A single crystal tail end process
By optimizing the parameter control in the single crystal finishing process, the problems of residual material in the quartz crucible and damage caused by overheating of the heater were solved, achieving full utilization of raw materials and improving production efficiency.
Patent Information
- Application Number
- CN202210105907.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-28
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-01-28
AI Technical Summary
In the existing single-crystal finishing process, the residual material at the bottom of the quartz crucible causes raw material waste, and the excessively high temperature of the main heater can easily damage the quartz crucible or cause it to curl, affecting production efficiency.
By adjusting parameters such as the power of the main heater and bottom heater, the rotation speed of the quartz crucible, the crystal rise rate compensation value, the rising speed of the quartz crucible, and the rotation speed of the single crystal, the finishing process is optimized to ensure that the raw material in the quartz crucible is completely pulled out, avoiding residual material and damage to the quartz crucible.
This achieves zero residue at the bottom of the quartz crucible, improves raw material conversion rate, protects the quartz crucible from damage, reduces costs, and improves production efficiency.
Abstract
Description
Technical Field
[0001] This invention belongs to the technical field of accessories used in Czochralski silicon single crystal furnaces, and in particular relates to a single crystal finishing process. Background Technology
[0002] Currently, in the production of Czochralski silicon single crystal furnaces, after the finishing process of existing technologies, there will be residual material at the bottom of the quartz crucible, resulting in material waste; and the temperature of the main heater is too high during the finishing process, which can easily cause damage to the quartz crucible or abnormalities such as edge curling, affecting production efficiency. Summary of the Invention
[0003] The problem this invention aims to solve is that in existing finishing processes, residual material remains at the bottom of the quartz crucible after finishing, resulting in raw material waste; and the main heater temperature is too high during finishing, which can easily cause damage to the quartz crucible or abnormalities such as edge curling, affecting production efficiency. This invention provides a single-crystal finishing process that eliminates residual material at the bottom of the quartz crucible after finishing, improving raw material conversion rate and preventing waste; furthermore, this process protects the quartz crucible from damage, reduces the risk of edge curling, lowers costs, and improves production efficiency.
[0004] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is as follows:
[0005] A single-crystal finishing process, comprising:
[0006] The power of the main heater at the beginning of the finishing process is set to the first power, and the power of the main heater from the beginning to the middle of the finishing process is set to the second power. From the beginning of the finishing process to the beginning of the finishing process, the first power is reduced to the second power at a constant speed. From the beginning of the finishing process to the first half of the middle of the finishing process, the power of the main heater is maintained at the second power. In the second half of the middle of the finishing process, the power of the main heater rises back to the first power. From the second half of the middle of the finishing process to the end of the finishing process, the power of the main heater is maintained at the first power.
[0007] The bottom heater power is set to the third power at the beginning of the finishing process, and the bottom heater power is set to the fourth power from the middle to the end of the finishing process. From the beginning to the middle of the finishing process, the third power is increased to the fourth power, and from the middle to the end of the finishing process, the bottom heater power is maintained at the fourth power.
[0008] Furthermore, the rotation speed of the quartz crucible at the beginning of the finishing process is set to the first rotation speed, and the rotation speed of the quartz crucible at the end of the finishing process is set to the minimum rotation speed. From the beginning of the finishing process to the middle of the finishing process, the rotation speed of the quartz crucible is maintained at the first rotation speed. From the middle of the finishing process to the end of the finishing process, the rotation speed of the quartz crucible is uniformly reduced from the first rotation speed to the minimum rotation speed.
[0009] Furthermore, the crystal rise rate compensation value at the start of the finishing process is set as the first rate, the crystal rise rate compensation value from the initial stage to the middle stage of the finishing process is set as the second rate, and the crystal rise rate compensation value at the end of the finishing process is set as the maximum rate. From the start of the finishing process to the initial stage of the finishing process, the first rate decreases to the second rate. In the first half of the middle stage of the finishing process, the second rate increases rapidly. From the second half of the middle stage of the finishing process to the end of the finishing process, the second rate increases uniformly to the maximum rate.
[0010] Furthermore, the rising speed of the quartz crucible at the beginning of the finishing process is set as the first rising speed, and the rising speed of the quartz crucible in the middle of the finishing process is set as the second rising speed. From the beginning of the finishing process to the middle of the finishing process, the first rising speed is reduced to the second rising speed. From the middle of the finishing process to the end of the finishing process, the rising speed of the quartz crucible is maintained at the second rising speed.
[0011] Furthermore, when the second acceleration is 0, from the beginning of the final stage to the middle of the final stage, the first acceleration is reduced to 0, and from the middle of the final stage to the end of the final stage, the rising speed of the quartz crucible is 0.
[0012] Furthermore, the single crystal rotation speed at the beginning of the finishing process is set as the first crystal speed, and the single crystal rotation speed in the middle of the finishing process is set as the second crystal speed. From the beginning of the finishing process to the first half of the middle of the finishing process, the single crystal rotation speed is the first crystal speed. In the second half of the middle of the finishing process, the first crystal speed is reduced to the second crystal speed. From the second half of the middle of the finishing process to the end of the finishing process, the single crystal rotation speed is the second crystal speed.
[0013] Furthermore, from the start of the finishing process to its completion, the pressure in the single crystal furnace remains constant.
[0014] Furthermore, from the start of the finishing process to its completion, the argon flow rate of the single crystal furnace remains constant.
[0015] This invention presents a single-crystal crystal finishing process. In the initial stage of finishing, the main heater power is reduced to facilitate the crystallization of raw materials in the quartz crucible. More material is pulled out in the initial stage. In the middle and later stages of finishing, the main heater power is increased. At this point, there is less raw material in the quartz crucible; increasing the power and temperature allows all remaining raw material to be pulled out, preventing it from cooling and solidifying inside the crucible, thus avoiding residue. The power of the bottom heater is increased, and the quartz crucible rotation speed is maintained from the initial to the middle stage of finishing. In the middle and later stages, the quartz crucible rotation speed is reduced, similarly preventing the remaining raw material from cooling and solidifying inside the crucible. In the middle and later stages of finishing, the quartz crucible's rising rate is reduced, and the upper edge of the quartz crucible is moved away from the main heater to avoid damage and the risk of edge curling. After finishing using this process, no residue remains at the bottom of the quartz crucible, improving the raw material conversion rate and eliminating waste. Furthermore, this process protects the quartz crucible from damage, reduces the risk of edge curling, lowers costs, and improves production efficiency. Detailed Implementation
[0016] Embodiments of the present invention are described in detail below, examples of which are illustrated in the accompanying drawings, wherein the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout. The embodiments described below with reference to the accompanying drawings are exemplary and intended to explain the present invention, and should not be construed as limiting the present invention.
[0017] This invention provides a single-crystal finishing process, including:
[0018] The power of the main heater at the beginning of the finishing process is set to the first power. The power of the main heater from the beginning of the finishing process to the middle of the finishing process is set to the second power. From the beginning of the finishing process to the beginning of the finishing process, the first power is reduced to the second power at a constant speed. From the beginning of the finishing process to the first half of the middle of the finishing process, the power of the main heater is maintained at the second power. In the second half of the middle of the finishing process, the power of the main heater rises back to the first power. From the second half of the middle of the finishing process to the end of the finishing process, the power of the main heater is maintained at the first power.
[0019] The bottom heater power is set to the third power at the beginning of the finishing phase, and the bottom heater power is set to the fourth power from the middle to the end of the finishing phase. From the beginning to the middle of the finishing phase, the third power is increased to the fourth power, and from the middle to the end of the finishing phase, the bottom heater power remains at the fourth power.
[0020] Specifically, the finishing process involves uniform crystal pulling. At the start of the finishing process, the initial power of the main heater is the first power. In the early stage of the finishing process, when the length of the pulled single crystal accounts for 10% of the total length of the single crystal, the first power is uniformly reduced to the second power, and the temperature decreases, which is conducive to the crystallization and pulling of the raw material in the quartz crucible. In the middle stage of the finishing process, when the length of the pulled single crystal accounts for 40%-50% of the total length of the single crystal, the power of the main heater is increased back to the first power until the finishing process is completed. In the middle and late stages of the finishing process, most of the raw material in the quartz crucible has been pulled out, leaving a small amount of residual material. At this time, the power of the main heater is increased, and the temperature of the main heater increases, so that the residual material in the quartz crucible is melted and pulled out, preventing the residual material from crystallizing in the quartz crucible and causing residual material, thus achieving no residual material after the finishing process.
[0021] Specifically, at the beginning of the finishing process, the initial power of the bottom heater is the third power. From the early to the middle stage of the finishing process, the power of the bottom heater is increased, and the power of the bottom heater and the main heater work together to heat the quartz crucible. In the middle and late stages of the finishing process, the power of the bottom heater is no longer increased, thus avoiding damage to the quartz crucible caused by excessive power of the bottom heater.
[0022] Preferably, the rotation speed of the quartz crucible at the beginning of the finishing process is set to the first rotation speed, and the rotation speed of the quartz crucible at the end of the finishing process is set to the minimum rotation speed. From the beginning of the finishing process to the middle of the finishing process, the rotation speed of the quartz crucible is maintained at the first rotation speed. From the middle of the finishing process to the end of the finishing process, the rotation speed of the quartz crucible is uniformly reduced from the first rotation speed to the minimum rotation speed.
[0023] Specifically, in the middle of the finishing process, when the length of the pulled single crystal accounts for 40%-50% of the total length of the single crystal, the rotation speed of the quartz crucible is reduced uniformly from the first rotation speed and reaches the minimum rotation speed at the end of the finishing process. At this time, there is no material left in the quartz crucible. The lower the rotation speed of the quartz crucible, the easier it is to be heated. The purpose of reducing the rotation speed of the quartz crucible is also to avoid the remaining raw material in the quartz crucible from crystallizing in the quartz crucible, resulting in the situation of leftover material after the finishing process.
[0024] Preferably, the crystal rise rate compensation value at the beginning of the finishing process is set as the first rate, the crystal rise rate compensation value from the initial stage to the middle stage of the finishing process is set as the second rate, and the crystal rise rate compensation value at the end of the finishing process is set as the maximum rate. From the beginning of the finishing process to the initial stage of the finishing process, the first rate decreases to the second rate. In the first half of the middle stage of the finishing process, the second rate increases rapidly. From the second half of the middle stage of the finishing process to the end of the finishing process, the second rate increases uniformly to the maximum rate.
[0025] Specifically, at the beginning of the finishing process, the initial crystal lifting rate compensation value is the first rate, which quickly retracts the diameter of the single crystal. In the early stage of the finishing process, when the length of the pulled single crystal accounts for 10% of the total length of the single crystal, the first rate is reduced to the second rate, which evenly pulls out the remaining material in the quartz crucible. In the first half of the middle stage of the finishing process, when the length of the pulled single crystal accounts for 45% of the total length of the single crystal, the second rate is rapidly increased, which gradually tapers and lifts the single crystal. In the second half of the middle stage of the finishing process until the end of the finishing process, the second rate is uniformly increased to the maximum rate, which pulls out all the remaining material in the quartz crucible.
[0026] Preferably, the rising speed of the quartz crucible at the beginning of the finishing process is set as the first rising speed, and the rising speed of the quartz crucible in the middle of the finishing process is set as the second rising speed. From the beginning of the finishing process to the middle of the finishing process, the first rising speed is reduced to the second rising speed, and from the middle of the finishing process to the end of the finishing process, the rising speed of the quartz crucible is maintained at the second rising speed.
[0027] Preferably, the second acceleration is 0, from the beginning of the finishing process to the middle of the finishing process, the first acceleration is reduced to 0, and from the middle of the finishing process to the end of the finishing process, the rising speed of the quartz crucible is 0.
[0028] Specifically, at the beginning of the finishing process, the quartz crucible has an initial rising speed, i.e., the first rising speed. From the beginning to the middle of the finishing process, the quartz crucible is in a state of rising with a continuously decreasing speed, i.e., it is approaching the main heater. From the middle to the end of the finishing process, the quartz crucible maintains a constant second rising speed, and its rising speed no longer changes, continuing to rise at the second rising speed. In a preferred embodiment, the quartz crucible drops to the second rising speed of 0, i.e., the quartz crucible stops rising and no longer approaches the main heater, and the upper edge of the quartz crucible is far from the main heater, effectively avoiding the phenomenon of quartz crucible edge curling.
[0029] Preferably, the single crystal rotation speed at the beginning of the finishing process is set as the first crystal speed, and the single crystal rotation speed in the middle of the finishing process is set as the second crystal speed. From the beginning of the finishing process to the first half of the middle of the finishing process, the single crystal rotation speed is the first crystal speed. In the second half of the middle of the finishing process, the first crystal speed is reduced to the second crystal speed. From the second half of the middle of the finishing process to the end of the finishing process, the single crystal rotation speed is the second crystal speed.
[0030] Specifically, from the beginning of the finishing process to the first half of the middle stage, the single crystal is pulled out at the first crystal speed. From the second half of the middle stage to the end of the finishing process, the single crystal is pulled out at the second crystal speed, and the pulling is slower, thus avoiding the possibility of breakage during the crystal pulling process.
[0031] Preferably, the pressure in the single crystal furnace remains constant from the start of the finishing process to its completion.
[0032] Preferably, the argon flow rate of the single crystal furnace remains constant from the start of the finishing process to its completion.
[0033] Specifically, the finishing process maintains stable furnace pressure and argon flow rate to ensure the stability and consistency of power and temperature changes within the single crystal furnace.
[0034] Example 1:
[0035] The single crystal furnace pressure is set to 15 Torr, the argon flow rate is 40 slpm, the main heater's first power is 60 kW, the second power is 30 kW, the bottom heater's first power is 35 kW, the second power is 40 kW, the quartz crucible's first rotation speed is 8 rpm, the minimum rotation speed is 1 rpm, the crystal rise rate compensation values are -10 mm / hr, -25 mm / hr, and the maximum rate is 50 mm / hr, the quartz crucible's first rise rate is 10 mm / hr, the second rise rate is 3 mm / hr, the single crystal's first crystal speed is 6 rpm, and the second crystal speed is 5 rpm. After using this process to finish, there is no residual material in the quartz crucible, and the quartz crucible is not damaged or has rolled edges.
[0036] Example 2:
[0037] The single crystal furnace pressure is set to 15 Torr, the argon flow rate is 40 slpm, the main heater's first power is 60 kW, the second power is 35 kW, the bottom heater's first power is 35 kW, the second power is 40 kW, the quartz crucible's first rotation speed is 8 rpm, the minimum rotation speed is 1 rpm, the crystal rise rate compensation values are -10 mm / hr for the first rate, -25 mm / hr for the second rate, and the maximum rate is 50 mm / hr, the quartz crucible's first rise rate is 10 mm / hr, the second rise rate is 0, the single crystal's first crystal velocity is 6 rpm, and the second crystal velocity is 5 rpm. After using this process to finish, there is no residual material in the quartz crucible, and the quartz crucible is not damaged or has rolled edges.
[0038] The advantages and beneficial effects of this invention are:
[0039] 1. The present invention provides a single-crystal finishing process. After finishing using this process, no residual material will remain at the bottom of the quartz crucible, which can improve the conversion rate of raw materials and eliminate waste. In addition, this process can protect the quartz crucible from damage, reduce the risk of quartz crucible edge curling, reduce costs, and improve production efficiency.
[0040] 2. The single-crystal finishing process designed in this invention first reduces the power of the main heater in the early stage of finishing to facilitate the crystallization of raw materials in the quartz crucible. More material is pulled out in the early stage of finishing. In the middle and late stages of finishing, the power of the main heater is increased. At this time, there is less raw material in the quartz crucible. Increasing the power and temperature can pull out all the remaining raw material in the quartz crucible, preventing the remaining raw material from cooling and solidifying in the quartz crucible and causing leftover material. In addition, the upper edge of the quartz crucible is far away from the main heater, avoiding the edge curling phenomenon caused by excessive temperature of the quartz crucible and protecting the quartz crucible from damage.
[0041] It should be understood that the specific embodiments described above are merely illustrative or explanatory of the principles of the invention and do not constitute a limitation thereof. Therefore, any modifications, equivalent substitutions, improvements, etc., made without departing from the spirit and scope of the invention should be included within the protection scope of the invention. Furthermore, the appended claims are intended to cover all variations and modifications falling within the scope and boundaries of the appended claims, or equivalent forms of such scope and boundaries.
Claims
1. A single crystal tail end process characterized by, include: The power of the main heater at the beginning of the finishing process is set to the first power, and the power of the main heater from the beginning to the middle of the finishing process is set to the second power. From the beginning of the finishing process to the beginning of the finishing process, the first power is reduced to the second power at a constant speed. From the beginning of the finishing process to the first half of the middle of the finishing process, the power of the main heater is maintained at the second power. In the second half of the middle of the finishing process, the power of the main heater rises back to the first power. From the second half of the middle of the finishing process to the end of the finishing process, the power of the main heater is maintained at the first power. The bottom heater power is set to the third power at the beginning of the finishing process, and the bottom heater power is set to the fourth power from the middle to the end of the finishing process. From the beginning to the middle of the finishing process, the third power is increased to the fourth power, and from the middle to the end of the finishing process, the bottom heater power is maintained at the fourth power.
2. The single-crystal finishing process according to claim 1, characterized in that: The rotation speed of the quartz crucible at the beginning of the finishing process is set to the first rotation speed, and the rotation speed of the quartz crucible at the end of the finishing process is set to the minimum rotation speed. From the beginning of the finishing process to the middle of the finishing process, the rotation speed of the quartz crucible is maintained at the first rotation speed. From the middle of the finishing process to the end of the finishing process, the rotation speed of the quartz crucible is uniformly reduced from the first rotation speed to the minimum rotation speed.
3. A single-crystal finishing process according to claim 1 or 2, characterized in that: The crystal rise rate compensation value at the beginning of the finishing process is set as the first rate, the crystal rise rate compensation value from the initial stage to the middle stage of the finishing process is set as the second rate, and the crystal rise rate compensation value at the end of the finishing process is set as the maximum rate. From the beginning of the finishing process to the initial stage of the finishing process, the first rate decreases to the second rate. In the first half of the middle stage of the finishing process, the second rate increases rapidly. From the second half of the middle stage of the finishing process to the end of the finishing process, the second rate increases uniformly to the maximum rate.
4. The single-crystal finishing process according to claim 3, characterized in that: The rising speed of the quartz crucible at the beginning of the finishing process is set as the first rising speed, and the rising speed of the quartz crucible in the middle of the finishing process is set as the second rising speed. From the beginning of the finishing process to the middle of the finishing process, the first rising speed is reduced to the second rising speed. From the middle of the finishing process to the end of the finishing process, the rising speed of the quartz crucible is maintained at the second rising speed.
5. The single-crystal finishing process according to claim 4, characterized in that: The second acceleration is 0. From the beginning of the final stage to the middle of the final stage, the first acceleration is reduced to 0. From the middle of the final stage to the end of the final stage, the rising speed of the quartz crucible is 0.
6. A single-crystal finishing process according to claim 1, 2, 4, or 5, characterized in that: The single crystal rotation speed at the beginning of the finishing process is set as the first crystal speed, and the single crystal rotation speed in the middle of the finishing process is set as the second crystal speed. From the beginning of the finishing process to the first half of the middle of the finishing process, the single crystal rotation speed is the first crystal speed. In the second half of the middle of the finishing process, the first crystal speed is reduced to the second crystal speed. From the second half of the middle of the finishing process to the end of the finishing process, the single crystal rotation speed is the second crystal speed.
7. A single-crystal finishing process according to claim 1, 2, 4, or 5, characterized in that: From the start of the finishing process to its completion, the pressure in the single crystal furnace remains constant.
8. The single-crystal finishing process according to claim 6, characterized in that: From the start of the finishing process to its completion, the pressure in the single crystal furnace remains constant.
9. The single-crystal finishing process according to claim 7, characterized in that: From the start of the finishing process to its completion, the argon flow rate of the single crystal furnace remains constant.
10. A single-crystal finishing process according to claim 8, characterized in that: From the start of the finishing process to its completion, the argon flow rate of the single crystal furnace remains constant.
Citation Information
Patent Citations
Tailing method and preparation method of direct-pulling silicon monocrystals
CN106676621A
Method for adjusting power of heaters for single crystal furnace and single crystal furnace
CN109750350A
Ending process of large-size single crystal and preparation process of large-size single crystal
CN112301414A