Polyphosphorus bacteria synthesizes lithium iron phosphate material and its preparation method and application
By synthesizing lithium iron phosphate materials through bio-preparation polyphosphate bacteria and combining them with hybrid capacitor deionization technology, the problem of insufficient lithium ion adsorption capacity of existing porous electrode materials has been solved, achieving efficient lithium ion recovery and low-cost environmentally friendly treatment.
Patent Information
- Application Number
- CN202310543206.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-15
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-05-15
AI Technical Summary
Existing porous electrode materials have limited adsorption capacity for lithium ions, making it difficult to improve recovery rates. Furthermore, traditional lithium iron phosphate materials suffer from defects in electrochemical performance and preparation methods, resulting in low lithium ion recovery efficiency, high costs, and severe environmental pollution.
A bio-based method was used to synthesize lithium iron phosphate materials from polyphosphate bacteria. By optimizing electrode materials and utilizing hybrid capacitor deionization technology, combined with the polyphosphate-synthesized lithium iron phosphate materials and activated carbon electrodes, efficient adsorption and recovery of lithium ions were achieved.
It improves the adsorption rate and capacity of lithium ions, reduces energy consumption and environmental pollution, and achieves efficient and low-cost lithium ion recycling. In addition, the material has good electrochemical performance and recycling capacity.
Smart Images

Figure CN116574763B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of electrochemical technology for resource recycling, specifically relating to a method for synthesizing lithium iron phosphate materials by polyphosphate bacteria, its preparation method, and its application. Background Technology
[0002] Driven by the global pursuit of clean energy for sustainable development, the demand for lithium has been growing rapidly, making lithium availability a major concern. Lithium is primarily stored in lithium-bearing ores (such as schist and sphalerite) and water-based lithium resources, with two-thirds of total lithium reserves found in brine and seawater. To date, various technologies have been explored for extracting lithium from brine and seawater, such as precipitation, solvent extraction, lithium-ion sieve adsorption, and membrane-based techniques. However, these technologies all have their drawbacks, including low extraction rates, the need for large amounts of acid causing environmental problems, time-consuming processes, and high costs. Therefore, there is an urgent need to develop a lithium extraction method that is highly efficient, environmentally friendly, and cost-effective.
[0003] Capacitive deionization (CDI) is a novel brine desalination technology. It involves applying an external voltage across a porous electrode, causing cations and anions to move towards the oppositely charged electrode under the influence of an electrostatic field. The cations and anions are then adsorbed within the micropores of the electrode, achieving ion recovery and brine desalination. After a period of operation, the porous electrode becomes saturated. At this point, by shorting or reversing the power supply, the adsorbed salt ions are released into the solution, regenerating the porous electrode. While CDI can recover lithium from water, addressing the time-consuming, costly, and environmentally polluting issues of other technologies, it still has drawbacks: existing porous electrodes generally use carbon-based electrodes (mostly activated carbon), which have limited lithium ion adsorption capacity, making it difficult to improve recovery rates. Summary of the Invention
[0004] To address the aforementioned problems, one objective of this invention is to provide a method for preparing lithium iron phosphate materials synthesized by polyphosphate bacteria. This method is simple, easy to operate, and can produce electrode material substrates capable of adsorbing large quantities of lithium ions.
[0005] To achieve the above objectives, the specific technical solution adopted by the present invention is as follows:
[0006] A method for preparing lithium iron phosphate materials synthesized by polyphosphate bacteria includes the following steps:
[0007] S1. Inoculate polyphosphate-accumulating bacteria with a phosphorus removal effect of 10-20 mg / L into LB liquid medium and culture in a shaker at 25°C and 120 r / min for 10-12 h;
[0008] S2. Add lithium hydrogen phosphate to the culture medium and continue culturing for 22-26 hours;
[0009] S3. Add ferrous sulfate to the culture medium and continue culturing for 24–36 h;
[0010] S4. Add lithium chloride to the culture medium and continue culturing for 22-26 hours;
[0011] S5. After centrifuging to remove the culture medium, dry the sample and then anneal it at 750-850℃ for 3-5 hours under a nitrogen atmosphere.
[0012] To improve the lithium-ion recovery rate of CDI technology, this invention starts by optimizing electrode materials, selecting lithium iron phosphate (LFP) to replace activated carbon in existing technologies. However, conventional LFP has significant drawbacks in both electrochemical performance and preparation methods. Specifically, existing LFP is primarily chemically synthesized, with methods including high-temperature solid-state methods, hydrothermal methods, and carbothermal reduction methods, which are complex and prone to pollution. Furthermore, existing LFP is limited by slow lithium-ion diffusion kinetics and its inherently low electronic conductivity, making efficient lithium-ion recovery difficult. In addition, LFP is prone to volume expansion after cycling, affecting its lifespan and electrochemical performance.
[0013] Therefore, this invention utilizes a self-developed bio-preparation method to produce lithium iron phosphate materials synthesized by polyphosphate bacteria. This bio-preparation method is simple, easy to operate, environmentally friendly, safe, and low-cost, offering significant advantages compared to existing chemical synthesis methods. The polyphosphate-synthesized lithium iron phosphate material prepared according to this invention overcomes the shortcomings of conventional lithium iron phosphate. The presence of polyphosphate-derived carbon effectively improves its conductivity while mitigating the volume expansion of lithium iron phosphate, resulting in a significant improvement in electrochemical performance. Electrodes made using this polyphosphate-synthesized lithium iron phosphate material exhibit faster adsorption rates and higher adsorption capacities compared to traditional carbon electrodes, showing promising application prospects in the field of lithium-ion recovery.
[0014] Preferably, in step S1, the polyphosphate-accumulating bacteria are obtained by the following method: a. Activated sludge treatment: Take activated sludge from the aerobic stage of a conventional AAO denitrification and phosphorus removal water treatment process (i.e., the aerobic stage of an anaerobic-anoxic-aerobic process), centrifuge to obtain activated sludge samples, and remove impurities such as silt for later use; b. Acclimation: Set up culture media with different phosphorus concentration gradients in the range of 50-500 mg / L, inoculate activated sludge into the gradient liquid culture media at an inoculation rate of 5-15%, and culture at 25℃ and 120 r / min for 24-48 h; c. Centrifugation separation: Select bacterial culture solutions with a phosphorus removal effect of 10-20 mg / L, centrifuge and wash to obtain polyphosphate-accumulating bacteria for later use. The strain obtained by this method has a strong phosphorus absorption capacity.
[0015] Preferably, the amount of lithium hydrogen phosphate added to the culture medium is 0.02–0.05 M, the amount of ferrous sulfate added to the culture medium is 0.02–0.05 M, and the amount of lithium chloride added to the culture medium is 0.16–0.2 M. Further, the molar ratio of lithium hydrogen phosphate, ferrous sulfate, and lithium chloride is 1:1:8. The types and amounts of phosphorus, iron, and lithium sources in this invention must be strictly added according to requirements: it must be lithium hydrogen phosphate, ferrous sulfate, and lithium chloride. If other substances are used or added, it is difficult to synthesize the target material. Below this molar ratio, the adsorbate mass of polyphosphate-accumulating bacteria is low, making product synthesis difficult; above this molar ratio, the growth and reproduction of the bacteria are affected, resulting in low biomass of polyphosphate-accumulating bacteria, making product synthesis impossible.
[0016] Preferably, in step S1, the culture time is 12h; in steps S2 and S4, the culture time is 24h; in step S5, the sample is annealed at 800℃ for 4h under a nitrogen atmosphere.
[0017] The second objective of this invention is to provide a polyphosphate-synthesized lithium iron phosphate material prepared by the above-described preparation method.
[0018] The third objective of this invention is to provide the application of lithium iron phosphate materials synthesized by polyphosphate bacteria using the above-mentioned preparation method in lithium-ion recovery, comprising the following steps:
[0019] (1) Preparation of lithium iron phosphate material electrode synthesized by polyphosphate bacteria: The lithium iron phosphate material synthesized by polyphosphate bacteria is ground into micron-sized powder, then mixed with PVDF and acetylene black, and then NMP is added and stirred for 6-12 hours to obtain a well mixed slurry. The slurry is spread on the graphite paper current collector and dried to obtain the lithium iron phosphate material electrode synthesized by polyphosphate bacteria.
[0020] (2) Preparation of activated carbon electrode: Activated carbon is mixed with PVDF and acetylene black, and then NMP is added and stirred for 6-12 hours to obtain a well mixed slurry. The slurry is spread on a graphite paper current collector and dried to obtain an activated carbon electrode.
[0021] (3) Assembly of the hybrid capacitor deionization device: The fixed plate, silicone gasket, current collector, lithium iron phosphate material electrode synthesized by polyphosphate bacteria, plexiglass water collection tank, diaphragm, anion exchange membrane, activated carbon electrode, current collector, silicone gasket, and fixed plate are assembled in the device in sequence; among them, the plexiglass water collection tank is a hollow plate with inlet and outlet ports to achieve the purpose of circulating water intake;
[0022] (4) Lithium ion recovery: After the hybrid capacitor deionization device is assembled, it is connected to the lithium ion recovery system. The recovery system includes a lithium chloride collection tank, a peristaltic pump, a hybrid capacitor deionization device, and a conductivity meter. During operation, the peristaltic pump inputs lithium chloride brine from the lithium chloride collection tank into the energized hybrid capacitor deionization device. During adsorption, the lithium iron phosphate material electrode synthesized by polyphosphate bacteria is connected to the negative electrode to adsorb lithium ions, and the activated carbon electrode is connected to the positive electrode to adsorb chloride ions. After adsorption, the brine is recycled back to the lithium chloride collection tank to test the conductivity.
[0023] (5) Electrode regeneration: Desorption can be achieved by reversing the power supply, and the operation is the same as that of adsorption.
[0024] Unlike existing dual-carbon-based capacitor deionization technologies, this invention employs lithium iron phosphate material electrodes synthesized by polyphosphate bacteria and activated carbon electrodes. It utilizes hybrid capacitor deionization technology to recover lithium ions from water, effectively improving recovery rate and efficiency while reducing energy consumption. The principle of the hybrid capacitor deionization recovery is as follows: Under an external voltage, lithium ions in the lithium iron phosphate composite material synthesized by microorganisms are released from their lattice. With a reverse voltage applied, lithium ions in the solution can re-enter the lattice, thus undergoing a Faraday reaction for lithium insertion and extraction, thereby recovering lithium ions from the water. Meanwhile, under an external voltage, chloride ions migrate towards the activated carbon electrode, forming a double layer on its surface and being stored. With a reverse voltage applied, the double layer disappears, and chloride ions desorb from the electrode. This achieves a process of material adsorption-desorption recycling.
[0025] Preferably, in step (1), the mass ratio of the polyphosphate-synthesized lithium iron phosphate material, PVDF and acetylene black is 8:1:1; in step (2), the mass ratio of the activated carbon, PVDF and acetylene black is 8:1:1.
[0026] Preferably, in step (4), the circulating water flow rate of the peristaltic pump is 20-30 mL / min.
[0027] Preferably, in step (4), the influent concentration is 400-600 mg / L.
[0028] Preferably, in step (4), the voltage range of the hybrid capacitor deionization device is -1.6 to 1.6V to -1.2 to 1.2V, and the constant current density range is 20 to 60mA / g.
[0029] The present invention has the following beneficial effects:
[0030] 1. The lithium iron phosphate material synthesized by polyphosphate bacteria prepared in this invention has a fast adsorption rate of lithium ions, a large adsorption capacity, good conductivity, can effectively alleviate the volume expansion of lithium iron phosphate, and has excellent electrochemical performance. Compared with traditional activated carbon and lithium iron phosphate, it has obvious advantages.
[0031] 2. The lithium iron phosphate material synthesized by polyphosphate bacteria in this invention is prepared by a biological method. The process is simple, easy to operate, environmentally friendly, safe and low cost.
[0032] 3. This invention utilizes hybrid capacitor deionization technology to recover lithium chloride from water based on Faraday capacitance and double-layer capacitance, achieving efficient, high-adsorption capacity, low-cost, low-energy consumption, and pollution-free recovery of lithium, and enabling its recycling. Attached Figure Description
[0033] Figure 1 SEM image of polyphosphate-accumulating bacteria in Example 1.
[0034] Figure 2 SEM image of lithium iron phosphate material synthesized by polyphosphate bacteria in Example 1.
[0035] Figure 3 Example 4: Graph showing the change in conductivity of hybrid capacitors during lithium-ion recovery.
[0036] Figure 4 Example 4: Adsorption capacity diagram of hybrid capacitor deionization under different current windows (20-60 mA / g).
[0037] Figure 5 Example 4: Adsorption capacity diagram of hybrid capacitor deionization at different voltages (-1.6 to 1.6V to -1.2 to 1.2V). Detailed Implementation
[0038] The present invention will be further described below with reference to the accompanying drawings and specific embodiments.
[0039] Example 1
[0040] A method for preparing lithium iron phosphate materials synthesized by polyphosphate bacteria includes the following steps:
[0041] S1. First, polyphosphate-accumulating bacteria were obtained using the following method: a. Activated sludge treatment: Activated sludge from the aerobic stage of a conventional AAO denitrification and phosphorus removal water treatment process (anaerobic-anoxic-aerobic process) was centrifuged to obtain activated sludge samples, and impurities such as silt were removed for later use; b. Acclimation: Culture media with different phosphorus concentration gradients (50, 100, 200, 500 mg / L) were set up, and activated sludge was inoculated into the gradient liquid culture media at an inoculation rate of 10%, and cultured at 25℃ and 120 r / min for 36 h; c. Centrifugation separation: After the culture was completed, the phosphorus content in the culture medium was measured. Based on the phosphorus removal effect (selecting the bacterial culture medium with a phosphorus removal effect of 10-20 mg / L), the polyphosphate-accumulating bacteria were obtained by centrifugation and washing for later use; then, all the obtained polyphosphate-accumulating bacteria were inoculated into 80 mL of LB liquid culture medium and cultured in a shaker at 25℃ and 120 r / min for 12 h;
[0042] S2. Add lithium hydrogen phosphate to the culture medium at a concentration of 0.02M and continue culturing for 24 hours;
[0043] S3. Add ferrous sulfate to the culture medium at a concentration of 0.02M and continue culturing for 36 hours;
[0044] S4. Add lithium chloride to the culture medium at a concentration of 0.16M and continue culturing for 24 hours;
[0045] S5. After centrifuging to remove the culture medium, dry the sample and then anneal it at 800℃ for 4 hours under a nitrogen atmosphere.
[0046] Example 2
[0047] S1. First, polyphosphate-accumulating bacteria were obtained using the following method: a. Activated sludge treatment: Activated sludge from the aerobic stage of a conventional AAO denitrification and phosphorus removal water treatment process (anaerobic-anoxic-aerobic process) was centrifuged to obtain activated sludge samples, and impurities such as silt were removed for later use; b. Acclimation: Culture media with different phosphorus concentration gradients (50, 100, 200, 500 mg / L) were set up, and activated sludge was inoculated into the gradient liquid culture media at an inoculation rate of 5%, and cultured at 25℃ and 120 r / min for 48 h; c. Centrifugation separation: After the culture was completed, the phosphorus content in the culture medium was measured. Based on the phosphorus removal effect (selecting the bacterial culture medium with a phosphorus removal effect of 10-20 mg / L), the polyphosphate-accumulating bacteria were obtained by centrifugation and washing for later use; then, all the obtained polyphosphate-accumulating bacteria were inoculated into 50 mL of LB liquid culture medium and cultured in a shaker at 25℃ and 120 r / min for 10 h;
[0048] S2. Add lithium hydrogen phosphate to the culture medium at a concentration of 0.02M and continue culturing for 24 hours;
[0049] S3. Add ferrous sulfate to the culture medium at a concentration of 0.02M and continue culturing for 36 hours;
[0050] S4. Add lithium chloride to the culture medium at a concentration of 0.16M and continue culturing for 24 hours;
[0051] S5. After centrifuging to remove the culture medium, dry the sample and then anneal it at 800℃ for 4 hours under a nitrogen atmosphere.
[0052] Example 3
[0053] S1. First, polyphosphate-accumulating bacteria were obtained using the following method: a. Activated sludge treatment: Activated sludge from the aerobic stage of a conventional AAO denitrification and phosphorus removal water treatment process (anaerobic-anoxic-aerobic process) was centrifuged to obtain activated sludge samples, and impurities such as silt were removed for later use; b. Acclimation: Culture media with different phosphorus concentration gradients (50, 100, 200, 500 mg / L) were set up, and activated sludge was inoculated into the gradient liquid culture media at an inoculation rate of 15%, and cultured at 25℃ and 120 r / min for 24 h; c. Centrifugation separation: After the culture was completed, the phosphorus content in the culture medium was measured. Based on the phosphorus removal effect (selecting the bacterial culture medium with a phosphorus removal effect of 10-20 mg / L), the polyphosphate-accumulating bacteria were obtained by centrifugation and washing for later use; then, all the obtained polyphosphate-accumulating bacteria were inoculated into 100 mL of LB liquid culture medium and cultured in a shaker at 25℃ and 120 r / min for 12 h;
[0054] S2. Add lithium hydrogen phosphate to the culture medium at a concentration of 0.025M, and continue culturing for 24 hours;
[0055] S3. Add ferrous sulfate to the culture medium at a concentration of 0.025M and continue culturing for 36 hours;
[0056] S4. Add lithium chloride to the culture medium at a concentration of 0.2M and continue culturing for 24 hours;
[0057] S5. After centrifuging to remove the culture medium, dry the sample and then anneal it at 800℃ for 4 hours under a nitrogen atmosphere.
[0058] Examples 1-3 all successfully prepared lithium iron phosphate materials synthesized by polyphosphate-accumulating bacteria. Taking Example 1 as an example, the SEM images of the polyphosphate-accumulating bacteria and the prepared lithium iron phosphate material synthesized by polyphosphate-accumulating bacteria are shown below. Figure 1-2 As shown.
[0059] Comparative Example
[0060] Compared with Example 1, the phosphorus source, iron source, and lithium source were changed in this comparative example, and the materials were prepared according to the method of Example 1. The specific materials and results are as follows:
[0061]
[0062] Example 4
[0063] This embodiment demonstrates the application of the lithium iron phosphate material synthesized by polyphosphate bacteria obtained in Example 1 in lithium-ion recovery, as detailed below:
[0064] (1) Preparation of lithium iron phosphate material electrode synthesized by polyphosphate bacteria: The lithium iron phosphate material synthesized by polyphosphate bacteria was ground in a mortar and mortar into fine powder with a particle size down to the micron level. Then, it was mixed with PVDF and acetylene black at a mass ratio of 8:1:1. NMP was added and stirred for 6 hours to obtain a well mixed slurry. The slurry was spread on a graphite paper current collector and dried under vacuum at 60°C to obtain the lithium iron phosphate material electrode synthesized by polyphosphate bacteria.
[0065] (2) Preparation of activated carbon electrode: Activated carbon, PVDF and acetylene black are mixed in a mass ratio of 8:1:1, and NMP is added and stirred for 6 hours to obtain a well mixed slurry. The slurry is spread on a graphite paper current collector and dried under vacuum at 60°C to obtain an activated carbon electrode.
[0066] (3) Assembly of the hybrid capacitor deionization device: The fixed plate, silicone gasket, current collector, lithium iron phosphate material electrode synthesized by polyphosphate bacteria, plexiglass water collection tank, diaphragm, anion exchange membrane, activated carbon electrode, current collector, silicone gasket, and fixed plate are assembled in the device in sequence; among them, the plexiglass water collection tank is a hollow plate with inlet and outlet ports to achieve the purpose of circulating water intake;
[0067] (4) Lithium-ion recovery: After the hybrid capacitor deionization device is assembled, it is connected to the lithium-ion recovery system. The recovery system includes a lithium chloride collection tank, a peristaltic pump, a hybrid capacitor deionization device, and a conductivity meter. All components are connected by hoses. During operation, the peristaltic pump inputs lithium chloride brine from the lithium chloride collection tank into the energized hybrid capacitor deionization device. During adsorption, the lithium iron phosphate material electrode synthesized by polyphosphate bacteria is connected to the negative electrode to adsorb lithium ions, and the activated carbon electrode is connected to the positive electrode to adsorb chloride ions. After adsorption, the brine is circulated back to the lithium chloride collection tank to test the conductivity. The influent concentration is 500 mg / L, and the circulating water flow rate of the peristaltic pump is 25 mL / min.
[0068] (5) Electrode regeneration: Desorption can be achieved by reversing the power supply so that it can be recycled. The operation is the same as that of adsorption.
[0069] In step (4), the lithium-ion recovery process was tested for recovery performance, as follows: using 500 mg·L⁻¹ -1 The hybrid capacitor deionization device was rinsed with lithium chloride solution, and then 50 mL of lithium chloride solution was added to the test solution tank and continuously circulated until the conductivity stabilized. Following the above steps, a constant current was applied to the electrodes to begin lithium ion recovery, and the changes in current and solution conductivity were recorded simultaneously. Current was recorded every 5 seconds, and conductivity was recorded every 10 seconds. When the solution conductivity reached a point of near stability, the adsorption experiment was complete. Specific conductivity changes are shown below. Figure 3 As shown. The adsorption performance of the lithium iron phosphate material electrode synthesized by polyphosphate bacteria is as follows. Figure 4-5As shown, compared with other current densities (40, 50 and 60 mA / g), the adsorption capacity reached its maximum of 11.05 mg·g at a current density of 20 mA / g. -1 (1.59 mmol / g); compared with other voltages (1.2 V and 1.4 V), the adsorption capacity reached its maximum of 15.11 mg·g at a voltage of 1.6 V. -1 (2.17mmol / g), compared with traditional carbon-based capacitor deionization, the adsorption capacity is effectively improved, and it has a broader application prospect.
[0070] This specific embodiment is merely an explanation of the present invention and is not intended to limit the present invention. Any changes made by those skilled in the art after reading the specification of the present invention, as long as they are within the scope of the claims of the present invention, will be protected by patent law.
Claims
1. A method for preparing lithium iron phosphate materials synthesized by polyphosphate bacteria, characterized in that: Includes the following steps: S1. Inoculate polyphosphate-accumulating bacteria with a phosphorus removal efficiency of 10–20 mg / L into LB liquid medium and culture in a shaker at 25°C and 120 r / min for 10–12 h; wherein, the polyphosphate-accumulating bacteria are obtained by the following method: a. Treatment of activated sludge: Take activated sludge from the aerobic section of a conventional AAO denitrification and phosphorus removal water treatment process, centrifuge to obtain activated sludge samples, remove impurities and set aside for later use; b.
1. Acclimation: Set up culture media with different phosphorus concentration gradients in the range of 50-500 mg / L, and inoculate activated sludge into the gradient liquid culture media at an inoculation rate of 5-15%, and culture at 25℃ and 120 r / min for 24-48 h; c. Centrifugation: Select bacterial culture solutions with phosphorus removal efficiency of 10-20 mg / L, centrifuge and wash to obtain polyphosphate-accumulating cells; S2. Add 0.02-0.05M lithium hydrogen phosphate to the culture medium and continue culturing for 22-26 hours; S3. Add 0.02-0.05M ferrous sulfate to the culture medium and continue culturing for 24-36 hours; S4. Add 0.16-0.2M lithium chloride to the culture medium and continue culturing for 22-26 hours; the molar ratio of lithium hydrogen phosphate, ferrous sulfate and lithium chloride is 1:1:8; S5. After centrifuging to remove the culture medium, dry the sample and then anneal it at 750-850℃ for 3-5 hours under a nitrogen atmosphere.
2. The polyphosphate-synthesized lithium iron phosphate material prepared by the method described in claim 1.
3. The application of the lithium iron phosphate material synthesized by polyphosphate bacteria prepared by the method of claim 1 in lithium-ion recovery, characterized in that: Includes the following steps: (1) Preparation of lithium iron phosphate material electrode synthesized by polyphosphate bacteria: The lithium iron phosphate material synthesized by polyphosphate bacteria is ground into micron-sized powder, then mixed with PVDF and acetylene black, and then NMP is added and stirred for 6-12 hours to obtain a well mixed slurry. The slurry is spread on a graphite paper current collector and dried to obtain the lithium iron phosphate material electrode synthesized by polyphosphate bacteria. (2) Preparation of activated carbon electrode: Activated carbon is mixed with PVDF and acetylene black, and then NMP is added and stirred for 6-12 hours to obtain a well mixed slurry. The slurry is spread on a graphite paper current collector and dried to obtain an activated carbon electrode. (3) Assembly of the hybrid capacitor deionization device: The fixed plate, silicone pad, current collector, lithium iron phosphate material electrode synthesized by polyphosphate bacteria, organic glass water collection tank, diaphragm, anion exchange membrane, activated carbon electrode, current collector, silicone pad, and fixed plate are assembled in the device in the following order. (4) Lithium ion recovery: After the hybrid capacitor deionization device is assembled, it is connected to the lithium ion recovery system. The recovery system includes a lithium chloride collection tank, a peristaltic pump, a hybrid capacitor deionization device, and a conductivity meter. During operation, the peristaltic pump inputs lithium chloride brine from the lithium chloride collection tank into the energized hybrid capacitor deionization device. During adsorption, the lithium iron phosphate material electrode synthesized by polyphosphate bacteria is connected to the negative electrode to adsorb lithium ions, and the activated carbon electrode is connected to the positive electrode to adsorb chloride ions. After adsorption, it is circulated back to the lithium chloride collection tank to test the conductivity. (5) Electrode regeneration: Desorption can be achieved by reversing the power supply, and the operation is the same as adsorption.
4. The application of the polyphosphate-synthesized lithium iron phosphate material according to claim 3 in lithium-ion recovery, characterized in that: In step (1), the mass ratio of the polyphosphate-synthesized lithium iron phosphate material, PVDF and acetylene black is 8:1:1; in step (2), the mass ratio of the activated carbon, PVDF and acetylene black is 8:1:
1.
5. The application of the polyphosphate-synthesized lithium iron phosphate material according to claim 3 in lithium-ion recovery, characterized in that: In step (4), the circulating water flow rate of the peristaltic pump is 20-30 mL / min.
6. The application of the lithium iron phosphate material synthesized by polyphosphate bacteria according to claim 3 in lithium-ion recovery, characterized in that: In step (4), the influent concentration is 400-600 mg / L.
7. The application of the polyphosphate-synthesized lithium iron phosphate material according to claim 3 in lithium-ion recovery, characterized in that: In step (4), the voltage range of the hybrid capacitor deionization device is -1.6 to 1.6 V to -1.2 to 1.2 V, and the constant current density range is 20 to 60 mA / g.
Citation Information
Patent Citations
Pseudomonas putida P.PAO-1 with dephosphorization function as well as acclimatization and culture method
CN104745512A
Co-enrichment method of nitrifying bacteria and denitrifying phosphorus-accumulating bacteria