Magnetic tunnel junction cell, method of making the same, magnetic tunnel junction device, and magnetic random access memory
By employing a three-layer synthetic antiferromagnetic sublayer structure and a ruthenium antiferromagnetic coupling layer in MRAM, the bounce problem in write operations is solved, the stability of the free layer and the data retention time are improved, and it is suitable for ultra-small magnetic tunnel junction arrays.
Patent Information
- Application Number
- CN202210079241.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-24
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2042-01-24
AI Technical Summary
In magnetic random access memory (MRAM), as device size shrinks, the bounce phenomenon during write operations becomes severe. Traditional synthetic antiferromagnetic layer structures cause leakage magnetic fields to affect the stability of the free layer and data retention time, and the process window is narrow, making it difficult to meet the needs of high-speed cache.
A magnetic tunnel junction structure with at least three synthetic antiferromagnetic sublayers is adopted, and adjacent synthetic antiferromagnetic sublayers are coupled through a ruthenium antiferromagnetic coupling layer. The second oscillation peak of RKKY is used to reduce the bounce phenomenon and reduce the influence of leakage magnetic field.
It effectively avoids the bounce phenomenon during the writing process of MRAM, improves the stability of the free layer and the data retention time, and is suitable for the application of ultra-small magnetic tunnel junction arrays.
Smart Images

Figure CN116546874B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of semiconductor devices, and more particularly to a magnetic tunnel junction unit having a multilayer synthetic antiferromagnetic sublayer, a method for preparing the same, a magnetic tunnel junction device, and a magnetic random access memory. Background Technology
[0002] Magnetic Random Access Memory (MRAM) is a random access memory that stores data using magnetoresistive properties. The core storage device of MRAM is the magnetic tunnel junction (MTJ).
[0003] Magnetic tunnel junctions (MTJs) are typically sandwich structures. Figure 1 This is a schematic diagram of the current magnetic tunnel junction structure. Figure 1 As shown, the current magnetic tunnel junction includes: a free layer (FL) 70, a reference layer (RL) 50, and a tunnel barrier layer (TBL) 60 sandwiched between them. To achieve effective pinning of the reference layer RL, a synthetic antiferromagnetic (SyAF) layer 30 is generally placed below the reference layer RL. In the conventional structure, the SyAF layer can be composed of a first synthetic antiferromagnetic sublayer 310 and a second synthetic antiferromagnetic sublayer 330. The first synthetic antiferromagnetic sublayer 310 and the second synthetic antiferromagnetic sublayer 330 achieve effective pinning of the reference layer RL through the RKKY (Ruderman-Kittel-Kasuya-Yosida) antiferromagnetic coupling effect.
[0004] As the size of the MRAM becomes smaller (e.g., shrinking to Sub-45nm), the back-hopping phenomenon will become increasingly severe during write operations on the MRAM. Figure 2 As shown. In this case, writing "0" or "1" will not succeed; moreover, the bounce phenomenon will become more and more obvious as the write pulse becomes shorter, which is very unfavorable for MRAM as a cache.
[0005] To reduce bounce during write operations, the first oscillation peak of Ru or Ir RKKY can be used as the coupling layer between the first and second synthetic antiferromagnetic sublayers, where the thickness of Ru or Ir is 0.35 nm–0.50 nm. The ultrathin Ru or Ir layer presents a significant challenge to the fabrication of superlattice SyAF layers: in most cases, such as… Figure 3As shown, due to interlayer diffusion, the first Ru RKKY oscillation peak disappears almost entirely after high-temperature annealing. In this case, the first and second synthetic antiferromagnetic sublayers will decouple. The decoupling phenomenon also applies to the first Ir RKKY oscillation peak. Therefore, using the first Ru or Ir oscillation peak to enhance the stability of RL will pose a significant challenge to the MTJ deposition process and will also hinder the expansion of the process window.
[0006] Figure 4(a) shows the leakage magnetic field (H) generated in the free layer. stray Figure 4(b) shows the principle diagram of the reversing current density and the critical reversing current density (J). c / J c0 The curve shows the variation of the reference layer RL and the synthetic antiferromagnetic SyAF layer with the pulse width. As shown in Figure 4(a), the bilayer structure of the reference layer RL and the synthetic antiferromagnetic SyAF layer will generate a leakage magnetic field (H). stray When H stray When the magnetization direction of H is parallel to the magnetic moment of the free layer FL, the thermal stability (Δ) of the free layer FL will increase, and further, the data retention time (τ) will also increase; conversely, when H... stray When the magnetization direction is antiparallel to the magnetic moment of the free layer FL, the thermal stability (Δ) of the free layer FL decreases, and further, the data retention time (τ) also decreases. The relevant formulas are as follows:
[0007]
[0008]
[0009]
[0010] Where τ is the data retention time; τ0 is the attempt time or characteristic relaxation time, where, When the pulse duration is long, it is generally taken as 1 ns of τ0; H stray For leakage magnetic field; H k α is the magnetic anisotropy field of the free layer; e is the free layer damping coefficient; μ0 is the free space permeability; η is the charge spin efficiency. M is the reduced Planck constant; s denoted as saturation magnetic susceptibility of the free layer.
[0011] Furthermore, based on the different pulse widths, as shown in Figure 4(b), the switching behavior of the free layer of the magnetic tunnel junction can be divided into three intervals: "thermal assisted switching" mode, "precessional switching" mode, and "dynamic switching" mode in between. It is generally believed that when the pulse width is greater than 10 ns, it is the "thermal assisted" switching mode; when the pulse width is greater than 1 ns but less than 10 ns, it is the "dynamic switching" mode; and when the pulse width is less than 1 ns, it is the "precessional switching" mode. When the pulse time is close to or less than the attempt time, a larger "overdrive" current needs to be added to make the free magnetic moment switch. Therefore, maintaining the balance of leakage magnetic flux is very helpful for the low pulse width writing process.
[0012] j = J c / J c0 -1 (4)
[0013] Among them, J c For the reversal current density; J c0 is the critical switching current density; j is the "overdrive" factor.
[0014] In summary, the presence of a leakage magnetic field reduces the thermal stability of states "1" or "0," which is highly detrimental to the development of MTJ devices. Furthermore, the presence of a leakage magnetic field also negatively impacts the switching current. With the miniaturization of MTJ devices, how to reduce H... stray It is becoming increasingly important that traditional structures containing double synthetic antiferromagnetic sublayers (Double SyAF sub-layers) are highly unfavorable for H due to process window limitations. stray The reduction. Summary of the Invention
[0015] The following is an overview of the subject matter described in detail herein. This overview is not intended to limit the scope of protection of this application.
[0016] This application provides a magnetic tunnel junction unit and its fabrication method, as well as a magnetic tunnel junction device and a magnetic random access memory including the magnetic tunnel junction unit. The magnetic tunnel junction unit can not only solve the back-hopping problem in the write process of the magnetic random access memory, but also avoid the influence of the leakage magnetic field generated by the reference layer and the synthetic antiferromagnetic layer on the free layer.
[0017] This application provides a magnetic tunnel junction unit for a magnetic tunnel junction device. The magnetic tunnel junction unit includes a free layer, a tunneling barrier layer, a reference layer, and a synthetic antiferromagnetic layer stacked sequentially. The synthetic antiferromagnetic layer includes at least three synthetic antiferromagnetic sublayers. The magnetization vectors of two adjacent synthetic antiferromagnetic sublayers are opposite, and two adjacent synthetic antiferromagnetic sublayers are coupled together through a ruthenium antiferromagnetic coupling layer. The thickness of the ruthenium antiferromagnetic coupling layer is 0.75nm-0.89nm, corresponding to the second oscillation peak of RKKY.
[0018] In the embodiments of this application, along the direction away from the reference layer, the synthetic antiferromagnetic layer sequentially includes a first synthetic antiferromagnetic sublayer, a second synthetic antiferromagnetic sublayer, ..., an Nth synthetic antiferromagnetic sublayer, where N is an integer and 3≤N≤10.
[0019] In embodiments of this application, the synthetic antiferromagnetic sublayer may be a layer formed of a ferromagnetic material having a single magnetization vector and containing Co.
[0020] In the embodiments of this application, the material of the first synthesized antiferromagnetic sublayer can be Co[Pt / Co]. a Co[Pd / Co] a Co[Ni / Co] a CoFe[Pt / CoFe] a CoFe[Pd / CoFe] a Or CoFe[Ni / CoFe] a , where 0≤a≤3.
[0021] In the embodiments of this application, the materials of the second synthetic antiferromagnetic sublayer to the Nth synthetic antiferromagnetic sublayer can each be independently Co[Pt / Co]. b Co[Pd / Co] b Co[Ni / Co] b CoFe[Pt / CoFe] b CoFe[Pd / CoFe] b Or CoFe[Ni / CoFe] b , where 1≤b≤4.
[0022] In the embodiments of this application, the thickness of Co, CoFe, Pt, Pd or Ni in the first synthetic antiferromagnetic sublayer can be 0.15nm-0.80nm.
[0023] In the embodiments of this application, the thicknesses of Co, CoFe, Pt, Pd, or Ni in the same first synthetic antiferromagnetic sublayer can be the same or different.
[0024] In the embodiments of this application, the thickness of Co, CoFe, Pt, Pd or Ni in the second synthetic antiferromagnetic sublayer or the Nth synthetic antiferromagnetic sublayer can be 0.15nm-0.80nm.
[0025] In the embodiments of this application, the thicknesses of Co, CoFe, Pt, Pd, or Ni can be the same or different in the same second synthetic antiferromagnetic sublayer or in the same Nth synthetic antiferromagnetic sublayer.
[0026] In the embodiments of this application, the structure of the magnetic tunnel junction unit can be any of the following:
[0027] (1) Co[Pt / Co] b2 / Ru / Co[Pt / Co] b1 / Ru / Co[Pt / Co] a1 ;
[0028] (2) Co[Pt / Co] b5 / Ru / Co[Pt / Co] b4 / Ru / Co[Pt / Co] b3 / Ru / Co[Pt / Co] a2 ;
[0029] (3) Co[Pt / Co] b9 / Ru / Co[Pt / Co] b8 / Ru / Co[Pt / Co] b7 / Ru / Co[Pt / Co] b6 / Ru / Co[Pt / Co] a3 ;
[0030] In each magnetic tunnel junction unit, from right to left, there are the first synthetic antiferromagnetic sublayer, the first ruthenium antiferromagnetic coupling layer, the second synthetic antiferromagnetic sublayer, the second ruthenium antiferromagnetic coupling layer, ... the Nth synthetic antiferromagnetic sublayer, a1 to a3 are each independently 0-3, and b1 to b9 are each independently 1-4.
[0031] In the embodiments of this application, the synthesized antiferromagnetic sublayer may have an FCC(111) superlattice structure, a BCC structure, or an HCP structure.
[0032] In embodiments of this application, the magnetic tunnel junction unit may further include a seed layer, which is disposed on the side of the synthetic antiferromagnetic layer away from the reference layer.
[0033] In the embodiments of this application, the material of the seed layer may be selected from any one or more of platinum, titanium, titanium nitride, tantalum, tantalum nitride, ruthenium, tungsten, tungsten nitride, palladium, chromium, oxygen, nitrogen, cobalt boride, iron boride, nickel-chromium alloy, and cobalt-iron-boron.
[0034] In embodiments of this application, the magnetic tunnel junction unit may further include a ferromagnetic coupling layer disposed between the reference layer and the synthetic antiferromagnetic layer.
[0035] In the embodiments of this application, the material of the ferromagnetic coupling layer may be selected from any one or more of tungsten, molybdenum, and tantalum.
[0036] This application also provides a magnetic tunnel junction device, including: a bottom electrode, a top electrode, and a magnetic tunnel junction unit disposed between the bottom electrode and the top electrode, wherein the magnetic tunnel junction unit is the magnetic tunnel junction unit as described above.
[0037] This application also provides a magnetic random access memory, including the magnetic tunnel junction device described above.
[0038] This application also provides a method for preparing the magnetic tunnel junction unit as described above, comprising: forming each layer of the magnetic tunnel junction unit using a sputtering deposition process; and after deposition, using a high-temperature annealing process to transform the reference layer and the free layer from an amorphous state into a crystalline structure.
[0039] This application employs a magnetic tunnel junction structure with at least three synthetic antiferromagnetic sublayers, and uses a ruthenium antiferromagnetic coupling layer with the second RKKY oscillation peak to couple two adjacent synthetic antiferromagnetic sublayers together. This can effectively avoid the back-hopping phenomenon in MRAM during the write process and reduce the influence of the leakage magnetic field generated by the reference layer and the synthetic antiferromagnetic layer on the free layer. The magnetic tunnel junction unit of this structure is very suitable for ultra-small magnetic tunnel junction arrays.
[0040] Other features and advantages of this application will be set forth in the following description, and will be apparent in part from the description, or may be learned by practicing the application. Other advantages of this application can be realized and obtained by means of the solutions described in the description and the accompanying drawings. Attached Figure Description
[0041] The accompanying drawings are used to provide an understanding of the technical solutions of this application and constitute a part of the specification. They are used together with the embodiments of this application to explain the technical solutions of this application and do not constitute a limitation on the technical solutions of this application.
[0042] Figure 1 This is a schematic diagram of the current magnetic tunnel junction structure;
[0043] Figure 2 This is a schematic diagram illustrating the bounce phenomenon in a magnetic tunnel junction.
[0044] Figure 3 A schematic diagram illustrating the principle of Ru forming the first and second RKKY oscillation peaks during deposition and the disappearance of the first RKKY oscillation peak after high-temperature annealing;
[0045] Figure 4(a) shows the leakage magnetic field (H) generated in the free layer. stray A schematic diagram illustrating the principle of ( );
[0046] Figure 4(b) shows the ratio of the reversing current density to the critical reversing current density (J). c / J c0 The curve showing the change in pulse width;
[0047] Figure 5 This is a schematic diagram of the structure of the magnetic tunnel junction unit according to an embodiment of this application;
[0048] Figure 6 This is a schematic diagram of the structure of a magnetic tunnel junction device, which is an exemplary embodiment of this application.
[0049] Figure 7 This is a schematic diagram illustrating the adjustment of the magnetic field and magnetic moment of a magnetic tunnel junction device, which is an exemplary embodiment of this application.
[0050] The symbols in the attached diagram have the following meanings:
[0051] 10-Bottom electrode; 20-Seed layer; 30-Synthetic antiferromagnetic layer; 310-First synthetic antiferromagnetic sublayer; 320-First ruthenium antiferromagnetic coupling layer; 330-Second synthetic antiferromagnetic sublayer; 340-Second ruthenium antiferromagnetic coupling layer; 350-Third synthetic antiferromagnetic sublayer; 360-Third ruthenium antiferromagnetic coupling layer; 370-Fourth synthetic antiferromagnetic sublayer; m-Nth synthetic antiferromagnetic sublayer; 40-Ferromagnetic coupling layer; 50-Reference layer; 60-Tunneling barrier layer; 70-Free layer; 80-Capping layer; 90-Top electrode. Detailed Implementation
[0052] To make the objectives, technical solutions, and advantages of this application clearer, the embodiments of this application will be described in detail below with reference to the accompanying drawings. It should be noted that, unless otherwise specified, the embodiments and features described in these embodiments can be arbitrarily combined with each other.
[0053] This application provides a magnetic tunnel junction unit for a magnetic tunnel junction device. Figure 5 This is a schematic diagram of the structure of a magnetic tunnel junction unit according to an embodiment of this application. Figure 5As shown, the magnetic tunnel junction unit includes a free layer 70, a tunneling barrier layer 60, a reference layer 50, and a synthetic antiferromagnetic layer 30. The tunneling barrier layer 60 is disposed on one side of the free layer 70, the reference layer 50 is disposed on the side of the tunneling barrier layer 60 away from the free layer 70, and the synthetic antiferromagnetic layer 30 is disposed on the side of the reference layer 50 away from the free layer 70. The synthetic antiferromagnetic layer 30 includes at least three synthetic antiferromagnetic sublayers, namely a first synthetic antiferromagnetic sublayer. 310, the second synthetic antiferromagnetic sublayer 330, and the Nth synthetic antiferromagnetic sublayer m, wherein the magnetization vectors of two adjacent synthetic antiferromagnetic sublayers are opposite, and two adjacent synthetic antiferromagnetic sublayers are coupled together through a ruthenium antiferromagnetic coupling layer (for example, the first synthetic antiferromagnetic sublayer 310 and the second synthetic antiferromagnetic sublayer 330 are coupled together through a first ruthenium antiferromagnetic coupling layer 320, and so on), wherein the thickness of the ruthenium antiferromagnetic coupling layer is 0.75nm-0.89nm, corresponding to the second oscillation peak of RKKY.
[0054] This application employs a magnetic tunnel junction structure with at least three synthetic antiferromagnetic sublayers, and uses a ruthenium antiferromagnetic coupling layer with the second RKKY oscillation peak to couple two adjacent synthetic antiferromagnetic sublayers together. This can avoid the back-hopping phenomenon in MRAM during the write process and reduce the influence of the leakage magnetic field generated by the reference layer and the synthetic antiferromagnetic layer on the free layer. The magnetic tunnel junction unit of this structure is very suitable for ultra-small magnetic tunnel junction arrays.
[0055] In the embodiments of this application, the thickness of the ruthenium antiferromagnetic coupling layer can be 0.75nm, 0.77nm, 0.79nm, 0.81nm, 0.83nm, 0.85nm, 0.87nm, or 0.89nm.
[0056] In the embodiments of this application, along the direction away from the reference layer, the synthetic antiferromagnetic layer sequentially includes a first synthetic antiferromagnetic sublayer, a second synthetic antiferromagnetic sublayer, ..., an Nth synthetic antiferromagnetic sublayer, where N is an integer and 3≤N≤10.
[0057] In embodiments of this application, the synthetic antiferromagnetic sublayer may be a layer formed of a ferromagnetic material having a single magnetization vector and containing Co.
[0058] In the embodiments of this application, the material of the first synthesized antiferromagnetic sublayer can be Co[Pt / Co]. a Co[Pd / Co] a Co[Ni / Co] a CoFe[Pt / CoFe] a CoFe[Pd / CoFe] a Or CoFe[Ni / CoFe] a, where 0≤a≤3, for example, a can be 0, 1, 2, or 3.
[0059] In the embodiments of this application, the thickness of Co, CoFe, Pt, Pd or Ni in the first synthetic antiferromagnetic sublayer can be 0.15nm-0.80nm, for example, it can be 0.15nm, 0.20nm, 0.25nm, 0.30nm, 0.35nm, 0.40nm, 0.45nm, 0.50nm, 0.55nm, 0.60nm, 0.65nm, 0.70nm, 0.75nm or 0.80nm.
[0060] In the embodiments of this application, the thickness of each layer of Co, CoFe, Pt, Pd or Ni in the same first synthetic antiferromagnetic sublayer may be the same or different.
[0061] In the embodiments of this application, the materials of the second synthetic antiferromagnetic sublayer to the Nth synthetic antiferromagnetic sublayer can each be independently Co[Pt / Co]. b Co[Pd / Co] b Co[Ni / Co] b CoFe[Pt / CoFe] b CoFe[Pd / CoFe] b Or CoFe[Ni / CoFe] b Where 1≤b≤4, for example, b can be 1, 2, 3, or 4.
[0062] In the embodiments of this application, the thickness of Co, CoF, Pt, Pd or Ni in the second synthetic antiferromagnetic sublayer or the Nth synthetic antiferromagnetic sublayer can be 0.15nm-0.80nm, for example, it can be 0.15nm, 0.20nm, 0.25nm, 0.30nm, 0.35nm, 0.40nm, 0.45nm, 0.50nm, 0.55nm, 0.60nm, 0.65nm, 0.70nm, 0.75nm or 0.80nm.
[0063] In the embodiments of this application, the thickness of each layer of Co, CoFe, Pt, Pd or Ni may be the same or different in the same second synthetic antiferromagnetic sublayer or in the same Nth synthetic antiferromagnetic sublayer.
[0064] In the embodiments of this application, the structure of the magnetic tunnel junction unit can be any of the following:
[0065] (1) Co[Pt / Co] b2 / Ru / Co[Pt / Co] b1 / Ru / Co[Pt / Co] a1 ;
[0066] (2) Co[Pt / Co] b5 / Ru / Co[Pt / Co] b4 / Ru / Co[Pt / Co] b3 / Ru / Co[Pt / Co] a2 ;
[0067] (3) Co[Pt / Co] b9 / Ru / Co[Pt / Co] b8 / Ru / Co[Pt / Co] b7 / Ru / Co[Pt / Co] b6 / Ru / Co[Pt / Co] a3 ;
[0068] In each magnetic tunnel junction unit, from right to left, there are the first synthetic antiferromagnetic sublayer, the first ruthenium antiferromagnetic coupling layer, the second synthetic antiferromagnetic sublayer, the second ruthenium antiferromagnetic coupling layer, ... the Nth synthetic antiferromagnetic sublayer, where a1 to a3 can be independently 0-3, and b1 to b9 can be independently 1-4.
[0069] In the embodiments of this application, the synthesized antiferromagnetic sublayer may have an FCC(111) superlattice structure, a BCC superlattice structure, or an HCP superlattice structure, etc.
[0070] Preferably, the synthesized antiferromagnetic sublayer has an FCC(111) superlattice structure.
[0071] In embodiments of this application, the magnetic tunnel junction unit may further include a seed layer disposed on the side of the synthesized antiferromagnetic sublayer away from the reference layer. The presence of the seed layer facilitates the growth of an FCC(111) superlattice structure from the synthesized antiferromagnetic sublayer using a sputtering deposition process.
[0072] In embodiments of this application, the material of the seed layer can be selected from any one or more of platinum (Pt), titanium (Ti), titanium nitride (TiN), tantalum (Ta), tantalum nitride (TaN), ruthenium (Ru), tungsten (W), tungsten nitride (W₂N), palladium (Pd), chromium (Cr), oxygen (O), nitrogen (N), cobalt boride (CoB), iron boride (FeB), nickel-chromium alloy (NiCr), and cobalt-iron-boron (CoFeB). For example, the material of the seed layer can be selected from any one or more of platinum (Pt), palladium (Pd), ruthenium (Ru), nickel-chromium alloy (NiCr), and cobalt-iron-boron (CoFeB). The seed layer may include a multilayer structure formed from the above materials.
[0073] In the embodiments of this application, the thickness of the seed layer can be 1.0nm-5.0nm, for example, it can be 1.0nm, 1.5nm, 2.0nm, 2.5nm, 3.0nm, 3.5nm, 4.0nm, 4.5nm, or 5.0nm.
[0074] In embodiments of this application, the magnetic tunnel junction unit may further include a ferromagnetic coupling layer disposed between the reference layer and the synthetic antiferromagnetic layer. The ferromagnetic coupling layer enables ferromagnetic coupling between the reference layer and the synthetic antiferromagnetic layer.
[0075] In the embodiments of this application, the material of the ferromagnetic coupling layer may be selected from any one or more of tungsten (W), molybdenum (Mo), and tantalum (Ta).
[0076] In the embodiments of this application, the thickness of the ferromagnetic coupling layer can be 0.15nm-0.7nm, for example, it can be 0.15nm, 0.2nm, 0.25nm, 0.3nm, 0.35nm, 0.4nm, 0.45nm, 0.5nm, 0.55nm, 0.6nm, 0.65nm, or 0.7nm.
[0077] In the embodiments of this application, the material of the reference layer may be selected from any one or more of cobalt boride (CoB), iron boride (FeB), cobalt iron boron (CoFeB), cobalt carbide (CoC), cobalt iron carbon (CoFeC), iron (Fe), and cobalt iron alloy (FeCo).
[0078] In the embodiments of this application, the thickness of the reference layer can be 0.7nm-1.4nm, for example, it can be 0.7nm, 0.8nm, 0.9nm, 1.0nm, 1.1nm, 1.2nm, 1.3nm, or 1.4nm.
[0079] In the embodiments of this application, the material of the tunneling barrier layer can be a non-magnetic metal oxide, such as magnesium oxide (MgO), zinc magnesium oxide (MgZnO), boron magnesium oxide (MgBO), or aluminum magnesium oxide (MgAlO).
[0080] In the embodiments of this application, the thickness of the tunneling barrier layer can be 0.8nm-2.0nm, for example, it can be 0.8nm, 0.9nm, 1.0nm, 1.1nm, 1.2nm, 1.3nm, 1.4nm, 1.5nm, 1.6nm, 1.7nm, 1.8nm, 1.9nm, or 2.0nm.
[0081] In the embodiments of this application, the free layer can be a single-layer structure of cobalt boride (CoB), iron boride (FeB), or cobalt iron boron (CoFeB); it can also be one of a double-layer structure of cobalt ferroide (CoFe) / cobalt iron boron (CoFeB) or iron (Fe) / cobalt iron boron (CoFeB); or it can be one of a three-layer structure of cobalt iron boron (CoFeB) / tantalum (Ta) / cobalt iron boron (CoFeB), cobalt iron boron (CoFeB) / tungsten (W) / cobalt iron boron (CoFeB), cobalt iron boron (CoFeB) / molybdenum (Mo) / cobalt iron boron (CoFeB), or cobalt iron boron (CoFeB) / hafnium (Hf) / cobalt iron boron (CoFeB). It can also be one of the four-layer structures of cobalt ferrophosphate (CoFe) / cobalt iron boron (CoFeB) / tungsten (W) / cobalt iron boron (CoFeB), cobalt ferrophosphate (CoFe) / cobalt iron boron (CoFeB) / molybdenum (Mo) / cobalt iron boron (CoFeB), cobalt ferrophosphate (CoFe) / cobalt iron boron (CoFeB) / hafnium (Hf) / cobalt iron boron (CoFeB), iron (Fe) / cobalt iron boron (CoFeB) / tungsten (W) / cobalt iron boron (CoFeB), iron (Fe) / cobalt iron boron (CoFeB) / molybdenum (Mo) / cobalt iron boron (CoFeB), and iron (Fe) / cobalt iron boron (CoFeB) / hafnium (Hf) / cobalt iron boron (CoFeB).
[0082] In the embodiments of this application, the thickness of the free layer can be 1.5nm-2.5nm, for example, it can be 1.5nm, 1.6nm, 1.7nm, 1.8nm, 1.9nm, 2.0nm, 2.1nm, 2.2nm, 2.3nm, 2.4nm, or 2.5nm.
[0083] This application embodiment also provides a magnetic tunnel junction device, the magnetic tunnel junction device comprising: a bottom electrode, a top electrode, and a magnetic tunnel junction unit disposed between the bottom electrode and the top electrode, the magnetic tunnel junction unit being the magnetic tunnel junction unit as described above.
[0084] In the embodiments of this application, the material of the bottom electrode may be selected from any one or more of titanium (Ti), titanium nitride (TiN), tungsten (W), tungsten nitride (WN), tantalum (Ta), and tantalum nitride (TaN).
[0085] In the embodiments of this application, the thickness of the bottom electrode can be 10nm-100nm, for example, it can be 10nm, 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm, or 100nm.
[0086] In the embodiments of this application, the material of the top electrode may be selected from any one or more of titanium (Ti), titanium nitride (TiN), tungsten (W), tungsten nitride (WN), tantalum (Ta), and tantalum nitride (TaN).
[0087] In the embodiments of this application, the thickness of the top electrode can be 10nm-100nm, for example, it can be 10nm, 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm, or 100nm.
[0088] In embodiments of this application, the magnetic tunnel junction device may further include a capping layer disposed between the top electrode and the free layer of the magnetic tunnel junction unit. The capping layer may comprise a multilayer structure formed of any two or more materials selected from magnesium oxide (MgO), cobalt iron boron (CoFeB), tungsten (W), platinum (Pt), ruthenium (Ru), tantalum (Ta), iron (Fe), cobalt (Co), cobalt boride (CoB), and iron boride (FeB).
[0089] In the embodiments of this application, the thickness of the covering layer can be 1.0nm-7.0nm, for example, it can be 1.0nm, 2.0nm, 3.0nm, 4.0nm, 5.0nm, 6.0nm, or 7.0nm.
[0090] This application also provides a magnetic random access memory, which includes the magnetic tunnel junction device described above.
[0091] This application embodiment also provides a method for preparing the magnetic tunnel junction unit as described above. The preparation method includes: forming each layer of the magnetic tunnel junction unit using a sputtering deposition process; after deposition, using a high-temperature annealing process to transform the reference layer and the free layer from an amorphous state to a crystalline structure, thereby obtaining a magnetic tunnel junction with a complete crystalline structure and improving its transmission and magnetic properties.
[0092] In embodiments of this application, the layers of the magnetic tunnel junction unit are formed under continuous vacuum conditions.
[0093] In the embodiments of this application, the annealing temperature of the high-temperature annealing process can be 350℃-450℃, for example, 350℃, 375℃, 400℃, 425℃ or 450℃; the annealing time can be 15min-180min, for example, 15min, 30min, 50min, 100min, 150min or 180min.
[0094] Example 1
[0095] Figure 6This is a schematic diagram of the structure of a magnetic tunnel junction device, which is an exemplary embodiment of this application. Figure 6 As shown, the magnetic tunnel junction device of this embodiment includes: a bottom electrode 10, a seed layer 20, a synthetic antiferromagnetic layer 30, a ferromagnetic coupling layer 40, a reference layer 50, a tunneling barrier layer 60, a free layer 70, a capping layer 80, and a top electrode 90, which are stacked sequentially.
[0096] The synthetic antiferromagnetic layer 30 comprises four antiferromagnetic sublayers, with the magnetization vectors of two adjacent synthetic antiferromagnetic sublayers being opposite, and two adjacent synthetic antiferromagnetic sublayers being coupled together through a ruthenium antiferromagnetic coupling layer. The thickness of the ruthenium antiferromagnetic coupling layer is 0.75nm-0.89nm, corresponding to the second oscillation peak of RKKY.
[0097] Specifically, along the direction away from the reference layer 50 (i.e. Figure 6 (From top to bottom) The synthetic antiferromagnetic layer 30 includes a multilayer structure comprising a first synthetic antiferromagnetic sublayer 310, a first ruthenium antiferromagnetic coupling layer 320, a second synthetic antiferromagnetic sublayer 330, a second ruthenium antiferromagnetic coupling layer 340, a third synthetic antiferromagnetic sublayer 350, a third ruthenium antiferromagnetic coupling layer 360, and a fourth synthetic antiferromagnetic sublayer 370.
[0098] The specific structure of the synthetic antiferromagnetic layer 30 is: Co[Pt / Co]. b5 / Ru / Co[Pt / Co] b4 / Ru / Co[Pt / Co] b3 / Ru / Co[Pt / Co] a2 Where 0≤a2≤3, 1≤b3≤4, 1≤b4≤4, 1≤b5≤4, that is, the first synthetic antiferromagnetic sublayer 310 is Co[Pt / Co]. a2 The second synthesized antiferromagnetic sublayer 330 is Co[Pt / Co]. b3 The third synthesized antiferromagnetic sublayer 350 is Co[Pt / Co]. b4 The fourth synthesized antiferromagnetic sublayer 370 is Co[Pt / Co]. b5 ;
[0099] The thickness of Co is 0.30 nm–0.80 nm, and the thickness of Pt is 0.15 nm–0.50 nm. Within the same synthesized antiferromagnetic sublayer, the thicknesses of Co or Pt can be the same or different. Furthermore, by adjusting the structure and material parameters of the synthesized antiferromagnetic layer 30, the H... ex and H stray Adjustments, such as Figure 7 As shown, this avoids the back-hopping phenomenon and reduces the impact of the leakage magnetic field on the free layer.
[0100] The formulas involved are as follows:
[0101]
[0102] Among them, H ex For exchange coupling field; J ex M is the exchange coupling constant. s t is the magnetic moment of the synthesized antiferromagnetic sublayer.
[0103] Exchange-coupled field (H ex The larger the value, the more stable the pinning of the reference layer, and the smaller the chance of back-hopping under current pulses, or even the absence of back-hopping.
[0104] Furthermore, it is generally believed that H ex The correlation between the flipped and reference layers 50 and the first synthetic antiferromagnetic sublayer 310 is relatively high, H ex The larger the value, the more stable the reference layer. For example... Figure 7 As shown, the outermost flipping magnetic field is generally called the saturated flipping magnetic field (H). sat Its physical origin is quite complex and will not be discussed in detail here.
[0105] For the entire synthetic antiferromagnetic layer 30, it generally has an FCC(111) superlattice structure. If the overall film thickness is too thin, it is very unfavorable to form an FCC(111) superlattice structure. In this case, compared with synthetic antiferromagnetic layers with two synthetic antiferromagnetic sublayers, synthetic antiferromagnetic layers with multiple synthetic antiferromagnetic sublayers are more likely to form an FCC(111) superlattice structure, and also have a larger process window; in order to obtain a larger H ex Compared to synthetic antiferromagnetic layers with two synthetic antiferromagnetic sublayers, synthetic antiferromagnetic layers with multiple synthetic antiferromagnetic sublayers have a better chance of making each synthetic antiferromagnetic sublayer relatively thin.
[0106] Meanwhile, within the multi-layered synthetic antiferromagnetic sublayer, the magnetization vector directions of adjacent synthetic antiferromagnetic sublayers are parallel. Compared to a magnetic tunnel junction with a double-layered synthetic antiferromagnetic sublayer, the magnetic tunnel junction with multiple layers of synthetic antiferromagnetic sublayers exhibits a larger leakage magnetic field (H). stray Balance adjustment window.
[0107] The material of the bottom electrode 10 can be selected from any one or more of titanium (Ti), titanium nitride (TiN), tungsten (W), tungsten nitride (WN), tantalum (Ta) and tantalum nitride (TaN), and the thickness can be 10nm-100nm.
[0108] The seed layer 20 can be made of any one or more of platinum (Pt), palladium (Pd), nickel-chromium alloy (NiCr), ruthenium (Ru) and cobalt-iron-boron (CoFeB), and its thickness can be 1.0 nm to 5.0 nm.
[0109] The material of the ferromagnetic coupling layer 40 can be selected from any one or more of tungsten (W), molybdenum (Mo) and tantalum (Ta), and the thickness can be 0.15nm-0.7nm.
[0110] The material of the reference layer 50 can be selected from any one or more of cobalt boride (CoB), iron boride (FeB), cobalt iron boron (CoFeB), cobalt carbide (CoC), cobalt iron carbon (CoFeC), iron (Fe), and cobalt iron alloy (FeCo), and the thickness can be 0.7nm-1.4nm.
[0111] The material of the tunneling barrier layer 60 can be a non-magnetic metal oxide, such as magnesium oxide (MgO), zinc magnesium oxide (MgZnO), boron magnesium oxide (MgBO), or aluminum magnesium oxide (MgAlO), and the thickness can be 0.8 nm to 2.0 nm.
[0112] The free layer 70 can be a single-layer structure of cobalt boride (CoB), iron boride (FeB), or cobalt iron boron (CoFeB); it can also be one of the following double-layer structures: cobalt iron boron (CoFe) / cobalt iron boron (CoFeB) or iron (Fe) / cobalt iron boron (CoFeB); it can also be one of the following triple-layer structures: cobalt iron boron (CoFeB) / tantalum (Ta) / cobalt iron boron (CoFeB), cobalt iron boron (CoFeB) / tungsten (W) / cobalt iron boron (CoFeB), cobalt iron boron (CoFeB) / molybdenum (Mo) / cobalt iron boron (CoFeB), or cobalt iron boron (CoFeB) / hafnium (Hf) / cobalt iron boron (CoFeB); it can also be cobalt iron boron (CoFe). One of the four-layer structures: / CoFeB / Tungsten(W) / CoFeB, CoFe / CoFeB / Mo / CoFeB, CoFe / CoFeB / Hf / CoFeB, Iron(Fe) / CoFeB / Tungsten(W) / CoFeB, Iron(Fe) / CoFeB / Mo / CoFeB, and Iron(Fe) / CoFeB / Hf / CoFeB, with a thickness of 1.5nm-2.5nm;
[0113] The capping layer 80 may comprise a multilayer structure formed by any two or more of the following materials: magnesium oxide (MgO), cobalt iron boron (CoFeB), tungsten (W), platinum (Pt), ruthenium (Ru), tantalum (Ta), iron (Fe), cobalt (Co), cobalt boride (CoB), and iron boride (FeB), with a thickness of 1.0 nm to 7.0 nm.
[0114] The material of the top electrode 90 can be selected from any one or more of titanium (Ti), titanium nitride (TiN), tungsten (W), tungsten nitride (WN), tantalum (Ta) and tantalum nitride (TaN), and the thickness can be 10nm-100nm.
[0115] The magnetic tunnel junction of the magnetic tunnel junction device in this embodiment can be formed using a sputtering deposition process. After deposition, a high-temperature annealing process is used to transform the reference layer 50 and the free layer 70 from an amorphous state to a crystalline state, thereby improving their transmission and magnetic properties. Alternatively, patterning techniques can be used to fabricate MTJ array devices of the appropriate size.
[0116] While the embodiments disclosed in this application are as described above, the content is merely for the purpose of facilitating understanding of this application and is not intended to limit this application. Any person skilled in the art to which this application pertains may make any modifications and changes in the form and details of the implementation without departing from the spirit and scope disclosed in this application; however, the scope of protection of this application shall still be determined by the scope defined in the appended claims.
Claims
1. A magnetic tunnel junction unit of a magnetic tunnel junction device, characterized in that, It includes a free layer, a tunneling barrier layer, a reference layer, and a synthetic antiferromagnetic layer stacked sequentially. The synthetic antiferromagnetic layer includes at least three synthetic antiferromagnetic sublayers. The magnetization vectors of two adjacent synthetic antiferromagnetic sublayers are opposite, and two adjacent synthetic antiferromagnetic sublayers are coupled together by a ruthenium antiferromagnetic coupling layer. The thickness of the ruthenium antiferromagnetic coupling layer is 0.75nm-0.89nm, corresponding to the second oscillation peak of RKKY. Along the direction away from the reference layer, the synthetic antiferromagnetic layer sequentially includes a first synthetic antiferromagnetic sublayer, a second synthetic antiferromagnetic sublayer, ..., an Nth synthetic antiferromagnetic sublayer, where N is an integer and 3≤N≤10; Each of the synthesized antiferromagnetic sublayers has an FCC(111) superlattice structure; or, each of the synthesized antiferromagnetic sublayers has a BCC structure; or, each of the synthesized antiferromagnetic sublayers has an HCP structure.
2. The magnetic tunnel junction unit according to claim 1, wherein, The synthetic antiferromagnetic sublayer is a layer formed of a ferromagnetic material with a single magnetization vector and containing Co. The material of the first synthesized antiferromagnetic sublayer is Co[Pt / Co]. a Co[Pd / Co] a Co[Ni / Co] a CoFe[Pt / CoFe] a CoFe[Pd / CoFe] a Or CoFe[Ni / CoFe] a Where 0 ≤ a ≤ 3; The materials of the second to the Nth synthetic antiferromagnetic sublayers are each independently Co[Pt / Co]. b Co[Pd / Co] b Co[Ni / Co] b CoFe[Pt / CoFe] b CoFe[Pd / CoFe] b Or CoFe[Ni / CoFe] b , where 1≤b≤4.
3. The magnetic tunnel junction unit according to claim 2, wherein, In the first synthetic antiferromagnetic sublayer, the thickness of Co, CoFe, Pt, Pd or Ni is 0.15nm-0.80nm; in the same first synthetic antiferromagnetic sublayer, the thickness of Co, CoFe, Pt, Pd or Ni may be the same or different. In the second synthetic antiferromagnetic sublayer or the Nth synthetic antiferromagnetic sublayer, the thickness of Co, CoFe, Pt, Pd or Ni is 0.15 nm to 0.80 nm; in the same second synthetic antiferromagnetic sublayer or the same Nth synthetic antiferromagnetic sublayer, the thickness of Co, CoFe, Pt, Pd or Ni is the same or different.
4. The magnetic tunnel junction unit according to any one of claims 1 to 3, wherein, The structure of the magnetic tunnel junction unit is any one of the following: (1)Co[Pt / Co] b2 / Ru / Co[Fri / Co] b1 / Ru / Co[Fri / Co] a1 ; (2)Co[Pt / Co] b5 / Ru / Co[Fri / Co] b4 / Ru / Co[Fri / Co] b3 / Ru / Co[Fri / Co] a2 ; (3)Co[Pt / Co] b9 / Ru / Co[Fri / Co] b8 / Ru / Co[Fri / Co] b7 / Ru / Co[Fri / Co] b6 / Ru / What[Fri / What] a3 ; In each magnetic tunnel junction unit, from right to left, there are the first synthetic antiferromagnetic sublayer, the first ruthenium antiferromagnetic coupling layer, the second synthetic antiferromagnetic sublayer, the second ruthenium antiferromagnetic coupling layer, ... the Nth synthetic antiferromagnetic sublayer, a1 to a3 are each independently 0-3, and b1 to b9 are each independently 1-4.
5. The magnetic tunnel junction unit according to any one of claims 1 to 3, further comprising a seed layer, the seed layer being disposed on the side of the synthetic antiferromagnetic layer away from the reference layer; The seed layer material is selected from any one or more of platinum, titanium, titanium nitride, tantalum, tantalum nitride, ruthenium, tungsten, tungsten nitride, palladium, chromium, oxygen, nitrogen, cobalt boride, iron boride, nickel-chromium alloy, and cobalt-iron-boron.
6. The magnetic tunnel junction unit according to any one of claims 1 to 3 further includes a ferromagnetic coupling layer, the ferromagnetic coupling layer being disposed between the reference layer and the synthetic antiferromagnetic layer; The material of the ferromagnetic coupling layer is selected from any one or more of tungsten, molybdenum, and tantalum.
7. A magnetic tunnel junction device, characterized in that, include: A bottom electrode, a top electrode, and a magnetic tunnel junction unit disposed between the bottom electrode and the top electrode, wherein the magnetic tunnel junction unit is a magnetic tunnel junction unit according to any one of claims 1 to 6.
8. A magnetic random access memory, characterized in that, Includes the magnetic tunnel junction device according to claim 7.
9. The method for preparing a magnetic tunnel junction unit according to any one of claims 1 to 6, characterized in that, include: The magnetic tunneling unit is formed using a sputtering deposition process; After deposition, a high-temperature annealing process is used to transform the reference layer and the free layer from an amorphous state into a crystalline structure.
Citation Information
Patent Citations
Magnetic random access device and magnetic tunnel junction memory cell
CN111864057A