Electrode for lithium secondary battery, method for preparing the same, and lithium secondary battery comprising the same

By using multi-directional fibrous binders in the electrodes for lithium secondary batteries, the problem of insufficient bonding between electrode active materials and conductive materials is solved, thereby improving the durability and overall performance of the electrodes.

CN116547826BActive Publication Date: 2026-11-20LG ENERGY SOLUTION LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202280007089.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2022-09-15
Filing Date
2022-09-16
Publication Date
2026-11-20
Estimated Expiration
2042-09-16

AI Technical Summary

Technical Problem

In the current process of preparing electrodes for lithium secondary batteries, the bonding force between the electrode active material, conductive material and binder is insufficient, resulting in poor electrode durability and affecting battery performance.

Method used

By fiberizing the adhesive in multiple directions and employing specific mixing and fiberization processes, including low-temperature mixing, primary fiberization, grinding, and secondary fiberization, the uniformity of adhesive distribution and bonding strength in the active layer can be improved.

Benefits of technology

It improves the bonding force between electrode active materials, conductive materials and binders, thereby enhancing the durability and overall performance of the electrode.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116547826B_ABST
    Figure CN116547826B_ABST
Patent Text Reader

Abstract

The present invention provides an electrode for a lithium secondary battery, which includes an electrode active material, a conductive material, and a binder, wherein the binder is fiberized in multiple directions. For the active layer, the average diameter (D 50 ) of the particles is 200 μm to 500 μm. In the electrode for a lithium secondary battery, the binder included in the active layer is fiberized in multiple directions, thus improving the binding force between the electrode active material, the conductive material, and the binder in the active layer, and further improving the durability of the electrode.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to an electrode for lithium secondary batteries, a method for preparing the same, and a lithium secondary battery comprising the electrode. Specifically, this invention relates to an electrode for lithium secondary batteries comprising an adhesive fibrous in multiple directions in an active layer, a method for preparing the same, and a lithium secondary battery comprising the electrode.

[0002] This application claims the benefit based on priority of Korean Patent Application No. 10-2021-0123848, filed September 16, 2021; Korean Patent Application No. 10-2021-0123856, filed September 16, 2021; and Korean Patent Application No. 10-2022-0116025, filed September 15, 2022, the entire contents of which are incorporated herein by reference. Background Technology

[0003] With technological advancements and increasing demands for mobile devices, the demand for secondary batteries as an energy source is also rapidly growing. Among these secondary batteries, lithium-ion batteries, characterized by high energy density and voltage, long cycle life, and low self-discharge rate, have been commercialized and are widely used.

[0004] When preparing electrodes for lithium-ion batteries, electrode active materials, conductive materials, and binders are mixed to prepare a mixture containing electrode active materials. This prepared mixture is applied to an electrode current collector, and then pressurized using equipment such as rollers to prepare the electrode. When pressing a binder such as polytetrafluoroethylene (PTFE), fibrosis occurs centered on the surface in contact with the rollers. This fibrosis occurs in the direction of roller movement (machine direction, MD direction) and is mainly formed in the binder located on the electrode surface. Even if the binder is fibrous, the electrode durability may be insufficient because the electrode active materials, conductive materials, and binder located inside the electrode are still dispersed in the form of small particles. Electrode durability is also a factor related to electrode life and can directly affect battery performance. In particular, when electrodes are prepared using a dry method, the bonding force between the electrode active material particles, conductive materials, and binders may be relatively reduced, and the fibrosis of the binder may play a more important role in improving electrode durability.

[0005] In this technical field, research is underway to improve the durability of electrodes used in lithium secondary batteries, and the inventors completed this invention following these studies.

[0006] [Existing Technical Documents]

[0007] [Patent Literature]

[0008] (Patent Document 1) Korean Patent Publication No. 10-2014-0136952 Summary of the Invention

[0009] [Technical Issues]

[0010] The purpose of this invention is to provide an electrode for a lithium secondary battery that can improve the bonding force between the electrode active material, the conductive material and the binder, a method for preparing the electrode thereon, and a lithium secondary battery comprising the electrode.

[0011] [Technical Solution]

[0012] According to a first aspect of the present invention, an electrode for a lithium secondary battery is provided, comprising an active layer comprising an electrode active material, a conductive material and an adhesive, wherein the adhesive is fibrous in multiple directions.

[0013] In one embodiment of the invention, for the active layer, the average diameter (D) of the particles when ground at 10,000 rpm for 30 seconds using a stirrer with four blades is used. 50 The range is from 200μm to 500μm.

[0014] In one embodiment of the present invention, the tensile strength of the active layer in the MD direction is 7.5 kgf / cm. 2 above.

[0015] In one embodiment of the present invention, the tensile strength ratio of the active layer in the MD direction to the TD direction is 1 to 1.3.

[0016] In one embodiment of the present invention, the electrode active material is an average particle size (D) 50 ) is a lithium transition metal oxide ranging from 7 μm to 30 μm.

[0017] In one embodiment of the present invention, the conductive material is a carbonaceous material or a metallic material.

[0018] In one embodiment of the invention, the adhesive comprises polytetrafluoroethylene.

[0019] In one embodiment of the invention, the binder content in the active layer is 0.5% to 5% by weight, based on the total weight of the electrode active material.

[0020] According to a second aspect of the present invention, a method for preparing an electrode for a lithium secondary battery is provided, comprising the following steps: preparing an active layer:

[0021] (1) Mix the electrode active material, conductive material and adhesive stored at low temperature, (2) Fiberize the mixed material at high temperature, (3) Grind the fiberized material at room temperature, and (4) Fiberize the ground material a second time.

[0022] In one embodiment of the present invention, in step (1), an electrode active material, a conductive material and a binder stored at -20°C to -1°C are mixed using a stirrer rotating at 5000 RPM to 20000 RPM.

[0023] In one embodiment of the invention, in step (2), a kneader is used to apply a shear force of 20 N·m to 200 N·m to the mixed material.

[0024] In one embodiment of the present invention, in step (2), the mixed material is fiberized once using a twin-screw kneader rotating at 10 RPM to 50 RPM at 50°C to 70°C.

[0025] In one embodiment of the invention, in step (3), the fibrous material is ground at room temperature using a stirrer rotating at 5000 RPM to 20000 RPM.

[0026] In one embodiment of the present invention, in step (4), the ground material is subjected to secondary fiberization at 40°C to 60°C using a three-roll mill rotating at 5 RPM to 20 RPM.

[0027] In one embodiment of the invention, the particles ground in step (3) are selected such that they contain only particles with a particle size of less than 1 mm before the secondary fiberization in step (4).

[0028] In one embodiment of the invention, the particles ground in step (3) are selected such that the Hausner ratio is 1.6 or less before the secondary fiberization in step (4).

[0029] [Beneficial Effects]

[0030] In the lithium secondary battery electrode of the present invention, the adhesive contained in the active layer is fibrous in multiple directions, thereby improving the bonding force between the electrode active material, the conductive material and the adhesive in the active layer, and further improving the durability of the electrode. Attached Figure Description

[0031] Figure 1 This is a schematic diagram illustrating an active layer prepared by rolling from the top and bottom in the prior art.

[0032] Figure 2 This diagram schematically illustrates an active layer prepared according to an embodiment of the present invention.

[0033] Figure 3a The image shows a SEM image (magnification: ×3000) of the interior of the active layer prepared according to Comparative Example 1.

[0034] Figure 3b The image is a SEM image (magnification: ×3000) of the outer surface of the active layer prepared according to Comparative Example 1.

[0035] Figure 4a The image shows a SEM image (magnification: ×3000) of the interior of the active layer prepared according to Example 1.

[0036] Figure 4b The image is a SEM image (magnification: ×3000) of the outer surface of the active layer prepared according to Example 1.

[0037] Figure 5 This is a graph showing the size distribution of particles after grinding the active layer prepared according to Example 1 and Comparative Example 1.

[0038] Figure 6 The graph shows the results of the bulk density and tap density measured according to Example 5.

[0039] Figure 7 This is a graph showing the flowability measured according to the Hausner ratio. Detailed Implementation

[0040] The embodiments provided by this invention can all be implemented through the following description. It should be understood that the following description should be construed as describing preferred embodiments of the invention, but does not necessarily limit the invention.

[0041] Regarding the physical properties described herein, if the measurement conditions and methods are not specifically described, these physical properties are measured according to the measurement conditions and methods commonly used by those skilled in the art.

[0042] According to one embodiment of the present invention, an electrode for a lithium secondary battery is provided, comprising an active layer containing an electrode active material, a conductive material, and a binder, wherein the binder is fibrous in multiple directions. As used herein, the term "fibrous in multiple directions" means that the linear structure formed by fibrosis is not aligned in a specific direction, but is irregularly positioned, such that the entire linear structure has no specific orientation. According to one embodiment of the present invention, the binder fibrous in multiple directions is not concentrated near the surface in a direction parallel to the surface of the active layer, but is uniformly distributed up to the center of the active layer, without a specific orientation.

[0043] Typically, when preparing electrodes for lithium-ion batteries, electrode active materials, conductive materials, and binders are mixed to prepare a mixture containing electrode active materials. Considering the processability of the mixture, it can also be added to a solvent such as water or an organic solvent and used in slurry form. After the mixture is applied to an electrode current collector, the electrode is prepared by pressing it using equipment such as rollers. In solvent-free dry manufacturing during mixture preparation, the functionality of the binder may be reduced, thus potentially decreasing the adhesion between the electrode active materials, conductive materials, and binder. These problems can be addressed by fibrousizing the binder with pressure. However, when the surface of the mixture is pressed using rollers, there are still shortcomings in ensuring the adhesion of the individual components, for example, such as... Figure 1 As shown, fibrosis occurs centered on the surface in contact with the roll, or it occurs only in a specific direction parallel to the roll's travel direction. In response, this invention provides an electrode for a lithium secondary battery, wherein multidirectional fibrosis using an adhesive improves the bonding strength between the components of the active layer in the electrode. Figure 1 The difference is that the active layer of the adhesive, which is fiberized in multiple directions, can have the same properties as... Figure 2 Same structure.

[0044] An active layer refers to a layer comprising electrode active materials, conductive materials, and a binder. If the electrode contains a current collector, the active layer refers to the material layer applied to the current collector, and is therefore a layer distinct from the electrode current collector. Because the active layer contains electrode active materials, it is active in the electrochemical reactions within the electrode; it can be referred to as an electrode active material layer in terms of containing electrode active materials, and as a mixed layer in terms of being formed by mixing electrode active materials, conductive materials, and a binder.

[0045] According to one embodiment of the invention, for the active layer, the average diameter (D) of the particles when milled at 10,000 rpm for 30 seconds using a stirrer with four blades (manufacturer: Waring, equipment: LB10S, grinding vessel: SS110) is... 50 The diameter is between 200 μm and 500 μm. The average diameter (D) 50 The median diameter (D) is the particle size at the point where the cumulative value reaches 50% of the total volume, calculated based on the particle size distribution. It refers to the particle size at this point in the cumulative curve obtained by calculating the particle size distribution based on volume and taking the total volume as 100%. The average diameter (D) is... 50 The average diameter (D) of the ground particles can be measured using laser diffraction. 50The average diameter (D) of these particles can be greater than 200 μm, greater than 210 μm, greater than 220 μm, greater than 230 μm, greater than 240 μm, or greater than 250 μm; it can also be less than 500 μm, less than 490 μm, less than 480 μm, less than 470 μm, less than 460 μm, or less than 450 μm; or it can be between 200 μm and 500 μm, between 230 μm and 470 μm, or between 250 μm and 450 μm. 50 It is significantly larger than the size of the individual particles of the electrode active material, conductive material and binder that make up the active layer, and it is a value that indicates the bonding of the components after the binder is fiberized.

[0046] In one embodiment of the present invention, the tensile strength of the active layer in the MD direction is 7.5 kgf / cm. 2 The tensile strength ratio in the active layer in the MD direction / TD direction is 1 to 1.3. In this text, the MD (machine direction) refers to the direction of roll movement before the final sheet-like active layer is formed, and the TD (transverse direction) refers to the direction perpendicular to the MD direction relative to the electrode plane. Specifically, the tensile strength of the active layer in the MD direction can be 7.5 kgf / cm². 2 Above, 7.6 kgf / cm 2 Above, 7.7 kgf / cm 2 Above, 7.8 kgf / cm 2 Above, 7.9kgf / cm 2 Above, 8.0kgf / cm 2 The higher the upper limit of the tensile strength of the active layer in the MD direction, the better the electrode durability. However, considering the electrode manufacturing process, it can be 20 kgf / cm. 2 Below, 18 kgf / cm 2 Below, 16kgf / cm 2 Below, 14 kgf / cm 2 Below, 12kgf / cm 2 Below, 10kgf / cm 2or less. Usually, due to calendering during final electrode fabrication, the tensile strength in the MD direction is higher than the tensile strength in the TD direction. The active layer of one embodiment of the present invention exhibits high tensile strength in the MD direction and also high tensile strength in the TD direction due to secondary fibrillation. Specifically, the tensile strength ratio in the MD direction / TD direction may be 1 or more, and since the tensile strength in the TD direction is high, the tensile strength ratio in the MD direction / TD direction may be 1.30 or less, 1.28 or less, 1.26 or less, 1.24 or less, 1.22 or less, 1.20 or less. In the active layer of one embodiment of the present invention, the binder is fibrillated in multiple directions through primary fibrillation and secondary fibrillation, thereby maintaining strong durability regardless of the specific direction. Since force is not only applied in a specific direction when driving the battery, having durability in all directions can help improve battery performance. Because the tensile strength ratio in the MD / TD direction is close to 1, the active layer of one embodiment of the present invention has excellent durability in almost all directions.

[0047] When applied to a positive electrode, the electrode active material may be a positive electrode active material, and when applied to a negative electrode, the electrode active material may be a negative electrode active material. The positive electrode active material or the negative electrode active material is not particularly limited as long as it is commonly used in the art.

[0048] According to one embodiment of the present invention, the positive electrode active material is a lithium transition metal oxide. In the lithium transition metal oxide, the transition metal has the form of Li 1+x M y O 2+Z (0≤x≤5, 0<y≤2, 0≤z≤2), wherein M is selected from the group consisting of Ni, Co, Mn, Fe, P, Al, Mg, Ca, Zr, Zn, Ti, Ru, Nb, W, B, Si, Na, K, Mo, V and combinations thereof, and is not particularly limited within the above range. More specifically, the lithium transition metal oxide is selected from LiCoO2, LiNiO2, LiMnO2, Li2MnO3, LiMn2O4, Li(Ni a Co b Mn c )O2 (0<a<1, 0<b<1, 0<c<1, a+b+c=1), LiNi 1-y Co y O2 (0<y<1), LiCo 1-y Mn y O2, LiNi 1- y Mn y O2 (0<y<1), Li(Ni a Co b Mn c)O4(0<a<2, 0<b<2, 0<c<2, a+b+c=2), LiMn 2-z Ni z O4(0<z<2), LiMn 2-z Co z O4(0<z<2) and combinations thereof.

[0049] According to one embodiment of the present invention, the negative electrode active material is a compound capable of reversibly intercalating and deintercalating lithium. Specific examples of the negative electrode active material may be: carbonaceous materials, such as artificial graphite, natural graphite, graphitized carbon fibers and amorphous carbon; metallic substances capable of alloying with lithium, such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys or Al alloys; metal oxides capable of doping and dedoping lithium, such as SiO β (0<β<2), SnO2, vanadium oxides and lithium vanadium oxides; or composites containing the above metallic substances and carbonaceous materials, such as Si-C composites or Sn-C composites, and any one or a mixture of two or more thereof may be used. In addition, a metallic lithium thin film may be used as the negative electrode active material. Further, as the carbon material, low-crystallinity carbon and high-crystallinity carbon can be used. Representative low-crystallinity carbons include soft carbon and hard carbon, while representative high-crystallinity carbons include amorphous, plate-like, flake-like, spherical or fibrous natural graphite or artificial graphite, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fibers, mesocarbon microbeads, mesophase pitch, and high-temperature calcined carbon (such as coke derived from petroleum or coal tar pitch).

[0050] According to one embodiment of the present invention, the electrode active material is a lithium transition metal oxide having an average particle diameter (D 50 ) of 7 μm to 30 μm. Specifically, the average particle diameter (D 50 ) may be 7 μm or more, 7.5 μm or more, 8 μm or more, 8.5 μm or more, 9 μm or more, 9.5 μm or more, 10 μm or more, may be 30 μm or less, 28 μm or less, 26 μm or less, 24 μm or less, 22 μm or less, 20 μm or less, and may be 7 μm to 30 μm, 8.5 μm to 24 μm, 10 μm to 20 μm. The average diameter (D 50 ) of these particles is significantly smaller than the average diameter (D 50 ) of the ground active layer particles described above. Within the above range, the binding force of the electrode active material can be improved through multidirectional fibrillation of the binder.

[0051] Conductive materials are used to impart conductivity to electrodes. They can be used without any particular restrictions as long as they possess electronic conductivity without causing chemical changes in the battery to be constructed. Specific examples of conductive materials can be: graphite, such as natural or artificial graphite; carbonaceous materials, such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermally cracked carbon black, single-walled or multi-walled carbon nanotubes, carbon fibers, graphene, activated carbon, activated carbon fibers, etc.; metal powders or fibers of copper, nickel, aluminum, silver, etc.; conductive whiskers, such as zinc oxide and potassium titanate; conductive metal oxides, such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and one or more mixtures of these can be used.

[0052] The conductive material can be a carbonaceous material or a metallic material, and the metallic material can include the aforementioned metal powder, metal fiber, conductive metal oxide, etc. The conductive material can be spherical particles or linear particles. If the conductive material is spherical particles, then the average particle size (D) 50 The diameter of the conductive material can range from 1 nm to 100 nm, specifically from 5 nm to 70 nm, and more specifically from 10 nm to 40 nm. If the conductive material is in the form of linear particles, the length of the linear particles can range from 1 μm to 10 μm, specifically from 2 μm to 9 μm, and more specifically from 3 μm to 8 μm. The diameter of the vertical cross-section can range from 10 nm to 500 nm, specifically from 50 nm to 350 nm, and more specifically from 100 nm to 200 nm. The particle size of the conductive material is significantly smaller than the average diameter (D) of the active layer particles after grinding. 50 ).

[0053] Adhesives are used to improve the adhesion between electrode active material particles and the adhesion between the electrode active material and the electrode current collector. To achieve the objectives of this invention, the adhesive is a material that can be fibrousized by pressure or the like, and there are no particular limitations as long as it is a fibrous material and is commonly used as an adhesive in the art. According to one embodiment of the invention, the adhesive comprises polytetrafluoroethylene (PTFE). As far as the adhesive is concerned, since it exists in a fibrous state within the active layer, its particle size is less important than that of other components.

[0054] According to one embodiment of the invention, based on the total weight of the electrode active material, the binder content in the active layer is from 0.5% to 5% by weight, specifically from 1% to 4.5% by weight, and more specifically from 1.5% to 4% by weight. The significance of this invention is that even using a small amount of binder can increase the overall adhesion of the active layer.

[0055] If the adhesive substantially comprises a fibrous adhesive, such as polytetrafluoroethylene (PTFE), it can be used by modifying the fibrous adhesive or by mixing in additional adhesives. The additional adhesives can be adhesives commonly used in the art, provided they function to improve the adhesion between electrode active material particles and between the electrode active material and the electrode current collector. According to one embodiment of the invention, the additional adhesive is selected from, but not limited to, polyvinylidene fluoride (PVDF), ethylene-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polyimide, polyamide-imide, polyethylene, polypropylene, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene-butadiene rubber, fluororubber, and combinations thereof.

[0056] The active layer can be applied to the electrode current collector and thus incorporated into the electrode. There are no particular limitations on the electrode current collector, as long as it is conductive without causing chemical changes in the battery, and it can be, for example, stainless steel, aluminum, nickel, titanium, sintered carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. Furthermore, the thickness of the electrode current collector can typically range from 3 μm to 500 μm, and the adhesion of the electrode active material can be increased by forming fine irregularities on the surface of the electrode current collector. For example, the electrode current collector can be used in various forms, such as films, sheets, foils, meshes, porous bodies, foams, and nonwoven fabrics.

[0057] According to one embodiment of the present invention, the present invention provides a method for preparing an electrode for a lithium secondary battery as described above. The method comprises preparing an active layer by the following steps: (1) mixing an electrode active material, a conductive material, and a binder stored at low temperature; (2) performing a primary fiberization of the mixed material at high temperature; (3) grinding the fiberized material at room temperature; and (4) performing a secondary fiberization of the ground material. The active layer prepared in this manner is then introduced onto an electrode current collector as needed, thereby preparing the final electrode.

[0058] Step (1) is a step of uniformly mixing the electrode active material, conductive material, and binder, wherein storing the electrode active material, conductive material, and binder at a low temperature prevents the aggregation of individual particles. According to one embodiment of the invention, the electrode active material, conductive material, and binder are stored at -20°C to -1°C. Specifically, the storage temperature can be above -20°C, above -19°C, above -18°C, above -17°C, above -16°C, or above -15°C; it can be below -1°C, below -2°C, below -3°C, below -4°C, or below -5°C; or it can be between -20°C and -1°C, -17°C and -3°C, or -15°C and -5°C. This storage temperature minimizes the adhesion between the particles of the electrode active material, conductive material, and binder, and then the particles can be uniformly distributed by mixing. The low-temperature storage time can be extended, but storage for about 5 to 15 minutes is sufficient to obtain the desired effect.

[0059] The electrode active material, conductive material, and binder, stored at low temperature, are mixed briefly at room temperature in a stirrer. According to one embodiment of the invention, the electrode active material, conductive material, and binder are mixed using a stirrer rotating at 5000 RPM to 20000 RPM. Specifically, the rotation speed can be above 5000 RPM, above 5500 RPM, above 6000 RPM, above 6500 RPM, above 7000 RPM, or above 7500 RPM; it can be below 20000 RPM, below 19000 RPM, below 18000 RPM, below 17000 RPM, below 16000 RPM, or below 15000 RPM; or it can be between 5000 RPM and 20000 RPM, 6000 RPM and 17000 RPM, or 7500 RPM and 15000 RPM. This rotation speed enables effective and uniform mixing in a short time. Mixing can be carried out in a short time of less than one minute to enhance the effect of low-temperature storage.

[0060] Step (2) is a first-stage fiberization step of the mixture, which fiberizes the binder contained in the mixture and then adheres it to the electrode active material and the conductive material. In the first fiberization step, a kneader capable of applying a shear force above a certain level to the mixture can be used. In this specification, a "kneader" refers to a device capable of applying a shear force of, for example, 20 N·m to 200 N·m to the mixture, and if such shear force can be applied, a "mixer" may also be included in the "kneader" in this specification. This shear force refers to the maximum shear force applied to the mixture by the device, which is measured by a torque rheometer. Specifically, the shear force can be 20 N·m or more, 25 N·m or more, 30 N·m or more, 35 N·m or more, 40 N·m or more, 45 N·m or more, or 50 N·m or more; it can be less than 200 N·m, less than 190 N·m, less than 180 N·m, less than 170 N·m, less than 160 N·m, or less than 150 N·m; or it can be between 20 N·m and 200 N·m, between 35 N·m and 170 N·m, or between 50 N·m and 150 N·m. The shear force generated by this device is suitable for the fiberization of adhesives. According to one embodiment of the invention, the kneader can be a twin-screw kneader or a paradoxical mixer, specifically a twin-screw kneader.

[0061] According to one embodiment of the invention, a twin-screw kneader rotating at 10 to 50 RPM is used to perform a single fiberization of the mixed material. Specifically, the rotation speed can be 10 RPM or higher, 12 RPM or higher, 14 RPM or higher, 16 RPM or higher, 18 RPM or higher, 20 RPM or higher, or 50 RPM or lower, 48 RPM or lower, 46 RPM or lower, 44 RPM or lower, 42 RPM or lower, 40 RPM or lower, or 10 to 50 RPM, 16 to 46 RPM, or 20 to 40 RPM. Unlike mixing, this rotation speed is a very slow speed to ensure sufficient time for fiberization. Using a twin-screw kneader, sufficient pressure is applied to the interior of the mixed material to achieve overall fiberization. Sufficient effect can be obtained by performing a single fiberization for approximately 5 to 10 minutes.

[0062] When using a twin-screw kneader for primary fiberization, the formability of the adhesive can be increased when carried out at a high temperature rather than at room temperature. According to one embodiment of the invention, the primary fiberization step is performed at 50°C to 70°C. Specifically, the high temperature can be above 50°C, above 51°C, above 52°C, above 53°C, above 54°C, or above 55°C; it can be below 70°C, below 69°C, below 68°C, below 67°C, below 66°C, or below 65°C; or it can be between 50°C and 70°C, 53°C and 67°C, or 55°C and 65°C. This temperature is suitable for the fiberization of the adhesive.

[0063] Step (3) is a primary grinding step of the fibrous material, wherein the primary fibers are rearranged by grinding, which enables more complex and multidirectional fiberization during secondary fiberization. According to one embodiment of the invention, the fibrous material is ground at room temperature using a stirrer rotating at 5000 RPM to 20000 RPM. Specifically, the rotation speed can be above 5000 RPM, above 5500 RPM, above 6000 RPM, above 6500 RPM, above 7000 RPM, above 7500 RPM, below 20000 RPM, below 19000 RPM, below 18000 RPM, below 17000 RPM, below 16000 RPM, below 15000 RPM, or between 5000 RPM and 20000 RPM, 6000 RPM and 17000 RPM, or 7500 RPM and 15000 RPM. This rotation speed allows for efficient grinding to a suitable size in a short time. If the mixing time is short, less than 1 minute, it can prevent the fibrous particles from being over-ground.

[0064] Step (4) is a secondary fiberization step of the ground material, wherein the rearranged primary fibers are reconnected through grinding, and any deficiencies in the fiberization are supplemented. According to one embodiment of the invention, the ground material is subjected to secondary fiberization using a three-roll mill rotating at 5 RPM to 20 RPM. Specifically, the rotation speed can be 5 RPM or higher, 6 RPM or higher, 7 RPM or higher, 8 RPM or higher, 9 RPM or higher, 10 RPM or higher, or 20 RPM or lower, 19 RPM or lower, 18 RPM or lower, 17 RPM or lower, 16 RPM or lower, 15 RPM or lower, or 5 RPM to 20 RPM, 8 RPM to 17 RPM, 10 RPM to 15 RPM. Unlike mixing and grinding, this rotation speed is a very slow rotation speed, which is to ensure sufficient time for fiberization. Using a three-roll mill, the gap between the rollers gradually narrows to allow for gradual fiberization, eventually processing the material into sheets. The secondary fiberization ends naturally when all the material has passed through the rollers.

[0065] When secondary fiberization is performed using a three-roll mill, the formability of the adhesive can be increased when it is carried out at a high temperature rather than at room temperature. According to one embodiment of the invention, the secondary fiberization step is performed at 40°C to 60°C. Specifically, the high temperature can be above 40°C, above 41°C, above 42°C, above 43°C, above 44°C, or above 45°C; it can be below 60°C, below 59°C, below 58°C, below 57°C, below 56°C, or below 55°C; or it can be between 40°C and 60°C, between 43°C and 57°C, or between 45°C and 55°C. This temperature is suitable for the fiberization of the adhesive and complements the primary fiberization, and processing can be carried out at a slightly lower temperature than the primary fiberization.

[0066] After grinding in step (3) and before secondary fiberization in step (4), the ground material can be screened. When preparing the active layer by screening materials that are well-coordinated with each other from the ground material and then fiberizing them, defects in the active layer can be minimized and it can be prepared into a uniform sheet. The ground material can be screened according to the particle size. When screening according to the particle size, a sieve can be used. According to one embodiment of the invention, materials with a particle size of less than 1 mm are selected from the material ground in step (3). If the particle size is less than 1 mm, there is no problem in forming a uniform sheet because the fluidity is higher than normal. If the particle size is greater than 1 mm, there may be disadvantages such as the formation of pores in the prepared sheet due to the poor fluidity. Since the particle size distribution determined by grinding increases the number of particles around the average particle size, the small-sized particles are not only fewer in number but also occupy a smaller volume, so they do not have a significant adverse effect on the formation of the sheet.

[0067] According to one embodiment of the present invention, the bulk density of the particles screened by the above method is from 0.8 g / ml to 1.5 g / ml. As used herein, bulk density refers to the density of the particles when they are resting and packed without special handling. Specifically, the bulk density can be 0.8 g / ml or more, 0.9 g / ml or more, or 1.0 g / ml or more; it can be 1.5 g / ml or less, 1.4 g / ml or less, or 1.3 g / ml or less; or it can be from 0.8 g / ml to 1.5 g / ml, 0.9 g / ml to 1.4 g / ml, or 1.0 g / ml to 1.3 g / ml. When the particles are screened within the above range, the flowability can be at a level that will not adversely affect the preparation of the sheet.

[0068] According to one embodiment of the present invention, the Hausner ratio of the particles screened by the above method is 1.6 or less. As used herein, the Hausner ratio refers to the value obtained by dividing the tapped density by the bulk density, which is the density after compression by additional tapping in the resting filled state when the bulk density is measured. In the case of compression by tapping, the tapped density is usually greater than the bulk density because the volume filled with particles is reduced, and therefore the Hausner ratio is 1.0 or more. Specifically, the Hausner ratio is 1.6 or less, 1.5 or less, and 1.4 or less. When the particles are screened within the above range, the flowability can be at a level that will not adversely affect the preparation of the sheet.

[0069] Electrodes manufactured using the method described above can be used in lithium secondary batteries. Lithium secondary batteries are typically manufactured by placing a separator between the positive and negative electrodes and then injecting an electrolyte, but they can be modified into various shapes as needed.

[0070] The separator separates the negative and positive electrodes and provides a channel for lithium-ion movement. It can be used without any particular limitations as long as it is commonly used as a separator in lithium-ion secondary batteries. In particular, it is preferable that the separator has low resistance to ion movement of the electrolyte and excellent impregnation ability with the electrolyte. Specifically, as the separator, porous polymer membranes can be used, such as porous polymer membranes made of polyolefin polymers (e.g., ethylene homopolymer, propylene homopolymer, ethylene / butene copolymer, ethylene / hexene copolymer, ethylene / methacrylate copolymer, etc.), or their two- or more-layered stacked structures. Alternatively, conventional porous nonwoven fabrics can be used, such as nonwoven fabrics made of high-melting-point glass fibers, polyethylene terephthalate fibers, etc. Furthermore, separators coated with ceramic components or polymer materials can be used to ensure heat resistance or mechanical strength, and can optionally use single-layer or multi-layer structures.

[0071] Electrolytes include, but are not limited to, organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used to manufacture lithium secondary batteries.

[0072] Specifically, the electrolyte may contain organic solvents and lithium salts.

[0073] Organic solvents can be used without any particular restrictions as long as they can serve as a medium through which ions participating in the electrochemical reaction of the battery can move. Specifically, organic solvents can be ester solvents, such as methyl acetate, ethyl acetate, γ-butyrolactone, or ε-caprolactone; ether solvents, such as dibutyl ether or tetrahydrofuran; ketone solvents, such as cyclohexanone; aromatic hydrocarbon solvents, such as benzene or fluorobenzene; carbonate solvents, such as dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl ethyl carbonate (MEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); alcohol solvents, such as ethanol and isopropanol; nitriles, such as R-CN (where R is a straight-chain, branched, or cyclic C2-C20 hydrocarbon group, which may contain double-bonded aromatic rings or ether bonds); amides, such as dimethylformamide; dioxolane, such as 1,3-dioxolane; or sulfones. Carbonate solvents are preferred, and even more preferred are mixtures of cyclic carbonate compounds (e.g., ethylene carbonate or propylene carbonate) with high ionic conductivity and high dielectric constant, and linear carbonate compounds (e.g., ethyl methyl carbonate, dimethyl carbonate, or diethyl carbonate) with low viscosity, which can improve the charge-discharge performance of the battery. In this case, when cyclic carbonates and linear carbonates are mixed in a volume ratio of about 1:1 to about 1:9, the performance of the electrolyte can be excellent.

[0074] Lithium salts can be used without particular restriction as long as they are compounds capable of providing lithium ions for lithium secondary batteries. Specifically, lithium salts can be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2. The concentration of the lithium salt is preferably in the range of 0.1 M to 2.0 M. If the concentration of the lithium salt is within this range, excellent electrolyte performance can be exhibited due to the suitable conductivity and viscosity of the electrolyte, and lithium ions can move efficiently.

[0075] To improve battery life characteristics, suppress battery capacity degradation, and improve battery discharge capacity, in addition to the electrolyte components mentioned above, the electrolyte may also contain one or more additives, such as: alkylene carbonate halogenated compounds, such as ethylene difluorocarbonate; pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, n-glycol dimethyl ether, triamide hexaphosphate, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinones, N,N-substituted imidazolides, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride. In this case, the content of additives may be from 0.1% by weight to 5% by weight, based on the total weight of the electrolyte.

[0076] As described above, since the lithium secondary battery incorporating the electrodes of the present invention stably exhibits excellent discharge capacity, output characteristics and capacity retention, it can be used in the field of portable devices, such as mobile phones, laptops, and digital cameras, as well as in the field of electric vehicles, such as hybrid electric vehicles (HEVs).

[0077] Therefore, according to another embodiment of the present invention, a battery module comprising the lithium secondary battery as a unit cell and a battery pack comprising the battery module are provided.

[0078] The battery module or battery pack can be used as a power source for any one or more of the following medium to large-sized devices: power tools; electric vehicles, including electric vehicles (EVs), hybrid electric vehicles and plug-in hybrid electric vehicles (PHEVs); or power storage systems.

[0079] Preferred embodiments are presented below to aid in understanding the invention, but the following embodiments are provided to facilitate a better understanding of the invention, and the invention is not limited thereto.

[0080] Example

[0081] Example 1

[0082] 96% by weight of LiNi was prepared as an electrode active material by storing it in a refrigerator at -10°C for 10 minutes. 0.5 Co 0.3 Mn 0.2 O2 (average particle size (D) 50 ): 10μm, manufacturer: LG Chem, product: HN803S), 2% by weight VGCF (vapor-grown carbon fiber, average diameter: 150nm, average length: 6μm, manufacturer: Showa Denko, product: VGCF-H) as conductive material, 2% by weight polytetrafluoroethylene (particle average particle size (D) as binder 50(500μm, Manufacturer: Chemours, Product: 601x). Remove the prepared electrode active material, conductive material, and binder from the refrigerator and mix at room temperature in a stirrer (manufacturer: Waring, Equipment: LB10S, Container: SS110) at 10000 RPM for 30 seconds. Fiberize the mixture once in a twin-screw kneader (manufacturer: Brabender, Product: Torque Rheometer) at 60°C and 30 RPM for 5 minutes. Grind the fiberized material in a stirrer (manufacturer: Waring, Equipment: LB10S, Container: SS110) at room temperature and 10000 RPM for 30 seconds. Among the ground particles, only particles with a diameter of less than 1 mm are selected and rolled on a three-roll mill (roll gap: 150 μm / 100 μm, manufacturer: Kmtech, product: KRM-80B) at a temperature of 50°C and a speed of 10 RPM to finally prepare a sheet-like active layer.

[0083] Comparative Example 1

[0084] 96% by weight of LiNi was prepared as an electrode active material by storing it in a refrigerator at -10°C for 10 minutes. 0.5 Co 0.3 Mn 0.2 O2 (average particle size (D) 50 ): 10μm, manufacturer: LG Chem, product: HN803S), 2% by weight VGCF (vapor-grown carbon fiber, average diameter: 150nm, average length: 6μm, manufacturer: Showa Denko, product: VGCF-H) as conductive material, 2% by weight polytetrafluoroethylene (particle average particle size (D) as binder 50 (100nm, Manufacturer: Chemours, Product: 601x). The prepared electrode active material, conductive material, and binder were removed from the refrigerator and mixed for 30 seconds at room temperature in a stirrer (Manufacturer: Waring, Equipment: LB10S, Container: SS110) at 10000 RPM. The mixed materials were then rolled using a three-roll mill (roll gap: 150μm / 100μm, Manufacturer: Kmtech, Product: KRM-80B) at 50°C and 10 RPM to finally prepare a sheet-like active layer.

[0085] Comparative Example 2

[0086] The active layer prepared in Comparative Example 1 was milled for 30 seconds at room temperature and 10,000 RPM in a stirrer (manufacturer: Waring, equipment: LB10S, container: SS110). From the milled particles, only particles with a diameter of 1 mm or less were selected, and these particles were then rolled in a three-roll mill (roll gap: 150 μm / 100 μm, manufacturer: Kmtech, product: KRM-80B) at 50°C and 10 RPM to finally prepare a sheet-like active layer.

[0087] Comparative Example 3

[0088] In addition to using average particle size (D) 50 LiNi with a thickness of 5 μm 0.5 Co 0.3 Mn 0.2 In addition to using O2 as the electrode active material, a sheet-like active layer was prepared in the same manner as in Example 1.

[0089] Experimental Example

[0090] Experimental Example 1

[0091] The internal and external structures of each active layer prepared in Example 1 and Comparative Example 1 were confirmed by scanning electron microscopy (SEM, magnification: ×3000, manufacturer: JEOL, product: JSM-7200F), and the results are as follows. Figure 3a (Inside the active layer of Comparative Example 1) Figure 3b (External active layer of Comparative Example 1) Figure 4a (Inside the active layer of Example 1) and Figure 4b (External active layer of Example 1) is shown.

[0092] Compare Figure 3a and Figure 4a Inside the active layer of Comparative Example 1, it was confirmed that polytetrafluoroethylene aggregated without becoming fibrous, but it was also confirmed that inside the active layer of Example 1 (… Figure 4a In this process, polytetrafluoroethylene (PTFE) is fibrous, and the electrode active material and conductive material are adhered to the fibrous PTFE.

[0093] Compare Figure 3b and Figure 4b Outside the active layer, in the case of the active layer outside Comparative Example 1 ( Figure 3b Although polytetrafluoroethylene is fibrous, the fibrous portion is not clearly identified; however, in the case of the active layer outside of Example 1 ( Figure 4b Because of the re-fiberization through roller pressing, the fibrous parts are more clearly identified.

[0094] Experiment Example 2

[0095] Each active layer prepared in Example 1 and Comparative Examples 1 and 2 was milled at 10,000 rpm for 30 seconds in a milling apparatus (manufacturer: Waring, equipment: LB10S, milling container: SS110), and the particle size after milling was analyzed by Optical PSD (Malvern Morphology). The results are as follows: Figure 5 As shown.

[0096] In the case of the active layer in Comparative Example 1, the adhesion between the materials constituting the active layer was not high, so the material was ground into individual particles or small aggregates. In the case of the active layer in Comparative Example 2, compared to Comparative Example 1, the adhesion between the materials constituting the active layer was improved by two rolling processes, and the material was ground into larger aggregates than in Comparative Example 1. In the case of the active layer in Example 1, the adhesion between the materials constituting the active layer was the highest by using a twin-screw kneader during one fiberization process, and the material was ground into relatively much larger aggregates compared to Comparative Examples 1 and 2. Figure 5 The particle size distributions of Comparative Examples 1 and 2, and Example 1, are shown respectively. In fact, it was found that the average diameter (D) of the milled particles in Comparative Example 1 was significantly larger. 50 The average diameter (D) of the ground particles in Comparative Example 2 is 50 μm. 50 The average diameter (D) of the milled particles in Example 1 is 150 μm. 50 The value is 400μm.

[0097] Experimental Example 3

[0098] The tensile strength of each active layer prepared in Example 1 and Comparative Examples 1 and 2 in the MD and TD directions was analyzed using a tensile strength measuring device (manufacturer: LLOYD, product: LS1). The results are shown in Table 1 below.

[0099] Table 1:

[0100] Tensile strength Example 1 Comparative Example 1 Comparative Example 2 <![CDATA[MD direction (kgf / cm 2 )]]> 8.3 3.3 6 <![CDATA[TD direction (kgf / cm 2 )]]> 7.1 1.9 5.2 MD direction / TD direction 1.16 1.7 1.15

[0101] According to Table 1, Examples 1 and Comparative Examples 1 and 2 all exhibited high tensile strength in the MD direction. However, for Examples 1 and Comparative Example 2, which were rolled after grinding, the tensile strength ratio in the MD direction / TD direction was also less than 1.2, indicating that the difference in tensile strength between the MD and TD directions was not significant. As in Example 1, when a twin-screw kneader was used for primary fiberization, the tensile strength in both the MD and TD directions was increased by more than 35% compared to Comparative Example 2, which was used for primary fiberization via a roller mill.

[0102] Experiment Example 4

[0103] The tensile strength in the MD direction of each active layer prepared in Example 1 and Comparative Example 3 was analyzed using a tensile strength measuring device. The results are shown in Table 2 below.

[0104] Table 2:

[0105] Tensile strength Example 1 Comparative Example 3 <![CDATA[MD direction (kgf / cm 2 )]]> 8.3 3.1

[0106] According to Table 2, in Comparative Example 3, the average particle size (D) of the electrode active material particles is... 50 The particle size is 5 μm, which is similar to the average particle size (D) of the electrode active material particles in Example 1. 50 Compared to 10 μm, the tensile strength in the MD direction is significantly lower.

[0107] Experimental Example 5

[0108] The particles ground in Example 1 were classified into five size ranges (based on particle size: Range 1: greater than 45 μm and less than 150 μm; Range 2: greater than 150 μm and less than 450 μm; Range 3: greater than 450 μm and less than 850 μm; Range 4: greater than 850 μm and less than 1000 μm; Range 5: greater than 1000 μm). The bulk density and tap density were measured, and the Hausner ratio was calculated, as shown in Table 3 below. Figure 6 As shown.

[0109] Table 3:

[0110] Particle size Bulk density (g / ml) Tap density (g / ml) Hausner First interval: greater than 45μm and less than 150μm 1.25 1.51 1.21 Second range: greater than 150μm and less than 450μm 1.20 1.45 1.20 Third interval: greater than 450μm and less than 850μm 1.07 1.36 1.27 Zone 4: Greater than 850 μm and less than 1000 μm 1.09 1.45 1.33 Zone 5: Greater than 1000μm 0.71 1.2 1.68

[0111] *Bulk density (g / ml): Measure the mass of the granules at rest when packed in a 100ml graduated cylinder and calculate the mass per unit volume (average of 5 repeated measurements) (Manufacturer: SEISHIN, Product: KYT-4000).

[0112] * Tapped density (g / ml): The granules are filled into a 100ml graduated cylinder at rest. Then, the graduated cylinder filled with granules is arbitrarily compressed by tapping with a constant force 1000 times using a tapped density volumetric meter. The mass is then measured and the mass per unit volume is calculated (average of 5 repeated measurements).

[0113] *Hausner ratio: The value obtained by dividing the tap density by the bulk density.

[0114] Based on the following criteria named after Henry H. Hausner, it can be seen in Table 4 and Figure 7 The assessment shown is based on the liquidity rating according to the Hausner ratio.

[0115] Table 4:

[0116] Hausner Liquidity assessment Greater than 1.60 Range Above 1.46 and below 1.60 Difference Above 1.35 and below 1.46 Slightly worse Above 1.26 and below 1.35 normal Above 1.19 and below 1.26 Slightly better Values ​​above 1.12 and below 1.19 good Above 1.00 and below 1.12 Excellent

[0117] Based on the flowability grades according to the Hausner ratio in Table 4, it can be seen that in Table 3, the 5th interval has extremely poor flowability, the 3rd and 4th intervals have normal flowability, and the 1st and 2nd intervals have slightly better flowability. If there are differences in flowability depending on the type of milled particles, unnecessary damage may occur during the subsequent electrode preparation via a secondary fiberization step.

[0118] All simple modifications and variations of this invention fall within its scope, and the specific scope of protection of this invention will be apparent from the appended claims.

Claims

1. An electrode for a lithium secondary battery, comprising an active layer including an electrode active material, a conductive material, and a binder, wherein, The adhesive is fiberized in multiple directions; The active layer is prepared by the following steps: (1) Mix the electrode active material, conductive material and adhesive stored at -20℃ to -1℃; (2) The mixed material is fiberized once at 50℃ to 70℃; (3) Grinding the fibrous material at room temperature; (4) The ground material is subjected to secondary fiberization.

2. The electrode for a lithium secondary battery as described in claim 1, wherein, For the active layer, the average diameter D of the particles when milled at 10,000 rpm for 30 seconds using a stirrer with 4 blades is... 50 It ranges from 200 μm to 500 μm.

3. The electrode for a lithium secondary battery as described in claim 1, wherein, The active layer has a tensile strength of 7.8 kgf / cm in the MD direction. 2 above.

4. The electrode for a lithium secondary battery as described in claim 1, wherein, The electrode active material has an average particle size D. 50 It is a lithium transition metal oxide with a thickness of 7 μm to 30 μm.

5. The electrode for a lithium secondary battery as described in claim 1, wherein, The conductive material is a carbonaceous material or a metallic material.

6. The electrode for a lithium secondary battery as described in claim 1, wherein, The adhesive contains polytetrafluoroethylene.

7. The electrode for a lithium secondary battery as described in claim 1, wherein, Based on the total weight of the electrode active material, the content of the adhesive in the active layer is from 1.5% to 4% by weight.

8. The electrode for a lithium secondary battery as described in claim 1, wherein, The tensile strength ratio of the active layer in the MD direction to the TD direction is 1 to 1.

3.

9. The electrode for a lithium secondary battery as described in claim 1, wherein, The active layer has a tensile strength of 7.5 kgf / cm in the MD direction. 2 above.

10. A method for preparing an electrode for a lithium secondary battery according to claim 1, the method comprising preparing an active layer by the following steps: (1) Mix the electrode active material, conductive material and adhesive stored at -20℃ to -1℃; (2) The mixed material is fiberized once at 50℃ to 70℃; (3) Grinding the fibrous material at room temperature; (4) The ground material is subjected to secondary fiberization.

11. The method for preparing an electrode for a lithium secondary battery as described in claim 10, wherein, In step (1), the electrode active material, conductive material and binder are mixed using a stirrer rotating at 5000 RPM to 20000 RPM.

12. The method for preparing an electrode for a lithium secondary battery as described in claim 10, wherein, In step (2), a kneader is used to apply a shear force of 20 N·m to 200 N·m to the mixture.

13. The method for preparing an electrode for a lithium secondary battery as described in claim 10, wherein, In step (2), the mixture is fiberized once using a twin-screw kneader rotating at 10 RPM to 50 RPM.

14. The method for preparing an electrode for a lithium secondary battery as described in claim 10, wherein, In step (3), the fibrous material is ground at room temperature using a stirrer rotating at 5000 RPM to 20000 RPM.

15. The method for preparing an electrode for a lithium secondary battery as described in claim 10, wherein, In step (4), the milled material is subjected to secondary fiberization at 40°C to 60°C using a three-roll mill rotating at 5 RPM to 20 RPM.

16. The method for preparing an electrode for a lithium secondary battery as described in claim 10, wherein, The particles ground in step (3) are selected such that only particles with a diameter of less than 1 mm are included before the secondary fiberization in step (4).

17. The method for preparing an electrode for a lithium secondary battery as described in claim 10, wherein, The particles ground in step (3) are selected such that the Hausner ratio is below 1.6 before the secondary fiberization in step (4).

Citation Information

Patent Citations

  • Cathode for lithium-containing batteries and solvent-free method for the production thereof

    KR1020140136952A

  • Medical multi way stop cock

    KR1020210123848A

  • User interface apparatus for automatic transmission of agricultural working machine

    KR1020210123856A

  • Method and device for processing system information requests in wireless communication systems

    KR1020220116025A

  • EDLC electrode and manufacturing process thereof

    CN105723484A