A polyvinylbenzyl chloride-based anion exchange membrane and a method for preparing the same
By introducing a hydrophilic flexible crosslinking agent and hydrophobic side chains into polyvinyl benzyl chloride, the flexibility and ionic conductivity of the anion exchange membrane are improved, solving the problems of poor flexibility and low ionic conductivity of polyvinyl benzyl chloride membranes in the prior art, and realizing the preparation of high-performance anion exchange membranes.
Patent Information
- Application Number
- CN202310600312.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-25
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-05-25
AI Technical Summary
Existing anion exchange membranes based on polyvinyl benzyl chloride suffer from poor flexibility and low ionic conductivity.
By introducing the hydrophilic flexible crosslinking agent Jeffamine and a primary amine containing hydrophobic side chains into polyvinyl benzyl chloride, a crosslinked polymer network is formed, which promotes the separation of hydrophilic and hydrophobic microphases and improves flexibility and ion conduction efficiency.
An anion exchange membrane with superior mechanical properties, high chemical stability, and high ionic conductivity was prepared, making it suitable for large-scale production.
Smart Images

Figure CN116535713B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of anion exchange membrane technology, and more specifically, relates to an anion exchange membrane based on polyvinylbenzyl chloride and its preparation method. Background Technology
[0002] Anion exchange membranes (AEMs) are solid electrolytes composed of cations immobilized on polymers and mobile anions, primarily serving to conduct ions and isolate the positive and negative electrodes. Excellent anion exchange membranes require high ion conductivity, excellent mechanical properties, and outstanding chemical stability. Most polymer grafting of cations is achieved by chloromethylating the polymer backbone and then reacting it with a tertiary amine to generate quaternary ammonium ions; however, this step is not only challenging but also often requires the use of highly toxic substances like chloromethyl ether. The mechanical properties of anion exchange membranes mainly depend on the polymer, but it is difficult for a single polymer to simultaneously possess both high tensile strength and excellent flexibility. For example, phenyl ether polymers are favored by many researchers because they are easily functionalized and have high strength; however, these materials lack sufficient flexibility. Polyolefin polymers, on the other hand, have excellent flexibility but insufficient rigidity. Modern research has shown that polar groups in the polymer backbone are the main factor leading to backbone degradation; however, modifying backbones without polar groups often faces significant challenges. Polyvinyl benzyl chloride has a chloromethyl group in its structural unit, so no additional functionalization reaction is required. In addition, its main chain does not contain polar groups and has high chemical stability, so it has attracted the attention of researchers. However, this polymer is brittle, not resistant to bending, and cannot even form a film.
[0003] In the literature (ACS Applied Energy Materials, 2018, 1, 7, 3479-3487), the authors synthesized a quaternized polyvinylbenzyl chloride crosslinked with a long-chain multi-cationic crosslinking agent. The long-chain multi-cationic crosslinking agent improves the rigidity and flexibility of polyvinylbenzyl chloride, and also constructs a hydrophilic-hydrophobic phase separation to enhance ion conductivity. The sample PVBC-50Q4 exhibits a hydroxide ion conductivity of 74.3 mS / cm at 80 °C. -1 The tensile strength is 16.5 MPa, and the elongation at break is 18.6%. After soaking in 2M KOH solution at 80℃ for 1300 h, the ionic conductivity is retained at 88%, and the ion exchange capacity is retained at 89%.
[0004] In the literature (Journal of The Electrochemical Society, 2019, 166, 15, F1134-F1141), the authors synthesized N-methylpyrrolidone-grafted polyvinylbenzyl chloride. To improve the mechanical properties of this anion exchange membrane, sulfonated polyether ether ketone was introduced for ionic crosslinking. The ion exchange capacity of the sample PVBC-MPy / 10% sPEEK was 2.98 mmol g. -1 The volume swelling ratio at room temperature is 45%; the water content is 20%; and the hydroxide ion conductivity at 80℃ is 28 mS / cm. -1 The tensile strength is 25.6 MPa, and the elongation at break does not exceed 9%. After soaking in 1M KOH solution at 80℃ for 410 h, the retention rate of ionic conductivity is 86.4%.
[0005] In the literature (Polymer, 2021, 212, 123156), the authors synthesized quaternized polyvinylbenzyl chloride based on N-methylpyrrolidone onon grafting. To improve the mechanical properties of this anion exchange membrane, a polysulfone backbone was introduced, and N,N,N',N'-tetramethyl-1,6-hexanediamine was used for chemical crosslinking. The ion exchange capacity of the sample PVBMPy-CL-15%PSF was 2.1 mmol / g. -1 The volume swelling ratio at 30℃ is 26.2%, and the water content is 40.0%; the hydroxide ion conductivity at 80℃ is 32.9 mS / cm. -1 The room temperature tensile strength is 13.1 MPa, and the elongation at break is not more than 10%. After soaking in 1M KOH solution at 80℃ for 580 h, the retention rate of ionic conductivity is 70.5%.
[0006] In summary, while polyvinylbenzyl chloride-based anion exchange membranes possess high chemical stability, they suffer from poor flexibility and low ionic conductivity. Therefore, developing a polyvinylbenzyl chloride-based anion exchange membrane that combines high ionic conductivity, a balance of rigidity and flexibility, and high chemical stability is of great significance. Summary of the Invention
[0007] The purpose of this invention is to provide an anion exchange membrane based on polyvinylbenzyl chloride and its preparation method, thereby improving the problems of poor flexibility and low ionic conductivity of the polymer network of polyvinylbenzyl chloride as anion exchange membrane.
[0008] To achieve the above objectives, one aspect of the present invention provides a method for preparing an anion exchange membrane based on polyvinyl benzyl chloride, the method comprising:
[0009] (1) In the presence of a first organic solvent and a protective gas, 4-chloromethylstyrene monomer is polymerized under the action of an initiator to obtain polyvinylbenzyl chloride;
[0010] (2) In the presence of a second organic solvent, the polyvinyl benzyl chloride and O,O”-di(2-aminopropyl)polypropylene glycol-block-polyethylene glycol-block-polypropylene glycol are reacted; then an organic solution of trimethylamine is added and the reaction is continued to obtain a cross-linked quaternized polyvinyl benzyl chloride film solution.
[0011] (3) Dissolve the polyvinylbenzyl chloride in a third organic solvent, add an organic solution of trimethylamine, and react; then add a primary amine or an organic solution of a primary amine, and continue the reaction to obtain a quaternized polyvinylbenzyl chloride film solution with hydrophobic side-linked branches.
[0012] (4) The cross-linked quaternized polyvinyl benzyl chloride membrane solution is mixed with the hydrophobic side-linked quaternized polyvinyl benzyl chloride membrane solution to obtain a mixed solution. The mixed solution is poured into a mold and dried to obtain a halogen-type anion exchange membrane. The halogen-type anion exchange membrane is subjected to ion exchange with an alkaline solution to obtain the polyvinyl benzyl chloride-based anion exchange membrane with hydroxide ions as the anion.
[0013] In this invention, polyvinylbenzyl chloride is selected as the polymer backbone, which has the advantages of simple synthesis steps, strong rigidity of anion exchange membrane and high chemical stability. A hydrophilic flexible crosslinking agent (Jeffamine) is introduced into polyvinylbenzyl chloride to achieve good flexibility and high water content of anion exchange membrane. A primary amine containing hydrophobic side chains is introduced into polyvinylbenzyl chloride to achieve hydrophilic and hydrophobic microphase separation in anion exchange membrane and promote ion conduction.
[0014] According to the present invention, preferably, in step (1), the first organic solvent is tetrahydrofuran; the initiator is azobisisobutyronitrile; and the protective gas is nitrogen.
[0015] According to the present invention, preferably, in step (1), the polymerization reaction is carried out at a temperature of 40 to 60°C for a time of 9 to 12 hours.
[0016] In this invention, preferably, the reaction is terminated with methanol after completion to obtain a white, flaky crude product. The crude product is then washed with methanol 3-5 times and dried.
[0017] According to the present invention, preferably, in step (2), in the presence of a second organic solvent, the polyvinyl benzyl chloride and O,O”-di(2-aminopropyl)polypropylene glycol-block-polyethylene glycol-block-polypropylene glycol are reacted at 50-60°C for 2-4 hours; the temperature is lowered to 40-45°C, and then an organic solution of trimethylamine is added, and the reaction is continued for 1-2 hours to obtain a crosslinked quaternized polyvinyl benzyl chloride film solution.
[0018] According to the present invention, preferably, in step (2), the second organic solvent is dimethyl sulfoxide; and the organic solution of trimethylamine is a trimethylamine methanol solution.
[0019] According to the present invention, preferably, in step (3), the polyvinylbenzyl chloride is dissolved in a third organic solvent, and an organic solution of trimethylamine is added, and the reaction is carried out at 40-45°C for 1-2 hours; the temperature is raised to 50-60°C, and then a primary amine or an organic solution of a primary amine is added, and the reaction is continued for 2-6 hours to obtain a quaternized polyvinylbenzyl chloride film solution with hydrophobic side-linked branches.
[0020] According to the present invention, preferably, in step (3), the third organic solvent is dimethyl sulfoxide;
[0021] The organic solution of trimethylamine is a trimethylamine methanol solution;
[0022] The organic solution of the primary amine is a tetrahydrofuran solution of the primary amine.
[0023] According to the present invention, preferably, in step (4), the mixing temperature is 40-60°C and the time is 2-4 hours;
[0024] Preferably, the mixed solution is filtered into the mold using a filter material.
[0025] According to the present invention, preferably, the alkaline solution is a KOH solution and / or a NaOH solution;
[0026] The temperature of the alkaline solution is 30-65℃;
[0027] The concentration of the alkaline solution is 1–2 mol / L.
[0028] In this invention, the prepared halogen-type anion exchange membrane is immersed in an alkaline solution to replace the halogen ions with hydroxide ions, ultimately obtaining the polyvinylbenzyl chloride-based anion exchange membrane with hydroxide ions as the anion.
[0029] In this invention, the ion exchange of the halogen-type anion exchange membrane with an alkaline solution involves immersing the halogen-type anion exchange membrane in the alkaline solution. The immersion time is preferably 12-24 hours, and the alkaline solution is preferably replaced 3-5 times during the immersion period.
[0030] Another aspect of the present invention provides an anion exchange membrane based on polyvinyl benzyl chloride prepared by the above preparation method.
[0031] This invention relates to an anion exchange membrane based on polyvinylbenzyl chloride. It utilizes the reaction of a hydrophilic flexible polyether amine with some of the benzyl chloride groups on the polyvinylbenzyl chloride to generate a cross-linked polymer network and improve polymer flexibility. Furthermore, it utilizes a primary amine containing hydrophobic side chains to react with some of the benzyl chloride groups on the polyvinylbenzyl chloride, inducing polymer phase separation and improving ion conduction efficiency. Finally, it utilizes trimethylamine to react with some of the benzyl chloride groups on the polyvinylbenzyl chloride to generate quaternary ammonium groups, which then conduct anions. This membrane exhibits a novel chemical structure, its fabrication process does not involve chloromethylation or highly toxic reactants, and the method is simple and efficient. The resulting anion exchange membrane exhibits uniform formation, high ionic conductivity, superior mechanical properties, and high chemical stability.
[0032] The anion exchange membrane of the present invention has the following characteristics: simple synthesis steps, low cost, uniform film formation, and easy large-scale production; a combination of rigid and flexible mechanical properties; and high ionic conductivity and high chemical stability.
[0033] The technical solution of the present invention has the following beneficial effects:
[0034] (1) The anion exchange membrane based on polyvinyl benzyl chloride disclosed in this invention is composed of a rigid main chain component and a flexible cross-linking component, exhibiting excellent mechanical properties.
[0035] (2) The anion exchange membrane based on polyvinyl benzyl chloride disclosed in this invention can be used to prepare a series of anion exchange membranes with different physical properties according to the different lengths of hydrophobic side chains.
[0036] (3) The anion exchange membrane based on polyvinyl benzyl chloride disclosed in this invention has a high water content, a hydrophilic-hydrophobic phase separation structure, promotes ion conduction, and has high ion conductivity.
[0037] (4) The main chain of the anion exchange membrane based on polyvinyl benzyl chloride disclosed in this invention does not contain polar groups and has high chemical stability.
[0038] (5) The method for preparing anion exchange membrane based on polyvinyl benzyl chloride disclosed in this invention has low requirements for equipment and reaction, simple synthesis steps, low cost, and is suitable for large-scale production.
[0039] Other features and advantages of the present invention will be described in detail in the following detailed description section. Attached Figure Description
[0040] The above and other objects, features and advantages of the present invention will become more apparent from the more detailed description of exemplary embodiments of the invention in conjunction with the accompanying drawings, wherein the same reference numerals generally represent the same components in the exemplary embodiments of the invention.
[0041] Figure 1 An optical photograph of an anion exchange membrane based on polyvinyl benzyl chloride according to Embodiment 3 of the present invention is shown.
[0042] Figure 2 The Fourier transform infrared spectrum of the polyvinylbenzyl chloride-based anion exchange membrane according to Embodiment 3 of the present invention is shown.
[0043] Figure 3 The small-angle X-ray scattering pattern of the anion exchange membrane based on polyvinyl benzyl chloride according to Embodiment 3 of the present invention is shown. Detailed Implementation
[0044] Preferred embodiments of the invention will now be described in more detail. While preferred embodiments of the invention are described below, it should be understood that the invention can be implemented in various forms and should not be limited to the embodiments set forth herein. Rather, these embodiments are provided so that the invention will be thorough and complete, and will fully convey the scope of the invention to those skilled in the art.
[0045] The present invention will be further illustrated by the following examples.
[0046] The O,O”-bis(2-aminopropyl)polypropylene glycol-block-polyethylene glycol-block-polypropylene glycol (Jeffamine) used in the following examples was purchased from Shanghai Yuanye Biotechnology Co., Ltd., Mw=1900, brand name J-2000.
[0047] The concentration of the trimethylamine methanol solution used was 3.2 M. The concentration of the ethylamine tetrahydrofuran solution was 2.0 M.
[0048] The corresponding performance testing methods in the test data of the following embodiments and comparative examples are as follows:
[0049] (1) Ion exchange capacity:
[0050] The ion exchange capacity of AEM was determined using the Mohr titration method, and the calculation formula is shown below. Where c (AgNO3) It is the concentration of AgNO3 solution, v (AgNO3) It is the volume of AgNO3 solution consumed, m dry(OH) This is the dry weight of AEM.
[0051]
[0052] IEC stands for ion exchange capacity.
[0053] (2) Dimensional stability:
[0054] First, record the dry film size x. dry(OH) Then, the dimensions of the AEM with OH- ions after fully absorbing water and swelling at different temperatures were measured and recorded as x. hyd(OH) The formula for calculating dimensional stability is shown below:
[0055]
[0056] SD represents the swelling ratio.
[0057] (3) Moisture content:
[0058] Take an AEM with OH- anion, wipe the water off its surface with filter paper, and weigh it under saturated water content conditions. hyd The membrane was then placed in a vacuum drying oven at 65°C for 12 hours to dry thoroughly until the membrane mass no longer decreased. Its mass W was then measured. dry The formula for calculating water content is as follows:
[0059]
[0060] (4) Gel content test:
[0061] The gel strength (GF) of AEM was calculated by recording the mass change after immersion in dimethyl sulfoxide solvent at 60°C for 24 hours. The dry weight before measurement was m. before The mass obtained after soaking, washing, and drying is m. after The ratio of the two is the gel strength. A higher gel strength indicates a more complete degree of cross-linking.
[0062]
[0063] GF% represents gel strength.
[0064] (5) Mechanical strength: The tensile strength and elongation at break of the AEM under test with saturated water content were tested at 25℃. In the tensile test, the tensile speed was 5 mm / min, and the two-dimensional dimensions of the anion exchange membrane under test were 1 cm × 3 cm.
[0065] (6) Ionic conductivity: The present invention uses AC impedance method to measure the ionic resistance of anion exchange membrane. The measurement frequency range is 1Hz-4MHz, the potential amplitude is 5mV, and the measured resistance Nyquist curve is fitted. The intersection of the curve with the real axis Z' is the ionic resistance value R of the anion exchange membrane.
[0066] The formula for calculating conductivity is shown below:
[0067]
[0068] σ is the ionic conductivity, l is the distance between the two electrodes, R is the ionic resistance of the sample being measured, and S is the cross-sectional area of the membrane.
[0069] (7) Alkali resistance stability: The stability test conditions of the example were 80℃ and soaking in 1mol / L NaOH solution for 720 hours to determine the retention rate of mass and ionic conductivity.
[0070] Example 1
[0071] A method for preparing an anion exchange membrane based on polyvinyl benzyl chloride specifically includes the following steps:
[0072] (a) Under nitrogen protection, 6 g of 4-chloromethylstyrene monomer was added to 50 mL of tetrahydrofuran solvent. After complete dissolution, 0.1 g of azobisisobutyronitrile was added. The mixture was heated under reflux at 60 °C for 9 h. The reaction was stopped and quenched with methanol to obtain a white flake-like crude product. After washing with methanol three times, the product was dried under vacuum at 40 °C to obtain the final product, polyvinylbenzyl chloride.
[0073] (b) Weigh 0.1 g of the synthesized polyvinyl benzyl chloride into 10 mL of dimethyl sulfoxide. After complete dissolution, add 77.81 mg of Jeffamine. React at 60 °C for 2 h, then cool to 40 °C. Add 81.9 μL of trimethylamine methanol solution and continue the reaction for 1 h to obtain a cross-linked quaternized polyvinyl benzyl chloride membrane solution.
[0074] (c) Weigh 0.1 g of the synthesized polyvinyl benzyl chloride into 5 mL of dimethyl sulfoxide. After complete dissolution, add 81.9 μL of trimethylamine methanol solution. React at 40 °C for 1 h, then raise the temperature to 60 °C and add 131.0 μL of ethylamine tetrahydrofuran solution. Continue the reaction for 2 h to obtain a quaternized polyvinyl benzyl chloride membrane solution with hydrophobic side-linked branches.
[0075] (d) The two membrane solutions synthesized in steps b and c above are mixed and stirred at 40°C for 2 hours. The mixed solution is filtered through a filter cloth into a clean glass plate mold and dried at 80°C to form a membrane, thus obtaining a halogen-type polymer electrolyte membrane (halogen-type anion exchange membrane). Then, it is soaked in a 1M potassium hydroxide solution at 60°C for 12 hours, during which the alkali solution is replaced 3 times. Finally, the membrane surface is rinsed with deionized water to remove residual alkali until the pH of the aqueous solution is 7, thus obtaining a hydroxide-type anion exchange membrane based on polyvinyl benzyl chloride.
[0076] The ion exchange capacity of the polyvinylbenzyl chloride-based anion exchange membrane was measured to be 1.76 mmol g. -1The gel strength was 93.1%; the swelling rate at 30℃ was 20.0%; the water content was 161.9%; and the hydroxide ion conductivity at 80℃ was 73.8 mS / cm. -1 The tensile strength and elongation at break at 100% relative humidity were 5.08 MPa and 168.3%, respectively; after soaking in 1M NaOH solution at 80℃ for 720 h, the mass retention rate and ionic conductivity retention rate of the anion exchange membrane were 89.6% and 80.1%, respectively.
[0077] Example 2
[0078] A method for preparing an anion exchange membrane based on polyvinyl benzyl chloride specifically includes the following steps:
[0079] (1) Under nitrogen protection, 6g of 4-chloromethylstyrene monomer was added to 50mL of tetrahydrofuran solvent. After complete dissolution, 0.1g of azobisisobutyronitrile was added. The mixture was heated under reflux at 60℃ for 9h. The reaction was stopped and quenched with methanol to obtain a white flake-like crude product. After washing with methanol three times, the product was dried under vacuum at 40℃ to obtain the final product, polyvinylbenzyl chloride.
[0080] (2) Weigh 0.1g of the synthesized polyvinyl benzyl chloride into 10mL of dimethyl sulfoxide. After it is completely dissolved, add 77.81mg of Jeffamine. React at 60℃ for 2h and then cool down to 40℃. Then add 81.9μL of trimethylamine methanol solution and continue to react for 1h to obtain a cross-linked quaternized polyvinyl benzyl chloride membrane solution.
[0081] (3) Weigh 0.1g of the synthesized polyvinyl benzyl chloride into 5mL of dimethyl sulfoxide. After it is completely dissolved, add 81.9μL of trimethylamine methanol solution. After reacting at 40℃ for 1h, raise the temperature to 60℃ and add 35.0μL of hexylamine. Continue to react for 4h to obtain a quaternized polyvinyl benzyl chloride membrane solution with hydrophobic side-linked branches.
[0082] (4) The two membrane solutions synthesized in steps b and c above are mixed and stirred at 40°C for 2 hours. The mixed solution is filtered through a filter cloth into a clean glass plate mold and dried at 80°C to form a membrane, thus obtaining a halogen-type polymer electrolyte membrane. Then, it is soaked in a 1M potassium hydroxide solution at 60°C for 12 hours, during which the fresh alkali solution is replaced 3 times. Finally, the membrane surface is rinsed with deionized water to remove residual alkali until the pH of the aqueous solution is 7, thus obtaining a hydroxide-type anion exchange membrane based on polyvinyl benzyl chloride.
[0083] The ion exchange capacity of the polyvinylbenzyl chloride-based anion exchange membrane was measured to be 1.65 mmol g. -1The gel strength was 94.9%; the swelling ratio at 30℃ was 17.3%, and the water content was 142.0%; the hydroxide ion conductivity at 80℃ was 99.3 mS / cm. -1 The tensile strength and elongation at break at 100% relative humidity were 5.49 MPa and 175.9%, respectively; after soaking in 1M NaOH solution at 80℃ for 720 h, the mass retention rate and ionic conductivity retention rate of the anion exchange membrane were 96.9% and 80.0%, respectively.
[0084] Example 3
[0085] A method for preparing an anion exchange membrane based on polyvinyl benzyl chloride specifically includes the following steps:
[0086] (1) Under nitrogen protection, 6g of 4-chloromethylstyrene monomer was added to 50mL of tetrahydrofuran solvent. After complete dissolution, 0.1g of azobisisobutyronitrile was added. The mixture was heated under reflux at 60℃ for 9h. The reaction was stopped and quenched with methanol to obtain a white flake-like crude product. After washing with methanol three times, the product was dried under vacuum at 40℃ to obtain the final product, polyvinylbenzyl chloride.
[0087] (2) Weigh 0.1g of the synthesized polyvinyl benzyl chloride into 10mL of dimethyl sulfoxide. After it is completely dissolved, add 77.81mg of Jeffamine. React at 60℃ for 2h and then cool down to 40℃. Then add 81.9μL of trimethylamine methanol solution and continue to react for 1h to obtain a cross-linked quaternized polyvinyl benzyl chloride membrane solution.
[0088] (3) Weigh 0.1g of the synthesized polyvinyl benzyl chloride into 5mL of dimethyl sulfoxide. After it is completely dissolved, add 81.9μL of trimethylamine methanol solution. After reacting at 40℃ for 1h, raise the temperature to 60℃ and add 61.6μL of dodecylamine. Continue to react for 6h to obtain a quaternized polyvinyl benzyl chloride film solution with hydrophobic side-linked branches.
[0089] (4) The two membrane solutions synthesized in steps b and c above are mixed and stirred at 40°C for 4 hours. The mixed solution is filtered through a filter cloth into a clean glass plate mold and dried at 80°C to form a membrane, yielding a halogenated polymer electrolyte membrane. This membrane is then immersed in a 1M potassium hydroxide solution at 60°C for 12 hours, with the alkali solution replaced three times during this period. Finally, the membrane surface is rinsed with deionized water to remove any residual alkali until the pH of the aqueous solution reaches 7, thus obtaining a hydroxide-type anion exchange membrane based on polyvinylbenzyl chloride (e.g., ...). Figure 1 (As shown).
[0090] The ion exchange capacity of the polyvinylbenzyl chloride-based anion exchange membrane was measured to be 1.56 mmol g. -1The gel strength was 94.0%; the swelling ratio at 30℃ was 15.4%, and the water content was 119.1%; the hydroxide ion conductivity at 80℃ was 110.4 mS / cm. -1 The tensile strength and elongation at break at 100% relative humidity were 7.40 MPa and 199.8%, respectively; after soaking in 1M NaOH solution at 80℃ for 720 h, the mass retention rate and ionic conductivity retention rate of the anion exchange membrane were 92.1% and 86.1%, respectively.
[0091] Example 4
[0092] A method for preparing an anion exchange membrane based on polyvinyl benzyl chloride specifically includes the following steps:
[0093] (1) Under nitrogen protection, 6g of 4-chloromethylstyrene monomer was added to 50mL of tetrahydrofuran solvent. After complete dissolution, 0.1g of azobisisobutyronitrile was added. The mixture was heated under reflux at 60℃ for 9h. The reaction was stopped and quenched with methanol to obtain a white flake-like crude product. After washing with methanol three times, the product was dried under vacuum at 40℃ to obtain the final product, polyvinylbenzyl chloride.
[0094] (2) Weigh 0.1g of the synthesized polyvinyl benzyl chloride into 10mL of dimethyl sulfoxide. After it is completely dissolved, add 77.81mg of Jeffamine. React at 60℃ for 2h and then cool down to 40℃. Then add 81.9μL of trimethylamine methanol solution and continue to react for 1h to obtain a cross-linked quaternized polyvinyl benzyl chloride membrane solution.
[0095] (3) Weigh 0.1g of the synthesized polyvinyl benzyl chloride into 5mL of dimethyl sulfoxide. After it is completely dissolved, add 81.9μL of trimethylamine methanol solution. After reacting at 40℃ for 1h, raise the temperature to 60℃ and add 78.48mg of octadecylamine. Continue to react for 6h to obtain a quaternized polyvinyl benzyl chloride membrane solution with hydrophobic side-linked branches.
[0096] (4) The two membrane solutions synthesized in steps b and c above are mixed and stirred at 40°C for 4 hours. The mixed solution is filtered through a filter cloth into a clean glass plate mold and dried at 80°C to form a membrane, thus obtaining a halogen-type polymer electrolyte membrane. Then, it is soaked in a 1M potassium hydroxide solution at 60°C for 12 hours, during which the fresh alkali solution is replaced 3 times. Finally, the membrane surface is rinsed with deionized water to remove residual alkali until the pH of the aqueous solution is 7, thus obtaining a hydroxide-type anion exchange membrane based on polyvinyl benzyl chloride.
[0097] The ion exchange capacity of the polyvinylbenzyl chloride-based anion exchange membrane was measured to be 1.46 mmol g. -1The gel strength was 92.8%; the swelling ratio at 30℃ was 11.0%; the water content was 104.4%; and the hydroxide ion conductivity at 80℃ was 92.2 mS / cm. -1 The tensile strength and elongation at break at 100% relative humidity were 6.81 MPa and 125.0%, respectively; after soaking in 1M NaOH solution at 80℃ for 720 h, the mass retention rate and ionic conductivity retention rate of the anion exchange membrane were 96.7% and 85.9%, respectively.
[0098] Since the polyvinylbenzyl chloride-based anion exchange membrane prepared in the final embodiment was insoluble, Fourier transform infrared spectroscopy was used to characterize the membrane material structure, and the results are as follows. Figure 2 As shown. Wavenumber 2875cm -1 1457cm -1 and 1106cm -1 The corresponding stretching vibrations of the –CH group, the scissor vibrations of the –CH2 group, and the stretching vibrations of the C–O–C group on Jeffamine indicate successful crosslinking of Jeffamine; wavenumber 1487 cm⁻¹. -1 and 974cm -1 The corresponding absorption peaks are characteristic peaks of quaternary ammonium cations; since both the main chain, Jeffamine, and the hydrophobic side chains contain –CH2 and –CH3, their infrared peaks are not easily distinguishable; furthermore, since a small number of benzyl groups on polyvinylbenzyl chloride remain unreacted, the peaks at a wavenumber of 1265 cm⁻¹ are not easily distinguishable. -1 and 672cm -1 The stretching vibration peak of C–Cl on benzyl chloride can be observed at this point.
[0099] The factors affecting the ionic conductivity of the polyvinylbenzyl chloride-based anion exchange membrane synthesized in this invention are mainly ion exchange capacity, water content, and ion conduction pathway. Generally speaking, the higher the ion exchange capacity and the greater the water content (except for cases where excessive water content leads to a decrease in ion concentration), the higher the ionic conductivity. However, the anion exchange membrane synthesized in Example 3 exhibits the highest ionic conductivity. Clearly, for Example 3, the superior ion conduction pathway is the main reason affecting its ionic conductivity. Therefore, the long-range ordered structure of the polymer is characterized by small-angle X-ray scattering. Figure 3 As shown, at 1.84nm -1 At this point, a distinct and sharp peak appears, indicating that this embodiment possesses a hydrophilic-hydrophobic phase separation structure. Calculated using the Bragg equation, the corresponding ion cluster size is 3.41 nm.
[0100] Comparative Example
[0101] In the literature (Polymer, 2021, 212, 123156), the authors synthesized quaternized polyvinylbenzyl chloride based on N-methylpyrrolidone grafting. The sample PVBMPy-CL-10%PSF had an ion exchange capacity of 2.4 mmol g. -1 The volume swelling ratio at 30℃ is 34.6%, and the water content is 49.4%; the hydroxide ion conductivity at 80℃ is 40.4 mS / cm. -1 The room temperature tensile strength was 1.3 MPa, and the elongation at break did not exceed 2%; stability data were not provided. The sample PVBMPy-CL-15%PSF had an ion exchange capacity of 2.1 mmol g. -1 The volume swelling ratio at 30℃ is 26.2%, and the water content is 40.0%; the hydroxide ion conductivity at 80℃ is 32.9 mS / cm. -1 The room temperature tensile strength is 13.1 MPa, and the elongation at break is not more than 10%. After soaking in 1 M KOH solution at 80°C for 580 h, the retention rate of ionic conductivity is 70.5%.
[0102] From the appendix Figure 2 As can be seen from the above experimental data, the polyvinylbenzyl chloride-based anion exchange membrane disclosed in the embodiments of the present invention exhibits uniform film formation and good flexibility. Compared with the comparative examples, the embodiments show lower ion exchange capacity, but higher water content, higher ionic conductivity, higher elongation at break, and higher chemical stability.
[0103] The various embodiments of the present invention have been described above. These descriptions are exemplary and not exhaustive, nor are they limited to the disclosed embodiments. Many modifications and variations will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.
Claims
1. A method for preparing an anion exchange membrane based on polyvinylbenzyl chloride, characterized in that, The preparation method includes: (1) In the presence of a first organic solvent and a protective gas, 4-chloromethylstyrene monomer is polymerized under the action of an initiator to obtain polyvinylbenzyl chloride; (2) In the presence of a second organic solvent, the polyvinyl benzyl chloride and O,O''-di(2-aminopropyl)polypropylene glycol-block-polyethylene glycol-block-polypropylene glycol are reacted; then an organic solution of trimethylamine is added and the reaction is continued to obtain a cross-linked quaternized polyvinyl benzyl chloride film solution. (3) Dissolve the polyvinylbenzyl chloride in a third organic solvent, add an organic solution of trimethylamine, and react; then add a primary amine or an organic solution of a primary amine, and continue the reaction to obtain a quaternized polyvinylbenzyl chloride film solution with hydrophobic side-linked branches. (4) The cross-linked quaternized polyvinyl benzyl chloride membrane solution is mixed with the hydrophobic side-linked quaternized polyvinyl benzyl chloride membrane solution to obtain a mixed solution. The mixed solution is poured into a mold and dried to obtain a halogen-type anion exchange membrane. The halogen-type anion exchange membrane is subjected to ion exchange with an alkaline solution to obtain the polyvinyl benzyl chloride-based anion exchange membrane with hydroxide ions as the anion. In step (4), the mixing temperature is 40~60℃ and the time is 2~4 h.
2. The preparation method according to claim 1, wherein, In step (1), the first organic solvent is tetrahydrofuran; the initiator is azobisisobutyronitrile; and the protective gas is nitrogen.
3. The preparation method according to claim 1, wherein, In step (1), the polymerization reaction is carried out at a temperature of 40-60°C for 9-12 hours.
4. The preparation method according to claim 1, wherein, In step (2), in the presence of a second organic solvent, the polyvinyl benzyl chloride and O,O''-di(2-aminopropyl)polypropylene glycol-block-polyethylene glycol-block-polypropylene glycol are reacted at 50-60°C for 2-4 h; the temperature is then lowered to 40-45°C, and then an organic solution of trimethylamine is added, and the reaction is continued for 1-2 h to obtain a crosslinked quaternized polyvinyl benzyl chloride film solution.
5. The preparation method according to claim 1, wherein, In step (2), the second organic solvent is dimethyl sulfoxide; the organic solution of trimethylamine is a trimethylamine methanol solution.
6. The preparation method according to claim 1, wherein, In step (3), the polyvinylbenzyl chloride is dissolved in a third organic solvent, and an organic solution of trimethylamine is added. The reaction is carried out at 40-45°C for 1-2 hours. The temperature is raised to 50-60°C, and then a primary amine or an organic solution of a primary amine is added. The reaction is continued for 2-6 hours to obtain a quaternized polyvinylbenzyl chloride film solution with hydrophobic side-linked branches.
7. The preparation method according to claim 1, wherein, In step (3), the third organic solvent is dimethyl sulfoxide; The organic solution of trimethylamine is a trimethylamine methanol solution; The organic solution of the primary amine is a tetrahydrofuran solution of the primary amine.
8. The preparation method according to claim 1, wherein, The mixed solution is filtered into the mold using a filter material.
9. The preparation method according to claim 1, wherein, The alkaline solution is a KOH solution and / or a NaOH solution; The temperature of the alkaline solution is 30-65℃; The concentration of the alkaline solution is 1~2 mol / L.
10. An anion exchange membrane based on polyvinylbenzyl chloride prepared by the preparation method according to any one of claims 1-9.
Citation Information
Patent Citations
Preparation method of polymer anionic membrane based on N-methylpyrrolidine cation
CN108570157A
Semi-interpenetrating anion exchange membrane as well as preparation method and application thereof
CN114695933A