Alloyed galvanized steel sheet, electrodeposited coated steel sheet, automobile part, method for manufacturing electrodeposited coated steel sheet, and method for manufacturing alloyed galvanized steel sheet

By forming an Fe-based electroplating layer on the surface of high-strength Si-containing cold-rolled steel sheet and then alloying it, the problem of grain boundary cracking during resistance welding was solved, the resistance welding cracking resistance characteristics of the welded part were improved, and in particular, the occurrence of internal cracking was suppressed.

CN116568869BActive Publication Date: 2026-11-24JFE STEEL CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202180074884.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-11-06
Filing Date
2021-11-05
Publication Date
2026-11-24
Estimated Expiration
2041-11-05

AI Technical Summary

Technical Problem

High-strength Si-containing steel plates are prone to grain boundary cracking (LME cracking) during resistance welding, especially when there is an angle between the electrode and the steel plate, which increases residual stress and leads to insufficient resistance welding cracking resistance of the welded part.

Method used

An Fe-based electroplating layer is formed on the surface of cold-rolled steel sheet, and a pre-plating layer is formed before annealing. Then, galvanizing and alloying treatments are carried out to integrate the crystal orientation of the Fe-based electroplating layer with that of the cold-rolled steel sheet, ensuring that the adhesion amount of the Fe-based electroplating layer is greater than 20.0 g/m², thus forming an alloyed galvanized steel sheet.

Benefits of technology

By integrating crystal orientation and alloying the Fe-based electroplating layer, the resistance to cracking of the welded part is significantly improved, the grain boundary intrusion and stress concentration of zinc are reduced, and the toughness and resistance to welding performance of the welded part are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116568869B_ABST
    Figure CN116568869B_ABST
Patent Text Reader

Abstract

This invention provides an alloyed galvanized steel sheet, which exhibits excellent resistance to resistance welding cracking characteristics at the weld joint when the crystal orientation of the Fe-based electroplating layer and the cold-rolled steel sheet is integrated at a high proportion at the interface between the Fe-based electroplating layer and the cold-rolled steel sheet. The alloyed galvanized steel sheet contains 0.1% to 3.0% by mass Si in a Si-containing cold-rolled steel sheet, and the amount of Si adhering to at least one side of the Si-containing cold-rolled steel sheet exceeds 20.0 g / m². 2 The Fe-based electroplated layer and the alloyed zinc plating layer formed on the Fe-based electroplated layer, and at the interface between the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet, the proportion of the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet being integrated in crystal orientation exceeds 50%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to alloyed galvanized steel sheets with excellent resistance to resistance welding cracking, electrodeposited coated steel sheets, automotive parts, methods for manufacturing electrodeposited coated steel sheets, and methods for manufacturing alloyed galvanized steel sheets. Background Technology

[0002] In recent years, from the perspective of protecting the Earth's environment, there has been a strong demand to improve automobile fuel efficiency. Furthermore, from the perspective of ensuring the safety of occupants in the event of a collision, there has also been a strong demand to improve automobile safety. To meet these demands, it is necessary to achieve both lightweight and high strength in automobile bodies. In the cold-rolled steel sheets used as raw materials for automobile components, the trend towards thinner walls based on high strength is actively developing. However, since most automobile components are manufactured by forming steel sheets, these steel sheets, in addition to high strength, also require excellent formability.

[0003] Various methods exist to improve the strength of steel sheets, but one method that achieves high strength without severely compromising the formability of the steel sheet is solid solution strengthening by adding silicon (Si). On the other hand, in the manufacture of automotive parts, pressure-formed components are mostly assembled by resistance welding (spot welding). When resistance-welded components contain high-strength galvanized steel sheets, residual stress is generated near the weld area during resistance welding. This causes the zinc coating to melt and diffuse into the grain boundaries, leading to liquid metal embrittlement (LME) and grain boundary cracking (LME cracking) in the steel sheet. When resistance welding is performed with the welding electrode at an angle to the steel sheet, residual stress increases, resulting in cracking. It is believed that residual stress increases with the increase in steel sheet strength, thus raising concerns about resistance welding cracking accompanying the increase in steel sheet strength. This LME cracking problem is particularly pronounced in steel sheets containing Si.

[0004] Based on the above, we are seeking high-strength steel plates with excellent resistance to resistance welding cracking characteristics in the welded parts.

[0005] Previously, improvement strategies for the aforementioned problems have been reported. For example, Patent Document 1 discloses a hot-dip galvanized steel sheet with an internal oxide layer covering at least a portion of the grain boundaries with oxides from the surface of the base material to a depth of 5.0 μm or more, and the grain boundary coverage of the oxides in the region from the surface of the base material to a depth of 5.0 μm is 60% or more. Furthermore, Patent Document 2 controls the hot rolling conditions to suppress grain boundary oxidation, and further performs Fe plating after cold rolling to suppress grain boundary oxidation during reduction annealing, reducing the grain boundary oxidation depth to 5.0 μm or less, thereby suppressing cracking of the weld under conditions of high current generating spatter.

[0006] Existing technical documents

[0007] Patent documents

[0008] Patent Document 1: Patent No. 6388099

[0009] Patent Document 2: Patent No. 4791992 Summary of the Invention

[0010] The inventors have recently discovered that forming an Fe-based electroplating layer on the surface of a steel sheet can improve its resistance to resistance welding cracking. Furthermore, they have found that when the steel sheet is annealed after forming the Fe-based electroplating layer, the crystal orientation of the Fe-based electroplating layer and the cold-rolled steel sheet is highly integrated at the interface due to the annealing conditions. The inventors have also found that in cold-rolled steel sheets with such a high degree of crystal orientation integration, molten zinc during resistance welding easily penetrates the grain boundaries of the cold-rolled steel sheet via the grain boundaries of the Fe-based electroplating layer. Moreover, the inventors have found that this phenomenon is even more pronounced when alloying is performed on hot-dip galvanizing, as the surface layer of the Fe-based electroplating is consumed by alloying. Patent Document 1, however, completely fails to address these phenomena.

[0011] Furthermore, as described later, LME cracking can be broadly categorized into "cracking occurring on the surface in contact with the electrode (hereinafter, surface cracking)" and "cracking occurring between steel plates near the corona bond (hereinafter, internal cracking)." The resistance welding cracking resistance characteristics described in this specification specifically refer to the characteristics that prevent internal cracking. Patent Document 2 provides no guidance on improving surface cracking, but rather on internal cracking that may occur within a suitable current range without spattering. Furthermore, Fe-based electroplating aims to function as a protective layer that inhibits grain boundary oxidation during reduction annealing, and does not explore any improvement effect on the resistance welding cracking resistance characteristics of Fe-based electroplating itself.

[0012] Therefore, the object of the present invention is to provide an alloyed galvanized steel sheet with excellent resistance to resistance welding cracking characteristics at the welded part, even when the crystal orientation of the Fe-based electroplated layer and the cold-rolled steel sheet is integrated at a high proportion at the interface of the Fe-based electroplated layer and the cold-rolled steel sheet.

[0013] To solve the aforementioned problems, the inventors conducted repeated and in-depth research, and discovered that in order to achieve high-level resistance to welding cracking in the welded parts, it is crucial to form a pre-plating layer as a pre-annealing Fe-based electroplating layer on the surface of the cold-rolled steel sheet before the annealing process following cold rolling. The resulting alloyed galvanized steel sheet exhibits an Fe-based electroplating layer with an adhesion amount greater than 20.0 g / m² per single side. 2 It was found that the amount of material adhering to each single side of the cold-rolled steel sheet was greater than 20.0 g / m². 2The invention is completed by forming a soft Fe-based electroplating layer, which alleviates the stress applied to the surface of the steel plate during welding. When the cold-rolled steel plate contains Si, the Fe-based electroplating layer acts as a Si depletion layer to suppress the reduction in toughness caused by Si solid solution. This improves the resistance to resistance welding cracking characteristics of the welded part.

[0014] This invention is based on the above-mentioned insights. That is, the essence of this invention is as follows.

[0015] [1] An alloyed galvanized steel sheet, comprising:

[0016] Si-containing cold-rolled steel sheet, containing 0.1% to 3.0% by mass of Si;

[0017] Fe-based electroplating layer, formed on at least one side of the aforementioned Si-containing cold-rolled steel sheet, wherein the amount of coating on each side is greater than 20.0 g / m². 2 ;

[0018] An alloyed zinc plating layer is formed on the aforementioned Fe-based electroplating layer;

[0019] The crystal orientation of the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet is integrated at the interface of the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet in a proportion greater than 50%.

[0020] [2] According to the alloyed galvanized steel sheet described in [1] above, wherein the above-mentioned Si-containing cold-rolled steel sheet contains 0.50% to 3.0% by mass of Si.

[0021] [3] According to the alloyed galvanized steel sheet described in [1] or [2] above, the adhesion amount of the Fe-based electroplating layer on each single side is 25.0 g / m. 2 above.

[0022] [4] The alloyed galvanized steel sheet according to any one of [1] to [3] above, wherein the above-mentioned Si-containing cold-rolled steel sheet, in addition to the above-mentioned Si, has the following composition: containing C: less than 0.8%, Mn: 1.0% to 12.0%, P: less than 0.1%, S: less than 0.03%, N: less than 0.010% and Al: less than 1.0% by mass, with the remainder consisting of Fe and unavoidable impurities.

[0023] [5] According to the alloyed galvanized steel sheet described in [4] above, wherein the above composition further contains one or more of the following: B: less than 0.005%, Ti: less than 0.2%, Cr: less than 1.0%, Cu: less than 1.0%, Ni: less than 1.0%, Mo: less than 1.0%, Nb: less than 0.20%, V: less than 0.5%, Sb: less than 0.200%, Ta: less than 0.1%, W: less than 0.5%, Zr: less than 0.1%, Sn: less than 0.20%, Ca: less than 0.005%, Mg: less than 0.005%, and REM: less than 0.005%.

[0024] [6] The alloyed galvanized steel sheet according to any one of [1] to [5] above, wherein the Fe-based electroplating layer has the following composition: containing one or more elements selected from B, C, P, N, O, Ni, Mn, Mo, Zn, W, Pb, Sn, Cr, V and Co in total of less than 10% by mass, and the remainder is composed of Fe and unavoidable impurities.

[0025] [7] An alloyed galvanized steel sheet, comprising: cold-rolled steel sheet;

[0026] Fe-based electroplating layer is formed on at least one side of the aforementioned cold-rolled steel sheet, with an adhesion amount greater than 20.0 g / m² on each side. 2 ;

[0027] An alloyed zinc plating layer is formed on the aforementioned Fe-based electroplating layer;

[0028] The crystal orientation of the Fe-based electroplated layer and the cold-rolled steel sheet is more than 50% integrated at the interface between the Fe-based electroplated layer and the cold-rolled steel sheet.

[0029] Here, in the aforementioned cold-rolled steel sheet, the adhesion amount of a 50×150mm test piece cut with the rolling right-angle direction as the long side, and the hot-dip galvanized layer cut to the same size on each single side, is 50g / m². 2 The test used alloyed hot-dip galvanized steel sheets to be stacked and made into a plate assembly.

[0030] Next, using a servo motor-driven, single-phase AC (50Hz) resistance welding machine, the aforementioned plate assembly was tilted 5° along its long side relative to the vertical plane of the line connecting the central axes of the electrode pairs (6mm front diameter) of the resistance welding machine. A gap of 60mm along the long side and 2.0mm along the thickness direction of the plate assembly was placed between the lower electrode of the electrode pair and the test piece. The lower electrode and the plate assembly were fixed, and with the upper electrode of the electrode pair movable, resistance welding was performed on the plate assembly under the conditions of a welding current and welding time of 3.5kN pressure, 0.16 seconds holding time, and a weld nugget diameter of 5.9mm, to produce a plate assembly with a welded section.

[0031] Next, the plate assembly with the welded part was cut in half along the long side of the test piece, including the welded part. When the cross-section of the welded part was observed with an optical microscope (200x magnification), cracks with a length of more than 0.1 mm were observed.

[0032] [8] According to the alloyed galvanized steel sheet described in [7] above, wherein the above-mentioned cold-rolled steel sheet is subjected to resistance welding under the condition of holding time of 0.24 seconds to obtain the above-mentioned plate assembly with welded part, when the cross section of the above-mentioned welded part is observed with the above-mentioned optical microscope (magnification of 200 times), a crack with a length of more than 0.1 mm is observed.

[0033] [9] An electrodeposited coated steel sheet, wherein the alloyed galvanized steel sheet described in any one of [1] to [8] above further has a chemical conversion treatment film and an electrodeposited coating film formed on the chemical conversion treatment film.

[0034]

[10] An automotive component, at least a portion of which is made of the electrodeposited coated steel sheet described above [9].

[0035]

[11] A method for manufacturing an electrodeposited coated steel sheet, comprising the following steps:

[0036] The chemical conversion treatment process involves performing chemical conversion treatment on the alloyed galvanized steel sheet described in any one of [1] to [8] above to obtain a chemically converted steel sheet with a chemical conversion treatment film formed on the alloyed galvanized layer.

[0037] In the electrodeposition coating process, the above-mentioned chemically converted steel sheet is subjected to electrodeposition coating treatment to obtain an electrodeposition coated steel sheet with an electrodeposition coating film formed on the above-mentioned chemically converted film.

[0038]

[12] A method for manufacturing an alloyed galvanized steel sheet, wherein an Fe-based electroplating is performed on a cold-rolled steel sheet containing 0.1% to 3.0% by mass of Si to produce an annealed Fe-based electroplated steel sheet having an annealed Fe-based electroplating layer formed on at least one side.

[0039] Next, the Fe-based electroplated steel sheet before annealing is annealed in an atmosphere with a dew point below -30°C to produce an Fe-based electroplated steel sheet.

[0040] Next, the above-mentioned Fe-based electroplated steel sheet is galvanized to produce galvanized steel sheet.

[0041] Next, the galvanized steel sheet is further alloyed to obtain a coating weight greater than 20.0 g / m² on each side. 2 Alloyed galvanized steel sheet with Fe-based electroplating layer.

[0042]

[13] According to the manufacturing method of the alloyed galvanized steel sheet described in

[12] above, wherein the cold-rolled steel sheet contains 0.5% to 3.0% by mass of Si.

[0043]

[14] According to the manufacturing method of alloyed galvanized steel sheet as described in

[12] or

[13] , wherein the adhesion amount CW of the Fe-based electroplated layer on each single side before annealing is... Fe0 (g / m 2 It satisfies the following equation (1).

[0044] (CW Fe0 >20.0+(CW) Zn )×[mass%Fe] / 100···(1)

[0045] Here, CW Zn Target value for the amount of alloyed zinc coating adhered to each single side (g / m²) 2 )

[0046] Among them, 25.0g / m 2 ≤CW Zn ≤80.0g / m 2

[0047] [mass%Fe]: The target value (mass%) of Fe content in the above alloyed zinc plating layer.

[0048]

[15] A method for manufacturing an alloyed galvanized steel sheet, wherein a cold-rolled steel sheet is subjected to Fe-based electroplating to produce an annealed Fe-based electroplated steel sheet having an annealed Fe-based electroplating layer formed on at least one side.

[0049] Next, the Fe-based electroplated steel sheet before annealing is annealed in an atmosphere with a dew point below -30°C to produce an Fe-based electroplated steel sheet.

[0050] Next, the above-mentioned Fe-based electroplated steel sheet is galvanized to produce galvanized steel sheet.

[0051] Next, the galvanized steel sheet is further alloyed to obtain a coating weight of more than 20.0 g / m² on each side. 2 Alloyed galvanized steel sheet with Fe-based electroplating layer.

[0052] Here, in the aforementioned cold-rolled steel sheet, the adhesion amount of a 50×150mm test piece cut with the rolling right-angle direction as the long side, and the hot-dip galvanized layer cut to the same size on each single side, is 50g / m². 2 The test used alloyed hot-dip galvanized steel sheets to be stacked and made into a plate assembly.

[0053] Next, using a servo motor-driven, pressurized single-phase AC (50Hz) resistance welding machine, the aforementioned plate assembly was tilted 5° along its long side relative to the vertical plane of the line connecting the central axes of the electrode pairs (6mm front diameter) of the resistance welding machine. A gap of 60mm along the long side and 2.0mm along the thickness direction of the plate assembly was placed between the lower electrode of the electrode pair and the test piece. The lower electrode and the plate assembly were fixed, and with the upper electrode of the electrode pair movable, resistance welding was performed on the plate assembly under the conditions of a welding current and welding time of 3.5kN pressure, 0.16 seconds holding time, and a weld nugget diameter of 5.9mm, to produce a plate assembly with a welded section.

[0054] Next, the plate assembly with the welded part was cut in half along the long side of the test piece, including the welded part. When the cross-section of the welded part was observed with an optical microscope (200x magnification), cracks with a length of more than 0.1 mm were observed.

[0055]

[16] In the manufacturing method of the alloyed galvanized steel sheet described above

[15] , when the cross section of the welded part is observed with an optical microscope (magnification 200x) under the condition that the cold-rolled steel sheet is held for 0.24 seconds, a crack with a length of more than 0.1 mm is observed.

[0056]

[17] In the manufacturing method of alloyed galvanized steel sheet described in

[15] or

[16] above, wherein the adhesion amount CW of the Fe-based electroplated layer on each single side before annealing is... Fe0 (g / m 2 It satisfies the following equation (1).

[0057] (CW Fe0 >20.0+(CW) Zn )×[mass%Fe] / 100···(1)

[0058] Here, CW Zn Target value for the amount of alloyed zinc coating adhered to each single side (g / m²) 2 ).

[0059] Among them, 25.0g / m 2 ≤CW Zn ≤80.0g / m 2

[0060] [mass%Fe]: The target value (mass%) of Fe content in the above alloyed zinc plating layer.

[0061]

[18] The method for manufacturing alloyed galvanized steel sheet according to any one of

[12] to

[17] above, wherein the above-mentioned Fe electroplating is performed using an Fe-based electroplating bath containing one or more elements selected from B, C, P, N, O, Ni, Mn, Mo, Zn, W, Pb, Sn, Cr, V and Co, such that the total content of these elements in the Fe-based electroplating layer before annealing is 10% by mass or less.

[0062] According to the present invention, an alloyed galvanized steel sheet can be provided that exhibits excellent resistance to welding cracking characteristics at the welded portion even when the crystal orientation of the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet is integrated in a high proportion at the interface between the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet. Attached Figure Description

[0063] Figure 1 It is a diagram showing a cross-section of an alloyed galvanized steel sheet.

[0064] Figure 2 These are (a) a perspective view and (b) an A-A cross-sectional view of an observation sample used to determine the proportion of crystal orientation integration.

[0065] Figure 3 The following figures illustrate the evaluation method for the proportion of crystal orientation integration: (a) is a figure depicting the boundary line at the interface between the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet in the SIM image; (b) is a figure depicting the boundary line and the decision region in the binarized image; and (c) is an enlarged view of the position enclosed by the quadrilateral in (b) above.

[0066] Figure 4 This is a diagram showing an observation image of the interface between the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet of Comparative Example No. 30.

[0067] Figure 5 This is a graph showing the boundary line and determination region depicted after binarization of the interface between the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet in Comparative Example No. 30.

[0068] Figure 6 This is a diagram showing an observation image of the interface between the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet of Invention Example No. 31.

[0069] Figure 7 This is a diagram showing the boundary line and determination region depicted after binarization of the interface between the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet in Invention Example No. 31.

[0070] Figure 8 (a) is a diagram illustrating the evaluation method for the resistance to welding cracking characteristics of the welded part, (b) is a top view of the welded plate assembly in this evaluation, and the bottom view is a B-B cross-sectional view of the top view. Detailed Implementation

[0071] The embodiments of the present invention will be described below.

[0072] Furthermore, in the following description, the units for the content of each element in the composition of Si-containing cold-rolled steel sheet and the content of each element in the coating composition are all "mass%" and are simply expressed as "%" unless otherwise specified. Additionally, in this specification, the numerical range indicated by "~" includes the values ​​listed before and after "~" as the lower and upper limits. Furthermore, in this specification, "high strength" steel sheet refers to a tensile strength TS of 590 MPa or higher as measured according to JIS Z 2241 (2011).

[0073] The aforementioned LME cracking can be broadly categorized into "cracking at the surface in contact with the electrode (hereinafter, surface cracking)" and "cracking near the ductile metal ring region between steel plates (hereinafter, internal cracking)." It is known that surface cracking is prone to occur during resistance welding in high-current regions that generate spatter, and this can be suppressed by adjusting the current to an appropriate range that prevents spatter. On the other hand, internal cracking can occur even when the current during resistance welding is within an appropriate range that prevents spatter. Furthermore, surface cracking is easily detected during visual inspection in the manufacturing process, while internal cracking is difficult to detect visually. For these reasons, internal cracking is a particularly significant issue in LME cracking. If resistance welding is performed with the welding electrode at an angle relative to the steel plate, residual stress increases, potentially leading to internal cracking. It is believed that residual stress increases with the strengthening of the steel plate, and therefore, internal cracking may occur along with the strengthening of the steel plate. This disclosure improves resistance welding cracking resistance characteristics, and particularly improves the characteristics that prevent internal cracking.

[0074] [Implementation Method 1]

[0075] Figure 1 The diagram shows a schematic cross-section of the alloyed galvanized steel sheet 1 according to this embodiment. Figure 1 As shown, the alloyed galvanized steel sheet 1 has at least one side of the Si-containing cold-rolled steel sheet 2 with an Fe-based electroplating layer 3 and an alloyed galvanized layer 4 formed on the Fe-based electroplating layer. First, the composition of the Si-containing cold-rolled steel sheet will be explained.

[0076] Si: 0.1%–3.0%

[0077] Si (Si) significantly enhances the strength of steel through solid solution treatment without noticeably impairing workability (solid solution strengthening ability), making it an effective element for achieving high strength in steel sheets. However, Si also negatively impacts the resistance to weld cracking characteristics of welded sections. To achieve high strength in steel sheets, Si needs to be added at least 0.1%. When Si content is less than 0.50%, the resistance to weld cracking characteristics of welded sections are not particularly problematic in welding with a holding time of approximately 0.24 seconds. However, from a production cost perspective, the production interval during spot welding in the assembly process of automotive parts becomes an issue. Even with Si content less than 0.50%, insufficient resistance to weld cracking characteristics may still occur when measures are taken to reduce holding time. On the other hand, if the Si content exceeds 3.0%, hot-rollability and cold-rollability are significantly reduced, adversely affecting productivity or leading to a decrease in the ductility of the steel sheet itself. Therefore, Si is added in the range of 0.1% to 3.0%. The Si content is preferably 0.50% or more, more preferably 0.7% or more, and even more preferably 0.9% or more, which has a greater impact on the resistance to welding cracking characteristics of the welded part. In addition, the Si content is preferably 2.5% or less, more preferably 2.0% or less, and even more preferably 1.7% or less.

[0078] In this embodiment, the presence of Si within the aforementioned range is essential for the Si-containing cold-rolled steel sheet. Other components are permissible as long as they fall within the typical composition range of cold-rolled steel sheets, and there are no particular limitations. However, to achieve a high strength (TS) of 590 MPa or higher for the Si-containing cold-rolled steel sheet of this embodiment, the following composition is preferred.

[0079] C: Below 0.8% (excluding 0%)

[0080] C improves workability by forming martensite and other structures within the steel. When C is present, the amount of C is preferably 0.8% or less, more preferably 0.3% or less, to obtain good weldability. There is no particular limitation on the lower limit of C, but to obtain good workability, the amount of C is preferably greater than 0%, more preferably 0.03% or more, and even more preferably 0.08% or more.

[0081] Mn: 1.0%~12.0%

[0082] Mn is an element that strengthens steel through solid solution treatment, increases its strength, improves hardenability, and promotes the formation of retained austenite, bainite, and martensite. This effect is achieved by adding 1.0% or more of Mn. Conversely, if the Mn content is 12.0% or less, the aforementioned effects can be obtained without increasing costs. Therefore, the Mn content is preferably 1.0% or more, more preferably 12.0% or less. The Mn content is more preferably 1.3% or more, further preferably 1.5% or more, and most preferably 1.8% or more. Furthermore, the Mn content is more preferably 3.5% or less, more preferably 3.3% or less.

[0083] P: Below 0.1% (excluding 0%)

[0084] By controlling the phosphorus (P) content, a decrease in weldability can be prevented. Furthermore, preventing P segregation at grain boundaries helps prevent deterioration in ductility, flexibility, and toughness. Additionally, adding large amounts of P accelerates ferrite transformation and increases crystal size. Therefore, the P content is preferably 0.1% or less. There is no particular lower limit for the P content; considering production technology constraints, it can be greater than 0% or more than 0.001%.

[0085] S: Less than 0.03% (excluding 0%)

[0086] The sulfur content is preferably 0.03% or less, more preferably 0.02% or less. By suppressing the sulfur content, it is possible to prevent a decrease in weldability and a decrease in hot ductility, suppress hot cracking, and significantly improve the surface shape. Furthermore, by suppressing the sulfur content, coarse sulfides are formed as impurity elements, which can prevent a decrease in the ductility, flexibility, and tensile flangeability of the steel sheet. These problems become significant when the sulfur content is greater than 0.03%, and the sulfur content is preferably minimized. There is no particular limitation on the lower limit of sulfur; considering production technology constraints, it can be greater than 0% or more than 0.0001%.

[0087] N: Less than 0.010% (excluding 0%)

[0088] The nitrogen (N) content is preferably 0.010% or less. With an N content of 0.010% or less, N forms coarse nitrides with Ti, Nb, and V at high temperatures, thereby preventing damage to the high-strength effect of the steel sheet caused by the addition of Ti, Nb, and V. Furthermore, an N content of 0.010% or less also prevents a decrease in toughness. Moreover, an N content of 0.010% or less prevents slab cracking and surface defects during hot rolling. The N content is preferably 0.005% or less, more preferably 0.003% or less, and even more preferably 0.002% or less. There is no particular limitation on the lower limit of the N content; considering production technology constraints, it can be greater than 0% or more.

[0089] A1: Below 1.0% (excluding 0%)

[0090] Al is thermodynamically the most readily oxidized, thus oxidizing before Si and Mn. It inhibits the oxidation of Si and Mn on the outermost surface of the steel sheet and promotes the oxidation of Si and Mn within the steel sheet. This effect is achieved when the Al content is 0.01% or higher. On the other hand, if the Al content exceeds 1.0%, the final cost increases. Therefore, when adding Al, the Al content is preferably 1.0% or less. More preferably, it is 0.1% or less. The lower limit for Al is not particularly limited; it can be greater than 0% or more, and can be 0.001% or higher.

[0091] The composition may further optionally contain one or more of the following: B: less than 0.005%, Ti: less than 0.2%, Cr: less than 1.0%, Cu: less than 1.0%, Ni: less than 1.0%, Mo: less than 1.0%, Nb: less than 0.20%, V: less than 0.5%, Sb: less than 0.200%, Ta: less than 0.1%, W: less than 0.5%, Zr: less than 0.1%, Sn: less than 0.20%, Ca: less than 0.005%, Mg: less than 0.005%, and REM: less than 0.005%.

[0092] B: Below 0.005%

[0093] Boron (B) is an effective element for improving the hardenability of steel. To improve hardenability, the amount of B is preferably 0.0003% or more, more preferably 0.0005% or more. However, if B is added excessively, the formability decreases, so the amount of B is preferably 0.005% or less.

[0094] Ti: below 0.2%

[0095] Ti is effective in precipitation strengthening of steel. There is no particular limit to the lower limit of Ti, but in order to achieve the effect of strength adjustment, it is preferable to be 0.005% or more. However, if too much Ti is added, the hard phase becomes too large and the formability deteriorates. Therefore, when adding Ti, the amount of Ti is preferably 0.2% or less, and more preferably 0.05% or less.

[0096] Cr: less than 1.0%

[0097] The Cr content is preferably 0.005% or more. By ensuring the Cr content is 0.005% or more, hardenability is improved, thereby enhancing the balance between strength and ductility. From the viewpoint of preventing cost increases, the Cr content is preferably 1.0% or less when added.

[0098] Cu: below 1.0%

[0099] The Cu content is preferably 0.005% or more. By making the Cu content 0.005% or more, the formation of the residual γ phase can be promoted. In addition, from the viewpoint of preventing cost increases, the Cu content is preferably 1.0% or less.

[0100] Ni: below 1.0%

[0101] The Ni content is preferably 0.005% or more. By making the Ni content 0.005% or more, the formation of the residual γ phase can be promoted. In addition, from the viewpoint of preventing cost increases, the Ni content is preferably 1.0% or less when adding Ni.

[0102] Mo: 1.0% or less

[0103] The preferred Mo content is 0.005% or more. By ensuring the Mo content is 0.005% or more, a strength adjustment effect can be achieved. Furthermore, from the viewpoint of preventing cost increases, the preferred Mo content is 1.0% or less.

[0104] Nb: below 0.20%

[0105] The strength is improved by containing 0.005% or more of Nb. Furthermore, from the viewpoint of preventing cost increases, the amount of Nb is preferably 0.20% or less.

[0106] V: Below 0.5%

[0107] The strength is improved by containing 0.005% or more of V. Furthermore, from the viewpoint of preventing increased costs, the amount of V is preferably 0.5% or less when it is present.

[0108] Sb: below 0.200%

[0109] Sb can be included to suppress nitriding, oxidation, or decarburization in the tens of micrometers of the steel plate surface caused by oxidation. By suppressing nitriding and oxidation on the steel plate surface, Sb prevents a reduction in the amount of martensite formed on the steel plate surface, thereby improving the fatigue properties and surface quality of the steel plate. To achieve this effect, the Sb content is preferably 0.001% or more. On the other hand, to obtain good toughness, the Sb content is preferably 0.200% or less.

[0110] Ta: below 0.1%

[0111] Ta contains 0.001% or more, which increases strength. Furthermore, from the viewpoint of preventing cost increases, the amount of Ta is preferably 0.1% or less.

[0112] W: below 0.5%

[0113] W increases strength by containing 0.005% or more. Furthermore, when W is present, from the viewpoint of preventing cost increases, the amount of W is preferably 0.5% or less.

[0114] Zr: below 0.1%

[0115] Zr content of 0.0005% or more results in increased strength. Furthermore, from the viewpoint of preventing increased costs, the Zr content is preferably 0.1% or less.

[0116] Sn: below 0.20%

[0117] Sn is an effective element for inhibiting the reduction of steel strength by suppressing denitrification and deboration. To achieve this effect, the content is preferably 0.002% or more. On the other hand, to obtain good impact resistance, the Sn content is preferably 0.20% or less.

[0118] Ca: below 0.005%

[0119] By controlling the morphology of sulfides with a content of 0.0005% or more, Ca can improve ductility and toughness. Furthermore, from the viewpoint of obtaining good ductility, the Ca content is preferably 0.005% or less.

[0120] Mg: less than 0.005%

[0121] By controlling the morphology of sulfides with Mg at a content of 0.0005% or more, ductility and toughness can be improved. Furthermore, from the viewpoint of preventing increased costs, the Mg content is preferably 0.005% or less when Mg is present.

[0122] REM: below 0.005%

[0123] REM, by controlling the morphology of sulfides with 0.0005% or more, can improve ductility and toughness. Furthermore, from the viewpoint of obtaining good toughness, the amount of REM is preferably 0.005% or less when it contains REM.

[0124] In this embodiment, the remaining components of the Si-containing cold-rolled steel sheet, other than those described above, are Fe and unavoidable impurities.

[0125] Next, we will describe the Fe-based electroplating layer formed on at least one side of the alloyed galvanized steel sheet before the formation of the galvanized layer by pre-plating the Fe-based electroplating layer before annealing and alloying treatment after galvanizing.

[0126] Fe-based electroplating layer: greater than 20.0 g / m 2

[0127] The amount of alloyed material adhered to each single side is greater than 20.0 g / m. 2 The mechanism by which the Fe-based electroplating layer improves the resistance to resistance welding cracking of the welded portion is not yet clear, but the inventors have considered the following. In this embodiment, as described later, annealing is performed after the Fe-based electroplating layer is formed. By annealing after the Fe-based electroplating layer is formed, it is possible to suppress the formation of "pick-up" marks, such as Si and Mn surface oxides formed during annealing, on the surface of the Fe-based coated steel sheet. Instead, the crystal orientation of the Fe-based electroplating layer and the Si-containing cold-rolled steel sheet is integrated at the interface of the Fe-based electroplating layer and the Si-containing cold-rolled steel sheet at a ratio greater than 50%. Therefore, molten zinc can easily penetrate the grain boundaries of the Si-containing cold-rolled steel sheet through the grain boundaries of the Fe-based electroplating layer. Furthermore, when the galvanized layer is alloyed, the surface layer of the Fe-based electroplating layer is consumed by alloying, making it difficult to improve the resistance to resistance welding cracking of the welded portion compared to galvanized steel sheets that are not alloyed. Therefore, in this embodiment, the adhesion amount after alloying treatment is greater than 20.0 g / m. 2 Fe-based electroplated layers. It is believed that by forming a layer with a density greater than 20.0 g / m²... 2 The Fe-based electroplating layer, with its sufficient amount of deposited Fe, can delay the time it takes for molten zinc to reach the grain boundaries of the Si-containing cold-rolled steel sheet during resistance welding, thus improving the resistance welding crack resistance characteristics of the weld (zinc grain boundary intrusion suppression effect). Furthermore, it is believed that the Fe-based electroplating layer functions as a soft layer, mitigating the stress applied to the steel sheet surface during welding and reducing residual stress in the resistance weld, thereby improving the resistance welding crack resistance characteristics of the weld (stress mitigation effect). Moreover, it is believed that when the amount of dissolved Si on the steel sheet surface is high, the weld toughness decreases, and the resistance welding crack resistance characteristics of the weld deteriorate. Conversely, it is believed that when there is a sufficient amount of Fe-based electroplating layer on the steel sheet surface, this Fe-based electroplating layer acts as a Si depletion layer, reducing the amount of dissolved Si in the weld, suppressing the reduction in weld toughness caused by Si solution, and improving the resistance welding crack resistance characteristics of the weld (toughness reduction suppression effect). The contribution of these Fe-based electroplating layers to the inhibition of grain boundary intrusion, stress mitigation, and toughness reduction in galvanized steel, thus improving resistance to welding cracking, is complex and has not yet been quantitatively determined. It is believed that they improve resistance to welding cracking through a combination of factors. To achieve the effect of improving the resistance to welding cracking of the welded area, the Fe-based electroplating layer in the alloyed galvanized steel sheet needs to have an adhesion amount greater than 20.0 g / m² on each single side. 2 There is no particular upper limit to the amount of Fe-based electroplated coating adhering to each single side, but from a cost perspective, an adhering amount of 60.0 g / m² per single side is preferred. 2 The preferred adhesion amount of the Fe-based electroplated layer is 25.0 g / m². 2 The above, more preferably 30.0 g / m2 The above is further preferred to be 35.0 g / m 2 The above describes the preferred alloyed galvanized steel sheet, which has an Fe-based electroplating layer on both sides of the Si-containing cold-rolled steel sheet. The Fe-based electroplating layer is designed to have an adhesion weight of 25.0 g / m². 2 The welded parts exhibit particularly good resistance to resistance welding cracking.

[0128] In addition, the thickness of the Fe-based electroplating layer was measured as follows. A 10×15mm sample was taken from an alloyed galvanized steel sheet and embedded in resin to create a cross-section of the embedded sample. A scanning electron microscope (SEM) was used at any three locations on this cross-section with an accelerating voltage of 15kV, and the thickness of the Fe-based electroplating layer was observed at magnifications of 2000–10000x. The amount of Fe-based electroplating layer deposited per single side was calculated by multiplying the average thickness of the three fields of view by the density of iron.

[0129] As Fe-based electroplating layers, in addition to pure Fe, alloy plating layers such as Fe-B alloys, Fe-C alloys, Fe-P alloys, Fe-N alloys, Fe-O alloys, Fe-Ni alloys, Fe-Mn alloys, Fe-Mo alloys, and Fe-W alloys can also be used. The composition of Fe-based electroplating layers is not particularly limited, but the following composition is preferred: containing one or more elements selected from B, C, P, N, O, Ni, Mn, Mo, Zn, W, Pb, Sn, Cr, V, and Co, totaling 10% or less, with the remainder consisting of Fe and unavoidable impurities. By ensuring that the amount of elements other than Fe is 10% or less in total, a decrease in electrolysis efficiency can be prevented, allowing for the formation of Fe-based electroplating layers at low cost. In the case of Fe-C alloys, the C content is preferably 0.08% or less by mass.

[0130] The proportion of the crystal orientation of the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet integrated at the interface is greater than 50%. This is because when the proportion of the crystal orientation of the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet integrated at the interface is greater than 50%, molten zinc can easily penetrate into the grain boundaries of the Si-containing cold-rolled steel sheet through the grain boundaries of the Fe-based electroplated layer. The effect obtained by setting the Fe-based electroplated layer in this embodiment becomes significant. In the alloyed galvanized steel sheet of this embodiment, the proportion of the crystal orientation of the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet integrated at the interface can be 70% or more, or 75% or more. Furthermore, there is no particular upper limit to the proportion of the crystal orientation of the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet integrated at the interface, and it can also be 100%.

[0131] As described above, the higher the proportion of crystal orientation integration between the Fe-based electroplating layer and the Si-containing cold-rolled steel sheet at the interface, the easier it is for molten zinc to penetrate the grain boundaries of the Si-containing cold-rolled steel sheet via the grain boundaries of the Fe-based electroplating layer. In particular, this trend becomes significant when the proportion of crystal orientation integration between the Fe-based electroplating layer and the Si-containing cold-rolled steel sheet at the interface is greater than 50%. In this embodiment, the Si-containing cold-rolled steel sheet is annealed after Fe-based electroplating, and annealed in a low dew point atmosphere as described later, resulting in a high proportion of crystal orientation integration between the Fe-based electroplating layer and the Si-containing cold-rolled steel sheet. Therefore, by forming a layer with a crystal orientation greater than 20.0 g / m², a high degree of integration is achieved. 2 The amount of Fe-based electroplating coating can be expected to delay the molten zinc from penetrating the grain boundaries of the Si-containing cold-rolled steel sheet through the grain boundaries of the Fe-based electroplating coating, thereby further improving the resistance to resistance welding cracking characteristics of the welded part.

[0132] Here, the proportion of crystal orientation integration between the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet at the interface was determined as follows. A 10×10mm sample was taken from the alloyed galvanized steel sheet. The sample was processed at an arbitrary location using a focused ion beam (FIB) device to form a 30μm wide section in the rolling right-angle direction (parallel to and perpendicular to the steel sheet surface) at a 45° angle to the T-section (a section perpendicular to the rolling right-angle direction of the steel sheet). This section, with a length of 50μm relative to the 45° direction of the T-section, served as the observation sample. Figure 2 The image shows a summary of the sample used for this observation. Figure 2 (a) is a three-dimensional view of the sample used for observation. Figure 2 (b) is Figure 2 (a) shows the A-A cross-sectional view of the sample for observation. Next, an 8-bit SIM image of 1024 pixels wide × 943 pixels high was captured by observing the central part of the 45° section of the sample for observation at 5000x magnification using a Scanning Ion Microscope (SIM). The proportion of the crystal orientation of the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet at the interface of the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet was calculated from the SIM images captured per 45° section based on the following equation (2). In addition, the decimal places were rounded to the nearest whole number.

[0133] (The proportion of the crystal orientation of the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet integrated at the interface of the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet) = (The length of the position where the crystal orientation of the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet is integrated at the interface of the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet) ÷ (The length of the interface of the observation field) × 100···(2)

[0134] Image processing was used to determine whether the crystal orientation of the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet was integrated at the interface. Figure 3 The evaluation method for the proportion of crystal orientation integration is explained. First, as... Figure 3 As shown in (a), a boundary line B was drawn at the interface between the Fe-based electroplated layer 3 and the Si-containing cold-rolled steel sheet 2 in the aforementioned SIM image using a scanning electron microscope. Next, an image of the SIM image was created, distinct from the image before the boundary line was drawn, and then image processing was performed. Specifically, firstly, the grain boundaries of the 8-bit SIM image (1024 pixels wide × 943 pixels high) were emphasized using a Sobel filter. Next, the image emphasizing the grain boundaries was smoothed using a Gaussian filter (radius (R): 10 pixels). Then, the smoothed image was binarized (threshold: 17). Next, the boundary line B of the image depicting the interface was transferred to the binarized image. Then, as... Figure 3 As shown in (b), the region of 40 pixels in width centered on boundary line B in the binarized image is defined along boundary line B in the binarized image. Figure 3 (b) The region enclosed by L1 and L2 is depicted. The length of the boundary line B is considered as the length of the position where the interface between the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet (the black and white boundary in the binarized image) does not exist within the judgment region. Here, the length of the boundary line B is calculated as follows: First, the two normals through the boundary line B are searched for positions that can divide the judgment region into approximately rectangular shapes, including only one color, black or white. Next, the maximum distance between the intersections of the boundary line and the two normals at this position is calculated over the entire judgment region, and this is considered as the length of the boundary line B that does not exist within the judgment region. Alternatively, the length of the position where the crystal orientation is integrated can be obtained by subtracting the length of the non-integrated crystal orientation position from the length of the interface in the field of view. For explanation, Figure 3 (c) shows the result of Figure 3 (b) Enlarged view of the area enclosed by the quadrilateral. First, as... Figure 3 As shown in (c), the search is performed across the entire decision region to find the two normal lines passing through boundary line B. Figure 3(c) In this case, l1 and l2, l3 and l4) can divide the judgment region into roughly rectangular positions using both white and black colors. Next, the maximum distance between the intersections of the boundary line and the two normals at each position is summed across the entire judgment region. This summates the length of the boundary line where the interface between the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet does not exist within the judgment region. By subtracting this length—the length of the non-integrated crystal orientation position—from the length of the interface in the observation field, the length of the integrated crystal orientation position can be determined.

[0135] Figure 4 The image shown is a SIM image of the interface between the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet of Comparative Example No. 30, which will be described later. The SIM image was processed as described above, and the binarized image is shown below. Figure 5 In Comparative Example No. 30, the crystal orientation of the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet was 97% integrated at the interface. Furthermore, Figure 6 The image shown is a SIM image of the interface between an Fe-based electroplated layer and a Si-containing cold-rolled steel sheet, according to Invention Example No. 31 of the embodiments described later. The SIM image was processed as described above, and the binarized image is shown below. Figure 7 In Invention Example No. 31, the crystal orientation of the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet is 100% integrated at the interface between the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet.

[0136] Next, the alloyed zinc plating layer formed on the aforementioned Fe-based electroplating layer will be described. Here, "alloyed zinc plating layer" refers to an alloyed zinc film formed on the surface of the steel plate. It is not limited to plating; any method of forming the zinc film, such as thermal spraying or cold spraying, is included in the term "alloyed zinc plating layer" as long as it is an alloyed zinc film formed on the surface of the steel plate. The alloyed zinc plating layer may contain one or more phases selected from the ζ phase, δ1 phase, Γ phase, and Γ1 phase.

[0137] Excellent corrosion resistance can be achieved by forming an alloyed zinc coating on the surface of steel sheet. However, during resistance welding, molten zinc penetrates the grain boundaries of the Si-containing cold-rolled steel sheet through the Fe-based electroplating layer, making it difficult to improve the resistance welding crack resistance of the welded joint. As mentioned above, by pre-coating the surface of the cold-rolled steel sheet before the annealing process after cold rolling with a pre-annealed Fe-based electroplating layer before forming the zinc coating, and then performing alloying treatment after zinc plating, with an adhesion amount greater than 20.0 g / m² per single side, the corrosion resistance of the welded joint is improved. 2The Fe-based electroplating layer formed on alloyed galvanized steel sheets can improve the resistance to resistance weld cracking characteristics of welded parts in alloyed galvanized steel sheets. The composition of the alloyed galvanized layer is not particularly limited, but it may contain, for example, Al, Zn, Fe, and unavoidable impurities. The Al content in the alloyed galvanized layer is not particularly specified; in one example, the Al content is 0.05% to 0.250% by mass. The Fe content in the alloyed galvanized layer is also not particularly limited, but in one example, the Fe content is 7.0% by mass or more and 15.0% by mass or less.

[0138] There is no particular limit to the amount of alloyed zinc plating applied per single side, but it can be up to 25 g / m². 2 The above, and can be 80g / m 2 The following is an example of achieving an alloyed zinc plating layer with an adhesion amount of 25 g / m² on each single side. 2 The above can further improve corrosion resistance and make it easier to control the coating adhesion. Additionally, if the adhesion of the alloyed zinc coating on each single side is 80 g / m²... 2 The following coating exhibits good adhesion.

[0139] According to this disclosure, it is possible to provide high-strength alloyed galvanized steel sheets with a tensile strength (TS) of 590 MPa or higher as measured according to JIS Z 2241 (2011). More preferably, the strength of the alloyed galvanized steel sheet is 800 MPa or higher.

[0140] The thickness of the alloyed galvanized steel sheet in this embodiment is not particularly limited, but it is generally 0.5 mm or more, and can be 3.2 mm or less.

[0141] <Manufacturing Method of Alloyed Galvanized Steel Sheet>

[0142] Next, the manufacturing method of alloyed galvanized steel sheet will be explained.

[0143] One embodiment of the method for manufacturing alloyed galvanized steel sheet may be the following method for manufacturing alloyed galvanized steel sheet:

[0144] Fe-based electroplating is performed on cold-rolled steel sheets containing 0.1% to 3.0% by mass of Si to produce Fe-based electroplated steel sheets before annealing, in which at least one side has an unannealed Fe-based electroplating layer.

[0145] Next, the Fe-based electroplated steel sheet before annealing is annealed in an atmosphere with a dew point below -30°C to produce an Fe-based electroplated steel sheet.

[0146] Next, the above-mentioned Fe-based electroplated steel sheet is galvanized to produce galvanized steel sheet.

[0147] Next, the galvanized steel sheet is further alloyed to obtain a coating weight greater than 20.0 g / m² on each side. 2 Alloyed galvanized steel sheet with Fe-based electroplating layer.

[0148] First, a cold-rolled steel sheet containing 0.1% to 3.0% by mass of Si is manufactured. Alternatively, the cold-rolled steel sheet may contain 0.50% to 3.0% by mass of Si. The manufacturing method of the cold-rolled steel sheet can follow the conventional method for manufacturing cold-rolled steel sheets. In one example, the cold-rolled steel sheet is manufactured by hot-rolling a steel slab having the above-mentioned composition into a hot-rolled sheet, then pickling the hot-rolled sheet, and finally cold-rolling the hot-rolled sheet into a cold-rolled steel sheet.

[0149] Next, the surface of the cold-rolled steel sheet is subjected to Fe-based electroplating treatment to produce a pre-annealed Fe-based electroplated steel sheet with a pre-annealed Fe-based electroplating layer formed on at least one side. The Fe-based electroplating treatment method is not particularly limited. For example, a sulfuric acid bath, a hydrochloric acid bath, or a mixture of both can be used as the Fe-based electroplating bath. Furthermore, pre-annealed Fe-based electroplated steel sheet refers to a steel sheet in which the Fe-based electroplating layer has not undergone an annealing process; this does not exclude the possibility of pre-annealing the cold-rolled steel sheet before the Fe-based electroplating treatment.

[0150] Before annealing, the adhesion amount of the Fe-based electroplated layer is defined as greater than 20.0 g / m² per single side of the alloyed galvanized steel sheet obtained after alloying treatment. 2 The amount of Fe-based electroplated layer adhered before annealing can be adjusted by factors such as the energizing time.

[0151] CW of Fe-based electroplated layer per single side before annealing Fe0 (g / m 2 It is preferable to satisfy the following formula (1).

[0152] (CW Fe0 >20.0+(CW) Zn )×[mass%Fe] / 100···(1)

[0153] Here, CW Zn Target value for the amount of alloyed zinc coating adhered to each single side (g / m²) 2 )

[0154] Among them, 25.0g / m 2 ≤CW Zn ≤80.0g / m 2

[0155] [mass%Fe]: The target value (mass%) of Fe content in the above alloyed zinc plating layer.

[0156] In other words, if the Fe content in the alloyed zinc coating forming the alloyed galvanized steel sheet is greater than the target value (g / m²), then... 2 )+20.0(g / m 2 If the amount of Fe-based electroplated layer before annealing is increased to a certain level, a final layer with a density greater than 20.0 g / m² can be obtained. 2 Fe-based electroplating layer.

[0157] Here, the target value CW for the amount of alloyed zinc coating adhered to per single side of the alloyed galvanized steel sheet is... Zn The target value for the Fe content in the alloyed zinc plating layer is determined based on the pre-determined specifications for each application. Furthermore, the amount of Fe-based electroplating layer deposited on each single side can be calculated through the aforementioned cross-sectional observation.

[0158] The Fe ion content in the Fe-based electroplating bath before energization is determined by Fe. 2+ The preferred concentration is 0.5 mol / L or higher. If the Fe ion content in the Fe-based electroplating bath is... 2+ A concentration of 0.5 mol / L or higher is required to achieve a sufficient amount of Fe adhesion. Furthermore, to ensure a sufficient amount of Fe adhesion, the Fe ion content in the Fe-based electroplating bath before energizing is preferably below 2.0 mol / L.

[0159] Furthermore, the Fe-based electroplating bath may contain Fe ions and at least one element selected from B, C, P, N, O, Ni, Mn, Mo, Zn, W, Pb, Sn, Cr, V, and Co. The total content of these elements in the Fe-based electroplating bath is preferably 10% by mass or less in the Fe-based electroplated layer before annealing. Additionally, metallic elements may be contained as metallic ions, and non-metallic elements may be contained as part of boric acid, phosphoric acid, nitric acid, organic acids, etc. Furthermore, the ferric sulfate plating solution may contain conductive additives, chelating agents, pH buffers, such as sodium sulfate and potassium sulfate.

[0160] Other conditions for the Fe-based electroplating bath are not particularly limited. Considering temperature stability, the temperature of the Fe-based electroplating bath is preferably 30°C or higher, and more preferably 85°C or lower. The pH of the Fe-based electroplating bath is not particularly specified, but from the viewpoint of preventing a decrease in current efficiency due to hydrogen generation, it is preferably 1.0 or higher. Furthermore, considering the conductivity of the Fe-based electroplating bath, it is preferably 3.0 or lower. From a productivity viewpoint, the current density is preferably 10 A / dm³. 2 From the perspective of easily controlling the adhesion amount of Fe-based electroplated layers, 150 A / dm is preferred. 2 The following applies to the plate speed. From a productivity point of view, a speed of 5 mpm or higher is preferred, and from the point of view of stable control of the amount of adhesion, a speed of 150 mpm or lower is preferred.

[0161] In addition, as a pretreatment before Fe-based electroplating, degreasing and rinsing of the cold-rolled steel sheet surface can be performed, as well as pickling and rinsing to activate the surface of the cold-rolled steel sheet. After these pretreatments, Fe-based electroplating is performed. The methods for degreasing and rinsing are not particularly limited, and conventional methods can be used. For pickling, various acids such as sulfuric acid, hydrochloric acid, nitric acid, and mixtures thereof can be used. Sulfuric acid, hydrochloric acid, or mixtures thereof are preferred. The concentration of the acid is not particularly specified, but considering the ability to remove the oxide film and prevent rough skin (surface defects) caused by over-pickling, a concentration of about 1 to 20 mass% is preferred. Furthermore, the pickling solution may contain defoamers, pickling accelerators, pickling inhibitors, etc.

[0162] Next, after Fe-based electroplating treatment, the Fe-based electroplated steel sheet before annealing is subjected to an annealing process. This process involves holding the sheet in a reducing atmosphere with a dew point below -30°C and a hydrogen concentration of 1.0% to 30.0% vol% at a temperature range of 650°C to 900°C for 30 to 600 seconds, followed by cooling. The annealing process is performed to improve the strength of the steel sheet by removing the strain caused by the rolling process and allowing the microstructure to recrystallize.

[0163] Dew point: below -30℃

[0164] In this embodiment, the dew point of the annealing atmosphere in the annealing process is a low dew point below -30°C, requiring no additional equipment such as humidification equipment. Controlling the dew point below -30°C is preferably performed within a temperature range of 650°C to 900°C. Through independent research, the inventors have discovered a correlation between the proportion of the crystal orientation of the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet integrated at the interface and the dew point of the annealing atmosphere in the annealing process after the formation of the Fe-based electroplated layer. That is, it is known that when annealing the Fe-based electroplated steel sheet before annealing after the formation of the Fe-based electroplated layer, the lower the dew point of the annealing atmosphere, the higher the proportion of the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet integrated in the annealed Fe-based electroplated steel sheet; conversely, the higher the dew point of the annealing atmosphere, the lower the proportion of the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet integrated in the crystal orientation. The reason why there is a correlation between the proportion of crystal orientation integration between the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet and the dew point is not yet clear, but it is speculated as follows: When the dew point is controlled at a certain high level, elements that diffuse from the steel sheet to the Fe-based electroplated layer during annealing form oxides inside the Fe-based electroplated layer. These oxides hinder the growth of the Fe-based electroplated layer's crystal grains, resulting in finer grains. On the other hand, when annealing is performed in a low dew point atmosphere after the formation of the Fe-based electroplated layer, it is difficult to form such oxides, and the crystal grain size of the Fe-based electroplated layer becomes coarser. Therefore, it can be considered that when annealing is performed at a low dew point, the crystal orientation of the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet are integrated to a high proportion. Due to the cost of the humidification equipment in the annealing furnace, when the dew point of the annealing atmosphere in the annealing process is below -30°C, the proportion of crystal orientation integration between the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet at the interface is high. As a result, when alloyed galvanized steel sheets are used, molten zinc during resistance welding easily penetrates the grain boundaries of the Si-containing cold-rolled steel sheet through the grain boundaries of the Fe-based electroplating layer. In this embodiment, by forming an Fe-based electroplating layer with a specific adhesion amount, the time it takes for molten zinc to reach the grain boundaries of the Si-containing cold-rolled steel sheet through the grain boundaries of the Fe-based electroplating layer during resistance welding is delayed, thereby improving the resistance welding crack resistance characteristics of the welded portion. The lower limit of the dew point of the annealing atmosphere is not particularly limited, but it is difficult to achieve below -80°C in industry; therefore, -80°C or higher is preferred. The dew point of the annealing atmosphere is more preferably -55°C or higher.

[0165] Hydrogen concentration: 1.0 vol% to 30.0 vol%

[0166] The annealing process is carried out in a reducing atmosphere with a hydrogen concentration of 1.0 vol% to 30.0 vol%. Hydrogen inhibits the oxidation of Fe on the surface of the Fe-based electroplated steel sheet before annealing, thus activating the steel sheet surface. If the hydrogen concentration is 1.0 vol% or higher, Fe oxidation on the steel sheet surface can be avoided, which would lead to deterioration of the plating adhesion when the zinc plating layer is applied, as described later. Therefore, the annealing process is preferably carried out in a reducing atmosphere with a hydrogen concentration of 1.0 vol% or higher, more preferably in a reducing atmosphere with a hydrogen concentration of 2.0 vol% or higher. There is no particular upper limit to the hydrogen concentration in the annealing process, but from a cost point of view, the hydrogen concentration is preferably 30.0 vol% or less, more preferably 20.0 vol% or less. The remainder of the annealing atmosphere other than hydrogen is preferably nitrogen.

[0167] Holding time in the temperature range of 650℃ to 900℃: 30 seconds to 600 seconds

[0168] In the annealing process, the holding time in the temperature range of 650°C to 900°C is preferably 30 to 600 seconds. By holding this temperature range for more than 30 seconds, the natural oxide film of Fe formed on the surface of the Fe-based electroplated layer before annealing is appropriately removed, which improves the coating adhesion when a zinc plating layer is applied to the surface of the Fe-based electroplated steel sheet, as described later. Therefore, the holding time in this temperature range is preferably 30 seconds or more. There is no particular upper limit to the holding time in this temperature range, but from a productivity point of view, the holding time in this temperature range is preferably 600 seconds or less.

[0169] Maximum temperature reached for Fe-based electroplated steel sheets before annealing: 650℃~900℃

[0170] The maximum temperature reached before annealing of Fe-based electroplated steel sheet is not particularly limited, but is preferably 650°C to 900°C. By setting the maximum temperature of the Fe-based electroplated steel sheet before annealing to 650°C or higher, the recrystallization of the steel sheet structure proceeds smoothly, and the desired strength can be obtained. In addition, the natural oxide film of Fe formed on the surface of the Fe-based electroplated layer before annealing can be appropriately reduced, which can improve the coating adhesion when zinc plating is applied to the surface of the Fe-based electroplated steel sheet as described later. Furthermore, if the maximum temperature reached before annealing of the Fe-based electroplated steel sheet is 900°C or lower, the diffusion rate of Si and Mn in the steel can be prevented from increasing excessively, and the diffusion of Si and Mn to the surface of the steel sheet can be prevented, thus improving the coating adhesion when zinc plating is applied to the surface of the Fe-based electroplated steel sheet as described later. In addition, if the maximum temperature reached before annealing is 900°C or lower, damage to the heat treatment furnace can be prevented, and costs can be reduced. Therefore, the maximum temperature reached before annealing of cold-rolled steel sheet is preferably 900°C or lower. In addition, the above-mentioned maximum temperature reached before annealing is based on the temperature measured on the surface of the cold-rolled steel sheet.

[0171] Next, the galvanizing process will be explained.

[0172] Following the annealing process described above, the Fe-based electroplated steel sheet is galvanized. The galvanizing method is not particularly limited, but can include, for example, hot-dip galvanizing, electroplating, cold spraying, and plasma spraying. In one example of hot-dip galvanizing, the Fe-based electroplated steel sheet can be cooled after the annealing process and then immersed in a hot-dip galvanizing bath to galvanize the surface of the steel sheet. The hot-dip galvanizing bath consists of Al, Zn, and unavoidable impurities. The composition of the hot-dip galvanizing bath is not specifically defined; generally, the Al concentration in the bath is 0.05% to 0.250% by mass. If the Al concentration in the bath is 0.05% by mass or higher, the formation of bottom dross can be prevented, and dross can be prevented from adhering to the steel sheet and becoming a defect. Furthermore, by keeping the Al concentration in the bath below 0.250% by mass, the increase of top dross is prevented, dross can be prevented from adhering to the steel sheet and causing defects, and costs are reduced. There are no restrictions on other conditions for hot-dip galvanizing, but for example, the bath temperature of the hot-dip galvanizing bath is usually in the range of 440 to 500°C, and the plate temperature is 440 to 550°C to immerse the steel plate in the hot-dip galvanizing bath.

[0173] The preferred adhesion amount of the galvanized layer on each single side is 25–80 g / m². 2 The amount. By making the amount of alloyed zinc plating on each single side 25g / m 2 The above can further improve corrosion resistance and make it easy to control the coating adhesion. Additionally, if the adhesion of the alloyed zinc coating on each single side is 80 g / m²... 2 The following coating exhibits good adhesion.

[0174] After galvanizing, the coating adhesion can be adjusted appropriately. There are no particular limitations on the method for adjusting the coating adhesion, but in hot-dip galvanizing, for example, it is generally adjusted by gas purging. In one example, the coating adhesion is adjusted by factors such as the gas pressure during purging and the distance between the purging nozzle and the steel plate.

[0175] After galvanizing, alloying treatment is further performed to obtain alloyed galvanized steel sheet. The galvanized layer is alloyed by heating. The alloying treatment is preferably performed at a temperature of 450°C to 600°C. By alloying at 450°C or higher, a steel sheet with excellent low-pressure formability and no residual η phase can be provided. Furthermore, by alloying at 600°C or lower, good coating adhesion is achieved. The alloying time is preferably 5s to 60s.

[0176] Next, the calculation method for the amount of alloyed zinc plating on each single side will be explained.

[0177] First, two 20×25mm samples were taken from the alloyed galvanized steel sheet. After measuring their respective weights, the alloyed galvanized coating on one side with the Fe-based electroplating layer was peeled off using the test solution specified in JIS H 0401 (2013) or ISO 17925 (2004), and the weight was measured again. The amount of alloyed galvanized coating adhering to each side can be calculated by subtracting the weight after peeling from the weight before peeling and then dividing by the surface area of ​​the peeled portion. Here, the average value of the two measurements is taken as the amount of alloyed galvanized coating adhering to each side.

[0178] Furthermore, the determination of the Fe content (mass%) in the alloyed zinc plating layer was performed according to ISO 17925 (2004). The test solution after peeling off the aforementioned plating layer was analyzed using an inductively coupled plasma (ICP) luminescence analyzer. The Fe content in the test solution was calculated by dividing the Fe content in the test solution by the total content of Fe, Zn, Al, and other components constituting the alloyed zinc plating layer, and then multiplying by 100. Here, the average value from two locations was taken as the Fe content in the alloyed zinc plating layer.

[0179] <Electrodeposited Coated Steel Sheets>

[0180] Furthermore, according to this embodiment, an electrodeposited coated steel sheet can also be provided, which further comprises a chemical conversion coating formed on the aforementioned alloyed galvanized layer and an electrodeposited coating formed on the chemical conversion coating. The alloyed galvanized steel sheet of this embodiment exhibits excellent resistance to resistance welding cracking at the welded portion, and the electrodeposited coated steel sheet formed using this alloyed galvanized steel sheet is particularly suitable for automotive parts. The types of chemical conversion coating and electrodeposited coating are not particularly limited, and can be any known chemical conversion coating or electrodeposited coating. As a chemical conversion coating, zinc phosphate coating, zirconium coating, etc., can be used. As for the electrodeposited coating, there are no particular limitations as long as it is an electrodeposited coating for automotive applications. The thickness of the electrodeposited coating varies depending on the application, and the coating in the dry state is preferably about 10 μm to 30 μm. Furthermore, according to this embodiment, an alloyed galvanized steel sheet for electrodeposited coating can be provided.

[0181] <Manufacturing Method of Electrodeposited Coated Steel Sheets>

[0182] Next, the manufacturing method of the above-mentioned electrodeposited coated steel sheet will be described. The above-mentioned electrodeposited coated steel sheet can be manufactured by the following method, which includes the following steps: a chemical conversion treatment step, in which an alloyed galvanized steel sheet is subjected to chemical conversion treatment to obtain a chemically converted steel sheet with a chemically converted coating film formed on the alloyed galvanized layer; and an electrodeposition coating step, in which the chemically converted steel sheet is subjected to electrodeposition coating treatment to obtain an electrodeposited coated steel sheet with an electrodeposited coating film formed on the chemically converted coating film. The chemical conversion treatment and electrodeposition coating treatment can be performed using known methods. Furthermore, as a pretreatment before performing the chemical conversion treatment, degreasing treatment, water washing, and surface conditioning treatment as needed can be performed on the surface of the alloyed galvanized steel sheet. The chemical conversion treatment is performed after these pretreatments. The methods for degreasing treatment and water washing are not particularly limited, and conventional methods can be used. In the surface conditioning treatment, surface conditioning agents containing Ti colloid or zinc phosphate colloid can be used. Applying these surface modifiers requires no special procedures and can be done using conventional methods. For example, the desired surface modifier is dissolved in a specified amount of deionized water, stirred thoroughly, and a treatment solution is prepared at a predetermined temperature (usually room temperature, 25–30°C). The steel sheet is then immersed in this treatment solution for a specified time (20–30 seconds). Then, without drying, the next step, chemical conversion treatment, is performed. Chemical conversion treatment can also be performed using conventional methods. For example, the desired chemical conversion agent is dissolved in a specified amount of deionized water, stirred thoroughly, and a treatment solution is prepared at a specified temperature (usually 35–45°C). The steel sheet is then immersed in this treatment solution for a specified time (60–120 seconds). Examples of chemical conversion agents include zinc phosphate for steel, zinc phosphate for steel and aluminum blends, and zirconium agents. Next, the next step, electrodeposition coating, is performed. Electrodeposition coating can also be performed using conventional methods. After pretreatment such as water washing as required, the steel plate is immersed in a thoroughly stirred electroplating coating, and an electrodeposition process is performed to obtain an electrodeposited coating of the desired thickness. In addition to cationic electrodeposited coatings, anionic electrodeposited coatings can also be used. Furthermore, a topcoat can be applied after the electrodeposited coating, depending on the application.

[0183] <Automotive Parts>

[0184] Furthermore, according to this embodiment, it is possible to provide automotive parts that are at least partially made using the aforementioned electrodeposited coated steel sheet. Because the alloyed galvanized steel sheet of this embodiment has excellent resistance to resistance weld cracking at the welded portion, the electrodeposited coated steel sheet using this alloyed galvanized steel sheet is particularly suitable for use in automotive parts. Automotive parts made using the electrodeposited coated steel sheet may include steel sheets other than the electrodeposited coated steel sheet of this embodiment as blanks. Because the electrodeposited coated steel sheet of this embodiment has excellent resistance to resistance weld cracking at the welded portion, it is possible to appropriately prevent LME cracking at the welded portion of automotive parts made using this alloyed galvanized steel sheet. The types of automotive parts that are at least partially made using the electrodeposited coated steel sheet are not particularly limited, but may include, for example, side beam components, pillar components, and automotive bodies.

[0185] [Implementation Method 2]

[0186] Next, the alloyed galvanized steel sheet of Embodiment 2 of the present invention will be described.

[0187] The alloyed galvanized steel sheet of this embodiment may have the following characteristics:

[0188] Cold-rolled steel sheet

[0189] The amount of material adhering to at least one side of the aforementioned cold-rolled steel sheet is greater than 20.0 g / m². 2 Fe-based electroplating layer

[0190] The alloyed zinc plating layer formed on the above-mentioned Fe-based electroplating layer,

[0191] The crystal orientation of the Fe-based electroplated layer and the cold-rolled steel sheet is more than 50% integrated at the interface between the Fe-based electroplated layer and the cold-rolled steel sheet.

[0192] Here, the aforementioned cold-rolled steel sheet is a test piece cut into 50×150mm sections with the rolling right-angle direction as the long side, and a hot-dip galvanized layer of the same size is cut into each single side with an adhesion amount of 50g / m. 2 The test used alloyed hot-dip galvanized steel sheets to be stacked and made into a plate assembly.

[0193] Next, using a servo motor-driven, pressurized single-phase AC (50Hz) resistance welding machine, the aforementioned plate assembly was tilted 5° along its long side relative to the vertical plane of the line connecting the central axes of the electrode pairs (6mm front diameter) of the resistance welding machine. A gap of 60mm along the long side and 2.0mm along the thickness direction of the plate assembly was placed between the lower electrode of the electrode pair and the test piece. The lower electrode and the plate assembly were fixed, and with the upper electrode of the electrode pair movable, resistance welding was performed on the plate assembly under the conditions of a welding current and welding time of 3.5kN pressure, 0.16 seconds holding time, and a weld nugget diameter of 5.9mm, to produce a plate assembly with a welded section.

[0194] Next, the plate assembly with the welded part was cut in half along the long side of the test piece, including the welded part. When the cross-section of the welded part was observed with an optical microscope (200x magnification), cracks with a length of more than 0.1 mm were observed.

[0195] The cold-rolled steel sheet of this embodiment is not particularly limited in that, when evaluated through the following tests, is a steel sheet whose weld joint has poor resistance to weld cracking characteristics when the sheet assembly is galvanized steel sheet. The composition of the cold-rolled steel sheet is also not particularly limited. The inventors found that cold-rolled steel sheets with a Si content of 0.1% by mass or more in the steel exhibit poor resistance to weld cracking characteristics in the weld joint, as evaluated through the following tests.

[0196] Cold-rolled steel sheets can be those obtained by resistance welding with a holding time of 0.24 seconds, resulting in a sheet assembly with a welded section. When the cross-section of the welded section is observed under an optical microscope (200x magnification), cracks longer than 0.1 mm are observed. Furthermore, for the same type of cold-rolled steel sheet, the resistance to resistance welding cracking of the welded section generally deteriorates as the holding time decreases. Therefore, if a cold-rolled steel sheet exhibits cracks longer than 0.1 mm when the welded section is observed under an optical microscope (200x magnification) after resistance welding with a holding time of 0.24 seconds, then even when resistance welding is performed with a holding time of 0.16 seconds, cracks longer than 0.1 mm are still observed under an optical microscope (200x magnification) on the cross-section of the welded section. It was also confirmed that if the cold-rolled steel sheet has a Si content of 0.50% by mass or more, the welded parts evaluated by the above tests have poor resistance to weld cracking characteristics. However, even cold-rolled steel sheets with a Si content of less than 0.50% by mass are examples of welded parts with poor resistance to weld cracking characteristics evaluated by the following tests.

[0197] <Characteristics of resistance welding cracking resistance of welded parts>

[0198] use Figure 8The evaluation method for the resistance to cracking of welded parts is explained. Test pieces 6, each 50×150mm, were cut with the rolling right-angle direction (TD) as the long side and the rolling direction as the short side. The adhesion amount of the hot-dip galvanized layer on each single side of the same size was 50g / m². 2 The test alloyed hot-dip galvanized steel sheets 5 were overlapped to form a plate assembly. The plate assembly was assembled with the evaluation surface (Fe-based electroplated layer side) of the test piece 6 facing each other against the galvanized layer of the test alloyed hot-dip galvanized steel sheet 5. The plate assembly was fixed to the mounting table 8 with 2.0 mm thick spacers 7 in between. Spacers 7 consisted of a pair of steel plates, each 50 mm long x 45 mm short x 2.0 mm thick. Figure 8 As shown in (a), the long side end faces of each pair of steel plates are aligned with the short side end faces of the plate assembly. Therefore, the distance between the pair of steel plates is 60 mm. The fixing platform 8 is a plate with a hole in the center.

[0199] Next, using a servo motor-driven single-phase AC (50Hz) resistance welding machine, while bending the plate assembly under pressure with a pair of electrodes 9 (front diameter: 6mm), resistance welding was performed with a welding current and welding time of 5.9mm weld nugget diameter r, under conditions of 3.5kN pressure and holding time of 0.18 seconds or 0.24 seconds, to produce a plate assembly with a welded section. At this time, the pair of electrodes 9 applied pressure to the plate assembly from vertically upwards and downwards, with the lower electrode applying pressure to the test piece 6 through a hole in the fixing table 8. During pressure application, the lower electrode of the pair of electrodes 9 was fixed to the fixing table 8 in such a way that it contacted a plane extending from the surface where the pad 7 contacts the fixing table 8, while the upper electrode was movable. Furthermore, the upper electrode contacted the center portion of the test alloyed hot-dip galvanized steel plate 5. Additionally, the plate assembly was positioned perpendicular to the line connecting the central axes of the electrode pairs of the resistance welding machine (…). Figure 8 (a) The plates are welded while tilted 5° along the long side of the plate assembly (in the horizontal direction). A gap of 60mm along the long side of the plate assembly and 2.0mm along the thickness direction is formed between the lower electrode and the test piece 6 using the aforementioned spacer. Furthermore, the holding time refers to the time from the end of the welding current flow to the start of electrode release. Here, refer to... Figure 8 (b) In the figure below, the diameter r of the melt core refers to the distance between the ends of the melt cores 10 in the long side direction of the plate assembly.

[0200] Next, the aforementioned plate assembly with welded portions is arranged along the center of the welded portion, including the weld nugget 10. Figure 8(b) Cut along line B-B in the above figure and observe the cross-section of the weld using an optical microscope (200x). Evaluate the resistance to welding cracking characteristics of the weld according to the following criteria. Furthermore, if the result is ◎ or ○, the weld is judged to have excellent resistance to welding cracking characteristics. If the result is ×, the weld is judged to have poor resistance to welding cracking characteristics.

[0201] ◎: No cracks longer than 0.1 mm were observed during a holding time of 0.14 seconds.

[0202] ○: Cracks longer than 0.1 mm were observed after a holding time of 0.14 seconds, but no cracks longer than 0.1 mm were observed after a holding time of 0.16 seconds.

[0203] ×: Cracks longer than 0.1 mm were observed after a holding time of 0.16 seconds.

[0204] Furthermore, as a relatively mild welding condition, the resistance to welding cracking characteristics of the welded part can be evaluated using the same criteria as below.

[0205] ◎: No cracks longer than 0.1 mm were observed during a holding time of 0.18 seconds.

[0206] ○: Cracks longer than 0.1 mm were observed after a holding time of 0.18 seconds, but no cracks longer than 0.1 mm were observed after a holding time of 0.24 seconds.

[0207] ×: Cracks longer than 0.1 mm were observed after a holding time of 0.24 seconds.

[0208] Additionally, in Figure 12(b), the symbol 11 is used to represent an example of a crack produced in test piece 6.

[0209] The Fe-based electroplated layer and the alloyed zinc layer of the alloyed galvanized steel sheet in this embodiment are the same as those in Embodiment 1 above, so descriptions are omitted here. Furthermore, the proportion of the crystal orientation of the Fe-based electroplated layer and the cold-rolled steel sheet integrated at the interface is the same as in Embodiment 1 above, exceeding 50%. The detailed proportion of the crystal orientation of the Fe-based electroplated layer and the cold-rolled steel sheet integrated at the interface is the same as in Embodiment 1 above, so descriptions are omitted here.

[0210] Next, the manufacturing method of the alloyed galvanized steel sheet of Embodiment 2 will be described.

[0211] One embodiment of the method for manufacturing alloyed galvanized steel sheet may be the following method for manufacturing alloyed galvanized steel sheet.

[0212] Fe-based electroplating is performed on cold-rolled steel sheets to produce Fe-based electroplated steel sheets before annealing, in which at least one side has a pre-annealed Fe-based electroplating layer.

[0213] Next, the Fe-based electroplated steel sheet before annealing is annealed in an atmosphere with a dew point below -30°C to produce an Fe-based electroplated steel sheet.

[0214] Next, the above-mentioned Fe-based electroplated steel sheet is galvanized to produce galvanized steel sheet.

[0215] Next, the galvanized steel sheet is further alloyed to obtain a coating weight of more than 20.0 g / m² on each side. 2 Alloyed galvanized steel sheet with Fe-based electroplating layer.

[0216] Here, the aforementioned cold-rolled steel sheet is a test piece cut into 50×150mm sections with the rolling right-angle direction as the long side, and a hot-dip galvanized layer of the same size is cut into each single side with an adhesion amount of 50g / m. 2 The test used alloyed hot-dip galvanized steel sheets to be stacked and made into a plate assembly.

[0217] Next, using a servo motor-driven, pressurized single-phase AC (50Hz) resistance welding machine, the aforementioned plate assembly was tilted 5° along its long side relative to the vertical plane of the line connecting the central axes of the electrode pairs (6mm front diameter) of the resistance welding machine. A gap of 60mm along the long side and 2.0mm along the thickness direction of the plate assembly was placed between the lower electrode of the electrode pair and the test piece. The lower electrode and the plate assembly were fixed, and with the upper electrode of the electrode pair movable, resistance welding was performed on the plate assembly under the conditions of a welding current and welding time of 3.5kN pressure, 0.16 seconds holding time, and a weld nugget diameter of 5.9mm, to produce a plate assembly with a welded section.

[0218] Next, the plate assembly with the welded part was cut in half along the long side of the test piece, including the welded part. When the cross-section of the welded part was observed with an optical microscope (200x magnification), cracks with a length of more than 0.1 mm were observed.

[0219] First, cold-rolled steel sheets are manufactured. The manufacturing method for cold-rolled steel sheets can follow the usual methods. In one example, a steel slab is hot-rolled to produce a hot-rolled sheet, which is then pickled, and finally cold-rolled to produce a cold-rolled steel sheet.

[0220] In this embodiment, the cold-rolled steel sheet is not particularly limited to any sheet that exhibits poor resistance to weld cracking characteristics at the welded portion when the sheet assembly is galvanized steel sheet, provided that the test evaluation described above is passed. The composition of the cold-rolled steel sheet is also not particularly limited, but it is recognized that cold-rolled steel sheets with a Si content of 0.1% by mass or more exhibit poor resistance to weld cracking characteristics at the welded portion, as evaluated by the following tests.

[0221] The cold-rolled steel sheet can be subjected to the aforementioned resistance welding under a holding time of 0.24 seconds, resulting in a sheet assembly with a welded portion. When the cross-section of the welded portion is observed using an optical microscope (200x magnification), cracks with a length of 0.1 mm or more are observed. Furthermore, for the same cold-rolled steel sheet, the resistance welding cracking resistance of the welded portion generally deteriorates as the holding time decreases. Therefore, if a cold-rolled steel sheet is subjected to resistance welding under a holding time of 0.24 seconds, and cracks with a length of 0.1 mm or more are observed when the cross-section of the welded portion is observed using an optical microscope (200x magnification), then when resistance welding is performed under a holding time of 0.16 seconds, cracks with a length of 0.1 mm or more are also observed when the cross-section of the welded portion is observed using an optical microscope (200x magnification). It was also confirmed that cold-rolled steel sheets with a Si content of 0.50% by mass or more in the steel exhibit poor resistance to weld cracking characteristics in the welded parts as evaluated by the above-mentioned tests. However, even cold-rolled steel sheets with a Si content of less than 0.50% by mass in the steel are examples of cold-rolled steel sheets with poor resistance to weld cracking characteristics in the welded parts as evaluated by the above-mentioned tests.

[0222] Next, the surface of the cold-rolled steel sheet is subjected to Fe-based electroplating treatment to obtain Fe-based electroplated steel sheet before annealing. The details of the Fe-based electroplating treatment have already been explained above, and will not be elaborated here.

[0223] Next, the Fe-based electroplated steel sheet before annealing is subjected to an annealing process in a reducing atmosphere with a dew point below -30°C and a hydrogen concentration of 1.0% to 30.0% by volume, held at a temperature range of 650°C to 900°C for 30 to 600 seconds, and then cooled to obtain the Fe-based electroplated steel sheet. The details of the annealing process are as described above and are omitted here.

[0224] Similar to Embodiment 1 described above, galvanizing is performed on the Fe-based electroplated steel sheet in this embodiment to obtain a galvanized steel sheet. The details of the galvanizing process are the same as in Embodiment 1 described above, so they are omitted here.

[0225] Similar to Embodiment 1 described above, this embodiment also provides an electrodeposited coated steel sheet further comprising a chemical conversion coating formed on the zinc plating layer and an electrodeposited coating film formed on the chemical conversion coating. Furthermore, an alloyed galvanized steel sheet for electrodeposited coating can also be provided. The details of the manufacturing method of the electrodeposited coated steel sheet and the electrodeposited coated steel sheet are the same as in Embodiment 1 described above, therefore, descriptions are omitted here.

[0226] Furthermore, this embodiment is the same as Embodiment 1 described above, and can provide automotive parts. The details of the automotive parts have already been described above, and will not be repeated here.

[0227] The present invention will now be described in detail based on embodiments.

[0228] Example 1

[0229] The steel with the chemical composition shown in Table 1 was melted to obtain a casting, which was then hot-rolled, pickled, and cold-rolled to produce a cold-rolled steel sheet with a thickness of 1.6 mm.

[0230]

[0231]

[0232] Next, the cold-rolled steel sheet was degreased with an alkaline solution. Then, it was electrolyzed under the conditions shown below, using the steel sheet as the cathode, to produce a pre-annealed Fe-based electroplated steel sheet with a pre-annealed Fe-based electroplating layer on one side. The adhesion amount of the pre-annealed Fe-based electroplating layer was calculated using the cross-sectional observation method described above and controlled by the energizing time. Next, the pre-annealed Fe-based electroplated steel sheet was subjected to reduction annealing with 15% H2-N2, a soaking zone temperature of 800°C, and the dew point of the atmosphere adjusted according to Tables 2-1, 2-2, and 4 to obtain the Fe-based electroplated steel sheet. After cooling the obtained Fe-based electroplated steel sheet to 440–550°C, it was then hot-dip galvanized in a 460°C hot-dip galvanizing bath with an effective Al concentration of 0.132% by mass and the remainder consisting of Zn and unavoidable impurities. The weight per unit area was then adjusted to approximately 50 g / m² per side by gas purging. 2 Galvanized steel sheets were obtained. Further, the galvanized steel sheets were alloyed at 490℃ for varying times to produce samples of alloyed galvanized steel sheets with different Fe contents diffused in the alloyed zinc layer.

[0233] [Electrolysis conditions]

[0234] Bath temperature: 50℃

[0235] pH: 2.0

[0236] Current density: 45A / dm 2

[0237] Fe-based electroplating bath: containing 1.5 mol / L Fe 2+ ion

[0238] Electrode (anode): Iridium oxide electrode

[0239] Based on the above method, the adhesion amount of the Fe-based electroplating layer on each single side, the adhesion amount of the alloyed zinc plating layer, the Fe content (mass%) in the alloyed zinc plating layer, and the proportion of the crystal orientation of the Fe-based electroplating layer and the Si-containing cold-rolled steel sheet integrated at the interface of the Fe-based electroplating layer and the Si-containing cold-rolled steel sheet are determined from the alloyed zinc plating sheet manufactured as described above.

[0240] The resistance to resistance welding cracking characteristics of the welded parts of the alloyed galvanized steel sheets obtained above were investigated. The following describes the methods for determining and evaluating the resistance to resistance welding cracking characteristics of the welded parts.

[0241] <Characteristics of resistance welding cracking resistance of welded parts>

[0242] For alloyed galvanized steel sheets, the evaluation method described above is used to assess the resistance to welding cracking characteristics of the sheet group under a holding time of 0.18 seconds, where Si content is less than 0.5%, tensile strength is 980 MPa, and adhesion weight per single side is 50 g / m². 2 The resistance to welding cracking characteristics of the welded portion of the test alloyed hot-dip galvanized steel sheet (1.6 mm thick) were investigated. The welding time was 0.36 seconds, and the holding time was 0.18 seconds and 0.24 seconds. For each Example No., the weld nugget diameter was measured by changing the welding current, and the evaluation was conducted at a welding current with a weld nugget diameter of 5.9 mm. Furthermore, the data for the test alloyed hot-dip galvanized steel sheet used as the plate group object was used as the example data, provided that no cracking occurred. This is because when cracking occurred in the plate group object, the stress dispersion of the alloyed galvanized steel sheet being evaluated could not be properly assessed.

[0243] The results of the above tests are shown in Tables 2-1, 2-2, and 4. The results indicate that, prior to the annealing process, the alloyed galvanized steel sheet of the inventive example, where the Fe-based electroplating layer is formed under conditions suitable for this invention, exhibits excellent resistance to weld cracking at the weld joint. Furthermore, in Reference Examples 1 and 2, since Si is less than 0.5%, there are no particular problems with the resistance to weld cracking at the weld joint. The Fe-based electroplating layer adhesion of the alloyed hot-dip galvanized steel sheet, which has an Fe-based electroplating layer formed before annealing and undergoes alloying treatment after galvanizing, is 25.0 g / m². 2 In the above-mentioned examples, no cracks longer than 0.1 mm were observed even under a holding time of 0.18 seconds, indicating particularly good resistance to resistance welding cracking in the welded parts. Furthermore, in Tables 2-1 and 2-2, examples where no Fe-based electroplating layer was formed are indicated by "-" for the adhesion amount of the Fe-based electroplating layer and the alloyed zinc plating layer. Additionally, in Reference Examples No. 17, 29, and 45, which underwent a high dew point annealing process greater than -30°C, the proportion of crystal orientation integration between the Fe-based electroplating layer and the Si-containing cold-rolled steel sheet at the interface was low due to the high dew point annealing, resulting in good resistance to resistance welding cracking in the welded parts. Furthermore, in these reference examples, the Fe-based electroplated steel sheet before annealing was heated to a soaking temperature of 800°C at an average heating rate of 10°C / second or higher in a temperature range of 400°C to 650°C, and then subjected to reduction annealing.

[0244]

[0245]

[0246]

[0247] Example 2

[0248] The steel with the chemical composition shown in Table 5 was melted to obtain castings, which were then hot-rolled, pickled, and cold-rolled to produce cold-rolled steel sheets with a thickness of 1.6 mm.

[0249]

[0250] Next, the cold-rolled steel sheet was degreased with an alkaline solution. Then, it was electrolyzed under the conditions shown below, using the steel sheet as the cathode, to produce a pre-annealed Fe-based electroplated steel sheet with a pre-annealed Fe-based electroplating layer on one side. The adhesion amount of the pre-annealed Fe-based electroplating layer was calculated using the cross-sectional observation method described above and controlled by the energizing time. Next, the pre-annealed Fe-based electroplated steel sheet was subjected to reduction annealing with 15% H2-N2, a soaking zone temperature of 800°C, and the dew point of the atmosphere adjusted as shown in Table 6, to obtain the Fe-based electroplated steel sheet. After cooling the obtained Fe-based electroplated steel sheet to 440–550°C, it was then hot-dip galvanized in a 460°C hot-dip galvanizing bath with an effective Al concentration of 0.132% by mass and the remainder consisting of Zn and unavoidable impurities. The weight per unit area was adjusted to approximately 50 g / m² per side by gas purging. 2 Galvanized steel sheets were obtained. Then, the galvanized steel sheets were alloyed at 490℃ for varying times to produce samples of alloyed galvanized steel sheets with different Fe contents diffused into the alloyed zinc layer.

[0251] [Electrolysis conditions]

[0252] Bath temperature: 50℃

[0253] pH: 2.0

[0254] Current density: 45A / dm 2

[0255] Fe-based electroplating bath: containing 1.5 mol / L Fe 2+ ion

[0256] Electrode (anode): Iridium oxide electrode

[0257] Alloyed galvanized steel sheets manufactured as described above are used to determine the amount of Fe-based electroplating on each side, the amount of alloyed galvanized layer, the Fe content (mass%) in the alloyed galvanized layer, and the proportion of the crystal orientation of the Fe-based electroplating layer and the Si-containing cold-rolled steel sheet integrated at the interface of the Fe-based electroplating layer and the Si-containing cold-rolled steel sheet, according to the above method.

[0258] The resistance to resistance welding cracking characteristics of the welded parts of the alloyed galvanized steel sheets obtained above were investigated. The methods for determining and evaluating the resistance to resistance welding cracking characteristics of the welded parts are shown below.

[0259] <Characteristics of resistance welding cracking resistance of welded parts>

[0260] For alloyed galvanized steel sheets, the evaluation criteria, based on the above method, included resistance welding cracking characteristics under a holding time of 0.14 seconds, a tensile strength of 590 MPa with Si content less than 0.1%, and an adhesion weight of 50 g / m² per single side. 2 The resistance to welding cracking characteristics of the welded portion of the test alloyed hot-dip galvanized steel sheet (1.6 mm thick) were examined. The welding time was 0.36 seconds, and the holding time was 0.14 seconds and 0.16 seconds. For each Example No., the weld nugget diameter was measured by changing the welding current, and evaluation was performed at a welding current with a weld nugget diameter of 5.9 mm. Furthermore, this is because the data for the examples uses the test alloyed hot-dip galvanized steel sheet that cracked as the subject of the plate group. When cracking occurred in the plate group, the stress dispersion of the alloyed galvanized steel sheet being evaluated could not be properly assessed.

[0261] The results of the above experiments are recorded in Table 6. The results show that, prior to the annealing process, the alloyed galvanized steel sheet of the invention example, under conditions suitable for this invention, exhibits excellent resistance to resistance welding cracking at the welded portion. Before forming the galvanized layer, an Fe-based electroplating layer is formed; after galvanizing, the Fe-based electroplating layer on the alloyed hot-dip galvanized steel sheet undergoes alloying treatment, with an adhesion amount of 25.0 g / m³. 2 In all the above-mentioned examples, no cracks longer than 0.1 mm were observed even under a holding time of 0.14 seconds, demonstrating particularly good resistance to resistance welding cracking in the welded parts. Furthermore, in Table 6, examples where no Fe-based electroplating layer was formed are indicated by "-" to represent the amount of Fe-based electroplating layer and alloyed zinc plating layer adhered.

[0262]

[0263] Industrial availability

[0264] The alloyed galvanized steel sheet manufactured by this invention not only has excellent resistance to resistance welding cracking characteristics in the welded parts, but also has high strength and excellent workability. Therefore, it can be used not only as a billet for use in automotive parts, but also as a billet for applications requiring the same characteristics in the fields of home appliances and building components.

[0265] Symbol Explanation

[0266] 1 Alloyed galvanized steel sheet

[0267] 2. Si-containing cold-rolled steel sheet

[0268] 3 Fe-based electroplating layer

[0269] 4 Alloyed zinc coating

[0270] 5. Experimental Alloyed Hot-Dip Galvanized Steel Sheets

[0271] 6 test pieces

[0272] 7 gaskets

[0273] 8 Fixed Platform

[0274] 9 electrodes

[0275] 10 Melting Core

[0276] 11 Cracks

Claims

1. An alloyed galvanized steel sheet, comprising: Si-containing cold-rolled steel sheet, containing 0.1% to 3.0% by mass of Si, Fe-based electroplating layer, formed on at least one side of the Si-containing cold-rolled steel sheet, wherein the amount of plating on each side exceeds 20.0 g / m². 2 ,and An alloyed zinc plating layer is formed on the Fe-based electroplating layer; The proportion of the crystal orientation of the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet being integrated at the interface between the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet is greater than 50%.

2. The alloyed galvanized steel sheet according to claim 1, wherein, The Si-containing cold-rolled steel sheet contains 0.50% to 3.0% by mass of Si.

3. The alloyed galvanized steel sheet according to claim 1 or 2, wherein, The Fe-based electroplated layer has an adhesion amount of 25.0 g / m² per single side. 2 above.

4. The alloyed galvanized steel sheet according to claim 1 or 2, wherein, The Si-containing cold-rolled steel sheet, in addition to Si, has the following composition: by mass % C: less than 0.8%, Mn: 1.0% to 12.0%, P: less than 0.1%, S: less than 0.03%, N: less than 0.010%, and Al: less than 1.0%, with the remainder consisting of Fe and unavoidable impurities.

5. The alloyed galvanized steel sheet according to claim 4, wherein, The composition further contains one or more of the following: B: less than 0.005%, Ti: less than 0.2%, Cr: less than 1.0%, Cu: less than 1.0%, Ni: less than 1.0%, Mo: less than 1.0%, Nb: less than 0.20%, V: less than 0.5%, Sb: less than 0.200%, Ta: less than 0.1%, W: less than 0.5%, Zr: less than 0.1%, Sn: less than 0.20%, Ca: less than 0.005%, Mg: less than 0.005%, and REM: less than 0.005%.

6. The alloyed galvanized steel sheet according to claim 1 or 2, wherein, The Fe-based electroplating layer has the following composition: it contains one or more elements selected from B, C, P, N, O, Ni, Mn, Mo, Zn, W, Pb, Sn, Cr, V and Co, totaling less than 10% by mass, with the remainder consisting of Fe and unavoidable impurities.

7. An alloyed galvanized steel sheet, comprising: Cold-rolled steel sheet containing 0.1% to 3.0% by mass of Si, Fe-based electroplating layer is formed on at least one side of the cold-rolled steel sheet, with an adhesion amount greater than 20.0 g / m² on each side. 2 ,and An alloyed zinc plating layer is formed on the Fe-based electroplating layer; The proportion of the crystal orientation of the Fe-based electroplated layer and the cold-rolled steel sheet that is integrated at the interface between the Fe-based electroplated layer and the cold-rolled steel sheet is greater than 50%. in, The cold-rolled steel sheet is as follows: The adhesion amount of a 50×150mm test piece cut with the rolling right angle as the long side and a hot-dip galvanized layer of the same size cut on each single side was 50g / m². 2 The experiment used alloyed hot-dip galvanized steel sheets stacked together to form a plate assembly. Next, using a servo motor-driven, pressure-applied, single-phase AC 50Hz resistance welding machine, the plate assembly was tilted 5° along its long side relative to the vertical plane of the line connecting the central axes of the 6mm diameter electrode pair at the front end of the welding machine. A gap of 60mm along the long side and 2.0mm along the thickness of the plate assembly was created between the lower electrode of the electrode pair and the test piece. The lower electrode and the plate assembly were fixed, and with the upper electrode of the electrode pair movable, resistance welding was performed on the plate assembly under the conditions of a pressure of 3.5kN, a holding time of 0.16 seconds, a welding current of 5.9mm, and a welding time, producing a plate assembly with a welded section. Next, the plate assembly with the welded part was cut in half along the long side of the test piece, including the welded part. When the cross-section of the welded part was observed with an optical microscope at a magnification of 200x, cracks with a length of more than 0.1 mm were observed.

8. The alloyed galvanized steel sheet according to claim 7, wherein, The cold-rolled steel sheet is as follows: when resistance welding is performed on the cold-rolled steel sheet under the condition of holding time of 0.24 seconds to obtain a plate assembly with the welded part, when the cross section of the welded part is observed with the optical microscope at a magnification of 200x, a crack with a length of more than 0.1 mm is observed.

9. An electrodeposited coated steel sheet, further comprising a chemical conversion treatment film and an electrodeposited coating film formed on the chemical conversion treatment film, on an alloyed galvanized steel sheet according to any one of claims 1 to 8.

10. An automotive component, at least a portion of which is made using the electrodeposited coated steel sheet of claim 9.

11. A method for manufacturing an electrodeposited coated steel sheet, comprising the following steps: The chemical conversion treatment process involves subjecting the alloyed galvanized steel sheet according to any one of claims 1 to 8 to chemical conversion treatment to obtain a chemical conversion treated steel sheet with a chemical conversion treatment film formed on the alloyed galvanized layer. In the electrodeposition coating process, the chemically converted steel plate is subjected to electrodeposition coating treatment to obtain an electrodeposition coated steel plate with an electrodeposition coating film formed on the chemically converted film.

12. A method for manufacturing alloyed galvanized steel sheet, comprising subjecting a cold-rolled steel sheet containing 0.1% to 3.0% by mass Si to Fe-based electroplating to produce a pre-annealed Fe-based electroplated steel sheet having a pre-annealed Fe-based electroplating layer formed on at least one side. Next, the Fe-based electroplated steel sheet before annealing is annealed in an atmosphere with a dew point below -30°C to produce an Fe-based electroplated steel sheet. Next, the Fe-based electroplated steel sheet is galvanized to produce a galvanized steel sheet. Next, the galvanized steel sheet is further alloyed to obtain a coating weight of more than 20.0 g / m² on each single side. 2 Alloyed galvanized steel sheet with Fe-based electroplating coating.

13. The method for manufacturing alloyed galvanized steel sheet according to claim 12, wherein, The cold-rolled steel sheet contains 0.5% to 3.0% by mass of Si.

14. The method for manufacturing alloyed galvanized steel sheet according to claim 12 or 13, wherein, The amount of adhesion CW per single side of the Fe-based electroplated layer before annealing Fe0 It satisfies the following equation (1). Among them, CW Zn The target value for the amount of alloyed zinc plating adhered to per side, and 25.0 g / m². 2 ≤CW Zn ≤80.0g / m 2 The CW Fe0 The target value for the amount of adhesion is in g / m³. 2 , [mass%Fe]: The target value of Fe content in the alloyed zinc plating layer, in mass%.

15. A method for manufacturing an alloyed galvanized steel sheet, comprising subjecting a cold-rolled steel sheet containing 0.1% to 3.0% by mass of Si to Fe-based electroplating, to produce an annealed Fe-based electroplated steel sheet having an annealed Fe-based electroplating layer formed on at least one side. Next, the Fe-based electroplated steel sheet before annealing is annealed in an atmosphere with a dew point below -30°C to produce an Fe-based electroplated steel sheet. Next, the Fe-based electroplated steel sheet is galvanized to produce a galvanized steel sheet. Next, the galvanized steel sheet is further alloyed to obtain a coating weight of more than 20.0 g / m² on each single side. 2 Alloyed galvanized steel sheet with Fe-based electroplating coating, in, The cold-rolled steel sheet is as follows: The adhesion amount of a 50×150mm test piece cut with the rolling right angle as the long side and a hot-dip galvanized layer of the same size cut on each single side was 50g / m². 2 The test used alloyed hot-dip galvanized steel sheets to be stacked and made into a plate assembly. Next, using a servo motor-driven, pressurized single-phase AC 50Hz resistance welding machine, the plate assembly is tilted 5° along its long side relative to the vertical plane of the line connecting the central axes of the 6mm diameter electrode pair at the front end of the welding machine. A gap of 60mm along the long side and 2.0mm along the thickness of the plate assembly is created between the lower electrode of the electrode pair and the test piece. The lower electrode and the plate assembly are fixed. With the upper electrode of the electrode pair movable, resistance welding is performed on the plate assembly under the following conditions: applied pressure: 3.5kN; holding time: 0.16 seconds; weld nugget diameter: 5.9mm; welding current and welding time, to produce a plate assembly with a welded section. Next, the plate assembly with the welded part was cut in half along the long side of the test piece, including the welded part. When the cross-section of the welded part was observed with an optical microscope at a magnification of 200x, cracks with a length of more than 0.1 mm were observed.

16. The method for manufacturing alloyed galvanized steel sheet according to claim 15, wherein, When the cross-section of the welded part was observed with an optical microscope at a magnification of 200x under the condition that the holding time was 0.24 seconds, a crack with a length of more than 0.1 mm was observed.

17. The method for manufacturing alloyed galvanized steel sheet according to claim 15 or 16, wherein, The amount of adhesion CW per single side of the Fe-based electroplated layer before annealing Fe0 It satisfies the following equation (1). Among them, CW Zn The target value for the amount of alloyed zinc plating adhered to per side, and 25.0 g / m². 2 ≤CW Zn ≤80.0g / m 2 The CW Fe0 The target value for the amount of adhesion is in g / m³. 2 , [mass%Fe]: The target value of Fe content in the alloyed zinc plating layer, in mass%.

18. The method for manufacturing alloyed galvanized steel sheet according to claim 12 or 15, wherein, The Fe-based electroplating is performed using an Fe-based electroplating bath containing one or more elements selected from B, C, P, N, O, Ni, Mn, Mo, Zn, W, Pb, Sn, Cr, V, and Co, such that the total content of these elements in the Fe-based electroplating layer before annealing is 10% by mass.

Citation Information