the polymerization reaction of the polymeric composition for optical materials due to external heating.

[0406] Therefore, based on the heating state formed by the self-heating of the monomers through optical materials, the ambient temperature in the reaction tank (constant temperature reaction tank) where the mold is placed can be kept at a constant temperature or a heat-preserving state, thus promoting the polymerization reaction more effectively.

[0407] As an insulated environment, an insulated reaction tank or a constant temperature reaction tank, such as the one described above, can be used.

[0408] For example, when a mold containing monomers is placed in a vacuum container that serves as an insulated reaction tank, insulated polymerization in an insulated environment using an insulated reaction tank (constant temperature reaction tank) can be carried out through the following steps.

[0409] The inner surface of the vacuum container is covered with heat-insulating components such as polyurethane foam and cork, and the mold containing monomers is wrapped with components such as cloth as needed. Then, the mold containing monomers is placed in the vacuum container to stand.

[0410] The aforementioned curing process can also be a process of curing the aforementioned optical material with a polymeric composition by allowing it to stand without external heating.

[0411] As described above, in the second embodiment, it is not necessary to heat the optical material using the polymeric composition.

[0412] External heating is sometimes required, which can increase the economic burden. However, methods that do not require external heating allow for the manufacture of optical materials using simpler techniques, thus reducing the economic burden.

[0413] The aforementioned curing process is preferably a process in which the aforementioned optical material is cured by allowing the polymeric composition to stand for 2 to 10 hours.

[0414] In the aforementioned curing process, it is more preferable to let the aforementioned optical material stand for 8 hours or less with the polymeric composition.

[0415] Furthermore, from the viewpoint of obtaining well-cured optical materials through polymerization, it is preferable to let the aforementioned optical materials stand with the polymeric composition for 2 hours or more, and more preferably for 3 hours or more.

[0416] In the aforementioned curing process, a microwave irradiation process can also be set up to irradiate the polymeric composition of the optical material with microwaves for a specified time, as needed.

[0417] As one method of the curing process in the second embodiment, the method described as one of the curing processes in the first embodiment can be cited as an example.

[0418] Annealing process As needed, the method for manufacturing the optical material in the second embodiment may include an annealing step of annealing the cured optical material with a polymeric composition.

[0419] The annealing temperature is typically between 50 and 150°C, but preferably between 90 and 140°C, and more preferably between 100 and 130°C.

[0420] Applications of Optical Materials The optical material manufactured using the optical material manufacturing method of the second embodiment can be used in plastic lenses, prisms, optical fibers, information recording substrates, filters, light-emitting diodes, etc.

[0421] Of the above, optical materials are suitable for use in plastic lenses, and even more suitable for use in plastic lenses for eyeglasses.

[0422] ≪Optical Materials Manufacturing Systems≫ The optical material manufacturing system of the second embodiment is a system for manufacturing optical materials using a polymerizable composition for optical materials containing two or more different monomers for optical materials and a polymerization catalyst, comprising: A shearing section applies shear force to the first raw material composition and the second raw material composition to manufacture the aforementioned polymeric composition for optical materials; The stirring section applies a stirring force to the aforementioned polymeric composition for optical materials; The casting section casts the aforementioned optical material into a mold using a polymeric composition; The curing section polymerizes two or more different optical materials in the polymeric composition of the aforementioned optical material in the aforementioned mold using monomers, thereby curing the aforementioned optical material in the polymeric composition; and Quantitative liquid delivery part.

[0423] <Cut section> In the shearing section, shear force is applied to the first raw material composition and the second raw material composition to manufacture the aforementioned polymeric composition for optical materials.

[0424] In the shearing section, as a method of applying force in a direction intersecting the flow direction, one example is using a powered mixer.

[0425] The preferred ranges for the flow rate of the polymeric composition for optical materials and the rotation speed of the power mixer in the shearing section are the same as the preferred ranges for the flow rate of the polymeric composition for optical materials and the rotation speed of the power mixer in the above-mentioned <shearing process>.

[0426] <Mixing Section> In the stirring section, a stirring force is applied to the polymeric composition for optical materials.

[0427] In the stirring section, as a method of applying force in a direction that is approximately parallel to and opposite to the flow direction, an example is the use of a stirring tank containing a stir bar.

[0428] The preferred ranges for the flow rate of the polymeric composition for optical materials and the rotation speed of the stirring tank in the stirring section are the same as the preferred ranges for the flow rate of the polymeric composition for optical materials and the rotation speed of the stirring tank in the above-mentioned <stirring process>.

[0429] Casting Department In the casting section, optical materials are cast into a mold using a polymeric composition.

[0430] The details regarding the specific casting method and the preferred viscosity range of the polymeric composition for optical materials in the casting section are the same as those in the above-mentioned <Casting Process>.

[0431] <Cure Department> In the curing section, the optical material in the mold is polymerized with monomers of two or more different optical materials in a polymeric composition, thereby curing the optical material with the polymeric composition.

[0432] The details of the specific methods and preferred methods in the curing section are the same as those in the above-mentioned <curing process>.

[0433] <Quantitative liquid delivery unit> In the metering delivery section, the first raw material composition and the second raw material composition are delivered to the shearing section.

[0434] Specific examples of quantitative liquid delivery systems include gear pumps and diaphragm pumps.

[0435] In the metering delivery section, the speed at which the first raw material composition and the second raw material composition are delivered to the shearing section can be appropriately adjusted.

[0436] Viscosity Control Department The optical material manufacturing system of the second embodiment preferably further includes a viscosity control unit, which controls the viscosity of the aforementioned optical material polymeric composition in the stirring unit, measured by a type B viscometer at 25°C and 60 rpm, based on at least one condition selected from the group consisting of the shear force of the aforementioned shearing unit, the temperature of the aforementioned polymeric composition for optical materials in the stirring unit, the optical quality of the cured product obtained by curing the aforementioned polymeric composition for optical materials in the curing unit, and a characteristic quantity associated with the viscosity (hereinafter also simply referred to as viscosity) of the aforementioned polymeric composition for optical materials measured by a type B viscometer at 25°C and 60 rpm using a type B viscometer.

[0437] By controlling the viscosity of the polymeric composition for optical materials in the stirring section according to the above conditions, U-shaped ripples can be suppressed more effectively. Furthermore, U-shaped ripples can be suppressed more effectively over a longer period of time.

[0438] The optical material manufacturing system of the second embodiment preferably further includes a temperature control unit, which controls the temperature in the stirring unit based on at least one of the following conditions: the shear force of the shearing unit, the temperature of the polymeric composition for optical materials in the stirring unit, the optical quality of the cured product obtained by curing the polymeric composition for optical materials in the curing unit, and a characteristic quantity related to the viscosity of the polymeric composition for optical materials measured using a type B viscometer at 25°C and 60 rpm.

[0439] By controlling the temperature in the stirring section according to the above conditions, U-shaped ripples can be suppressed more effectively. Furthermore, U-shaped ripples can be suppressed more effectively over longer periods.

[0440] In the viscosity control unit and temperature control unit, the determination of whether the above conditions are met can be carried out in the manufacturing apparatus or outside the manufacturing apparatus by means of online connection or other means.

[0441] In addition, the determination of whether the above conditions are met can also be made using a learned model generated in advance through statistical machine learning.

[0442] In the viscosity control unit and temperature control unit, other controls besides viscosity and temperature can also be performed.

[0443] For example, the liquid level of the polymeric composition for optical materials in the stirring section can also be controlled. That is, when the liquid level of the polymeric composition for optical materials drops, the polymeric composition for optical materials is fed using a metering delivery section (e.g., a pump), thereby raising the liquid level.

[0444] The following uses Figures 1-4An example of a control routine based on a viscosity control unit and a temperature control unit will be explained.

[0445] Figure 1 This is a flowchart illustrating an example of a control routine that utilizes a viscosity control unit and a temperature control unit to obtain shear force information.

[0446] Figure 2 This is a flowchart illustrating an example of a control routine in which temperature information of a polymeric composition for optical materials in a stirring section is obtained using a viscosity control unit and a temperature control unit.

[0447] Figure 3 This is a flowchart illustrating an example of a control routine in which information related to the viscosity of a polymeric composition for optical materials is obtained using a viscosity control unit and a temperature control unit.

[0448] Figure 4 This is a flowchart illustrating an example of a control routine in which optical quality information of the cured material is obtained using a viscosity control unit and a temperature control unit.

[0449] The optical material manufacturing system of the second embodiment begins by preparing a first raw material composition and a second raw material composition, and then delivers the prepared first raw material composition and the second raw material composition to the shearing section. It should be noted that the first raw material composition and the second raw material composition, as a whole, contain two or more different monomers for optical materials and polymerization catalysts.

[0450] While allowing the first and second raw material compositions to flow through the liquid, a force is applied to the first and second raw material compositions in a direction intersecting the flow direction.

[0451] Here, Figure 1 In step 200, the viscosity control unit and the temperature control unit acquire information about the shear force of the shearing unit. In step 210, the acquired shear force information is determined. Specifically, for example, the viscosity control unit and the temperature control unit determine whether the shear force of the shearing unit is above a certain value.

[0452] If the shearing force of the shearing section is above a certain value, control is performed in step 220.

[0453] Specifically, the viscosity of the polymeric composition for optical materials in the stirring section is reduced to an appropriate range using a viscosity control unit. Additionally, the temperature in the stirring section is increased to an appropriate range using a temperature control unit.

[0454] In steps 200 to 220, the viscosity of the polymeric composition for optical materials and the temperature in the stirring section are controlled based on the shear force of the shear section.

[0455] That is, in steps 200 to 220, it is determined whether the above conditions are met. If not, the viscosity of the polymeric composition of the optical material in the stirring section is controlled within an appropriate range by the viscosity control unit, and the temperature in the stirring section is controlled within an appropriate range by the temperature control unit.

[0456] After steps 200 to 220 are completed, the sheared optical material is fed into the stirring section using a polymeric composition.

[0457] In the stirring section, while the polymeric composition for optical materials is flowing, a force is applied to the polymeric composition for optical materials in a direction that is approximately parallel to and opposite to the flow direction to stir it; or, the flow is temporarily stopped and the polymeric composition for optical materials is stirred.

[0458] Here, Figure 2 In step 230, the viscosity control unit and the temperature control unit acquire temperature information of the polymeric composition for optical materials in the stirring unit. In step 240, the acquired temperature information is determined. Specifically, for example, the viscosity control unit and the temperature control unit determine whether the temperature of the polymeric composition for optical materials in the stirring unit is above a certain value.

[0459] When the temperature of the polymeric composition for optical materials in the stirring section is above a certain value, control is performed in step 250.

[0460] Specifically, the viscosity of the polymeric composition for optical materials in the stirring section is increased to an appropriate range using a viscosity control unit. Additionally, the temperature in the stirring section is decreased to an appropriate range using a temperature control unit.

[0461] By implementing the above-described controls, the temperature rise of the polymeric composition for optical materials can be suppressed. Furthermore, at the same time, heat generation can also be suppressed by reducing the rotational speed of the shear section.

[0462] In steps 230 to 250, in the viscosity control section and the temperature control section, the viscosity of the polymeric composition for optical materials in the stirring section and the temperature in the stirring section are controlled according to the temperature of the polymeric composition for optical materials in the stirring section.

[0463] Here, Figure 3 In step 260, the viscosity control unit and the temperature control unit acquire information on characteristic quantities related to the viscosity of the polymeric composition for optical materials. In step 270, the acquired information on the aforementioned characteristic quantities is determined.

[0464] Specifically, it determines whether a characteristic quantity associated with the viscosity of a polymeric composition for optical materials exceeds a certain range.

[0465] Characteristic quantities related to the viscosity of polymeric compositions for optical materials include, for example, the resistance value of the polymeric composition for optical materials in the stirring section, the refractive index of the polymeric composition for optical materials in the stirring section, the electrical conductivity of the polymeric composition for optical materials in the stirring section, and the spectrum of the polymeric composition for optical materials in the stirring section.

[0466] Regarding the viscosity control unit and the temperature control unit, if the characteristic quantity associated with the viscosity of the polymeric composition for optical materials exceeds a certain range, control is performed in step 280.

[0467] In the viscosity control section and temperature control section, the viscosity of the polymeric composition for optical materials in the stirring section can be directly measured, or it can be calculated from the characteristic quantity associated with the viscosity of the polymeric composition for optical materials.

[0468] As a method for calculating the viscosity of the polymeric composition for optical materials in the stirring section from a characteristic quantity associated with the viscosity of the polymeric composition for optical materials, an example is the method of calculating the viscosity from the resistance value of the polymeric composition for optical materials in the stirring section.

[0469] Specifically, a standard curve of resistance versus viscosity is generated by passing an electric current through a testing instrument in a polymeric composition for optical materials, and the viscosity is calculated from the resistance value. It should be noted that polymerization through a curing reaction increases the resistance value.

[0470] Similarly, for example, the viscosity can be calculated from the refractive index of the polymeric composition for optical materials in the stirring section, the electrical conductivity of the polymeric composition for optical materials in the stirring section, the spectrum of the polymeric composition for optical materials in the stirring section, etc.

[0471] Regarding the control performed in step 280, specifically, for example, when the aforementioned characteristic quantity exceeds a certain range, in order to control the viscosity calculated from the characteristic quantity within a certain range, the viscosity of the polymeric composition of the optical material in the stirring section is controlled within an appropriate range by the viscosity control unit, and the temperature in the stirring section is controlled within an appropriate range by the temperature control unit.

[0472] Methods for controlling the viscosity of the polymeric composition for optical materials in the stirring section within an appropriate range include, for example, adjusting the shear force of the shearing section, adjusting the stirring force of the stirring section, discarding and replacing a portion of the polymeric composition for optical materials, and adjusting the liquid delivery speed of the metering liquid delivery section in the optical material manufacturing system.

[0473] Specifically, a method for discarding and replacing a portion of the polymeric composition for optical materials is, for example, the following method: discharging at least a portion of the polymeric composition for optical materials from the stirring section through the casting section, and replacing at least a portion of the polymeric composition for optical materials.

[0474] Methods for controlling the temperature in the stirring section within an appropriate range include, for example, controlling the stirring speed in the stirring section, and controlling the temperature of the water bath in the stirring section.

[0475] In the stirring section, after steps 260 to 280 are completed, the optical material polymeric composition is fed into the casting section.

[0476] In the casting section, optical materials are cast into a mold using a polymeric composition. After casting is completed, the optical materials are transferred to the curing section using the polymeric composition.

[0477] In the curing section, the optical material in the mold is polymerized with monomers of two or more different optical materials in a polymeric composition, thereby curing the optical material with the polymeric composition.

[0478] Here, Figure 4 In step 290, the viscosity control unit and the temperature control unit obtain optical quality information of the cured product obtained by curing the optical material with a polymeric composition in the curing unit.

[0479] Information about the optical quality of a cured product can include, for example, whether ridges are formed in the cured product.

[0480] In step 300, the obtained optical quality information is determined.

[0481] Specifically, for example, the viscosity control unit and the temperature control unit determine whether ripples are generated in the cured product.

[0482] If ripples are generated in the cured material, control is performed in step 310.

[0483] Specifically, a viscosity control unit is used to increase or decrease the viscosity of the polymeric composition for optical materials in the stirring section within an appropriate range. Additionally, a temperature control unit is used to raise or lower the temperature in the stirring section within an appropriate range.

[0484] In steps 290 to 310, it is determined whether ripples are generated in the cured product obtained by curing the optical material with the polymeric composition in the curing section. If ripples are generated, the viscosity of the optical material with the polymeric composition in the stirring section is increased or decreased by the viscosity control section, and the temperature in the stirring section is increased or decreased by the temperature control section.

[0485] Step 310 is complete, and this routine ends here.

[0486] Figure 5 This is a schematic diagram illustrating an example of an optical material manufacturing system.

[0487] Figure 5 In this process, a first raw material composition and a second raw material composition are prepared for manufacturing a polymeric composition for optical materials. The first raw material composition and the second raw material composition are stirred, thereby becoming a polymeric composition for optical materials containing two or more different monomers for optical materials and a polymerization catalyst. Therefore, the first raw material composition and the second raw material composition only need to be stirred to become a polymeric composition for optical materials, and the first raw material composition and the second raw material composition as a whole only need to contain two or more different monomers for optical materials and a polymerization catalyst.

[0488] In addition, the first raw material composition and the second raw material composition may also include a prepolymer obtained by polymerizing a portion of two or more different optical material monomers.

[0489] Separately, the first raw material composition prepared above is loaded into liquid tank 1 (A), and the second raw material composition is loaded into liquid tank 2 (B). Then, while adjusting the liquid temperature using cooler 3, and using nitrogen back pressure or the like, the first raw material composition is pumped from liquid tank 1 to liquid metering unit 4 (A) (e.g., a gear pump), and the second raw material composition is pumped from liquid tank 2 to liquid metering unit 6 (B) (e.g., a gear pump). At this time, the pumping speeds of liquid metering unit 4 (A) and liquid metering unit 6 (B) can be the same or different.

[0490] Then, the first raw material composition is fed from the A liquid metering unit 4 to the upper power mixer 8, which serves as a shearing unit, via the A liquid flow sensor head 5, and the second raw material composition is fed from the B liquid metering unit 6 to the upper power mixer 8, which serves as a shearing unit, via the B liquid flow sensor head 7.

[0491] In this stage, the first raw material composition and the second raw material composition are sheared by applying force in a direction intersecting the flow direction using a host power mixer 8 to obtain a polymeric composition for optical materials.

[0492] For polymeric compositions for optical materials, after shearing using the upper-level power mixer 8, the mixture can be filtered using the capsule filter 10 and further fed to the lower-level power mixer 9, which serves as the shearing unit. Then, the lower-level power mixer 9 can be used to shear the polymeric composition for optical materials.

[0493] In addition, the polymeric composition for optical materials can be sheared using multiple power mixers as described above, or it can be sheared using a single power mixer.

[0494] For example, polymeric compositions for optical materials can be sheared using only a host power mixer 8.

[0495] For polymeric compositions used in optical materials, after shearing using a lower-level power mixer 9, the mixture is filtered using a capsule filter 10 and then fed into a stirring tank 11, which serves as the stirring unit. The stirring tank 11 includes a stirrer 12.

[0496] In the stirring tank 11, the polymeric composition for optical materials is stirred by applying force in a direction that is approximately parallel to and opposite to the flow direction.

[0497] Then, the optical material polymeric composition is further mixed or stirred using a static mixer 13, and then cast into a mold 14, which serves as a curing part, using a casting section.

[0498] Then, in mold 14, two or more different optical material monomers in the polymeric composition are polymerized, thereby curing the optical material in the polymeric composition.

[0499] Figure 5 The control panel 15 in the middle is the viscosity control section and the temperature control section.

[0500] In control panel 15, the conditions described above are determined, and the viscosity of the polymeric composition for optical materials in the stirring section is measured or calculated. Based on the results, the viscosity and temperature can be controlled as described above.

[0501] For example, the foot switch 16 can be turned on (ON), thereby discharging at least a portion of the polymeric composition for optical materials from the casting section in order to replace at least a portion of the polymeric composition for optical materials.

[0502] Figure 6 This diagram illustrates an example of the configuration of a computer that implements the viscosity control unit and the temperature control unit.

[0503] For example, the viscosity control unit and temperature control unit can utilize Figure 6The computer 60 shown is implemented as described. The computer 60, which implements the viscosity control unit and temperature control unit, includes a central processing unit (CPU) 61, a memory 62 as a temporary storage area, and a non-volatile storage unit 63. Additionally, the computer includes an input / output interface (I / F) 64 for connecting input / output devices (not shown), and a read / write (R / W) unit 65 for controlling the reading and writing of data to the recording medium 68. Furthermore, the computer includes a network I / F 66 for connecting to a network such as the Internet. The CPU 61, memory 62, storage unit 63, I / F 64, R / W unit 65, and network I / F 66 are interconnected via a bus 67. The storage unit 63 can be implemented using a hard disk drive (HDD), solid-state drive (SSD), flash memory, etc. The storage unit 63, which serves as the storage medium, stores programs used to enable the computer's functions. CPU 61 reads the program from storage unit 63, displays it in memory 62, and executes the process described in the program sequentially. Thus, the above is achieved. Figures 1-4 Each control routine.

[0504] [Third Implementation] Manufacturing Methods of Optical Components The method for manufacturing the optical component according to the third embodiment includes the following steps: a space-forming step, in which a film is attached to the outer peripheral surface of two mold substrates arranged at predetermined intervals to form a space surrounded by the two mold substrates and the film; an injection step, in which a polymeric composition is injected into the space; and a curing step, in which the polymeric composition injected into the space is cured to obtain a cured product. The film is a film that has been completely peeled off from glass after being attached to glass and subjected to a heat resistance index test at 85°C, and the heat distortion temperature of the film is 70°C or higher. Furthermore, in the curing step, the curing time is preferably 10 hours or less. Additionally, the polymeric composition preferably exhibits a viscosity-enhancing curve (y=ae) at 25°C. bx The slope of ) is above 0.4.

[0505] The method for manufacturing an optical component according to the third embodiment, by including the above-described configuration, enables the manufacture of an optical component with a smooth outer peripheral surface.

[0506] In the third embodiment, the term "smooth outer peripheral surface" means, for example, that the outer peripheral surface of the cured material is preferably mirror-like, and the shape between the intersection of one main surface and the outer peripheral surface and the intersection of another main surface and the outer peripheral surface is approximately a straight line.

[0507] Furthermore, the optical component manufacturing method of the third embodiment can manufacture optical components with smooth outer peripheral surfaces without grinding operations or with a small amount of grinding.

[0508] The film in the third embodiment has relatively weak static adhesion. Therefore, when the polymeric composition shrinks during the curing process, the mold substrate can move on the contact surface with the film. This suppresses phenomena such as indentation or unevenness on the inward side of the contact surface between the film and the polymeric composition.

[0509] In addition, adhesives in films with weak static adhesion sometimes dissolve into the polymeric composition. This dissolved adhesive can contribute to whitening, voids, and other defects in the resulting cured product.

[0510] Regarding the manufacturing method of the optical component in the third embodiment, the combination of the above-described configuration can also effectively suppress the aforementioned cloudiness, voids, etc.

[0511] In particular, in the curing process of the third embodiment, when the curing time is less than 10 hours, there is a tendency for the amount of adhesive dissolution to be significantly suppressed, and the above-mentioned turbidity, voids, etc. can be suppressed more effectively.

[0512] <Space Formation Process> The space forming process in the third embodiment is as follows: a film is attached to the outer peripheral surface of two mold substrates arranged in a manner that is opposed at a predetermined interval, thereby forming a space surrounded by the two mold substrates and the aforementioned film.

[0513] use Figure 7 An example of a space-forming process will be provided.

[0514] Figure 7 This is a schematic diagram used to illustrate the space-forming process.

[0515] First, such as Figure 7 As shown, a lens casting molding die 110 is fabricated. For example, a first mold substrate 111 for forming a convex surface and a second mold substrate 112 for forming a concave surface are prepared from glass. The outer diameters of the mold substrates 111 and 112 can be the same as the final outer diameter of the plastic lens.

[0516] With mold substrates 111 and 112 arranged opposite each other at a predetermined interval, a film (e.g., adhesive tape) 113 is wrapped around the outer peripheral surfaces of mold substrates 111 and 112 in a manner slightly more than one circumference. The mold substrates 111 and 112 are fixed with the adhesive tape, and the gap between the mold substrates 111 and 112 is sealed. This forms a space surrounded by the two mold substrates and the aforementioned film (i.e., the mold cavity 114 for forming the lens). The film 113 can be a heat-peelable or re-peelable adhesive tape.

[0517] In the manufacturing method of the optical component in the third embodiment, a mold is used.

[0518] The mold in the third embodiment (also called an optical component manufacturing mold) is preferably a mold for manufacturing optical components by means of the following process: attaching a film to the outer peripheral surface of two mold substrates arranged in a manner that is opposed at a predetermined interval, forming a space surrounded by the two mold substrates and the film, placing a polymeric composition in the space, and curing the polymeric composition to obtain a cured product.

[0519] In the third embodiment, the approximate diameter of the main surface of the mold is preferably 60cm to 80cm.

[0520] As described above, when using the manufacturing method of the optical component according to the third embodiment, it is possible to manufacture an optical component with a smooth outer peripheral surface without performing a grinding operation or with a small amount of grinding.

[0521] Therefore, the approximate diameter of the main surface of the mold can be reduced accordingly without grinding.

[0522] <membrane> The method for manufacturing the optical component in the third embodiment uses the film in the third embodiment (also called the film for manufacturing optical components).

[0523] The membrane in the third embodiment is preferably an optical component manufacturing membrane for manufacturing optical components by means of the following process: attaching a membrane to the outer peripheral surface of two mold substrates arranged in a manner that is opposed at a predetermined interval, forming a space surrounded by the two mold substrates and the membrane, placing a polymeric composition in the space, and curing the polymeric composition for 10 hours or less to obtain a cured product.

[0524] The film in the third embodiment (also known as a film for manufacturing optical components) preferably includes at least a substrate layer and an adhesive layer.

[0525] [Heat Resistance Index Test] The film in the third embodiment is a film that is attached to glass and completely peeled off from the glass after a heat resistance index test at 85°C.

[0526] The static adhesive strength of a film can be determined using a heat resistance index test.

[0527] Since the film in the third embodiment is a film that is attached to glass and completely peeled off from the glass after a heat resistance index test at 85°C, it is able to suppress static adhesive force.

[0528] The film in the third embodiment has relatively weak static adhesion. Therefore, when the polymeric composition shrinks during the curing process, the mold substrate can move on the contact surface with the film. This suppresses phenomena such as indentation or unevenness on the inward side of the contact surface between the film and the polymeric composition.

[0529] The specific method for the heat resistance index test is as follows.

[0530] (method) At room temperature, the exposed surface of the adhesive layer of a membrane with a width of 25 mm ± 0.5 mm and a length of 80 mm ± 0.5 mm has an area of ​​625 mm². 2 ±25mm 2 Partially sealed to the glass plate, at 1 kg / cm² 2 The film is then subjected to load pressing. A 1kg weight is then attached to the folded end of the film that is not sealed tightly to the glass plate, and the film is placed in a constant temperature bath at 85°C with the glass plate vertical. Thirty minutes after placement in the constant temperature bath, the position of the top of the tape is measured, and the distance (mm) moved from the position immediately after attaching the 1kg weight is calculated as the heat resistance index.

[0531] The phrase "completely peeling off the glass after being attached to it and undergoing a heat resistance index test" means that, after the aforementioned heat resistance index test, the film adhered to the glass plate detaches from the glass plate within 30 minutes of being placed in the constant temperature bath, and the part that was in close contact with the glass plate disappears.

[0532] In the third embodiment, when the film is attached to glass and subjected to a heat resistance index test at 22°C, the heat resistance index is preferably 0.4 mm or less, and more preferably 0.3 mm or less.

[0533] By ensuring the heat resistance index meets the aforementioned range, the membrane can effectively fix the mold substrate. Furthermore, during the injection of the polymeric composition, leakage of the polymeric composition from the space can be suppressed.

[0534] For the membrane in the third embodiment, the heat resistance index can be 0 or higher when the heat resistance index test is conducted at 22°C.

[0535] [Heat distortion temperature] In the third embodiment, the heat distortion temperature of the film is preferably 70°C or higher, and also preferably higher than the highest temperature of the mold in the curing process.

[0536] By setting the heat distortion temperature to above 70°C, it is possible to manufacture optical components with smooth outer surfaces.

[0537] From the same perspective mentioned above, the heat distortion temperature is preferably 80°C or higher, more preferably 90°C or higher, even more preferably 120°C or higher, and particularly preferably 150°C or higher.

[0538] The heat distortion temperature can be below 500℃ or below 400℃.

[0539] For heat distortion temperature, according to ASTM-D648-56, a heat distortion temperature measuring device is used, with a value of 4.6 kgf·cm. 2 Load determination.

[0540] For the membrane in the third embodiment, when the glass ball adhesion test was conducted at 80°C, the movement distance of the glass ball is preferably 200 mm or less.

[0541] The dynamic adhesive force of a membrane can be determined using a glass ball adhesion test.

[0542] Since the membrane in the third embodiment exhibits excellent dynamic adhesion, with a glass ball movement distance of less than 200 mm after a glass ball adhesion test at 80°C.

[0543] Therefore, the membrane in the third embodiment can fix the mold substrate more effectively.

[0544] The glass ball adhesion test in the third embodiment is performed using a ball adhesion tester in accordance with JIS-Z0237.

[0545] First, prepare a plate with a film on its surface. Tilt the prepared plate at 30° so that the adhesive side of the film is positioned on the upper surface.

[0546] Next, at a specified temperature, a measuring glass ball (4.65 ± 0.03 g) is rolled from a specified position on the membrane, and the distance moved until the glass ball stops is measured.

[0547] For the membrane in the third embodiment, when a glass ball adhesion test was conducted at 25°C to 80°C, the movement distance of the glass ball is preferably 200 mm or less.

[0548] That is, preferably, when the glass ball adhesion test is carried out at 25℃~80℃, the movement distance of the glass ball is less than 200mm in the entire temperature range of 25℃~80℃.

[0549] For the membrane in the third embodiment, it is also preferable that, when the glass ball adhesion test is performed at 120°C, the movement distance of the glass ball is less than 200 mm.

[0550] For the membrane in the third embodiment, when a glass ball adhesion test is conducted at 25°C, 80°C, or 120°C, the movement distance of the glass ball is preferably 10 mm or more, more preferably 20 mm or more, and even more preferably 30 mm or more.

[0551] By keeping the movement distance of the glass sphere within the aforementioned range, the gap between the mold substrates decreases at a suitable speed during curing, reducing the likelihood of leakage of the polymeric composition. Furthermore, it prevents the formation of adhesive residue (also known as adhesive residue) on the outer surface of the cured product.

[0552] For the membrane in the third embodiment, the energy storage elastic modulus at 80°C is preferably 1.0 × 10⁻⁶. 10 Pa or higher, more preferably 2.0 × 10 Pa. 10 Pa or higher, more preferably 3.0 × 10 Pa. 10 Pa or above.

[0553] For the membrane in the third embodiment, the energy storage elastic modulus at 80°C is preferably 10.0 × 10⁻⁶. 10 Pa or less, more preferably 8.0 × 10 Pa. 10 Pa below, more preferably 6.0 × 10 Pa 10 Below Pa.

[0554] The following conditions can be cited as specific examples of detailed conditions for the test of energy storage elastic modulus determination.

[0555] Measurement method: DMA single cantilever measurement • Type of testing machine: DMA8000 • Test temperature: 0~120℃ • Frequency: 1.0Hz • Heating rate: 3℃ / min • Measured area: 1.2 (cm²) 2 ) • Chalcolide distance: 12.5mm <Injection Process> The injection process in the third embodiment is the process of injecting a polymeric composition into the aforementioned space.

[0556] use Figure 8 An example of the injection process will be provided.

[0557] Figure 8 This is a schematic diagram used to illustrate the injection process.

[0558] like Figure 8As shown, in the injection process, the adhesive tape 113 is peeled off to create a gap that allows the polymeric composition to be injected into the mold cavity 114. The polymeric composition 120 is then injected into the mold cavity 114 through the gap, and the gap is sealed again using the adhesive tape 113.

[0559] The temperature during the injection process is preferably below 30°C, more preferably below 27°C, and even more preferably below 25°C.

[0560] The temperature during the injection process is preferably 15°C or higher, more preferably 18°C ​​or higher, and even more preferably 20°C or higher.

[0561] <Polymerizing Compositions> The polymeric composition in the third embodiment can be a polymeric composition containing two or more different monomers for optical materials and a polymerization catalyst.

[0562] The slope of the viscosity-enhancing curve (y=ae) of the polymeric composition in the preferred third embodiment at 25°C bx The value is above 0.4.

[0563] By ensuring that the slope of the viscosity-enhancing curve of the polymeric composition at 25°C is 0.4 or higher, the contact time between the polymeric composition with the film and the lower viscosity composition can be shortened. As a result, the amount of binder leaching can be suppressed, and turbidity, voids, etc., can be suppressed more effectively.

[0564] From the same point of view, the slope of the thickening curve of the polymeric composition at 25°C is more preferably 0.5 or more, and even more preferably 0.6 or more.

[0565] By ensuring that the slope of the thickening curve of the polymeric composition in the third embodiment is less than 8.0 at 25°C, the polymeric composition exhibits excellent workability.

[0566] From the same point of view, the slope of the thickening curve of the polymeric composition at 25°C is more preferably 7.0 or less, and even more preferably 6.0 or less.

[0567] y=ae bx The symbols in the text are explained below.

[0568] y: viscosity a: slice e: Napier constant b: Slope x: time The slope of the viscosity-enhancing curve of the polymeric composition at 25°C was determined using the following method.

[0569] The polymerizable composition was placed in a water bath preheated to 25°C and stirred. Then, the viscosity was measured at regular time intervals (e.g., 5-minute intervals, 1-hour intervals, etc.) using a type B viscometer at 60 rpm. A viscosity-enhancing curve (y=ae) was constructed by plotting viscosity (in mPa·s) on the y-axis and time (in h) on the x-axis. bx ), calculate the slope.

[0570] The polymerizable composition of the third embodiment preferably contains two or more different monomers for optical materials and a polymerization catalyst. The content of the polymerization catalyst is 0.010 parts by mass to 2.0 parts by mass relative to a total of 100 parts by mass of the two or more different monomers for optical materials, and the viscosity measured using a type B viscometer at 25°C and 60 rpm is 10 mPa·s to 1000 mPa·s.

[0571] (Single for optical materials) The polymeric composition of the third embodiment may contain two or more different monomers for optical materials.

[0572] As a monomer for optical materials, any monomer used in optical applications is acceptable; there are no particular limitations.

[0573] For example, it can be a monomer used to manufacture optical materials having any of the following properties.

[0574] The total light transmittance of optical materials obtained using monomers can be above 10%. The total light transmittance of the aforementioned optical materials can be measured according to JIS K 7361-1 (1997).

[0575] The haze (i.e., total haze) of the optical material obtained using the optical material monomer can be 10% or less, preferably 1% or less, and more preferably 0.5% or less. The haze of the optical material is measured according to JIS-K7105 at 25°C using a haze measuring machine [(available) Tokyo Denshoku Co., Ltd., TC-HIII DPK].

[0576] The refractive index of the optical material obtained using the optical material monomer is preferably 1.58 or higher. The refractive index of the optical material obtained using the optical material monomer can be 1.80 or lower, or 1.75 or lower. The refractive index of the optical material can be measured according to JIS K7142 (2014).

[0577] The shape of optical materials obtained from monomers is not particularly limited and can be plate-shaped, cylindrical, cuboid, etc.

[0578] Examples of monomers used in optical materials include polymerizable monomers polymerized using polymerization catalysts described later.

[0579] The details of specific examples, preferred methods, preferred contents, etc. of the monomer for optical materials in the third embodiment are the same as those of the specific examples, preferred methods, preferred contents, etc. of the monomer for optical materials in the first embodiment.

[0580] [Isocyanate compounds] Examples of isocyanate compounds include aliphatic isocyanate compounds, alicyclic isocyanate compounds, aromatic isocyanate compounds, and heterocyclic isocyanate compounds; one type or a mixture of two or more types may be used. These isocyanate compounds may include dimers, trimers, and prepolymers. Examples of such isocyanate compounds include compounds exemplified in International Publication No. 2011 / 055540.

[0581] In addition, as isocyanate compounds, the following can also be used: halogen-substituted derivatives (e.g., chlorinated derivatives, bromine-substituted derivatives, etc.), alkyl-substituted derivatives, alkoxy-substituted derivatives, carbodiimide-modified derivatives, urea-modified derivatives, and biuret-modified derivatives. The above-mentioned compounds, together with nitro-substituted derivatives, polyols, etc., form prepolymer-type modified products. The dimerization or trimerization reaction products of the above-mentioned compounds, etc.

[0582] These compounds can be used alone or in combination of two or more.

[0583] The definitions of alicyclic isocyanate compounds, aromatic isocyanate compounds, heterocyclic isocyanate compounds, and aliphatic isocyanate compounds in the third embodiment are the same as those in the first embodiment.

[0584] The aforementioned isocyanate compound preferably includes at least one selected from the group consisting of aliphatic isocyanate compounds, alicyclic isocyanate compounds, aromatic isocyanate compounds, and heterocyclic isocyanate compounds.

[0585] At least one of the monomers used in the optical material in the third embodiment can be an isocyanate compound having an aromatic ring. Specifically, examples of isocyanate compounds having an aromatic ring include aromatic isocyanate compounds, and more specifically, examples include isocyanate compounds with isocyanate groups directly bonded to the aromatic ring, and isocyanate compounds with isocyanate groups bonded to the benzyl position of the aromatic ring.

[0586] Monomers used in optical materials may also contain isocyanate compounds other than isocyanate compounds with aromatic rings, i.e., isocyanate compounds without aromatic rings.

[0587] There are no particular limitations on isocyanate compounds other than those with aromatic rings, and examples include isocyanate compounds without aromatic rings. When the monomer for optical materials comprises both isocyanate compounds without aromatic rings and isocyanate compounds with aromatic rings, it is preferable that the molar number of isocyanate groups in the isocyanate compound without aromatic rings is less than the molar number of isocyanate groups in the isocyanate compound with aromatic rings.

[0588] In the third embodiment, from the viewpoint of maintaining the quality of the optical material and shortening the manufacturing time of the optical material, the aforementioned isocyanate compound preferably includes at least one selected from the group consisting of isophorone diisocyanate, 2,5-bis(isocyanate-methyl)bicyclo-[2.2.1]-heptane, 2,6-bis(isocyanate-methyl)bicyclo-[2.2.1]-heptane, m-phenylene diisocyanate, 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, dicyclohexylmethane diisocyanate, 1,3-bis(isocyanate-methyl)cyclohexane, 1,4-bis(isocyanate-methyl)cyclohexane, 1,6-hexanediisocyanate, and 1,5-pentanediisocyanate. More preferably, it comprises at least one selected from the group consisting of isophorone diisocyanate, 2,5-bis(isocyanate-methyl)bicyclo-[2.2.1]-heptane, 2,6-bis(isocyanate-methyl)bicyclo-[2.2.1]-heptane, m-phenylene diisocyanate, 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, dicyclohexylmethane diisocyanate, and 1,3-bis(isocyanate-methyl)cyclohexane. Further preferably, it comprises at least one of the following: selected from 2,5-bis(isocyanate-methyl)bicyclo-[2.2.1]-heptane, 2,6-bis(isocyanate-methyl)bicyclo-[2.2.1]-heptane, and isophthalic diisocyanate.

[0589] [Active hydrogen compounds] The details of specific examples, preferred methods, preferred contents, etc. of the active hydrogen compound in the third embodiment are the same as those of the specific examples, preferred methods, preferred contents, etc. of the active hydrogen compound in the first embodiment.

[0590] (Polythiol compounds with two or more thiol groups) The details of specific examples, preferred methods, preferred contents, etc. of the polythiol compounds having two or more thiol groups in the third embodiment are the same as those of the specific examples, preferred methods, preferred contents, etc. of the polythiol compounds having two or more thiol groups in the first embodiment.

[0591] (Polythiol compounds with 3 or more thiol groups) As active hydrogen compounds, polythiols with three or more thiol groups can also be cited.

[0592] In the case where the polymerizable composition of the third embodiment contains a polythiol compound having three or more thiol groups as an active hydrogen compound, from the viewpoint of promoting the polymerization reaction, it is preferable to include a compound (also called compound (N1)) obtained by replacing at least one of the three or more thiol groups contained in the aforementioned polythiol compound having three or more thiol groups with a group represented by the following formula (N1).

[0593] [Chemical Formula 3] In equation (N1), Indicates the bonding location.

[0594] For the polymerizable composition of the third embodiment, from the viewpoint of easily adjusting the polymerization reaction, when the peak area is determined by high performance liquid chromatography, the peak area of ​​compound (N1) is preferably 3.0 or less, more preferably 1.5 or less, relative to the peak area 100 of the aforementioned polythiol compound having 3 or more thiol groups.

[0595] It should be noted that, when using high performance liquid chromatography to determine the peak area, the peak area of ​​compound (N1) is preferably 0.01 or more from the viewpoint of promoting polymerization, relative to the peak area 100 of the aforementioned polythiol compounds having 3 or more thiol groups.

[0596] It should be noted that the peak area based on high performance liquid chromatography can be determined using the method described in paragraph 0146 of International Publication No. 2014 / 027665.

[0597] (Hydroxythiol compounds containing one or more thiol groups and one or more hydroxyl groups) The details of specific examples, preferred methods, preferred contents, etc. of the hydroxythiol compounds having one or more thiol groups and one or more hydroxyl groups in the third embodiment are the same as those of the specific examples, preferred methods, preferred contents, etc. of the hydroxythiol compounds having one or more thiol groups and one or more hydroxyl groups in the first embodiment.

[0598] (Polyol compounds containing two or more hydroxyl groups) The details of specific examples, preferred methods, preferred contents, etc. of the polyol compound having two or more hydroxyl groups in the third embodiment are the same as those of the specific examples, preferred methods, preferred contents, etc. of the polyol compound having two or more hydroxyl groups in the first embodiment.

[0599] (Amine compounds) The details of specific examples, preferred methods, preferred content, (NCO group / (OH group + SH group)), viscosity Va, viscosity difference V, etc. of the amine compound in the second embodiment are the same as those of the specific examples, preferred methods, preferred content, (NCO group / (OH group + SH group)), viscosity Va, viscosity difference V, etc. of the amine compound in the first embodiment.

[0600] <Polymerization Catalyst> The details of the specific examples, preferred methods, preferred contents, etc. of the polymerization catalyst in the third embodiment are the same as those of the specific examples, preferred methods, preferred contents, etc. of the polymerization catalyst in the first embodiment.

[0601] (Alkaline catalyst) The details of specific examples, preferred methods, preferred pKa, etc. of the alkaline catalyst in the third embodiment are the same as those of the specific examples, preferred methods, preferred pKa, etc. of the alkaline catalyst in the first embodiment.

[0602] As an alkaline catalyst, the pKa value is preferably 1 or higher, more preferably 3 or higher, and even more preferably 4 or higher.

[0603] As an alkaline catalyst, the pKa value is preferably 9 or less, and more preferably 8 or less.

[0604] (Organometallic catalysts) The details of specific examples and preferred embodiments of the organometallic catalyst in the third embodiment are the same as those of the specific examples and preferred embodiments of the organometallic catalyst in the first embodiment.

[0605] By ensuring that the content of the aforementioned polymerization catalyst is 0.010 parts by mass or more relative to the total 100 parts by mass of the monomers used in the two or more different optical materials, the polymerization reaction can be effectively promoted, thus enabling the production of high-quality optical materials in a short time. Furthermore, by effectively promoting the polymerization reaction, the demolding properties when removing the cured material from the mold can be improved.

[0606] From the above perspective, the content of the aforementioned polymerization catalyst is preferably 0.02 parts by mass or more, more preferably 0.03 parts by mass or more, relative to a total of 100 parts by mass of the aforementioned two or more different monomers for optical materials.

[0607] By making the content of the aforementioned polymerization catalyst less than 2.0 parts by mass relative to the total of 100 parts by mass of the monomers for the two or more different optical materials mentioned above, it is possible to improve, for example, the operability when injecting the polymeric composition into a mold.

[0608] From the above perspective, the content of the aforementioned polymerization catalyst relative to a total of 100 parts by mass of the aforementioned two or more different monomers for optical materials is preferably 0.20 parts by mass or less, more preferably 0.10 parts by mass or less, and even more preferably 0.09 parts by mass or less.

[0609] It should be noted that the content of the above-mentioned polymerization catalyst can be appropriately set according to the type of polymerization catalyst, the type and amount of monomers used (isocyanate compounds, active hydrogen compounds, other components, etc.), and the desired shape of the molded body.

[0610] The polymerization catalyst preferably satisfies the following condition 1.

[0611] [Condition 1] -Ea / R is above -7100 and below -2900.

[0612] (Ea is the activation energy calculated from the Arrhenius curve of the reaction rate constants of the aforementioned two or more different optical materials at two or more different temperatures using monomers; R is the gas constant (8.314 J / mol / K).) The details of the meaning and measurement method of condition 1 in the third embodiment are the same as those of the meaning and measurement method of condition 1 in the second embodiment.

[0613] (Other additives) The polymeric composition of the third embodiment may contain any additives.

[0614] Examples of any additive include photochromic compounds, internal mold release agents, bluing agents, and ultraviolet absorbers.

[0615] The details of specific examples and preferred embodiments of the photochromic compound, internal mold release agent, blueing agent, and ultraviolet absorber in the third embodiment are the same as those in the first embodiment.

[0616] (Viscosity) For the polymerizable composition of the third embodiment, from the viewpoint of suppressing corrugations and suppressing the dissolution of the adhesive, the viscosity measured by a type B viscometer at 25°C and 60 rpm is 10 mPa·s or more, preferably 40 mPa·s or more, more preferably 70 mPa·s or more, even more preferably 80 mPa·s or more, particularly preferably 100 mPa·s or more, and even more preferably 120 mPa·s or more.

[0617] For the polymerizable composition of the third embodiment, from the viewpoint of maintaining operability when molding the optical material into the desired shape, the viscosity measured by a type B viscometer at 25°C and 60 rpm is 1000 mPa·s or less, preferably 700 mPa·s or less, and more preferably 400 mPa·s or less.

[0618] The viscosity of the polymeric composition in the third embodiment can be adjusted according to the intended use of the resulting cured product.

[0619] For example, when a cured material is obtained using a mold for a convex lens, the end face (or injection port) is narrow (e.g., 1 mm to 3 mm). Therefore, from the viewpoint of suppressing ripples, the viscosity of the polymeric composition of the third embodiment is preferably 10 mPa·s to 100 mPa·s.

[0620] On the other hand, when a cured material is obtained using a mold for a conventional lens other than a convex lens, the end face (i.e., the injection port) is wide (for example, 5 mm to 15 mm). Therefore, from the viewpoint of suppressing ripples, the viscosity of the polymeric composition of the third embodiment is preferably 10 mPa·s to 1000 mPa·s, more preferably 100 mPa·s to 1000 mPa·s.

[0621] By increasing the viscosity of the polymerizable composition, when heat is applied to the composition from the outside, thermal convection caused by the temperature difference between the inside and outside of the composition can be suppressed, and ripples caused by thermal convection can be reduced.

[0622] However, if the amount of catalyst is insufficient, the viscosity increase during polymerization will be inadequate. Therefore, the viscosity will not increase to a level that can suppress thermal convection, and the temperature cannot rise rapidly in a short period of time. In addition, the time required until polymerization is complete will also be longer.

[0623] On the other hand, in the third embodiment, considering the reactivity of the isocyanate compound, the amount of catalyst is increased to an optimal range, thereby enabling a faster increase in the overall viscosity of the above composition. This suppresses both uneven polymerization and thermal convection caused by a rapid temperature rise, allowing polymerization to proceed in a short time.

[0624] For the polymerizable composition of the third embodiment, from the viewpoint of suppressing corrugations and suppressing the dissolution of the adhesive, the viscosity measured by a type B viscometer at 40°C and 60 rpm at the time point after the start of polymerization when the temperature of the polymerizable composition reaches 40°C is preferably 100 mPa·s or more, more preferably 200 mPa·s or more, and even more preferably 500 mPa·s or more.

[0625] For the polymerizable composition of the third embodiment, from the viewpoint of maintaining good operability when injecting the polymerizable composition, the viscosity measured by a type B viscometer at 40°C and 60 rpm at the time point after the start of polymerization when the temperature of the polymerizable composition reaches 40°C is preferably 2000 mPa·s or less, more preferably 1500 mPa·s or less.

[0626] The polymerizable composition of the third embodiment preferably comprises two or more different monomers for optical materials, a polymerization catalyst, and a prepolymer having polymerizable functional groups, wherein the prepolymer is a polymer of two or more different monomers for optical materials.

[0627] A prepolymer is a polymer of two or more different monomers used in optical materials, and it is a polymer with polymerizable functional groups.

[0628] Cured products obtained by polymerizing prepolymers with monomers of two or more different optical materials can be used as optical materials.

[0629] Examples of prepolymers include polymers in which two types of optical material monomers are not polymerized in a 1:1 equivalence ratio; and polymers in which two types of optical material monomers are polymerized in an unbalanced equivalence ratio.

[0630] It should be noted that the aforementioned polymerizable functional groups refer to functional groups that can polymerize with other polymerizable functional groups. Specifically, examples include isocyanate groups, mercapto groups, and other functional groups with active hydrogen, which will be discussed later.

[0631] The so-called 1:1 equivalent ratio polymerization means, for example, when using isocyanate compounds and polythiols for polymerization, the isocyanate groups of the isocyanate compound and the mercapto groups of the polythiols compound are polymerized in a molar ratio of 1:1.

[0632] <Curing Process> The curing process in the third embodiment is a process of curing the polymeric composition injected into the space to obtain a cured product.

[0633] The method for manufacturing an optical component according to the third embodiment includes a curing step, thereby enabling the aforementioned polymeric composition to be polymerized and optical materials to be manufactured.

[0634] During the curing process, the curing time is preferably less than 10 hours.

[0635] In particular, in the curing process of the third embodiment, when the curing time is less than 10 hours, there is a tendency for the amount of adhesive dissolution to be significantly suppressed, and the above-mentioned turbidity, voids, etc. can be suppressed more effectively.

[0636] In the third embodiment, the curing time refers to the time from when the temperature of the polymeric composition reaches 30°C until the polymeric composition is completely cured.

[0637] From the above perspective, the curing time is more preferably 7 hours or less, and even more preferably 5 hours or less.

[0638] From the viewpoint of the curability of the polymerizable composition, the curing time is preferably 1 hour or more, and more preferably 3 hours or more.

[0639] The maximum curing temperature in the curing process is preferably below 150°C, more preferably below 130°C, even more preferably below 100°C, and particularly preferably below 80°C.

[0640] The maximum curing temperature in the curing process is preferably above 50°C, more preferably above 60°C, and even more preferably above 70°C.

[0641] In the curing process, preferably, as the aforementioned polymeric composition cures, at least one of the aforementioned two mold substrates moves on the contact surface with the aforementioned film, and the gap between the aforementioned mold substrates becomes smaller than the gap between the aforementioned mold substrates in the aforementioned space forming process.

[0642] use Figure 9 This point will be explained in detail.

[0643] Figure 9 A schematic diagram illustrating the movement of the mold substrate during the curing process.

[0644] like Figure 9 As shown, in the curing process, the polymeric composition 120 in the mold cavity 114 is cured. The polymeric composition 120 is polymerized by, for example, heating, active energy rays, etc., resulting in polymerization shrinkage. When this polymerization shrinkage occurs most intensely, the holding force of the film (e.g., adhesive tape) 113 on the mold substrate decreases.

[0645] The reduced holding and adhesive forces of the film 113 result in the stress and self-weight associated with the polymerization shrinkage of the polymeric composition 120 in the mold cavity 114, primarily causing the upper mold substrate to move from its fixed position during the space-forming process (by...). Figure 9 (As shown by the dashed line) it slides and descends on the inner surface of the film 113, approaching the mold substrate on the lower side. At this time, the amount of movement of the mold substrate is approximately equal to the amount of polymerization shrinkage of the polymeric composition 120.

[0646] Therefore, by moving the mold substrates 111 and 112, the volume shrinkage of the polymeric composition 120 is absorbed, preventing the film 113 from deforming. The resulting cured product (plastic lens) 130 has the shape of the undeformed film 113 transferred to its side, resulting in an aesthetically pleasing shape.

[0647] Therefore, the outer diameters of the mold substrates 111 and 112 can be the same as the final outer diameter of the plastic lens. This eliminates the waste of the several millimeters of outer periphery that was previously removed through grinding. In the case of lenses with thick outer peripheries, this results in a reduction of over ten percent of the polymeric composition. Furthermore, it eliminates the advantage of not requiring grinding operations.

[0648] Traditionally, polymerization reactions are initiated by heating the polymerizable composition.

[0649] For the polymerizable composition in the third embodiment, the polymerization reaction of the monomers for optical materials in the polymerizable composition can also be promoted by generating the heat of reaction associated with the polymerization reaction (i.e., heat generated due to self-heating) in a short time.

[0650] Therefore, in the manufacturing method of the optical component of the third embodiment, it is not necessary to heat the polymeric composition, but heating is also possible.

[0651] That is, in the curing process of the third embodiment, the polymeric composition can be left to stand, thereby allowing the polymeric composition to cure through polymerization.

[0652] By promoting the polymerization reaction of the monomers for optical materials in a polymeric composition by generating the heat of reaction associated with the polymerization reaction (i.e., heat generated due to self-heating) in a short time, the polymerization time can be shortened.

[0653] In the past, in order to improve the quality of optical materials, the temperature was slowly increased while the polymerization reaction took several hours to tens of hours during the heat curing process. Specifically, it usually takes about 20 to 48 hours.

[0654] As mentioned above, when the polymerization reaction of the monomers for optical materials in the polymeric composition is promoted by generating reaction heat (i.e., heat generated due to self-heating) associated with the polymerization reaction in a short period of time, the curing time is mostly completed within a few hours to 20 hours.

[0655] In the curing process, it is preferable to cure the polymeric composition by allowing it to stand in a closed space. This results in a cured product with excellent end-face condition.

[0656] Furthermore, by placing the polymerizable composition in a confined space, heat generated by the self-heating of the polymerizable composition can be prevented from being released to the outside. This allows the heat generated by self-heating to be retained within the confined space, thus promoting the polymerization reaction more efficiently and enabling the manufacture of optical materials in a shorter time.

[0657] As an enclosed space, an example is an insulated environment.

[0658] An insulated environment refers to an environment that retains heat internally and inhibits heat conduction between the interior and exterior. An environment that inhibits heat conduction between the interior and exterior is one in which the heat conduction between the interior and exterior of the enclosed space is sufficient to allow the polymeric composition to solidify when the polymeric composition is left to stand in an enclosed space.

[0659] Thermal insulation environments can be created, for example, using thermal insulation materials.

[0660] That is, the polymeric composition can be placed in an insulated container formed of insulating material, thereby retaining heat inside the insulated container and inhibiting heat conduction between the inside and the outside.

[0661] The thermal conductivity of the insulation material is preferably below 0.50 W / mK, more preferably below 0.10 W / mK, and even more preferably below 0.05 W / mK.

[0662] The density of the thermal insulation material is preferably 10 kg / m³. 3 The above, preferably 15 kg / m 3 The above is further optimized to 20 kg / m 3 above.

[0663] In the "heat insulation" or "heat insulation environment" of the third embodiment, it is preferable to perform heating to make the heat insulation reaction tank a constant temperature state (constant temperature reaction tank) within a range that does not hinder the polymerization reaction based on the heat of reaction of the polymerizable composition, or excessively promote the polymerization reaction of the polymerizable composition due to external heating.

[0664] Therefore, based on the heating state formed by the self-heating of the monomers through optical materials, the ambient temperature in the reaction tank (constant temperature reaction tank) where the mold is placed can be kept at a constant temperature or a heat-preserving state, thus promoting the polymerization reaction more effectively.

[0665] As an insulated environment, an insulated reaction tank or a constant temperature reaction tank, such as the one described above, can be used.

[0666] For example, when a mold containing monomers is placed in a vacuum container that serves as an insulated reaction tank, insulated polymerization in an insulated environment using an insulated reaction tank (constant temperature reaction tank) can be carried out through the following steps.

[0667] The inner surface of the vacuum container is covered with heat-insulating and heat-preserving components such as polyurethane foam and cork. The mold containing the monomer is then wrapped with materials such as cloth, as needed. The mold containing the monomer is then left to stand inside the vacuum container.

[0668] The curing process can also be a process of curing the polymeric composition by allowing it to stand without external heating.

[0669] As described above, in the third embodiment, it is not necessary to heat the polymeric composition.

[0670] In order to heat from the outside, a device is sometimes used, which sometimes increases the economic burden. If the optical component is manufactured by the method of the third embodiment, the optical material can be manufactured by a simple method, thus reducing the economic burden.

[0671] The curing process is preferably a process in which the polymeric composition is cured by allowing it to stand for 2 to 10 hours.

[0672] According to conventional methods, polymerization typically occurs by slowly heating the material while the temperature is gradually increased over several hours to tens of hours (e.g., about 20 to 48 hours).

[0673] If the polymerization reaction time is short, the polymeric composition will not be fully cured, and therefore, optical materials cannot be obtained, or the quality of the optical materials will be reduced.

[0674] However, according to the third embodiment, the quality of the obtained optical material can be maintained, and the optical material can be manufactured in a short time. Specifically, the optical material can be manufactured by letting the polymeric composition stand for 10 hours or less.

[0675] From the above perspective, it is more preferable to let the polymeric composition stand for 8 hours or less during the curing process.

[0676] Furthermore, from the viewpoint of obtaining well-cured optical materials through polymerization, it is preferable to let the polymeric composition stand for 2 hours or more, and more preferably for 5 hours or more.

[0677] In the curing process, a microwave irradiation process can also be set up to irradiate the polymeric composition with microwaves for a specified time, as needed.

[0678] As one method of the curing process in the third embodiment, one example is process b, which is described as one method of the curing process in the first embodiment.

[0679] (cured material) The cured product of the third embodiment is the cured product of the polymeric composition of the third embodiment.

[0680] For the cured product of the third embodiment, from the viewpoint of reducing ripples, when using an amine catalyst as the polymerization catalyst, the amine content is preferably 0.03% by mass or more, more preferably 0.05% by mass or more, and even more preferably 0.07% by mass or more.

[0681] Furthermore, for the cured product of the third embodiment, from the viewpoint of improving the operability of the polymerizable composition for optical materials, the amine content is preferably 2.5% by mass or less, more preferably 2.0% by mass or less, and even more preferably 1.5% by mass or less.

[0682] It should be noted that the amine content mentioned above is the content of amines determined by gas chromatography-mass spectrometry of a dichloromethane composition obtained by dispersing the solidified material in dichloromethane and extracting it with ultrasound.

[0683] For the cured product of the third embodiment, from the viewpoint of reducing ripples, when using an organotin catalyst, the tin content is preferably 0.05% by mass or more, more preferably 0.1% by mass or more, and even more preferably 0.2% by mass or more.

[0684] Furthermore, for the cured product of the third embodiment, from the viewpoint of improving the operability of the polymeric composition for optical materials, the tin content is preferably 2.5% by mass or less, more preferably 2.0% by mass or less, and even more preferably 1.5% by mass or less.

[0685] For the cured product of the third embodiment, for example, the amine content determined by gas chromatography-mass spectrometry is preferably 0.03% by mass or more and 2.5% by mass or less.

[0686] The method for determining the amine content in the solidified product is as follows.

[0687] 200 mg of the solidified material, which was formed into powder by a metal file, and 3 mL of dichloromethane were placed into a centrifuge tube (volume 10 mL). The mixture was ultrasonically extracted for 10 minutes at room temperature using an ultrasonic cleaner (IUCHI, US-4). The mixture was then centrifuged for 10 minutes at 4000 rpm using a centrifuge (KUBOTA, benchtop mini centrifuge 2410).

[0688] Collect the supernatant, redisperse the residue in 3 mL of dichloromethane, perform the above ultrasonic extraction and centrifugation, and collect the supernatant (hereinafter also referred to as "residue extraction").

[0689] After performing the above residue extraction twice more, dichloromethane was added to the obtained supernatant to make the total volume 10 mL.

[0690] The obtained 10 mL supernatant was filtered and analyzed using gas chromatography-mass spectrometry (GC-MS) (GC-MS apparatus: Agilent Technologies, 6890GC / 5973N MSD, column: CP-Sil 8 CB for Amine (0.25 mm ID × 30 m FT = 0.25 μm)) to obtain the peak area values ​​of the amine. A standard curve was constructed based on the obtained peak area values ​​of the amine and the amount of amine, and the amine content in the solidified product was determined.

[0691] It should be noted that the amines mentioned above refer to amine compounds that can be used as polymerization catalysts, or amine compounds derived from the amine compounds mentioned above.

[0692] Especially in optical applications where light transmittance is required, the devitrification of the cured product of the third embodiment is preferably less than 50, more preferably less than 35.

[0693] Devitrification can be determined using the following methods.

[0694] In a dark environment, light from a light source (e.g., a Luminar Ace LA-150A manufactured by Hayashi-Repic Co., Ltd.) is passed through a cured material. An image of the light passing through the cured material is acquired and sent to an image processing device (e.g., an image processing device manufactured by Ube InformationSystems Inc.). The acquired image is processed to achieve varying degrees of density, and the density of the processed image is quantified for each pixel. The value calculated as the average of the density values ​​of each pixel is used as the opacity.

[0695] For the cured product of the third embodiment, it is preferable that there are no corrugations with a length of 1.0 mm or more within a radius of 15 mm from the center of the cured product, and more preferably that there are no corrugations with a length of 1.0 mm or more within and outside a radius of 15 mm from the center of the cured product.

[0696] More specifically, the cured product of the third embodiment can be a cured product of two or more different optical monomers, wherein at least one of the two or more different optical monomers is an isocyanate compound without an aromatic ring, there are no ridges of more than 1.0 mm in length within a radius of 15 mm from the center of the cured product, and the amine content determined by gas chromatography-mass spectrometry is more than 0.03% by mass and less than 2.5% by mass.

[0697] The cured product of the third embodiment is preferably a cured product of two or more different optical monomers, and there are no ridges with a length of 1.0 mm or more within a radius of 15 mm from the center of the cured product. The outer peripheral surface of the cured material is mirror-like, and the shape between the intersection of one main surface and the outer peripheral surface, and the intersection of the other main surface and the outer peripheral surface, is approximately a straight line.

[0698] The cured material of the third embodiment preferably includes a protrusion that is substantially parallel to the aforementioned outer peripheral surface at the intersection of the aforementioned one main surface and the outer peripheral surface, and at the intersection of the aforementioned other main surface and the outer peripheral surface.

[0699] When the polymeric composition is cured, small gaps (also called chamfers) are often provided in the mold at the intersection of the main surface of one mold and the film, and at the intersection of the main surface of the other mold and the film.

[0700] The aforementioned protrusions are formed when the polymeric composition enters the aforementioned gaps and is cured.

[0701] The cured product of the third embodiment preferably includes at least one selected from the group consisting of polyurethane resin, thiourethane resin and cyclic sulfur resin, and more preferably includes thiourethane resin.

[0702] Annealing process As needed, the method for manufacturing the optical component of the third embodiment may include an annealing process for annealing the cured polymeric composition.

[0703] The annealing temperature is typically between 50 and 150°C, but preferably between 90 and 140°C, and more preferably between 100 and 130°C.

[0704] <Optical Components> The cured material in the third embodiment can be suitably used as an optical component.

[0705] For example, the thickness of the optical component in the third embodiment can be 1mm to 20mm, or 4mm to 16mm.

[0706] <Applications of Optical Components> The optical components in the third embodiment can be plastic lenses, prisms, optical fibers, information recording substrates, filters, light-emitting diodes, etc.

[0707] Of the above, the optical component in the third embodiment can be suitably used for plastic lenses, and can be more suitably used for plastic lenses for eyeglasses.

[0708] [Fourth Implementation] Manufacturing Methods of Optical Components The method for manufacturing an optical component according to the fourth embodiment includes the following steps: a space-forming step, in which a film is attached to the outer peripheral surfaces of two mold substrates arranged at predetermined intervals to form a space surrounded by the two mold substrates and the film; an injection step, in which a polymeric composition is injected into the space; and a curing step, in which the polymeric composition injected into the space is cured to obtain a cured product. The film, when attached to glass and subjected to a heat resistance index test at 85°C, has a heat resistance index of 1 mm or more (excluding cases where it completely peels off from the glass), and a heat distortion temperature of 120°C or less. Furthermore, in the curing step, the curing time is preferably 10 hours or less. Additionally, the polymeric composition preferably has a viscosity-enhancing curve slope of 0.4 or more at 25°C.

[0709] The method for manufacturing an optical component according to the fourth embodiment, by including the above-described configuration, enables the manufacture of an optical component with a smooth outer peripheral surface.

[0710] In the fourth embodiment, the term "smooth outer peripheral surface" means, for example, that the outer peripheral surface of the cured material is preferably mirror-like, and the shape between the intersection of one main surface and the outer peripheral surface and the intersection of another main surface and the outer peripheral surface is a concave curve.

[0711] Furthermore, the optical component manufacturing method of the fourth embodiment can manufacture optical components with smooth outer peripheral surfaces without grinding operations or with a small amount of grinding.

[0712] When the polymeric composition shrinks during the curing process, movement of the mold substrate on the contact surface with the film can be suppressed. Therefore, the contact surface between the film and the polymeric composition can be recessed inwards.

[0713] In addition, the binder in the membrane sometimes dissolves into the polymerizable composition. The binder dissolved into the polymerizable composition can cause whitening, voids, etc. in the resulting cured product.

[0714] Regarding the manufacturing method of the optical component in the fourth embodiment, the combination of the above-described configuration can also effectively suppress the aforementioned cloudiness, voids, etc.

[0715] In particular, during the curing process in the fourth embodiment, when the curing time is less than 10 hours and the viscosity of the polymeric composition is a certain value or higher as described later, there is a tendency for the amount of adhesive dissolution to be significantly suppressed, and the aforementioned wrinkles, turbidity, voids, etc. can be suppressed more effectively.

[0716] <Space Formation Process> The details of the specific method and preferred method of the space forming process in the fourth embodiment are the same as those of the specific method and preferred method of the space forming process in the third embodiment.

[0717] In the manufacturing method of the optical component in the fourth embodiment, a mold is used.

[0718] The details of the specific method and preferred method of the mold in the fourth embodiment are the same as those of the specific method and preferred method of the mold in the third embodiment.

[0719] <membrane> The method for manufacturing the optical component in the fourth embodiment uses the film in the fourth embodiment (also called the film for manufacturing optical components).

[0720] The membrane in the fourth embodiment is preferably an optical component manufacturing membrane for manufacturing optical components by the following process: attaching a membrane to the outer peripheral surface of two mold substrates arranged in a manner that is opposed at a predetermined interval, forming a space surrounded by the two mold substrates and the membrane, placing a polymeric composition in the space, and curing the polymeric composition for 10 hours or less to obtain a cured product.

[0721] The film in the fourth embodiment (also known as a film for manufacturing optical components) preferably includes at least a substrate layer and an adhesive layer.

[0722] [Heat Resistance Index Test] The film in the fourth embodiment has a heat resistance index of 1 mm or more when it is attached to glass and subjected to a heat resistance index test at 85°C (excluding cases where it is completely peeled off from the glass).

[0723] The static adhesive strength of a film can be determined using a heat resistance index test.

[0724] Since the film in the fourth embodiment has a heat resistance index of 1 mm or more when it is attached to glass and subjected to a heat resistance index test at 85°C (excluding cases where it completely peels off from the glass), it is able to effectively adjust the static adhesion force.

[0725] That is, when the polymeric composition is cured and shrinks during the curing process, movement of the mold substrate on the contact surface with the film can be suppressed. Therefore, the contact surface between the film and the polymeric composition can be recessed to the inward side.

[0726] From the above perspective, the heat resistance index is preferably 2 mm or more, and more preferably 3 mm or more.

[0727] For the membrane in the fourth embodiment, as long as it does not completely peel off from the glass after being attached to it and subjected to a heat resistance index test at 85°C, there is no particular limit to the upper limit of the heat resistance index.

[0728] For example, regarding the heat resistance index, it is preferably 15 mm or less, more preferably 10 mm or less, and even more preferably 7 mm or less.

[0729] By ensuring the heat resistance index meets the aforementioned range, leakage of the polymeric composition from the space can be suppressed during injection. Misalignment of the mold substrates (i.e., spatial deformation) can be suppressed when at least one of the two mold substrates moves on the contact surface with the film during the curing of the polymeric composition.

[0730] The specific method for the heat resistance index test in the fourth embodiment is the same as that in the third embodiment.

[0731] [Heat distortion temperature] The details of the preferred range and measurement method of the heat distortion temperature and glass bead adhesion test of the membrane in the fourth embodiment are the same as those of the preferred range and measurement method of the heat distortion temperature and glass bead adhesion test of the membrane in the third embodiment.

[0732] For the membrane in the fourth embodiment, the energy storage elastic modulus at 80°C is preferably 3.0 × 10⁻⁶. 10 Pa or higher, more preferably 5.0 × 10 Pa. 10 Pa or higher, more preferably 7.0 × 10 Pa. 10 Pa or above.

[0733] For the membrane in the fourth embodiment, the energy storage elastic modulus at 80°C is preferably 40.0 × 10⁻⁶. 10 Pa or less, more preferably 30.0 × 10 Pa. 10 Pa below, more preferably 20.0 × 10 Pa 10 Below Pa.

[0734] The specific examples of detailed conditions for the energy storage elastic modulus measurement test in the fourth embodiment are the same as those for the specific examples of detailed conditions for the energy storage elastic modulus measurement test in the third embodiment.

[0735] [Adhesive strength] In the fourth embodiment, when the membrane includes at least a substrate layer and an adhesive layer, the adhesive strength of the adhesive layer is preferably 1.0 N / 10 mm to 10.0 N / 10 mm, more preferably 2.0 N / 10 mm to 7.0 N / 10 mm, and even more preferably 3.0 N / 10 mm to 5.0 N / 10 mm.

[0736] Adhesive strength was measured in accordance with JIS Z 0237:2009.

[0737] <Injection Process> The details of the injection process in the fourth embodiment, including the specific method and preferred method, are the same as those in the third embodiment.

[0738] <Polymerizing Compositions> The polymeric composition of the fourth embodiment can be a polymeric composition containing two or more different monomers for optical materials and a polymerization catalyst.

[0739] Preferably, the polymeric composition in the fourth embodiment has a viscosity-enhancing curve with a slope of 0.4 or higher at 25°C.

[0740] The preferred range of the slope of the viscosity-enhancing curve of the polymeric composition at 25°C in the fourth embodiment, the measurement method, and other details are the same as those in the third embodiment.

[0741] The polymerizable composition of the fourth embodiment preferably contains two or more different monomers for optical materials and a polymerization catalyst. The content of the polymerization catalyst is 0.010 parts by mass to 2.0 parts by mass relative to a total of 100 parts by mass of the two or more different monomers for optical materials, and the viscosity measured using a type B viscometer at 25°C and 60 rpm is 10 mPa·s to 1000 mPa·s.

[0742] (Single for optical materials) The details of the specific examples, preferred methods, preferred contents, etc. of the optical material monomer in the fourth embodiment are the same as those of the specific examples, preferred methods, preferred contents, etc. of the optical material monomer in the third embodiment.

[0743] [Isocyanate compounds] The details of specific examples, preferred methods, preferred contents, definitions, etc. of the isocyanate compound in the fourth embodiment are the same as those of the specific examples, preferred methods, preferred contents, definitions, etc. of the isocyanate compound in the third embodiment.

[0744] The aforementioned isocyanate compound preferably includes at least one selected from the group consisting of aliphatic isocyanate compounds, alicyclic isocyanate compounds, aromatic isocyanate compounds, and heterocyclic isocyanate compounds. In particular, from the viewpoint of suppressing polymerization reactivity to a certain extent and thus improving the state of the end face, it is preferable that the isocyanate compound does not contain aromatic isocyanate compounds.

[0745] Furthermore, when the isocyanate compound includes an aromatic isocyanate compound, from the same point of view as above, it is also preferable that the monomer for optical materials includes an aromatic isocyanate compound and a polythiol compound with four or more functions.

[0746] [Active hydrogen compounds] The details of specific examples, preferred methods, preferred contents, etc. of the active hydrogen compound in the fourth embodiment are the same as those of the specific examples, preferred methods, preferred contents, etc. of the active hydrogen compound in the third embodiment.

[0747] (Polythiol compounds with two or more thiol groups) The details of specific examples, preferred methods, preferred contents, etc. of the polythiol compounds having two or more thiol groups in the fourth embodiment are the same as those of the polythiol compounds having two or more thiol groups in the third embodiment.

[0748] (Polythiol compounds with 3 or more thiol groups) The details of specific examples, preferred methods, preferred contents, etc. of the polythiol compounds having three or more thiol groups in the fourth embodiment are the same as those of the polythiol compounds having three or more thiol groups in the third embodiment.

[0749] (Hydroxythiol compounds containing one or more thiol groups and one or more hydroxyl groups) The details of specific examples, preferred methods, preferred contents, etc. of the hydroxythiol compound having one or more thiol groups and one or more hydroxyl groups in the fourth embodiment are the same as those of the specific examples, preferred methods, preferred contents, etc. of the hydroxythiol compound having one or more thiol groups and one or more hydroxyl groups in the third embodiment.

[0750] (Polyol compounds containing two or more hydroxyl groups) The details of specific examples, preferred methods, preferred contents, etc. of the polyol compound having two or more hydroxyl groups in the fourth embodiment are the same as those of the specific examples, preferred methods, preferred contents, etc. of the polyol compound having two or more hydroxyl groups in the third embodiment.

[0751] (Amine compounds) The details of specific examples, preferred methods, preferred contents, (NCO group / (OH group + SH group)), viscosity Va, viscosity difference V, etc. of the amine compound in the fourth embodiment are the same as those of the specific examples, preferred methods, preferred contents, (NCO group / (OH group + SH group)), viscosity Va, viscosity difference V, etc. of the amine compound in the third embodiment.

[0752] <Polymerization Catalyst> The details of the specific examples, preferred methods, preferred content, and condition 1 (-Ea / R) of the polymerization catalyst in the fourth embodiment are the same as those of the specific examples, preferred methods, preferred content, and condition 1 (-Ea / R) of the polymerization catalyst in the third embodiment.

[0753] (Alkaline catalyst) The specific examples, preferred methods, preferred pKa, and other details of the alkaline catalyst in the fourth embodiment are the same as those of the alkaline catalyst in the third embodiment.

[0754] (Organometallic catalysts) The details of specific examples and preferred embodiments of the organometallic catalyst in the fourth embodiment are the same as those of specific examples and preferred embodiments of the organometallic catalyst in the third embodiment.

[0755] (Other additives) The polymeric composition of the fourth embodiment may contain any additives.

[0756] Examples of any additive include photochromic compounds, internal mold release agents, bluing agents, and ultraviolet absorbers.

[0757] The details of specific examples and preferred embodiments of the photochromic compound, internal mold release agent, blueing agent, and ultraviolet absorber in the fourth embodiment are the same as those in the third embodiment.

[0758] (Viscosity) The details of the preferred range of viscosity, adjustment method, etc. of the polymeric composition of the fourth embodiment are the same as those of the preferred range of viscosity, adjustment method, etc. of the polymeric composition of the third embodiment.

[0759] <Curing Process> The details of the curing process, including the specific method, preferred method, preferred time, and preferred temperature, in the fourth embodiment are the same as those in the third embodiment.

[0760] In the curing process, preferably, as the polymeric composition cures, the shape of the film between the intersection of one main surface and the outer peripheral surface and the intersection of another main surface and the outer peripheral surface becomes a concave curve.

[0761] use Figure 10 This point will be explained in detail.

[0762] Figure 10 This is a schematic diagram used to illustrate the shape changes of the film during the curing process.

[0763] like Figure 10 As shown, in the curing process, the polymeric composition 120 in the mold cavity 114 is cured. The polymeric composition 120 is polymerized by, for example, heating, active energy rays, etc., resulting in polymerization shrinkage. When this polymerization shrinkage occurs most intensely, the shape-retaining force that maintains the shape of the film (e.g., adhesive tape) 113 decreases.

[0764] The reduced shape-holding force of membrane 113 results in the membrane shape deforming in a concave curve between the intersection of one main surface and the outer peripheral surface, and the intersection of the other main surface and the outer peripheral surface, due to the stress associated with the polymerization shrinkage of the polymeric composition 120 in the mold cavity 114. At this point, the amount of membrane deformation is approximately equal to the amount of polymerization shrinkage of the polymeric composition 120.

[0765] Therefore, by making the shape of the film between the intersection of one main surface and the outer peripheral surface, and the intersection of the other main surface and the outer peripheral surface, a concave curve, the volume shrinkage of the polymerizable composition 120 can be absorbed. The resulting cured product 130 has a concave curve on its side surface.

[0766] Therefore, the outer diameters of the mold substrates 111 and 112 can be the same as the final outer diameter of the plastic lens. This eliminates the waste of the several millimeters of outer periphery that was previously removed through grinding. In the case of lenses with thick outer peripheries, this results in a reduction of over ten percent of the polymeric composition. Furthermore, it eliminates the advantage of not requiring grinding operations.

[0767] Traditionally, polymerization reactions are initiated by heating the polymerizable composition.

[0768] In the polymerizable composition of the fourth embodiment, the polymerization reaction of the monomers for optical materials in the polymerizable composition can also be promoted by generating the heat of reaction associated with the polymerization reaction (i.e., heat generated due to self-heating) in a short time.

[0769] The details in the fourth embodiment regarding the specific method, preferred method, definition of enclosed space and insulation environment, thermal conductivity and density of insulation material, polymerization time, etc., for promoting the polymerization reaction by utilizing the heat of reaction associated with the polymerization reaction are the same as those in the third embodiment.

[0770] As one method of the curing process in the fourth embodiment, one example is process b, which is described as one method of the curing process in the third embodiment.

[0771] (cured material) The details of the specific manner, preferred manner, preferred amine content, method for determining amine content, preferred tin content, devitrification, presence or absence of corrugations, etc. of the cured product in the fourth embodiment are the same as those of the specific manner, preferred manner, preferred amine content, method for determining amine content, preferred tin content, devitrification, method for determining devitrification, presence or absence of corrugations, etc. of the cured product in the third embodiment.

[0772] Annealing process As needed, the method for manufacturing the optical component of the fourth embodiment may include an annealing process for annealing the cured polymeric composition.

[0773] The annealing temperature is typically between 50 and 150°C, but preferably between 90 and 140°C, and more preferably between 100 and 130°C.

[0774] <Optical Components> The cured material in the fourth embodiment can be suitably used as an optical component.

[0775] For example, the thickness of the optical component in the fourth embodiment can be 1mm to 20mm or 4mm to 16mm.

[0776] <Applications of Optical Components> The optical components in the fourth embodiment can be plastic lenses, prisms, optical fibers, information recording substrates, filters, light-emitting diodes, etc.

[0777] Of the above, the optical component in the fourth embodiment can be suitably used for plastic lenses, and can be more suitably used for plastic lenses for eyeglasses.

[0778] Example Hereinafter, an embodiment of the first embodiment will be specifically described using examples, but the first embodiment is not limited to these examples.

[0779] The viscosity measurement method in the examples is the same as that described above.

[0780] The molded articles obtained in each embodiment or comparative example were evaluated as follows.

[0781] (Waves) The molded body was projected using an ultra-high pressure mercury lamp (light source model OPM-252HEG: manufactured by USHIO Inc.), and the transmitted image was observed visually. The evaluation was carried out according to the following criteria.

[0782] A: No ribs were observed, or ribs were not clearly observed.

[0783] B: Although slight ripples are observed, it is generally acceptable for the product.

[0784] C: Many ridges were observed, which is unacceptable for a finished product.

[0785] [Example 1] A mixture was prepared by adding 0.1 parts by weight of Mitsui Chemicals' internal release agent for MR applications, 1.5 parts by weight of Tinuvin 329 (UV absorber), and 40.6 parts by weight of 2,5(6)-bis(isocyanate methyl)-bicyclo-[2.2.1]-heptane (monomer for optical materials). The mixture was stirred at 25°C for 1 hour to ensure complete dissolution. Then, 23.9 parts by weight of pentaerythritol tetra(3-mercaptopropionate) (monomer for optical materials) and 25.5 parts by weight of 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane (monomer for optical materials) were added to the mixture, and the mixture was stirred at 25°C for 5 minutes to prepare a homogeneous solution. Further, 0.05 parts by mass of 3,5-dimethylpyridine [polymerization catalyst] (pKa value = 6.14) was added to the obtained homogeneous solution, and the mixture was degassed at 400 Pa and 25 °C while stirring for 1 hour. The viscosity was adjusted while the optical material was polymerized with monomers to obtain a first mixture containing the prepolymer. The viscosity of the mixture containing the prepolymer is shown in Table 1.

[0786] 10.0 parts by weight of 2,5(6)-bis(isocyanate-methyl)-bicyclo-[2.2.1]-heptane [monomer for optical materials] and 0.15 parts by weight of 3,5-dimethylpyridine [polymerization catalyst] were added to prepare a mixture. The mixture was stirred at 25°C for 15 minutes to obtain a second mixture.

[0787] Then, the first mixture and the second mixture are mixed at 20°C to obtain a polymeric composition for optical materials.

[0788] The obtained optical material is fed into a casting mold (i.e., a casting mold) while being further mixed with a polymeric composition in a static mixer.

[0789] The viscosity (also known as casting viscosity) of the polymeric composition of the optical material is adjusted to the values ​​shown in Table 1 when the liquid is fed into the mold and cast.

[0790] During the liquid delivery of the polymeric composition for optical materials, while filtering the polymeric composition for optical materials using a 1μm PTFE filter, it is injected at a rate of 10g / second into the cavity of a casting mold for lens manufacturing, which consists of a glass mold (upper mold) with a diameter of 78mm and a glass mold (lower mold) with a diameter of 78mm and a diameter of 4 or 2 curved surfaces, and has the set center thickness described in Table 1.

[0791] The casting is placed in an insulated container at 25°C and left to stand for 2 hours for insulated polymerization. After that, the casting is removed from the insulated container and further heated at 120°C for 1 hour for polymerization.

[0792] The solidified molded body is demolded from the casting mold and further annealed at 120°C for 2 hours to obtain the molded body (lens).

[0793] [Examples 2-4] The amount of polymerization catalyst and the stirring time of the first mixture in the prepolymerization process were changed to the values ​​shown in Table 1, and the casting viscosity of the polymeric composition for optical materials was adjusted to the values ​​shown in Table 1. Otherwise, the molded body (lens) was obtained using the same method as in Example 1.

[0794] [Example 5] A mixture was prepared by adding 0.1 parts by weight of an internal release agent for MR manufactured by Mitsui Chemicals, 1.5 parts by weight of Tinuvin 329 (UV absorber), and 50.6 parts by weight of 2,5(6)-bis(isocyanate methyl)-bicyclo-[2.2.1]-heptane (monomer for optical materials). The mixture was stirred at 25°C for 1 hour to completely dissolve it. Then, 1.7 parts by weight of pentaerythritol tetra(3-mercaptopropionate) (monomer for optical materials) and 1.8 parts by weight of 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane (monomer for optical materials) were added to the mixture, and it was stirred at 25°C for 5 minutes to prepare a homogeneous solution. Further, 0.2 parts by weight of 3,5-dimethylpyridine (polymerization catalyst) were added to the obtained homogeneous solution, and it was stirred at 40°C for 3 hours. Thus, the monomer for optical materials was polymerized while adjusting the viscosity to obtain a mixture containing prepolymer. The viscosity of the mixture containing the prepolymer is shown in Table 1.

[0795] Then, the mixture containing the prepolymer was degassed for 1 hour at 400 Pa and 25 °C to obtain the first mixture.

[0796] 22.2 parts by weight of pentaerythritol tetra(3-mercaptopropionate) [monomer for optical materials] and 23.7 parts by weight of 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane [monomer for optical materials] were added to prepare a mixture. The mixture was then degassed at 400 Pa and 25 °C for 1 hour to obtain a second mixture.

[0797] Then, the first mixture and the second mixture are mixed at 20°C to obtain a polymeric composition for optical materials.

[0798] Using the obtained polymeric composition for optical materials, the liquid was fed into a casting mold in the same manner as in Example 1, and the casting viscosity was adjusted to the values ​​shown in Table 1.

[0799] The casting is placed in an insulated container at 25°C and left to stand for 2 hours for insulated polymerization. After that, the casting is removed from the insulated container and further heated at 120°C for 1 hour for polymerization.

[0800] The solidified molded body is demolded from the casting mold and further annealed at 120°C for 2 hours to obtain the molded body (lens).

[0801] [Examples 6-7] The contents of pentaerythritol tetra(3-mercaptopropionate) and 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane in the prepolymerization process were changed to the values ​​shown in Table 1, and the casting viscosity of the polymeric composition for optical materials was adjusted to the values ​​shown in Table 1. Otherwise, the molded body (lens) was obtained using the same method as in Example 5.

[0802] [Example 8] The casting is placed in an insulated container at 25°C and left to stand for 3 hours for insulated polymerization. The casting is then removed from the insulated container and demolded. Otherwise, the molded body (lens) is obtained using the same method as in Example 7.

[0803] [Example 9] Without subjecting the casting to heat insulation polymerization, the temperature was increased from 30°C to 120°C over time and heated for 3 hours for polymerization. Otherwise, the molded body (lens) was obtained using the same method as in Example 7.

[0804] [Examples 10-11] The contents of pentaerythritol tetra(3-mercaptopropionate) and 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane in the prepolymerization process were changed to the values ​​shown in Table 1, and the casting viscosity of the polymeric composition for optical materials was adjusted to the values ​​shown in Table 1. Otherwise, the molded body (lens) was obtained using the same method as in Example 5.

[0805] [Comparative Example 1] A mixture was prepared by adding 0.1 parts by weight of Mitsui Chemicals' internal release agent for MR applications, 1.5 parts by weight of Tinuvin 329 (UV absorber), and 40.6 parts by weight of 2,5(6)-bis(isocyanate methyl)-bicyclo-[2.2.1]-heptane (monomer for optical materials). The mixture was stirred at 25°C for 1 hour to ensure complete dissolution. Then, 23.9 parts by weight of pentaerythritol tetra(3-mercaptopropionate) (monomer for optical materials) and 25.5 parts by weight of 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane (monomer for optical materials) were added to the mixture, and the mixture was stirred at 25°C for 5 minutes to form a homogeneous solution. The solution was degassed at 400 Pa and 25°C for 1 hour to obtain the first mixture.

[0806] 10.0 parts by weight of 2,5(6)-bis(isocyanate methyl)-bicyclo-[2.2.1]-heptane [monomer for optical materials] and 0.035 parts by weight of dibutyltin dichloride (also known as DBC) [polymerization catalyst] were stirred at 25°C for 30 minutes to completely dissolve them, thus obtaining the second mixture.

[0807] Then, the first mixture and the second mixture are mixed at 25°C to obtain a polymeric composition for optical materials.

[0808] Using the obtained polymeric composition for optical materials, the liquid was fed into a casting mold in the same manner as in Example 1. For the casting, no heat insulation polymerization was performed, and the temperature was increased from 10°C to 120°C over time for 38 hours for heat polymerization. Then, a molded body (lens) was obtained using the same method as in Example 1.

[0809] [Comparative Example 2] The first mixture was obtained using the same method as in Comparative Example 1.

[0810] 10.0 parts by weight of 2,5(6)-bis(isocyanate methyl)-bicyclo-[2.2.1]-heptane [monomer for optical materials] and 0.2 parts by weight of 3,5-dimethylpyridine [polymerization catalyst] were stirred at 25°C for 30 minutes to completely dissolve them, thus obtaining the second mixture.

[0811] The first and second mixtures were mixed at 20°C to obtain a polymeric composition for optical materials.

[0812] Using the obtained polymeric composition for optical materials, the liquid was fed into a casting mold in the same manner as in Example 1, and the casting viscosity was adjusted to the values ​​shown in Table 1.

[0813] The casting is placed in an insulated container at 25°C and left to stand for 2 hours for insulated polymerization. After that, the casting is removed from the insulated container and further heated at 120°C for 1 hour for polymerization.

[0814] The solidified molded body is demolded from the casting mold and further annealed at 120°C for 2 hours to obtain the molded body (lens).

[0815] [Table 1] The monomer types recorded in Tables 1 to 3 are as follows.

[0816] a1: A mixture of 2,5-bis(isocyanate-methyl)bicyclo-[2.2.1]-heptane and 2,6-bis(isocyanate-methyl)bicyclo-[2.2.1]-heptane. a2: Isophthalimide diisocyanate a3: Dicyclohexylmethane diisocyanate a4: 1,3-bis(isocyanate-methyl)cyclohexane b1: 4-Mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane b2: Pentaerythritol tetra(3-mercaptopropionate) b3: A mixture of 5,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, and 4,8-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane. b4: Pentaerythritol tetra(2-mercaptoacetate) b5: 2,5-bis(mercaptomethyl)-1,4-dithionecyclohexane As shown in Table 1, embodiments using a manufacturing method for optical materials that includes the following steps can suppress ripples in the obtained optical materials and shorten the manufacturing time of the optical materials: The preparation process involves preparing a total of 100 parts by weight of two or more different monomers for optical materials and 0.010 to 2.0 parts by weight of polymerization catalyst. The prepolymerization process involves mixing two or more different optical materials with a portion of a monomer and at least a portion of a polymerization catalyst, and polymerizing the two or more different optical materials with at least a portion of the monomer to obtain a prepolymer, thereby obtaining a mixture containing the prepolymer. A manufacturing process for a polymeric composition for optical materials involves adding the remainder of at least two different monomers for optical materials to a mixture containing a prepolymer, thereby obtaining a polymeric composition for optical materials containing at least two different monomers for optical materials, a prepolymer, and a polymerization catalyst; and The curing process involves curing two or more different optical material monomers in a polymeric composition for optical materials, thereby obtaining an optical material as a cured product of the polymeric composition for optical materials.

[0817] On the other hand, Comparative Example 2, which did not undergo a prepolymerization process, could not suppress ripples. In Comparative Example 1, although ripples could be suppressed, the manufacturing time of the optical material was a long time of 38 hours, which could not shorten the manufacturing time.

[0818] In the examples, Examples 2 to 4 and Examples 6 to 11, where the viscosity (i.e. casting viscosity) of the polymeric composition for optical materials used during casting is 70 mPa·s or higher, can suppress ripples more effectively.

[0819] [Example 12] 0.03 parts by weight of JP-506H (manufactured by Jōhoku Chemical Industry Co., Ltd.), an acidic phosphate ester, 1.5 parts by weight of Tinuvin 329 [UV absorber], and 40.7 parts by weight of isophthalic diisocyanate [monomer for optical materials] were stirred at 25°C for 1 hour until completely dissolved to prepare a mixture. Then, 49.3 parts by weight of a mixture of 5,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, and 4,8-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane [monomer for optical materials] were added to this mixture and stirred at 25°C for 5 minutes to prepare a homogeneous solution.

[0820] Further, 0.015 parts by mass of 3,5-dimethylpyridine [polymerization catalyst] (pKa value = 6.14) were added to the obtained homogeneous solution, and the mixture was degassed at 400 Pa and 25 °C while stirring for 1 hour. The viscosity was adjusted while the optical material was polymerized with monomers to obtain a first mixture containing the prepolymer. The viscosity of the mixture containing the prepolymer is shown in Table 2.

[0821] Add 10 parts by weight of isophthalene diisocyanate [monomer for optical materials] and 0.01 parts by weight of 3,5-dimethylpyridine [polymerization catalyst] to prepare a mixture. Stir the mixture at 25°C for 15 minutes to obtain a second mixture.

[0822] Then, the first mixture and the second mixture are mixed at 20°C to obtain a polymeric composition for optical materials.

[0823] Using the obtained polymeric composition for optical materials, the liquid was fed into a casting mold in the same manner as in Example 1, and the casting viscosity was adjusted to the values ​​shown in Table 2.

[0824] The casting is placed in an insulated container at 25°C and left to stand for 2 hours for insulated polymerization. After that, the casting is removed from the insulated container and further heated at 120°C for 1 hour for polymerization.

[0825] Then, the molded body (lens) is obtained using the same method as in Example 1.

[0826] [Example 13] The amount of polymerization catalyst and the stirring time of the first mixture in the prepolymerization process were changed to the values ​​shown in Table 2, and the casting viscosity of the polymeric composition for optical materials was adjusted to the values ​​shown in Table 2. Otherwise, the molded body (lens) was obtained using the same method as in Example 12.

[0827] [Example 14] A mixture was prepared by adding 0.03 parts by weight of JP-506H (manufactured by Jōhoku Chemical Industry Co., Ltd.) as an acidic phosphate ester, 1.5 parts by weight of Tinuvin 329 [UV absorber], and 50.7 parts by weight of isophthalene diisocyanate [monomer for optical materials]. The mixture was stirred at 25°C for 1 hour to ensure complete dissolution. Then, 6.9 parts by weight of a mixture of 5,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, and 4,8-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane was added to the mixture, and it was stirred at 25°C for 5 minutes to prepare a homogeneous solution. Further, 0.025 parts by mass of 3,5-dimethylpyridine [polymerization catalyst] were added to the obtained homogeneous solution, and the mixture was stirred at 40°C for 3 hours. This process adjusted the viscosity while polymerizing the optical material with monomers, resulting in a mixture containing the prepolymer. The viscosity of the mixture containing the prepolymer is shown in Table 2.

[0828] Then, the mixture containing the prepolymer was degassed for 1 hour at 400 Pa and 25 °C to obtain the first mixture.

[0829] A mixture of 42.4 parts by mass of 5,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, and 4,8-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane was added and degassed at 400 Pa and 25 °C for 1 hour to obtain a second mixture.

[0830] Then, the first mixture and the second mixture are mixed at 20°C to obtain a polymeric composition for optical materials.

[0831] Using the obtained polymeric composition for optical materials, the liquid was fed into a casting mold in the same manner as in Example 1, and the casting viscosity was adjusted to the values ​​shown in Table 2.

[0832] The casting is placed in an insulated container at 25°C and left to stand for 2 hours for insulated polymerization. After that, the casting is removed from the insulated container and further heated at 120°C for 1 hour for polymerization.

[0833] The solidified molded body is demolded from the casting mold and further annealed at 120°C for 2 hours to obtain the molded body (lens).

[0834] [Examples 15-19] The amount of polymerization catalyst, the content of 5,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, and the mixture of 4,8-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, and the stirring time in the prepolymerization process were changed to the values ​​shown in Table 2. The casting viscosity of the polymerizable composition for optical materials was adjusted to the values ​​shown in Table 2. Otherwise, the molded body (lens) was obtained using the same method as in Example 14.

[0835] [Example 20] The casting is placed in an insulated container at 25°C and left to stand for 3 hours for insulated polymerization. The casting is then removed from the insulated container and demolded. Otherwise, the molded body (lens) is obtained using the same method as in Example 19.

[0836] [Example 21] The casting was not subjected to heat insulation polymerization. Instead, it was heated from 30°C to 120°C over time and polymerized over 3 hours. Otherwise, the molded body (lens) was obtained using the same method as in Example 19.

[0837] [Comparative Example 3] 0.1 parts by weight of an internal release agent for MR (Metallurgical Resin) manufactured by Mitsui Chemicals, 1.5 parts by weight of Tinuvin 329 [UV absorber], and 40.7 parts by weight of isophthalic diisocyanate [monomer for optical materials] were stirred at 25°C for 1 hour until completely dissolved to prepare a mixture. Then, 49.3 parts by weight of a mixture of 5,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, and 4,8-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane were added to this mixture and stirred at 25°C for 5 minutes to prepare a homogeneous solution. The solution was degassed at 400 Pa for 1 hour to obtain the first mixture.

[0838] In addition, 10.0 parts by weight of isophthalene diisocyanate [monomer for optical materials] and 0.008 parts by weight of dimethyl tin dichloride (DMC) [polymerization catalyst] were stirred at 25°C for 10 minutes to completely dissolve them, thus obtaining the second mixture.

[0839] Then, the first mixture and the second mixture are mixed at 20°C to obtain a polymeric composition for optical materials.

[0840] Using the obtained polymeric composition for optical materials, the liquid was fed into a casting mold in the same manner as in Example 1, and the casting viscosity was adjusted to the values ​​shown in Table 2.

[0841] For the casting, no heat insulation polymerization was performed; instead, the temperature was increased from 20°C to 120°C over time, and the polymerization was carried out over 30 hours. Then, the molded body (lens) was obtained using the same method as in Example 1.

[0842] [Comparative Example 4] Instead of 0.1 parts by weight of the internal release agent for MR manufactured by Mitsui Chemicals, 0.03 parts by weight of JP-506H (manufactured by Jōhoku Chemical Industry Co., Ltd.) were used, the first mixture was obtained using the same method as in Comparative Example 3.

[0843] 10.0 parts by weight of isophthalene diisocyanate [monomer for optical materials] and 0.025 parts by weight of 3,5-dimethylpyridine [polymerization catalyst] were stirred at 25°C for 30 minutes until completely dissolved to obtain the second mixture.

[0844] The first and second mixtures were mixed at 20°C to obtain a polymeric composition for optical materials.

[0845] Using the obtained polymeric composition for optical materials, the liquid was fed into a casting mold in the same manner as in Example 1, and the casting viscosity was adjusted to the values ​​shown in Table 2.

[0846] The casting is placed in an insulated container at 25°C and left to stand for 2 hours for insulated polymerization. After that, the casting is removed from the insulated container and further heated at 120°C for 1 hour for polymerization.

[0847] The solidified molded body is demolded from the casting mold and further annealed at 120°C for 2 hours to obtain the molded body (lens).

[0848] [Table 2] As shown in Table 2, embodiments using a manufacturing method for optical materials that includes the following steps can suppress ripples in the obtained optical materials and shorten the manufacturing time of the optical materials: The preparation process involves preparing a total of 100 parts by weight of two or more different monomers for optical materials and 0.010 to 2.0 parts by weight of polymerization catalyst. The prepolymerization process involves mixing two or more different optical materials with a portion of a monomer and at least a portion of a polymerization catalyst, and polymerizing the two or more different optical materials with at least a portion of the monomer to obtain a prepolymer, thereby obtaining a mixture containing the prepolymer. A manufacturing process for a polymeric composition for optical materials involves adding the remainder of at least two different monomers for optical materials to a mixture containing a prepolymer, thereby obtaining a polymeric composition for optical materials containing at least two different monomers for optical materials, a prepolymer, and a polymerization catalyst; and The curing process involves curing two or more different optical material monomers in a polymeric composition for optical materials, thereby obtaining an optical material as a cured product of the polymeric composition for optical materials.

[0849] On the other hand, Comparative Example 4, which did not undergo a prepolymerization process, could not suppress ripples, and the optical material of Comparative Example 3, with a polymerization catalyst content of less than 0.010 parts by mass, had a long manufacturing time of 30 hours, which could not be shortened. In addition, Comparative Example 3 showed poor ripple performance when manufacturing an optical material with a thickness of 15.6 mm (front side: 6 curved surfaces, back side: 2 curved surfaces).

[0850] In the examples, Examples 11-12 and Examples 14-21, where the viscosity (i.e. casting viscosity) of the polymeric composition for optical materials used during casting is 120 mPa·s or higher, can suppress ripples more effectively.

[0851] [Example 22] A mixture was prepared by adding 0.05 parts by weight of JP-506H (manufactured by Jōhoku Chemical Industry Co., Ltd.) as an acidic phosphate ester, 1.5 parts by weight of Tinuvin 329 [UV absorber], and 52 parts by weight of isophthalic acid diisocyanate [monomer for optical materials]. The mixture was stirred at 25°C for 1 hour to ensure complete dissolution. Then, 7.7 parts by weight of 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane [monomer for optical materials] were added to the mixture, and it was stirred at 25°C for 5 minutes to prepare a homogeneous solution. Further, 0.02 parts by weight of 3,5-dimethylpyridine [polymerization catalyst] were added to the obtained homogeneous solution, and the mixture was stirred at 40°C for 3 hours. This process adjusted the viscosity while polymerizing the monomer for optical materials, resulting in a mixture containing a prepolymer. The viscosity of the mixture containing the prepolymer is shown in Table 3.

[0852] Then, the mixture containing the prepolymer was degassed for 1 hour at 400 Pa and 25 °C to obtain the first mixture.

[0853] Add 40.3 parts by mass of 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane and degas the mixture for 1 hour at 400 Pa and 25 °C to obtain the second mixture.

[0854] Then, the first mixture and the second mixture are mixed at 20°C to obtain a polymeric composition for optical materials.

[0855] Using the obtained polymeric composition for optical materials, the liquid was fed into a casting mold in the same manner as in Example 1, and the casting viscosity was adjusted to the values ​​shown in Table 3.

[0856] The casting is placed in an insulated container at 25°C and left to stand for 2 hours for insulated polymerization. After that, the casting is removed from the insulated container and further heated at 120°C for 1 hour for polymerization.

[0857] The solidified molded body is demolded from the casting mold and further annealed at 120°C for 2 hours to obtain the molded body (lens).

[0858] [Examples 23-25] The content of 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane in the prepolymerization process was changed to the values ​​shown in Table 3, and the casting viscosity of the polymeric composition for optical materials was adjusted to the values ​​shown in Table 3. Otherwise, the molded body (lens) was obtained using the same method as in Example 22.

[0859] [Example 26] The casting is placed in an insulated container at 25°C and left to stand for 3 hours for insulated polymerization. The casting is then removed from the insulated container and demolded. Otherwise, the molded body (lens) is obtained using the same method as in Example 25.

[0860] [Example 27] The casting was not subjected to heat insulation polymerization. Instead, it was heated from 30°C to 120°C over time and polymerized over 3 hours. Otherwise, the molded body (lens) was obtained using the same method as in Example 25.

[0861] [Comparative Example 5] 0.1 parts by weight of an internal release agent for MR (Metallurgical Resin) manufactured by Mitsui Chemicals, 1.5 parts by weight of Tinuvin 329 [UV absorber], and 42.0 parts by weight of isophthalic diisocyanate [monomer for optical materials] were stirred at 25°C for 1 hour until completely dissolved to prepare a mixture. Then, 48.0 parts by weight of 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane were added to this mixture, and the mixture was stirred at 25°C for 5 minutes to prepare a homogeneous solution. The solution was degassed at 400 Pa for 1 hour to obtain the first mixture.

[0862] In addition, 10.0 parts by weight of isophthalene diisocyanate [monomer for optical materials] and 0.01 parts by weight of dimethyl tin dichloride (DMC) [polymerization catalyst] were stirred at 25°C for 10 minutes to completely dissolve them, thus obtaining the second mixture.

[0863] Then, the first mixture and the second mixture are mixed at 20°C to obtain a polymeric composition for optical materials.

[0864] Using the obtained polymeric composition for optical materials, the liquid was fed into a casting mold in the same manner as in Example 1, and the casting viscosity was adjusted to the values ​​shown in Table 3.

[0865] For the casting, no heat insulation polymerization was performed; instead, the temperature was increased from 20°C to 120°C over time, and the polymerization was carried out over 38 hours. Then, the molded body (lens) was obtained using the same method as in Example 1.

[0866] [Comparative Example 6] Instead of 0.1 parts by weight of the internal release agent for MR manufactured by Mitsui Chemicals, 0.05 parts by weight of JP-506H (manufactured by Jōhoku Chemical Industry Co., Ltd.) were used, the first mixture was obtained using the same method as in Comparative Example 5.

[0867] 10.0 parts by weight of isophthalene diisocyanate [monomer for optical materials] and 0.02 parts by weight of 3,5-dimethylpyridine [polymerization catalyst] were stirred at 25°C for 30 minutes until completely dissolved to obtain the second mixture.

[0868] The first and second mixtures were mixed at 20°C to obtain a polymeric composition for optical materials.

[0869] Using the obtained polymeric composition for optical materials, the liquid was fed into a casting mold in the same manner as in Example 1, and the casting viscosity was adjusted to the values ​​shown in Table 3.

[0870] The casting is placed in an insulated container at 25°C and left to stand for 2 hours for insulated polymerization. After that, the casting is removed from the insulated container and further heated at 120°C for 1 hour for polymerization.

[0871] The solidified molded body is demolded from the casting mold and further annealed at 120°C for 2 hours to obtain the molded body (lens).

[0872] [Table 3] As shown in Table 3, embodiments using a manufacturing method for optical materials that includes the following steps can suppress ripples in the obtained optical materials and shorten the manufacturing time of the optical materials: The preparation process involves preparing a total of 100 parts by weight of two or more different monomers for optical materials and 0.010 to 2.0 parts by weight of polymerization catalyst. The prepolymerization process involves mixing two or more different optical materials with a portion of a monomer and at least a portion of a polymerization catalyst, and polymerizing the two or more different optical materials with at least a portion of the monomer to obtain a prepolymer, thereby obtaining a mixture containing the prepolymer. A manufacturing process for a polymeric composition for optical materials involves adding the remainder of at least two different monomers for optical materials to a mixture containing a prepolymer, thereby obtaining a polymeric composition for optical materials containing at least two different monomers for optical materials, a prepolymer, and a polymerization catalyst; and The curing process involves curing two or more different optical material monomers in a polymeric composition for optical materials, thereby obtaining an optical material as a cured product of the polymeric composition for optical materials.

[0873] On the other hand, Comparative Example 6, which did not undergo a prepolymerization process, could not suppress the ribs. In Comparative Example 5, the manufacturing time of the optical material was a long time of 38 hours, and the manufacturing time could not be shortened.

[0874] In the examples, Examples 23 to 27, where the viscosity (i.e. casting viscosity) of the polymeric composition for optical materials used during casting is 230 mPa·s or higher, can suppress ripples more effectively.

[0875] [Example 28] Add 58.9 parts by weight of dicyclohexylmethane diisocyanate [monomer for optical materials], 1.5 parts by weight of Tinuvin 329 [ultraviolet absorber], and 0.1 parts by weight of Mitsui Chemicals' internal release agent for MR [internal release agent] to prepare a mixed solution. Stir the mixture at 25°C for 1 hour until completely dissolved. Then, add 4.1 parts by weight of a mixture of 5,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, and 4,8-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane to the mixture and stir at 25°C for 5 minutes to prepare a homogeneous solution. Further, 1.5 parts by weight of 3,5-dimethylpyridine [polymerization catalyst] were added to the obtained homogeneous solution, and the mixture was stirred at 40°C for 4 hours. This process adjusted the viscosity while polymerizing the optical material with monomers, resulting in a mixture containing the prepolymer. The viscosity of the mixture containing the prepolymer is shown in Table 4.

[0876] Then, the mixture containing the prepolymer was degassed for 1 hour at 400 Pa and 25 °C to obtain the first mixture.

[0877] 37.0 parts by mass of a mixture of 5,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, and 4,8-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane were added, and the mixture was degassed at 400 Pa and 25 °C for 1 hour to obtain a second mixture.

[0878] Then, the first mixture and the second mixture are mixed at 20°C to obtain a polymeric composition for optical materials.

[0879] Using the obtained polymeric composition for optical materials, the liquid was fed into a casting mold in the same manner as in Example 1, and the casting viscosity was adjusted to the values ​​shown in Table 4.

[0880] The casting is placed in an insulated container at 25°C and left to stand for 3 hours for insulated polymerization. After that, the casting is removed from the insulated container and further heated at 130°C for 2 hours for polymerization.

[0881] The solidified molded body is demolded from the casting mold and further annealed at 120°C for 2 hours to obtain the molded body (lens).

[0882] [Table 4] As shown in Table 4, embodiments using a manufacturing method for optical materials that includes the following steps can suppress ripples in the obtained optical materials and shorten the manufacturing time of the optical materials: The preparation process involves preparing a total of 100 parts by weight of two or more different monomers for optical materials and 0.010 to 2.0 parts by weight of polymerization catalyst. The prepolymerization process involves mixing two or more different optical materials with a portion of a monomer and at least a portion of a polymerization catalyst, and polymerizing the two or more different optical materials with at least a portion of the monomer to obtain a prepolymer, thereby obtaining a mixture containing the prepolymer. A manufacturing process for a polymeric composition for optical materials involves adding the remainder of at least two different monomers for optical materials to a mixture containing a prepolymer, thereby obtaining a polymeric composition for optical materials containing at least two different monomers for optical materials, a prepolymer, and a polymerization catalyst; and The curing process involves curing two or more different optical material monomers in a polymeric composition for optical materials, thereby obtaining an optical material as a cured product of the polymeric composition for optical materials.

[0883] [Example 29] A mixed solution was prepared by adding 48 parts by weight of 1,3-bis(isocyanate-methyl)cyclohexane [monomer for optical materials], 1.5 parts by weight of Tinuvin 329 [ultraviolet absorber], and 0.18 parts by weight of JP-506H (manufactured by Jōhoku Chemical Industry Co., Ltd.). The mixture was stirred at 25°C for 1 hour to ensure complete dissolution. Then, 4.0 parts by weight of pentaerythritol tetra(2-mercaptoacetate) and 3.9 parts by weight of 2,5-bis(mercaptomethyl)-1,4-dithiacyclohexane were added to the mixture, and it was stirred at 25°C for 5 minutes to prepare a homogeneous solution. Further, 0.1 parts by weight of 3,5-dimethylpyridine [polymerization catalyst] were added to the obtained homogeneous solution, and the mixture was stirred at 40°C for 3 hours. This process adjusted the viscosity while polymerizing the monomer for optical materials, resulting in a mixture containing the prepolymer. The viscosity of the mixture containing the prepolymer is shown in Table 5.

[0884] Then, the mixture containing the prepolymer was degassed for 1 hour at 400 Pa and 25 °C to obtain the first mixture.

[0885] 22.7 parts by weight of pentaerythritol tetra(2-mercaptoacetate) and 22.3 parts by weight of 2,5-bis(mercaptomethyl)-1,4-dithiacyclohexane were added, and the mixture was degassed for 1 hour at 400 Pa and 25 °C to obtain the second mixture.

[0886] Then, the first mixture and the second mixture are mixed at 20°C to obtain a polymeric composition for optical materials.

[0887] Using the obtained polymeric composition for optical materials, the liquid was fed into a casting mold in the same manner as in Example 1, and the casting viscosity was adjusted to the values ​​shown in Table 5.

[0888] The casting is placed in an insulated container at 25°C and left to stand for 2 hours for insulated polymerization. After that, the casting is removed from the insulated container and further heated at 120°C for 1 hour for polymerization.

[0889] The solidified molded body is demolded from the casting mold and further annealed at 120°C for 2 hours to obtain the molded body (lens).

[0890] [Table 5] As shown in Table 5, embodiments using a manufacturing method for optical materials that includes the following steps can suppress ripples in the obtained optical materials and shorten the manufacturing time of the optical materials: The preparation process involves preparing a total of 100 parts by weight of two or more different monomers for optical materials and 0.010 to 2.0 parts by weight of polymerization catalyst. The prepolymerization process involves mixing two or more different optical materials with a portion of a monomer and at least a portion of a polymerization catalyst, and polymerizing the two or more different optical materials with at least a portion of the monomer to obtain a prepolymer, thereby obtaining a mixture containing the prepolymer. A manufacturing process for a polymeric composition for optical materials involves adding the remainder of at least two different monomers for optical materials to a mixture containing a prepolymer, thereby obtaining a polymeric composition for optical materials containing at least two different monomers for optical materials, a prepolymer, and a polymerization catalyst; and The curing process involves curing two or more different optical material monomers in a polymeric composition for optical materials, thereby obtaining an optical material as a cured product of the polymeric composition for optical materials.

[0891] [Examples 101-103] In the prepolymerization process, the isocyanate and thiol [monomers for optical materials] listed in Table 6 were used in the amounts listed in Table 6, 3,5-dimethylpyridine [polymerization catalyst] was used in the amounts listed in Table 6, and MR internal release agent [release agent] was used in the amounts listed in Table 6. The preparation was carried out in the manner described in Table 7, with the amount of optical material monomers added to the polymerizable composition for optical materials being adjusted as described in Table 6. Otherwise, the molded article (lens) was obtained using the same method as in Example 5. The evaluation of the corrugations is shown in Table 6.

[0892] [Examples 104-105] In the prepolymerization process, the isocyanate and thiol [monomers for optical materials] listed in Table 6 were used in the amounts listed in Table 6, 3,5-dimethylpyridine [polymerization catalyst] was used in the amounts listed in Table 6, and JP-506H [release agent] was used in the amounts listed in Table 6. The preparation was carried out in the manner described in Table 7, with the amount of optical material monomers added to the polymerizable composition for optical materials being adjusted as described in Table 6. Otherwise, the molded article (lens) was obtained using the same method as in Example 22. The evaluation of the corrugations is shown in Table 6.

[0893] [Example 106] A mixture was prepared by adding 1.5 parts by weight of Tinuvin 329 [UV absorber] and 48.9 parts by weight of isophthalene diisocyanate [monomer for optical materials]. The mixture was stirred at 25°C for 1 hour to ensure complete dissolution. Then, 10.1 parts by weight of 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane [monomer for optical materials] was added to the mixture, and it was stirred at 25°C for 5 minutes to form a homogeneous solution. Further, 0.025 parts by weight of 3,5-dimethylpyridine [polymerization catalyst] was added to the resulting homogeneous solution, and the mixture was stirred at 40°C for 1 hour. This process adjusted the viscosity while polymerizing the monomer for optical materials, yielding a mixture containing the prepolymer. The viscosity of the mixture containing the prepolymer is shown in Table 6.

[0894] Then, the mixture containing the prepolymer was degassed for 1 hour at 400 Pa and 25 °C, and 0.1 parts by weight of JP-506H [release agent] was added and stirred for 10 minutes to obtain the first mixture.

[0895] A mixture was prepared by adding 37.9 parts by mass of 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane and 3.1 parts by mass of m-phenylene diisocyanate [a monomer for optical materials]. The mixture was stirred at 25°C for 5 minutes to obtain a homogeneous solution. Further, 0.005 parts by mass of 3,5-dimethylpyridine [a polymerization catalyst] were added to the obtained homogeneous solution, and the mixture was stirred at 40°C for 1 hour. This process adjusted the viscosity while polymerizing the monomer for optical materials, resulting in a mixture containing the prepolymer. The viscosity of the mixture containing the prepolymer is shown in Table 6. The mixture was degassed at 400 Pa and 25°C for 1 hour to obtain a second mixture.

[0896] Then, the first mixture and the second mixture are mixed at 20°C to obtain a polymeric composition for optical materials.

[0897] Using the obtained polymeric composition for optical materials, the liquid was fed into a casting mold in the same manner as in Example 1, and the casting viscosity was adjusted to the values ​​shown in Table 6.

[0898] The casting is placed in an insulated container at 25°C and left to stand for 2 hours for insulated polymerization. After that, the casting is removed from the insulated container and further heated at 120°C for 1 hour for polymerization.

[0899] The cured molded body was demolded from the casting mold and further annealed at 120°C for 2 hours to obtain the molded body (lens). The evaluation of the corrugations is shown in Table 6.

[0900] [Examples 107-108] In the prepolymerization process, the isocyanate and thiol [monomers for optical materials] listed in Table 6 were used in the amounts listed in Table 6, 3,5-dimethylpyridine [polymerization catalyst] was used in the amounts listed in Table 6, and JP-506H [release agent] was used in the amounts listed in Table 6. The preparation was carried out in the manner described in Table 7, with the amount of optical material monomers added to the polymerizable composition for optical materials being adjusted as described in Table 6. Otherwise, the molded article (lens) was obtained using the same method as in Example 14. The evaluation of the corrugations is shown in Table 6.

[0901] [Table 6] [Table 7] The details of the records for each item in Tables 6 and 7 are as follows.

[0902] ·NBDI 2,5(6)-bis(isocyanate-methyl)-bicyclo-[2.2.1]-heptane XDI (isophthalamide diisocyanate) ·PEMP Pentaerythritol tetra(3-mercaptopropionate) ·GST 4-Mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane • A mixture of FSH 5,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, and 4,8-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane Hereinafter, an embodiment of the second embodiment will be specifically described using examples, but the second embodiment is not limited to these examples.

[0903] The viscosity measurement method in the examples is the same as that described above.

[0904] The molded articles obtained in each embodiment or comparative example were evaluated as follows.

[0905] (Waves) The molded body was projected using an ultra-high pressure mercury lamp (light source model OPM-252HEG: manufactured by USHIO Inc.), and the transmitted image was observed visually. The evaluation was carried out according to the following criteria.

[0906] A: No U-shaped ribs were observed, or, no U-shaped ribs were clearly observed.

[0907] B: Although a slight U-shaped rib is observed, it is generally acceptable as a finished product.

[0908] C: U-shaped ribs are clearly observed, which is unacceptable as a finished product.

[0909] [Examples 201-211] (Preparation of the composition) A mixture was prepared by adding 0.1 parts by weight of Mitsui Chemicals' internal release agent for MR applications, 1.5 parts by weight of Tinuvin 329 (UV absorber), and 50.6 parts by weight of 2,5(6)-bis(isocyanate methyl)-bicyclo-[2.2.1]-heptane (monomer for optical materials). The mixture was stirred at 25°C for 1 hour to ensure complete dissolution. Then, 3.6 parts by weight of pentaerythritol tetra(3-mercaptopropionate) (monomer for optical materials) and 3.8 parts by weight of 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane (monomer for optical materials) were added to the mixture, and the mixture was stirred at 25°C for 5 minutes to prepare a homogeneous solution. Further, 0.2 parts by mass of 3,5-dimethylpyridine [polymerization catalyst] (pKa = 6.14, -Ea / R = -3397) were added to the obtained homogeneous solution, and the mixture was stirred at 40°C for 3 hours. This process adjusted the viscosity while polymerizing the optical material with monomers, resulting in a mixture containing the prepolymer. The mixture containing the prepolymer was then degassed at 400 Pa and 25°C for 1 hour to obtain the first raw material composition.

[0910] The viscosity Va of the first raw material composition is shown in Table 8.

[0911] 20.3 parts by weight of pentaerythritol tetra(3-mercaptopropionate) [monomer for optical materials] and 21.7 parts by weight of 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane [monomer for optical materials] were added and stirred at 25°C for 15 minutes to prepare a homogeneous solution. The mixture was then degassed at 400 Pa and 25°C for 1 hour to obtain the second raw material composition.

[0912] The viscosity Vb of the second raw material composition is shown in Table 8.

[0913] (Shearing and stirring of the composition) The first raw material composition is loaded into the first can, and the second raw material composition is loaded into the second can.

[0914] Using a gear pump, each composition was fed into a power mixer at the flow rate described in Table 8.

[0915] Next, using a power mixer, shear force is applied to the first and second raw material compositions after they have been fed with liquid, at the rotation speeds specified in Table 8, and the mixture is then passed through a capsule filter (manufactured by F-tech Corporation) with the filtration accuracy specified in Table 8.

[0916] The polymeric composition for optical materials, after passing through the filter, is fed into a stirring tank and stirred at the rotation speeds described in Table 8. Thus, a force is applied to the polymeric composition for optical materials in a direction that is approximately parallel to and opposite to the flow direction to achieve stirring.

[0917] At this point, back pressure is applied using nitrogen from the liquid surface side of the stirred tank at the pressure described in Table 8.

[0918] Then, using a static mixer with the inner diameter and number of elements listed in Table 8, the polymeric composition of the optical material is stirred and then cast into a lens manufacturing mold with a diameter of 78 mm, 4 curved surfaces, and a set center thickness listed in Table 8. The number of casting axes and the amount of casting discharged are shown in Table 8.

[0919] (Cure of the composition) Polymerization reactions can be carried out using any of the following methods.

[0920] • Place the cast mold into an insulated container at 25°C and let it stand for 2 hours for insulated polymerization. Then, remove the casting from the insulated container and further heat it at 120°C for 1 hour for polymerization.

[0921] • Using an oven, heat the cast mold from 30°C to 70°C over 1.5 hours, then from 70°C to 120°C over 0.5 hours, and then maintain the temperature at 120°C for 1 hour for heating polymerization.

[0922] After the polymerization reaction, the mold is allowed to cool naturally. The solidified molded body is then demolded from the mold and further annealed at 120°C for 2 hours to obtain the molded body (lens).

[0923] [Table 8] In Table 8, "-" indicates that no corresponding operation was performed or that no corresponding value exists.

[0924] As shown in Table 8, the embodiments using the manufacturing method of the optical material described below are excellent in the evaluation of corrugations and can suppress U-shaped corrugations in the optical material. The manufacturing method of the optical material is a method for manufacturing optical material using a polymeric composition for optical material containing two or more different optical material monomers and a polymerization catalyst. It includes the following steps: a raw material composition preparation step, preparing a first raw material composition and a second raw material composition; a shearing step, applying shear force to the first raw material composition and the second raw material composition to manufacture the polymeric composition for optical material; a stirring step, applying a stirring force to the polymeric composition for optical material; a casting step, casting the polymeric composition for optical material into a mold after the stirring step; and a curing step, polymerizing the two or more different optical material monomers in the polymeric composition for optical material in the mold, thereby curing the polymeric composition for optical material.

[0925] Hereinafter, an embodiment of the third embodiment will be specifically described using examples, but the third embodiment is not limited to these examples.

[0926] The viscosity measurement method in the examples is the same as that described above.

[0927] The method for the heat resistance index test in the examples is the same as the method described above.

[0928] The method for determining the heat distortion temperature in the embodiments is the same as the method described above.

[0929] The method for determining the energy storage elastic modulus in the embodiments is the same as the method described above.

[0930] The method for the glass ball adhesion test in the embodiments is the same as the method described above.

[0931] The method for measuring adhesive force in the embodiments is the same as that described above.

[0932] The following evaluations were conducted on the cured products (i.e. lenses) obtained in each embodiment or comparative example.

[0933] [End face smoothness] The smoothness of the outer surface of the cured material is confirmed by visual inspection.

[0934] The case where there are no bumps or depressions with a depth of more than 1 mm on the outer peripheral surface is denoted as A, and the case where there are bumps or depressions with a depth of more than 1 mm on the outer peripheral surface is denoted as B.

[0935] [Residual glue] Visual inspection confirmed the presence of residual adhesive in the cured lens and mold.

[0936] Case A is defined as having no adhesive residue, case B is defined as having adhesive residue but being easily removed, and case C is defined as having adhesive residue and being difficult to remove. It should be noted that when adhesive residue is present, the outer surface appears cloudy to the naked eye; when adhesive residue is absent, the outer surface is mirror-like and appears almost transparent.

[0937] [Gap] Visual inspection confirmed whether voids had been formed in the solidified material.

[0938] Let A be the case where no gap is generated, and B be the case where a gap is generated.

[0939] [leakage] Monomer leakage rate: "Monomer leakage" refers to the phenomenon of monomers leaking from the mold inside the oven after injection. The monomer leakage rate is defined and calculated using the following formula: the amount of monomer injected into the mold and the weight of the polymerized resin are measured.

[0940] Cases with a monomer leakage rate of less than 1% are denoted as A, and cases with a monomer leakage rate of more than 1% are denoted as B.

[0941] Monomer injection volume = X (g) Mass of resin after polymerization = Y (g) Individual leakage amount = XY (g) Monomer leakage rate = (XY) / X × 100 (%) [The formation of resin burrs] The so-called "resin burr generation" refers to the phenomenon that burrs are generated when the cured material is demolded from the glass mold due to defects in the cured material.

[0942] Let A be the case where no burrs are generated, and B be the case where burrs are generated.

[0943] [White turbidity / dissolution] Visual inspection confirmed whether any white turbidity or dissolution of the adhesive had occurred in the cured material.

[0944] Cases where no turbidity or dissolution of the adhesive is confirmed are denoted as A, and cases where turbidity or dissolution of the adhesive is confirmed are denoted as B.

[0945] [Sudden rise] Visual inspection confirmed whether the intersection of one main surface and the outer peripheral surface of the cured material, and the intersection of the other main surface and the outer peripheral surface, contained a protrusion that was approximately parallel to the outer peripheral surface.

[0946] Record the case where a protrusion is confirmed as A, and the case where a protrusion is not confirmed as B.

[0947] <membrane> The membrane used in this embodiment is described below.

[0948] A: SLIONTEC #6261 (manufactured by Maxell Corporation) B: Mending tape #810 (manufactured by 3M Japan Co., Ltd.) C: SLIONTEC 6263-73 (manufactured by Maxell Corporation) Details of each membrane are shown in Table 9.

[0949] [Example 301] A mixture was prepared by adding 0.1 parts by weight of Mitsui Chemicals' internal release agent for MR applications, 1.5 parts by weight of Tinuvin 329 (UV absorber), and 50.6 parts by weight of 2,5(6)-bis(isocyanate methyl)-bicyclo-[2.2.1]-heptane (monomer for optical materials). The mixture was stirred at 25°C for 1 hour to ensure complete dissolution. Then, 3.1 parts by weight of pentaerythritol tetra(3-mercaptopropionate) (monomer for optical materials) and 3.3 parts by weight of 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane (monomer for optical materials) were added to the mixture, and the mixture was stirred at 25°C for 5 minutes to prepare a homogeneous solution. Furthermore, the polymerization catalysts listed in Table 9 are added to the obtained homogeneous solution in an amount equal to that listed in Table 9, and stirred at 40°C for 3 hours. Thus, the optical material is polymerized with monomers while adjusting the viscosity, resulting in a mixture containing prepolymers.

[0950] Then, the mixture containing the prepolymer was degassed for 1 hour at 400 Pa and 25 °C to obtain the first mixture.

[0951] 20.8 parts by weight of pentaerythritol tetra(3-mercaptopropionate) [monomer for optical materials] and 22.2 parts by weight of 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane [monomer for optical materials] were added to prepare a mixture. The mixture was then degassed at 400 Pa and 25 °C for 1 hour to obtain a second mixture.

[0952] Then, the first and second mixtures were mixed at 20°C to obtain a polymerizable composition. The slope of the viscosity-enhancing curve of the obtained polymerizable composition at 25°C was 4.6822.

[0953] A film as described in Table 9 is attached to the outer peripheral surfaces of two mold substrates arranged at a predetermined interval to form a space surrounded by the two mold substrates and the aforementioned film, thereby creating a casting mold.

[0954] While the obtained polymeric composition is further mixed in a static mixer, it is injected at a rate of 6 g / s into the aforementioned space with a center thickness of 10 mm, which is composed of a four-curved glass mold (upper mold) with a diameter of 80 mm and a four-curved glass mold (lower mold) with a diameter of 80 mm.

[0955] The viscosity (also known as casting viscosity) of the polymeric composition when the liquid is fed into the mold and cast is adjusted to the values ​​shown in Table 9.

[0956] The castings are heated in an oven at the temperatures and times specified in Table 9 to induce polymerization.

[0957] The cured material is demolded from the casting mold and further annealed at 120°C for 2 hours to obtain the cured material (lens).

[0958] [Example 302] The casting was placed in an insulated container at 25°C and allowed to stand for the curing time specified in Table 9 for insulated polymerization. Otherwise, the procedure was the same as in Example 301 to obtain a lens. The maximum curing temperature is shown in Table 9.

[0959] [Example 303] A mixture was prepared by adding 0.05 parts by weight of JP-506H (manufactured by Jōhoku Chemical Industry Co., Ltd.) as an acidic phosphate ester, 1.5 parts by weight of Tinuvin 329 [UV absorber], and 52.0 parts by weight of isophthalene diisocyanate [monomer for optical materials]. The mixture was stirred at 25°C for 1 hour to ensure complete dissolution. Then, 12.0 parts by weight of 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane [monomer for optical materials] was added to the mixture, and it was stirred at 25°C for 5 minutes to prepare a homogeneous solution. Further, the polymerization catalyst listed in Table 9 was added to the obtained homogeneous solution in an amount equal to that listed in Table 9, and the mixture was stirred at 40°C for 3 hours. This process was used to adjust the viscosity while polymerizing the monomer for optical materials, resulting in a mixture containing the prepolymer. The viscosity of the mixture containing the prepolymer is shown in Table 9.

[0960] Then, the mixture containing the prepolymer was degassed for 1 hour at 400 Pa and 25 °C to obtain the first mixture.

[0961] Add 36.0 parts by mass of 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane and degas the mixture for 1 hour at 400 Pa and 25 °C to obtain the second mixture.

[0962] Then, the first mixture and the second mixture were mixed at 20°C to obtain a polymerizable composition.

[0963] The slope of the thickening curve of the obtained polymeric composition at 25°C was 1.8476.

[0964] Using the obtained polymeric composition, the liquid was fed into a casting mold in the same manner as in Example 301, and the casting viscosity was adjusted to the values ​​shown in Table 9.

[0965] The castings are heated in an oven at the temperatures and times specified in Table 9 to induce polymerization.

[0966] The cured material is demolded from the casting mold and further annealed at 120°C for 2 hours to obtain the cured material (lens).

[0967] [Example 304] The casting was placed in an insulated container at 25°C and allowed to stand for the curing time specified in Table 9 for insulated polymerization. Otherwise, the procedure was the same as in Example 303 to obtain the lens. The maximum curing temperature is shown in Table 9.

[0968] [Example 305] 0.1 parts by weight of JP-506H were added, and the polymerization catalyst was added in the amounts listed in Table 9. Otherwise, the procedure was the same as in Example 303 to obtain the lens. The maximum curing temperature is shown in Table 9.

[0969] The slope of the viscosity-enhancing curve of the obtained polymeric composition at 25°C was 0.9010.

[0970] It should be noted that in Examples 301 and 302, for the polymerizable composition, at the point when the temperature of the polymerizable composition reaches 40°C after the start of polymerization, the viscosity measured by a Type B viscometer at 40°C and 60 rpm is 164 mPa·s.

[0971] [Comparative Example 301] The lens was obtained by changing the membrane to the one described in Table 9, otherwise operating in the same manner as in Example 301. The maximum curing temperature is shown in Table 9.

[0972] [Comparative Example 302] The lens was obtained by changing the membrane to the one described in Table 9, otherwise operating in the same manner as in Example 302. The maximum curing temperature is shown in Table 9.

[0973] [Comparative Example 303] A mixed solution was prepared by adding 0.035 parts by weight of dibutyltin dichloride (II) [polymerization catalyst], 0.1 parts by weight of internal release agent for MR manufactured by Mitsui Chemicals Co., Ltd. [internal release agent], 1.5 parts by weight of Tinuvin 329 [ultraviolet absorber], and 50.6 parts by weight of 2,5(6)-bis(isocyanate methyl)-bicyclo-[2.2.1]-heptane [monomer for optical materials...

Claims

1. A method for manufacturing optical materials, comprising using two or more different optical material monomers totaling 100 parts by mass and 0.010 to 2.0 parts by mass of a polymerization catalyst as raw materials to manufacture optical materials. The monomers used in the two or more different optical materials include isocyanate compound (A) and polythiol compound having two or more thiol groups. The manufacturing method includes the following steps: The preparation process involves preparing a total of 100 parts by weight of the two or more different monomers for optical materials and 0.010 to 2.0 parts by weight of the polymerization catalyst. The prepolymerization process involves mixing a portion of the monomers of the two or more different optical materials with at least a portion of the polymerization catalyst, and polymerizing at least a portion of the monomers of the two or more different optical materials to obtain a prepolymer, thereby obtaining a mixture containing the prepolymer. A manufacturing process for a polymeric composition for optical materials involves adding the remainder of at least two different monomers for optical materials to a mixture comprising the prepolymer, thereby obtaining a polymeric composition for optical materials comprising the two or more different monomers for optical materials, the prepolymer, and the polymerization catalyst. and The curing process involves curing two or more different optical material monomers in the polymeric composition for optical materials, thereby obtaining an optical material as a cured product of the polymeric composition for optical materials. After the manufacturing process of the polymeric composition for optical materials and before the curing process, a liquid feeding process is included, in which the polymeric composition for optical materials is liquided and fed into a casting mold. The liquid delivery process involves simultaneously mixing the polymeric composition of the optical material in a static mixer and delivering it to a casting mold. The viscosity of the polymeric composition of the optical material at the time of delivery to the mold and casting is referred to as the casting viscosity. A portion of the two or more different optical material monomers used in the prepolymerization process comprises at least one selected from 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane, 5,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,8-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, and pentaerythritol tetra(3-mercaptopropionate). The casting viscosity of the polymeric composition for the optical material, measured using a Type B viscometer at 25°C and 60 rpm, is 110 mPa·s to 1000 mPa·s.

2. The method for manufacturing the optical material as described in claim 1, wherein, The prepolymerization process is as follows: mixing a portion of the monomers of the two or more different optical materials and all of the polymerization catalyst, and polymerizing at least a portion of the portion of the monomers of the two or more different optical materials to obtain a prepolymer, thereby obtaining a mixture containing the prepolymer.

3. The method for manufacturing the optical material as described in claim 2, wherein, A portion of the two or more different optical material monomers consists of all of one of the two or more different optical material monomers and a portion of the other optical material monomers besides the one optical material monomer.

4. The method for manufacturing the optical material as described in claim 1, wherein, The prepolymerization process is as follows: mixing a portion of the monomers of the two or more different optical materials and a portion of the polymerization catalyst, and polymerizing at least a portion of the monomers of the two or more different optical materials to obtain a prepolymer, thereby obtaining a mixture containing the prepolymer; The manufacturing process of the polymeric composition for optical materials is as follows: adding at least the remaining portions of the two or more different monomers for optical materials and the remaining portions of the polymerization catalyst to a mixture containing the prepolymer, thereby obtaining a polymeric composition for optical materials containing the two or more different monomers for optical materials, the prepolymer, and the polymerization catalyst.

5. The method for manufacturing the optical material as described in claim 4, wherein, A portion of the two or more different optical material monomers comprises a portion of isocyanate compound (A), and the remaining portion of the two or more different optical material monomers comprises the remaining portion of isocyanate compound (A).

6. The method for manufacturing the optical material as described in claim 4 or claim 5, wherein, A portion of the polymerization catalyst is 5 to 80 parts by mass out of 100 parts by mass of the polymerization catalyst.

7. The method for manufacturing the optical material according to any one of claims 1 to 5, wherein, A portion of the two or more different optical material monomers is 5 to 95 parts by mass out of 100 parts by mass of the two or more different optical material monomers.

8. A method for manufacturing an optical material according to any one of claims 1 to 5, wherein, After the prepolymerization process and before the manufacturing process of the polymeric composition for the optical material, a viscosity adjustment process is included, in which the viscosity of the mixture containing the prepolymer, measured using a Type B viscometer at 25°C and 60 rpm, is adjusted to 30 mPa·s to 2000 mPa·s.

9. The method for manufacturing the optical material as described in claim 1, further comprising the following steps: In the second prepolymerization step, the remaining portions of the monomers of the two or more different optical materials and the remaining portions of the polymerization catalyst are mixed, and at least a portion of the remaining portions of the monomers of the two or more different optical materials are polymerized to obtain a second prepolymer, thereby obtaining a mixture containing the second prepolymer. A manufacturing process for a polymerizable composition for optical materials involves adding a mixture containing the second prepolymer to a mixture containing the prepolymer, thereby obtaining a polymerizable composition for optical materials containing the prepolymer, the second prepolymer, and the polymerization catalyst; and The curing process cures the prepolymer and the second prepolymer in the polymeric composition for optical materials, thereby obtaining an optical material as a cured product of the polymeric composition for optical materials.

10. A method for manufacturing an optical material according to any one of claims 1 to 5, wherein, The curing process includes a step of curing the optical material with the polymeric composition by allowing the optical material to stand in a static state.

11. A method for manufacturing an optical material according to any one of claims 1 to 5, wherein, The curing process includes a step of curing the optical material with a polymeric composition by placing the optical material in a closed space and allowing it to stand.

12. The method for manufacturing the optical material according to any one of claims 1 to 5, wherein, The curing process includes a step of curing the optical material with the polymeric composition by allowing it to stand without external heating.

13. The method for manufacturing the optical material according to any one of claims 1 to 5, wherein, The curing process includes a step of curing the optical material with the polymeric composition by letting the optical material stand for 2 to 10 hours.

14. A method for manufacturing an optical material according to any one of claims 1 to 5, wherein, The isocyanate compound (A) comprises at least one of an alicyclic isocyanate compound and an aromatic isocyanate compound.

15. A method for manufacturing an optical material according to any one of claims 1 to 5, wherein, The polymerization catalyst comprises at least one selected from the group consisting of basic catalysts with a pKa value of 4 to 8 and organometallic catalysts.

16. A method for manufacturing an optical material according to any one of claims 1 to 5, wherein, The polymerization catalyst comprises at least one selected from the group consisting of amine catalysts and organotin catalysts.

17. A method for manufacturing an optical material according to any one of claims 1 to 5, wherein, The polymerization catalyst comprises at least one selected from the group consisting of 3,5-dimethylpyridine, 2,4,6-trimethylpyridine, triethylenediamine, N,N-dimethylethanolamine, triethylamine, N-ethylmorpholine, dibutyltin dichloride, dimethyltin dichloride, dibutyltin dilaurate, and dibutyltin diacetate.

18. A method for manufacturing an optical material according to any one of claims 1 to 5, wherein the method comprises manufacturing an optical material using a polymerizable composition for optical materials containing two or more different monomers for optical materials and a polymerization catalyst, the method comprising the following steps: The raw material composition preparation process includes preparing the first raw material composition and the second raw material composition; A shearing process is performed by applying shear force to the first raw material composition and the second raw material composition to manufacture the polymeric composition for optical materials; The stirring process involves applying a stirring force to the polymeric composition for the optical material. The casting process involves casting the optical material into a mold using a polymeric composition after the stirring process. and The curing process involves polymerizing the optical material in the mold with monomers of two or more different optical materials from the polymeric composition, thereby curing the optical material with the polymeric composition. At least one of the first raw material composition and the second raw material composition contains a mixture comprising the prepolymer.

19. The method for manufacturing the optical material as described in claim 18, wherein, The absolute value V of the difference between the viscosity Va of the first raw material composition measured by a type B viscometer at 25°C and 60 rpm and the viscosity Vb of the second raw material composition measured by a type B viscometer at 25°C and 60 rpm is in the range of 20 mPa·s to 1500 mPa·s.

20. The method for manufacturing the optical material as described in claim 19, wherein, The viscosity Va is in the range of 10 mPa·s to 2000 mPa·s.

21. The method for manufacturing the optical material as described in claim 18, wherein, The polymerization catalyst satisfies the following condition 1. [Condition 1] -Ea / R is above -7100 and below -2900 Ea is the activation energy calculated from the reaction rate constants of the monomers of the two or more different optical materials at two or more different temperatures using an Arrhenius curve, and R is the gas constant with a value of 8.314 J / mol / K.

22. The method for manufacturing the optical material as described in claim 18, wherein, The polymerization catalyst comprises at least one of the following groups: basic catalysts with a pKa value of 4 to 8 and organometallic catalysts.

Citation Information

Patent Citations

  • LED lighting device

    JP2020194660A

  • Lithium composite oxide and lithium secondary battery comprising the same

    JP2021084856A

  • Extended reality instrument interaction zone for navigated robotic surgery

    JP2021122743A

  • Display control apparatus, display control method, and program

    JP2021124696A

  • Image forming apparatus

    JP2021124697A