Secondary battery activation method

By deriving the reduction reaction voltage and setting the pre-charge termination voltage, pre-charge and pre-aging operations are performed, solving the problem of uneven film formation of electrolyte additives on the negative electrode surface in secondary batteries, thereby improving battery life and safety.

CN116529927BActive Publication Date: 2026-11-24LG ENERGY SOLUTION LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202280007536.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-09-10
Filing Date
2022-09-06
Publication Date
2026-11-24
Estimated Expiration
2042-09-06

AI Technical Summary

Technical Problem

In the pre-charging process of secondary batteries, the electrolyte additives form an uneven film on the surface of the negative electrode, which reduces the battery life characteristics and cannot effectively suppress low voltage faults caused by metal foreign objects.

Method used

By deriving the reduction reaction voltage, setting the charging termination voltage of the pre-charging operation to be less than the reduction reaction voltage, performing pre-charging and pre-aging operations, forming a uniform solid electrolyte interface (SEI) film, reducing the negative electrode potential, and preventing metal elution.

Benefits of technology

It effectively suppresses the negative electrode reaction of electrolyte additives, prevents low voltage failure, uniformly forms SEI film, and improves battery life and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116529927B_ABST
    Figure CN116529927B_ABST
Patent Text Reader

Abstract

A method for activating a secondary battery is provided, the method comprising: deriving a reduction reaction voltage based on an electrolyte additive; a pre-charging operation of pre-charging a secondary battery in which an electrolyte containing an electrolyte additive has been injected; and a pre-aging operation of immersing an electrode assembly contained in the secondary battery with the injected electrolyte and aging the electrode assembly, wherein the charging termination voltage in the pre-charging operation is less than the reduction reaction voltage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0121099, filed on September 10, 2021, the entire contents of which are incorporated herein by reference.

[0002] This invention relates to a method for activating a secondary battery, and more specifically, to a method for activating a secondary battery that can reduce the potential of the negative electrode only by pre-charging before immersion, while suppressing the negative electrode reaction of some additives contained in the electrolyte. Background Technology

[0003] Unlike primary batteries, which cannot be recharged, secondary batteries are rechargeable and dischargeable batteries, widely used in electronic devices such as mobile phones, laptops, computers, cameras, and electric vehicles. In particular, lithium-ion secondary batteries have a larger capacity and higher energy density per unit weight compared to nickel-cadmium or nickel-metal hydride batteries; therefore, their utilization is rapidly increasing.

[0004] In this type of lithium secondary battery, lithium-based oxides and carbon materials are mainly used as positive and negative electrode active materials, respectively. The lithium secondary battery includes: an electrode assembly, wherein a positive electrode plate coated with positive and negative electrode active materials respectively has a separator inserted between it; and a coating material that seals and contains the electrode assembly together with the electrolyte.

[0005] Meanwhile, based on the shape of the battery casing, lithium secondary batteries are classified into can-type secondary batteries and pouch-type secondary batteries. In can-type secondary batteries, the electrode assembly is embedded in a metal can, while in pouch-type secondary batteries, the electrode assembly is embedded in a pouch of aluminum laminated sheet.

[0006] Typically, secondary batteries are manufactured by injecting a liquid electrolyte—that is, a liquid electrolyte solution—with the electrode assembly housed in a battery casing and then sealing the battery casing.

[0007] During manufacturing or use, these lithium secondary batteries may exhibit various types of defects for a variety of reasons. In particular, some manufactured secondary batteries have shown low-voltage failure due to high self-discharge rates or higher voltage drops.

[0008] Low voltage failures in secondary batteries are typically caused by metallic foreign objects located inside the battery. Specifically, when a metallic foreign object such as iron or copper is present on the positive electrode, it can grow as dendrites in the negative electrode. Furthermore, such dendrites can cause internal short circuits in the secondary battery, leading to malfunction or damage, or in severe cases, combustion.

[0009] To address the above issues, various attempts have been made, one of which is pre-charging as a representative method. This involves charging the negative electrode after electrolyte injection, prior to electrolyte wetting, to reduce the electrode potential. The negative electrode potential before charging is greater than or equal to 3V, which is the reduction potential of Li and corresponds to a higher potential than the reduction potential of iron (2.59V) and nickel (2.78V) within the monomer. After electrolyte injection, the electrolyte gradually wets the interior of the electrode pores. In this situation, foreign matter or Cu may be oxidized and eluted. Therefore, by performing a pre-charging process after electrolyte injection when electrolyte wetting is complete, the negative electrode potential can be reduced to prevent the elution of foreign matter or metals such as Cu.

[0010] However, since pre-charging begins and proceeds before the electrolyte fully wets the interior of the electrode pores, some additives contained in the electrolyte may induce reduction reactions on the surface of the negative electrode during pre-charging, forming an inhomogeneous film. Therefore, the battery's lifespan characteristics may be reduced due to the formation of this inhomogeneous film. Thus, it is necessary to develop a technique for suppressing the reactions of additives contained in the electrolyte during pre-charging. Summary of the Invention

[0011] Technical issues

[0012] The purpose of this invention is to provide a technique for reducing the potential of the negative electrode current collector only when precharging is performed before immersing a secondary battery, while suppressing the formation of a film by reacting additives on the surface of the negative electrode.

[0013] Technical solution

[0014] This invention aims to solve the above-mentioned problems and provides a method for activating a secondary battery. The method includes: deriving a reduction reaction voltage based on an electrolyte additive; a pre-charging operation of pre-charging a secondary battery in which an electrolyte containing an electrolyte additive has been injected; and a pre-aging operation of immersing an electrode assembly contained in the secondary battery with the injected electrolyte and aging the electrode assembly, wherein the charging termination voltage in the pre-charging operation is less than the reduction reaction voltage.

[0015] The reduction reaction voltage can be the voltage at the starting point of the reduction reaction in the dQ / dV curve, which is obtained by differentiating the voltage-capacity curve during the first charge of a secondary battery in which an electrolyte containing electrolyte additives has been injected.

[0016] The charging termination voltage during pre-charging can be set within the range of 70% to 99% of the reduction reaction voltage.

[0017] The pre-charging operation can begin within 3 hours immediately following the injection of electrolyte.

[0018] The pre-charge operation can be performed using a constant current charging method.

[0019] During the pre-charge operation, the secondary battery can be charged at a C- rate of 0.01 to 0.5.

[0020] The method may further include: a first charge operation that charges the pre-aged secondary battery after the pre-aging operation is performed; and an aging operation that ages the first-charged secondary battery.

[0021] During the initial charging operation, the secondary battery can be charged while being pressurized.

[0022] The method may further include a complete discharge and a complete charge operation for the secondary battery, which involves completely discharging and fully charging the secondary battery.

[0023] The method may further include an aging process that ages the secondary battery after performing a full discharge and a full charge operation.

[0024] Beneficial effects

[0025] The method for activating a secondary battery according to the present invention can reduce the potential of the negative electrode to prevent low voltage failure and uniformly form a solid electrolyte interface (SEI) film while suppressing the negative electrode reaction of the electrolyte additive. Attached Figure Description

[0026] Figures 1 to 3 This is a flowchart of a method for activating a secondary battery according to an embodiment of the present invention.

[0027] Figure 4 The dQ / dV curve is obtained by differentiating the voltage-capacity curve for each type of additive during the first charge of the secondary battery. Detailed Implementation

[0028] In the following description, exemplary embodiments of the invention will be described in detail with reference to the accompanying drawings. Prior to this, the terms and words used in this specification and claims should not be construed as limited to their common or dictionary meanings, but should be interpreted in a meaning and concept consistent with the technical scope of the invention, based on the principle that the inventors have appropriately defined the terms for the purpose of best describing the invention.

[0029] Therefore, since the embodiments described in this specification and the configurations illustrated in the accompanying drawings are merely exemplary embodiments and do not represent the overall technical scope of the invention, it should be understood that the invention covers various equivalents, modifications and alternatives at the time of filing of this application.

[0030] Figure 1 This is a flowchart of a method for activating a secondary battery according to an embodiment of the present invention. (See reference) Figure 1 The method for activating a secondary battery according to an embodiment of the present invention includes: operation S100, deriving a reduction reaction voltage based on an electrolyte additive; pre-charging operation S200, pre-charging a secondary battery in which an electrolyte containing an electrolyte additive has been injected; and pre-aging operation S300, immersing an electrode assembly contained in the secondary battery with the injected electrolyte and aging the electrode assembly.

[0031] Typically, when a secondary battery is assembled, an activation process is performed on the assembled battery, including processes such as charging, aging, and discharging, to stabilize the battery structure and make it usable. Before initiating the activation process, a pre-aging operation is performed first: the secondary battery, which has been injected with electrolyte, is left at room temperature for a certain period of time to stabilize it, allowing the electrolyte injected into the secondary battery to fully wet the interior of the electrode assembly.

[0032] refer to Figure 1 After the electrolyte is injected into the secondary battery, a pre-aging operation of wetting the electrode assembly with the electrolyte is performed. As described above, in order to suppress low voltage failures caused by the elution of foreign matter or metal, a technique is provided in which a pre-charging operation S200 is performed after the electrolyte is injected and before the pre-aging operation S300 is completed, charging the secondary battery at a predetermined charging rate.

[0033] The introduction of pre-charging has the following advantages: it can reduce the potential of the negative electrode while the electrolyte wets the electrode, thus preventing metal oxidation and leaching, thereby suppressing low-voltage faults. However, the inventors of this invention have discovered that during pre-charging, when the state of charge (SOC) is high, some additive components in the electrolyte are reduced and decomposed to form a non-uniform film on the negative electrode, and this non-uniformity may be further aggravated under high electrode load conditions. Therefore, this invention was conceived to provide a pre-charging method that can reduce the potential of the negative electrode while suppressing the negative electrode reaction of electrolyte additives.

[0034] To improve the ionic conductivity of the electrolyte and the lifespan or safety of the battery, various types of additives are included in the electrolyte. These additives can be categorized according to their function as solid electrolyte interface (SEI) forming / controlling agents on the surface of the negative electrode, overcharge inhibitors in secondary batteries, electrolyte ionic conductivity improvers, flame retardants, etc. These additives have different reduction potentials that react on the surface of the negative electrode.

[0035] Therefore, in this invention, after deriving the reduction reaction voltage according to the type of electrolyte additive, in the pre-charging operation, by setting the charging termination voltage to be less than the reduction reaction voltage, the reduction decomposition reaction of the additive is initiated after wetting with electrolyte, thereby forming a uniform SEI film, and by reducing the potential of the negative electrode before wetting with electrolyte, low voltage faults can be suppressed.

[0036] <Derivation of operation based on the reduction reaction voltage of the additive>

[0037] The operation S100, which derives the reduction reaction voltage based on the electrolyte additive, involves deriving the reduction reaction voltage of the secondary battery as a reference for the charging termination voltage based on the electrolyte additive, in order to set the charging termination voltage during the pre-charging operation. Since aspects of the reduction decomposition reaction and the reduction decomposition voltage vary depending on the type of additive, a suitable reference for the charging termination voltage during the pre-charging operation can be derived through the operation of deriving the reduction reaction voltage according to the present invention.

[0038] In a particular example, the reduction reaction voltage of the additive can be defined as the voltage at the starting point of the reduction reaction of the electrolyte in the dQ / dV curve, which is obtained by differentiating the voltage-capacity curve during the first charge of the secondary battery including the electrolyte additive.

[0039] Figure 4 This is a dQ / dV curve obtained by differentiating the voltage-capacity curve during the first charge of a secondary battery according to an embodiment of the invention, based on the type of additive (Ref. indicates the control group without additives). Reference Figure 4 It shows that the shape of the dQ / dV curve varies depending on the type of additive. No peak was observed for dQ / dV of additive A, while peaks were observed for each dQ / dV of additives B and C. Here, the peak is the point where the slope of dQ / dV increases rapidly and then decreases rapidly, while the starting point can be defined as the point where the slope of dQ / dV begins to increase. Specifically, as... Figure 4 As illustrated in the diagram, the starting point for additive B is observed around 1.5V, while the starting point for additive C is observed around 1.9V. Therefore, the pre-charge termination voltage for a battery including additive B can be set based on 1.5V, and the pre-charge termination voltage for a battery including additive C can be set based on 1.9V.

[0040] A charging method for obtaining a voltage-capacity curve can be performed according to known methods, and in a particular example, a secondary battery including a corresponding electrolyte additive used as an electrolyte is charged at a driving voltage range of 1.0 to 2.7V at room temperature (23°C) and charged at a charging rate of 0.1C-rate until SOC 40% is reached, and the voltage-capacity curve can be obtained by observing the capacity change according to the voltage, but the present invention is not limited thereto.

[0041] In addition, in a specific example, the secondary battery can be a fully single-cell secondary battery.

[0042] <Precharge Operation>

[0043] The pre-charging operation S200 of the present invention is an operation performed after the electrolyte is injected and before immersion in the electrolyte to reduce the potential of the negative electrode and prevent metal leaching. In the present invention, the charging termination voltage in the pre-charging operation is set to be less than the reduction reaction voltage of the electrolyte additive.

[0044] In the pre-charge operation, when charging is performed after setting the charging termination voltage to a voltage exceeding the reaction voltage of the additive, some of the additive is reduced and decomposed to form a non-uniform film on the surface of the negative electrode. In this invention, by setting the charging termination voltage in the pre-charge operation to be less than the reduction reaction voltage of the additive, the reduction and decomposition reaction of the additive takes place after wetting with electrolyte to form a uniform SEI film, thus improving lifetime characteristics.

[0045] In a specific example, the charging termination voltage during the pre-charging operation can be set within a range of 70% to 99% of the reduction reaction voltage of the electrolyte additive, and more preferably within a range of 75% to 95%. A charging termination voltage that is too high is undesirable because there is a possibility that the electrolyte additive will be reduced and decomposed; while a charging termination voltage that is too low is undesirable because it is insufficient to reduce the potential of the negative electrode. Therefore, the above-mentioned ranges are desirable.

[0046] The pre-charging operation of this invention begins after the electrolyte is injected. Immediately following the electrolyte injection, the electrolyte can gradually move into the electrode assembly, and the reduction and decomposition reaction of the electrolyte additives can take place. Therefore, it is preferable that the time interval between the start of electrolyte injection and the start of the pre-charging operation is short. In a specific example, the pre-charging operation can be performed within 6 hours after electrolyte injection, more preferably within 3 hours, and most ideally, immediately after electrolyte injection.

[0047] The charging method in the pre-charging operation of this invention can be performed by a constant current (CC) charging method or a constant voltage-constant current (CC-CV) charging method. Since the pre-charging operation of this invention aims to reduce the potential of the negative electrode, the CC charging method using a constant current is generally suitable. However, in some cases, when an overcurrent flows through the battery, a constant voltage (CV) charging method can be used to control the current.

[0048] In this case, the charging rate of the pre-charge operation can be appropriately set considering the desired time required for the pre-charge operation. Specifically, the C-rate can range from 0.01 to 0.5, preferably 0.02 to 0.4, and more preferably 0.03 to 0.3, but the invention is not limited thereto. When the charging rate is low, the potential of the negative electrode can be steadily reduced, but the time required for pre-charging becomes longer, and the additive may be reduced and decomposed before impregnation. Therefore, a charging rate that is too low is undesirable; conversely, when the charging rate is too high, the potential of the negative electrode drops suddenly, which may cause side effects.

[0049] <Pre-aging process>

[0050] The pre-aging operation S300 is an operation that ages the battery after it has been assembled so that the electrolyte can fully wet the electrode assembly.

[0051] More specifically, when a secondary battery is charged, electrons move along the conductive wires to the negative electrode and are charged, while lithium ions are retained in the negative electrode to achieve charge neutralization. In this case, lithium ions can be retained in areas sufficiently wetted by the electrolyte, i.e., in the areas that maintain the path through which the ions move (wetting areas), but lithium ions are relatively difficult to retain in areas not wetted by the electrolyte (non-wetting areas). Therefore, through a pre-aging process, the battery can be aged in an environment with constant humidity and temperature conditions, allowing the electrolyte to permeate well into both the positive and negative electrodes.

[0052] After the pre-aging operation is performed, an activation process series including an initial charging operation to charge the secondary battery to a predetermined depth of charge and an aging operation to age the charged battery is carefully performed, and in this invention, all process series including the pre-aging process will be described as being included in the concept of the activation process.

[0053] In a specific example, the required time for the pre-aging process can range from 3 hours to 72 hours, 6 hours to 60 hours, or 12 hours to 48 hours, and can be appropriately adjusted according to the materials of the positive electrode, negative electrode, and electrolyte, as well as the design capacity of the secondary battery.

[0054] In addition, the pre-aging process can be performed at room temperature of 20°C to 30°C, specifically 22°C to 28°C, more specifically 23°C to 27°C, and even more specifically 25°C to 27°C, but the present invention is not limited thereto, and the temperature can be appropriately changed according to the characteristics of the battery.

[0055] The activation process of the present invention is performed on a lithium secondary battery. Such a lithium secondary battery is assembled by the following process and then undergoes a pre-aging operation.

[0056] An electrode mixture, including electrode active materials and binders, is applied to an electrode current collector to create a positive and a negative electrode, and then a separator is inserted between the positive and negative electrodes to create an electrode assembly.

[0057] Electrode assemblies manufactured in this way are housed in a battery casing, then an electrolyte is injected, and the battery casing is sealed to assemble the battery.

[0058] Such battery assembly operations are not particularly restricted and can be performed according to known methods.

[0059] Furthermore, the electrode assembly is not particularly limited, as long as it has a structure including a positive electrode, a negative electrode and a separator inserted between the positive electrode and the negative electrode, and can be, for example, a jelly roll type electrode assembly, a stacked type electrode assembly, a stacked / folded type electrode assembly, etc.

[0060] The battery casing is not particularly limited, as long as it is used as a covering material for battery encapsulation, and cylindrical battery casings, prismatic battery casings, or pouch-shaped battery casings can be used.

[0061] Electrolytes may include organic solvents, lithium salts, and additives.

[0062] The organic solvent is not particularly limited, as long as it minimizes decomposition due to redox reactions during battery charging or discharging, and can be, for example, cyclic carbonates, linear carbonates, esters, ethers, or ketones. These materials can be used alone, or in combination of two or more materials.

[0063] Among organic solvents, carbonate organic solvents are particularly preferred. Representative examples of cyclic carbonates may include ethylene carbonate (EC), propylene carbonate (PC), and butenyl carbonate (BC), while representative examples of linear carbonates may include dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), ethyl methyl carbonate (EMC), methyl propyl carbonate (MPC), and ethyl propyl carbonate (EPC).

[0064] Examples of lithium salts can be unlimited and include lithium salts commonly used in electrolytes of lithium secondary batteries, such as LiPF6, LiAsF6, LiCF3SO3, LiN(CF3SO2)2, LiBF4, LiBF6, LiSbF6, LiN(C2F5SO2)2, LiAlO4, LiAlCl4, LiSO3CF3, LiClO4, etc., and these materials can be used alone or in combination of two or more materials.

[0065] Furthermore, the electrolyte further includes additives, and examples of such additives may include any one selected from the group consisting of: vinylene carbonate, ethylene ethylene carbonate, fluoroethylene carbonate, cyclic sulfite, saturated sulfone, unsaturated sulfone, acyclic sulfone, lithium difluoroborate oxalate (LiODFB) and its derivatives, or mixtures of two or more thereof, in order to stably form an SEI film, but the invention is not limited thereto.

[0066] Examples of cyclic sulfites may include vinyl sulfite, methyl vinyl sulfite, ethyl vinyl sulfite, 4,5-dimethyl vinyl sulfite, 4,5-diethyl vinyl sulfite, propylene sulfite, 4,5-dimethyl propylene sulfite, 4,5-diethyl propylene sulfite, 4,6-dimethyl propylene sulfite, 4,6-diethyl propylene sulfite, 1,3-butanediol sulfite, etc. Examples of saturated sulfones may include 1,3-propane sulfone, 1,4-butane sulfone, etc. Examples of unsaturated sulfones may include vinyl sulfone, 1,3-propene sulfone, 1,4-butene sulfone, 1-methyl-1,3-propene sulfone, etc., and examples of cyclic sulfones may include divinyl sulfone, dimethyl sulfone, diethyl sulfone, methyl ethyl sulfone, methyl vinyl sulfone, etc.

[0067] The above additives are added to the electrolyte to improve low-temperature output characteristics by firmly forming an SEI film on the negative electrode, suppress surface decomposition of the positive electrode that may occur during high-temperature cycling operation, and prevent oxidation of the electrolyte.

[0068] When the battery casing is a pouch-type battery casing, an aluminum laminated bag including an aluminum layer can be used. After the electrolyte is injected, the opening of the aluminum laminated bag can be sealed by heat welding or heat sealing.

[0069] Figure 2 This is a flowchart of a method for activating a secondary battery according to an embodiment of the present invention. (See reference) Figure 2 The method for activating a secondary battery according to the present invention further includes: a first charging operation S400 of charging the pre-aged secondary battery after performing a pre-aging operation S300; and an aging operation S500 of aging the first-charged secondary battery.

[0070] <Initial Charging Operation>

[0071] The initial charge operation S400 is an operation that charges the pre-aged secondary battery until the pre-aged secondary battery reaches a predetermined depth of charge. This initial charge operation activates the secondary battery.

[0072] During the initial charge operation, the secondary battery does not need to be fully charged. Specifically, the depth of charge during the initial charge operation can be 75% or less, 15% to 70%, or 30% to 60% of the battery's design capacity (SOC 100%). However, even within these ranges, the SEI film can be sufficiently and stably formed and initial gas generation can be initiated. The set depth of charge value is not limited to this and can be appropriately changed according to the purpose of the activation process.

[0073] As the charging conditions for the first charging operation, charging can be performed based on conditions known in the art.

[0074] In one specific example, during the initial charging operation, charging can be performed with a charging termination voltage of 2.5 to 4.0V and a C-rate of 1.0C or less. However, such a charging termination voltage can vary depending on battery characteristics such as battery capacity and battery materials.

[0075] In addition, the first charge can be performed at temperatures of 20°C to 30°C, specifically 22°C to 28°C, and more specifically 23°C to 27°C.

[0076] Furthermore, the initial charging operation can be performed simultaneously with pressurizing the secondary battery. When the secondary battery is pressurized and undergoing its first charge, the trapping of internal gas within the electrodes can be prevented.

[0077] <Aging Operation>

[0078] In order to stabilize the battery that has been charged for the first time according to the above method or to accelerate the stabilization of the SEI film formed by the first charge, an aging operation S500 is performed to age the secondary battery under various conditions.

[0079] In the aging process, a room temperature aging process can be performed to age the secondary battery for a defined period of time under room temperature / atmospheric pressure conditions. Depending on the purpose, a high temperature aging process can be performed instead of a room temperature aging process, or both a room temperature aging process and a high temperature aging process can be performed. The high temperature aging process is a process of aging the battery in a high temperature environment that can accelerate the stabilization of the SEI film. The high temperature aging process and the room temperature aging process can be performed sequentially on batteries undergoing their first charge.

[0080] In a specific example, a high-temperature aging process can be performed at a temperature of 50°C to 100°C, and preferably 50°C to 80°C. The high-temperature aging process can be performed for 1 hour to 30 hours, and preferably 2 hours to 24 hours.

[0081] In a specific example, the room temperature aging process can be performed at temperatures ranging from 20°C to 30°C, specifically from 22°C to 28°C, more specifically from 23°C to 27°C, and even more specifically from 25°C to 27°C. The room temperature aging process can be performed for 12 hours to 120 hours or 18 hours to 72 hours.

[0082] Figure 3 This is a flowchart of a method for activating a secondary battery according to an embodiment of the present invention. (See reference) Figure 3 It can further perform a full discharge and full charge operation, which involves completely discharging the secondary battery to near 0% SOC and then charging it to 95% (95% SOC) or higher of the designed capacity of the discharged secondary battery. The full discharge and full charge operation can be performed once or repeated two or more times.

[0083] In a specific example, after performing a full discharge and full charge operation, the method for activating a secondary battery according to the invention may further include an additional aging operation. The additional aging operation is a process for stabilizing the secondary battery and can be performed at room temperature or high temperature, specifically, it can be performed for 1 to 21 days. The additional aging operation may include a monitoring (open circuit voltage (OCV) tracking) process, including measuring the battery's OCV at regular time intervals to select low-voltage defective batteries that experience voltage drops exceeding the battery's self-discharge range.

[0084] As needed, the method for activating a secondary battery according to the present invention may further include a degassing operation to release the gas inside the secondary battery to the outside. During the initial charging operation and aging operation, gas is generated inside the secondary battery through a reaction between the electrolyte and the electrodes, and a degassing operation can be performed to release the internal gas to the outside of the battery. In this case, the degassing operation can be performed simultaneously with the aging operation, or it can be performed after the aging operation.

[0085] The invention will be described in more detail below with reference to examples. However, since the configurations described in the embodiments described in this specification are merely exemplary embodiments and do not represent the overall technical scope of the invention, it should be understood that the invention covers various equivalents, modifications, and alternatives at the time of filing.

[0086] Manufacturing Example

[0087] 100 parts by weight of NCM(Li[Ni) used as positive electrode active material 0.8 Co 0.1 Mn 0.1 O2), 1.5 parts by weight of carbon black (FX35, Denka) used as a conductive material, and 2.3 parts by weight of polyvinylidene fluoride (KF9700, Kureha) used as a binder polymer were added to NMP (N-methyl-2-pyrrolidone) used as a solvent to prepare a positive electrode active material slurry. The two side surfaces of the aluminum foil were treated with 640 mg / 25 cm⁻¹. 2 The positive electrode active material slurry is coated with a certain amount of loading and then vacuum dried to obtain the positive electrode.

[0088] 100 parts by weight of artificial graphite (GT, Zichen (China)) used as the negative electrode active material, 1.1 parts by weight of carbon black (Super-P), 2.2 parts by weight of styrene-butadiene rubber and 0.7 parts by weight of carboxymethyl cellulose used as the conductive material were added to water as a solvent to prepare a negative electrode active material slurry. Copper foil was then coated with the negative electrode active material slurry, dried and calendered to manufacture the negative electrode.

[0089] Meanwhile, after preparing a polyethylene separator with a microporous structure incorporating an inorganic layer, the polyethylene separator is inserted between the positive and negative electrodes to manufacture an electrode assembly. This electrode assembly is then embedded in a pouch-type battery casing. Finally, an electrolyte containing 1M LiPF6 and 1wt% additive B (used as an electrolyte additive) is injected into an organic solvent in a 3:7 (volume ratio) mixture of EC and EMC to complete the battery manufacturing process.

[0090] Example

[0091] The battery in the manufacturing example was charged to 40% SOC at room temperature (under charging conditions at a rate of 0.1C, at a temperature of 23°C, and within a driving voltage range of 1.0 to 2.7V) at room temperature, and the resulting voltage-capacity curve obtained by differentiating the capacity curve obtained by observing the change in capacity according to voltage is shown in the figure. Figure 4 (Chinese) Reference Figure 4 It can be seen that the starting point of the reduction reaction of additive B is at a voltage of approximately 1.5V.

[0092] At a point 30 minutes after the electrolyte was injected into the battery in the manufacturing example, the charging termination voltage was set to 1.4V at 23°C, and the battery in the manufacturing example was pre-charged at a constant current rate of 0.1C. Subsequently, the pre-charged battery was aged for 48 hours at 23°C and atmospheric pressure to complete the pre-aging process.

[0093] The initial charge is completed by charging the pre-aged batteries at a C-rate of 0.2C until 65% of the single-cell design capacity (SOC 65%). The batteries undergo a high-temperature aging process at 60°C for 24 hours, followed by a room-temperature aging process at 25°C for 4 days. Afterward, a full discharge and full charge process is performed to activate the secondary batteries.

[0094] Comparison Example 1

[0095] Except for the omission of the operations for deriving the reduction reaction voltage of the additive and the pre-charge operation in Example 1 above, the activation process is performed in the same manner as in Example 1.

[0096] Comparison Example 2

[0097] Except that the charging termination voltage for the pre-charge operation in Example 1 above is set to 2.0V, the activation process is performed in the same manner as in Example 1.

[0098] Experimental Example 1: Pressure Drop After High-Temperature Storage

[0099] For each secondary battery manufactured in the example and comparative examples, the secondary battery was fully charged (SOC 100%) at 0.33C-rate under constant current / constant voltage conditions at 25°C until a cutoff of 4.2V, 50mA was achieved. The initial voltage V1 before storage was then measured using a PNE-0506 charger (manufacturer: Pne Solution Co., Ltd.). After storage at 60°C for one month, the voltage V2 was measured using the same charger and discharger, and the voltage drop is shown in Table 1.

[0100] Experimental Example 2: Capacity retention after 100 cycles

[0101] Each secondary battery manufactured in the example and comparative examples was charged at a C-rate of 0.8C under constant current / constant voltage conditions up to 4.35V, with the charge cut-off at 0.05C, and discharged at 0.5C and 3.0V. Then, charging under constant current / constant voltage conditions at a rate of 0.8C and a charge cut-off at 0.05C up to 4.35V and discharging at 0.5C and 3.0V at room temperature was defined as one cycle, and the cycle capacity retention after 100 cycles is shown as a percentage of the capacity after one cycle in Table 1.

[0102] [Table 1]

[0103]

[0104] Referring to Table 1, in Comparative Example 1 without pre-charging, the voltage drop after one month of storage is much greater than that of the example battery. This is because the example battery underwent pre-charging, which is therefore interpreted as an effect of preventing the leaching of foreign objects or metals.

[0105] Meanwhile, although the battery of Comparative Example 2 underwent a pre-charge operation, the charging termination voltage was set to a voltage exceeding the voltage at which the reductive decomposition reaction of the electrolyte additives occurs during the pre-charge operation. This is therefore interpreted as the reductive decomposition reaction of the additives occurring before sufficient wetting with the electrolyte, and the capacity retention is worse than that of the example battery due to the formation of an uneven SEI film.

[0106] As described above, the method for activating a secondary battery according to the present invention has the following effects: it prevents low-voltage faults and uniformly forms an SEI film by reducing the potential of the negative electrode and suppressing the negative electrode reaction of the electrolyte additive.

Claims

1. A method for activating a secondary battery, comprising: The operation of deriving the reduction reaction voltage based on electrolyte additives; A pre-charging operation is performed on a secondary battery that has been injected with an electrolyte containing the electrolyte additive. A pre-aging process in which the electrode assembly housed in the secondary battery is immersed in the injected electrolyte and the electrode assembly is aged. Wherein, the charging termination voltage in the pre-charging operation is less than the reduction reaction voltage, and The pre-charging operation is performed after the electrolyte is injected and before the electrode assembly is wetted with the electrolyte.

2. The method according to claim 1, wherein, The reduction reaction voltage is the voltage at the starting point of the reduction reaction in the dQ / dV curve, which is obtained by differentiating the voltage-capacity curve during the first charge of the secondary battery containing the electrolyte additive.

3. The method according to claim 2, wherein, The charging termination voltage in the pre-charging operation is set within the range of 70% to 99% of the reduction reaction voltage.

4. The method according to claim 1, wherein, The pre-charging operation begins within 3 hours immediately following the injection of the electrolyte.

5. The method according to claim 1, wherein, The pre-charging operation is performed using a constant current charging method.

6. The method according to claim 5, wherein, During the pre-charge operation, the secondary battery is charged at a C-rate of 0.01 to 0.

5.

7. The method of claim 1, further comprising: After the pre-aging operation is performed The first charging operation for charging a pre-aged secondary battery; as well as An aging process that ages a secondary battery during its first charge.

8. The method according to claim 7, wherein, During the initial charging operation, the secondary battery is charged while being pressurized.

9. The method according to claim 7, further comprising a complete discharge and a complete charge operation of the secondary battery.

10. The method of claim 9, further comprising: An aging process is performed to age the secondary battery after the complete discharge and complete charge operations.

Citation Information

Patent Citations

  • Suppression of algae from pesticide-treated materials

    KR1020210121099A

  • Method for producing lithium ion secondary battery

    CN108808098A