Catalytic layer, method for producing the same, membrane electrode, and fuel cell

By alternating coatings of graphene-based catalysts and conductive materials, the problem of stacking graphene-based Pt catalysts in the membrane electrode catalytic layer was solved, thereby improving the conductivity and mass transfer performance of the catalytic layer and increasing the utilization rate of the catalytic material.

CN116581311BActive Publication Date: 2026-11-20BEIJING GRAPHENE TECH RES INST CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202310629233.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2026-11-20
Estimated Expiration
2043-05-31

AI Technical Summary

Technical Problem

Graphene-based Pt catalysts tend to stack during the preparation of membrane electrode catalytic layers, resulting in low porosity, increased contact resistance and mass transfer resistance, which in turn affects the conductivity of the catalytic layer and the utilization rate of Pt.

Method used

A method of alternating coating of graphene-based catalysts and conductive materials is adopted to form alternating layers of graphene and conductive support layers, avoiding the stacking of graphene sheets, preserving the properties of graphene, and improving the utilization rate of catalytic materials.

Benefits of technology

This effectively avoids graphene sheet stacking, improves the conductivity and mass transfer performance of the catalyst layer, enhances the utilization rate of the catalyst material, and improves the overall performance of the membrane electrode.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116581311B_ABST
    Figure CN116581311B_ABST
Patent Text Reader

Abstract

The application provides a catalytic layer and a preparation method thereof, a membrane electrode and a fuel cell. The preparation method comprises the following steps: preparing a first slurry, wherein the first slurry comprises a graphene-based catalyst, and the graphene-based catalyst comprises a graphene substrate and a catalytic material loaded on the surface of the graphene substrate; preparing a second slurry, wherein the second slurry comprises a conductive material; alternately applying the first slurry and the second slurry on the surface of a substrate to respectively prepare a graphene layer and a conductive support layer, and alternately stacking the graphene layer and the conductive support layer to obtain the catalytic layer. The catalytic layer is prepared by using the alternately coating method, and the conductive material is used as the support structure between the graphene layers, so that the stacking problem between two adjacent graphene layers can be avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of fuel cell technology, and in particular to a catalyst layer and its preparation method, a membrane electrode assembly, and a fuel cell. Background Technology

[0002] The most crucial component of a fuel cell is the membrane electrode assembly (MEA). Catalytic reactions occur within the catalytic layer of the MEA. Graphene-based Pt-supported catalysts exhibit excellent performance in aqueous oxygen reduction (ORR) environments. However, when used as a catalyst in the MEA catalytic layer, graphene sheets are prone to stacking, leading to low porosity, increased contact resistance, and increased mass transfer resistance. This, in turn, results in poor conductivity and low Pt utilization. Furthermore, if the stacking reaches a certain level, the graphene-based Pt-supported catalyst can transform into graphite, completely losing the large specific surface area, good conductivity, and multiple active sites characteristic of graphene. This renders it impossible to reproduce the catalytic activity in an aqueous ORR environment, severely impacting MEA performance.

[0003] Therefore, finding a catalytic layer that can avoid the stacking of graphene sheets has become an urgent technical problem to be solved. Summary of the Invention

[0004] Therefore, it is necessary to provide a catalyst layer and its preparation method, a membrane electrode and a fuel cell, which utilizes conductive materials as a supporting structure between graphene layers to avoid stacking problems between adjacent graphene layers.

[0005] In a first aspect, this application provides a method for preparing a catalyst layer, the method comprising:

[0006] A first slurry is prepared, the first slurry comprising a graphene-based catalyst, the graphene-based catalyst comprising a graphene substrate and a catalytic material supported on the surface of the graphene substrate;

[0007] Prepare a second slurry, the second slurry comprising a conductive material;

[0008] The first slurry and the second slurry are alternately applied to the surface of the substrate to prepare a graphene layer and a conductive support layer, respectively. The graphene layer and the conductive support layer are alternately stacked to obtain the catalyst layer.

[0009] In some embodiments, the thickness of each graphene layer is 10 nm to 50 nm.

[0010] In some embodiments, the thickness of each conductive support layer is 20 nm to 100 nm.

[0011] In some embodiments, the graphene substrate comprises ≤10 graphene layers.

[0012] In some embodiments, the graphene substrate includes at least one of exfoliated graphene, graphene oxide, reduced graphene oxide, and doped graphene.

[0013] In some embodiments, the catalytic material includes a metal catalytic material.

[0014] Optionally, the catalytic material includes at least one of Pt and Pt alloys.

[0015] In some embodiments, the mass percentage of the catalytic material in the graphene-based catalyst is 5% to 70%.

[0016] In some embodiments, the conductive material includes at least one of carbon black and carbon nanotubes.

[0017] In some embodiments, the particle size of the conductive material is 10 nm to 50 nm.

[0018] In some embodiments, the first slurry further includes a perfluorosulfonic acid resin.

[0019] Optionally, in the first slurry, the mass ratio of the graphene-based catalyst to the perfluorosulfonic acid resin is 1:(0.15-0.35).

[0020] In some embodiments, the second slurry further includes a perfluorosulfonic acid resin.

[0021] Optionally, in the second slurry, the mass ratio of the conductive material to the perfluorosulfonic acid resin is 1:(0.15 to 0.35).

[0022] In some embodiments, the mass-volume concentration of the graphene-based catalyst in the first slurry is 0.1 mg / mL to 3 mg / mL.

[0023] In some embodiments, the mass-volume concentration of the conductive material in the second slurry is 0.1 mg / mL to 3 mg / mL.

[0024] In some embodiments, the mass ratio of the graphene substrate in the first slurry to the mass of the conductive material in the second slurry is (1-10):1.

[0025] In some embodiments, the application methods of the first slurry and the second slurry independently include at least one of spraying, scraping, transfer, and sputtering.

[0026] Secondly, this application provides a catalytic layer comprising alternating layers of graphene and a conductive support layer, wherein the graphene layers include a graphene-based catalyst, and the graphene-based catalyst includes a graphene substrate and a catalytic material supported on the surface of the graphene substrate.

[0027] Thirdly, this application provides a membrane electrode comprising a catalytic layer prepared by the method described in the first aspect, or a catalytic layer as described in the second aspect.

[0028] Fourthly, this application provides a fuel cell, the fuel cell including the membrane electrode assembly as described in the third aspect.

[0029] Compared with traditional technologies, this application has at least the following beneficial effects:

[0030] This application employs alternating coatings of graphene-based catalysts and conductive materials to form graphene layers and conductive support layers, respectively. The conductive materials are inserted between adjacent graphene layers to provide support, preventing stacking between adjacent graphene layers, effectively preserving the properties of graphene, and exposing the catalytic materials on the graphene substrate, thereby improving the utilization rate of catalytic materials in the graphene-based catalyst. Attached Figure Description

[0031] Figure 1 This is a cross-sectional schematic diagram of the catalyst layer provided in one embodiment of this application.

[0032] Among them, 10-catalyst layer; 11-graphene layer; 12-conductive support layer. Detailed Implementation

[0033] To facilitate understanding of this application, a more complete description will be provided below with reference to the accompanying drawings. Preferred embodiments of this application are shown in the drawings. However, this application can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided to provide a thorough and complete understanding of the disclosure of this application.

[0034] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs. The terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting of the application. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.

[0035] In this application, when numerical intervals (i.e., numerical ranges) are involved, unless otherwise specified, the distribution of selectable numerical values ​​within the numerical interval is considered continuous, and includes the two endpoints of the numerical interval (i.e., the minimum and maximum values), as well as every numerical value between these two endpoints. Unless otherwise specified, when a numerical interval refers only to integers within that numerical interval, it includes the two endpoint integers of the numerical range, as well as every integer between the two endpoints, which is equivalent to directly listing every integer. When multiple numerical ranges are provided to describe features or characteristics, these numerical ranges can be merged. In other words, unless otherwise specified, the numerical ranges disclosed in this application should be understood to include any and all subranges included therein. The "numerical value" in the numerical interval can be any quantitative value, such as a number, percentage, ratio, etc. The term "numerical interval" can be broadly included to include percentage intervals, ratio intervals, proportion intervals, etc.

[0036] In this application, "optionally," "optionally," and "optional" mean that something is optional, that is, it means that it is selected from either "with" or "without." If there are multiple "optional" entries in a technical solution, unless otherwise specified, and there are no contradictions or mutual constraints, each "optional" entry shall be independent.

[0037] In this application, the terms "first aspect," "second aspect," "third aspect," etc., are used for descriptive purposes only and should not be construed as indicating or implying relative importance or quantity, nor should they be construed as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first," "second," "third," etc., serve only as a non-exhaustive enumeration and should be understood not to constitute a closed limitation on quantity.

[0038] In traditional techniques, when preparing the catalytic layer of a membrane electrode using a graphene-based Pt catalyst, a layer-by-layer coating of catalytic slurry is employed. This leads to the stacking of graphene sheets, even forming graphite, which negates the superior properties of graphene. Consequently, the porosity of the catalytic layer and the utilization rate of Pt are reduced, resulting in poor conductivity, increased contact resistance, and increased mass transfer resistance, thus degrading the performance of the membrane electrode. In contrast, this application employs alternating coatings of graphene slurry and conductive materials. The conductive material serves as a supporting structure for adjacent graphene layers, preventing the stacking of graphene sheets and thereby improving catalytic activity.

[0039] A first aspect of this application provides a method for preparing a catalyst layer, the method comprising:

[0040] A first slurry is prepared, the first slurry comprising a graphene-based catalyst, the graphene-based catalyst comprising a graphene substrate and a catalytic material supported on the surface of the graphene substrate;

[0041] Prepare a second slurry, the second slurry comprising a conductive material;

[0042] The first slurry and the second slurry are alternately applied to the surface of the substrate to prepare a graphene layer and a conductive support layer, respectively. The graphene layer and the conductive support layer are alternately stacked to obtain the catalyst layer.

[0043] This application employs alternating coatings of a first slurry and a second slurry to form alternatingly stacked graphene layers and a conductive support layer. The conductive material in the conductive support layer is dispersed, allowing it to act as a structural support and preventing the stacking of graphene sheets between adjacent graphene layers. This effectively preserves the properties of graphene, fully exposes the catalytic material of the graphene-based catalyst, improves the utilization rate of the catalytic material, and ensures its full participation in the catalytic reaction. Furthermore, the conductive material increases the porosity between graphene layers and possesses good conductivity, thereby reducing the mass transfer resistance and contact resistance of the catalyst layer. Therefore, the preparation method of this application is simple, and the resulting catalyst layer structure is stable.

[0044] It should be noted that the substrate in this application can be reasonably selected according to actual needs. The substrate is only used as the base layer for preparing the catalyst layer. The substrate can be part of the product preparation or only used as an auxiliary layer for the preparation of the catalyst layer. After the catalyst layer is prepared, the catalyst layer is separated from the substrate.

[0045] In some embodiments, the thickness of each graphene layer is 10nm to 50nm, for example, 10nm, 15nm, 20nm, 23nm, 26nm, 29nm, 32nm, 35nm, 38nm, 41nm, 44nm, 47nm or 50nm.

[0046] This application controls the thickness of the graphene layer to ensure the loading of the catalytic material while minimizing graphene stacking and preserving the good properties of graphene. If the graphene layer thickness is relatively low, a low concentration of spray slurry will be used, which will exacerbate the swelling of the proton exchange membrane during the formation of the graphene layer and affect the membrane electrode performance. If the graphene layer thickness is relatively high, graphene stacking may occur, resulting in the loss of graphene properties and the formation of graphite.

[0047] In some embodiments, the thickness of each conductive support layer is 20nm to 100nm, for example, 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm or 100nm.

[0048] This application controls the thickness of the conductive support layer to ensure good support while effectively guaranteeing mass transfer between adjacent graphene layers. If the thickness of the conductive support layer is relatively low, the support effect of the conductive support layer is poor; if the thickness of the conductive support layer is relatively high, some conductive material may enter the graphene layer, thereby covering the catalytic material on the surface of the graphene substrate, affecting the catalytic performance. Moreover, the thickness of the catalytic layer is relatively thick, resulting in poor mass transfer performance.

[0049] It should be noted that the conductive material is distributed in a dispersed manner in the conductive support layer, which is sufficient to support the two adjacent graphene layers.

[0050] In some embodiments, the graphene substrate comprises ≤10 graphene layers, for example, 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10 layers.

[0051] In some embodiments, the graphene substrate comprises at least one selected from exfoliated graphene, graphene oxide, reduced graphene oxide, and doped graphene. Optionally, the doping element in the doped graphene comprises at least one selected from N, B, S, and P.

[0052] In some embodiments, the catalytic material includes a metal catalytic material.

[0053] Optionally, the catalytic material includes at least one of Pt and Pt alloys. Optionally, the Pt alloy includes at least one of PtNi alloy, PtCo alloy, and PtPd alloy.

[0054] In some embodiments, the mass percentage of the catalytic material in the graphene-based catalyst is 5% to 70%, for example, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, or 70%.

[0055] In some embodiments, the conductive material includes at least one of carbon black and carbon nanotubes.

[0056] In some embodiments, the particle size of the conductive material is 10nm to 50nm, for example, 10nm, 15nm, 20nm, 25nm, 30nm, 35nm, 40nm, 45nm or 50nm.

[0057] This application controls the particle size of the conductive material to achieve both good support and to avoid affecting the catalytic activity of the catalyst layer. If the particle size is relatively small, the resulting conductive support layer will be too dense, affecting mass transfer performance and thus hindering the catalytic effect of the catalyst material in the graphene layer. If the particle size is relatively large, the resulting conductive support layer will be thicker, resulting in a larger catalyst layer thickness under the same catalyst material loading, which is not conducive to mass transfer in the membrane electrode and fuel cell discharge process.

[0058] In some embodiments, the first slurry further includes a perfluorosulfonic acid resin.

[0059] Optionally, in the first slurry, the mass ratio of the graphene-based catalyst to the perfluorosulfonic acid resin is 1:(0.15-0.35), preferably 1:(0.25-0.3).

[0060] This application controls the mass ratio of graphene-based catalyst to perfluorosulfonic acid resin, which is beneficial for constructing proton channels in the catalyst layer, facilitating proton transport, and acting as both a proton transporter and a binder. If the amount of perfluorosulfonic acid resin added is high, it may coat the catalyst material, thereby blocking the pores and affecting the conductivity of the graphene layer, increasing the contact resistance and mass transfer overpotential of the catalyst layer. If the amount of perfluorosulfonic acid resin added is low, the graphene layer is unstable, easily detaches, and has a large proton transport resistance, resulting in poor stability and durability.

[0061] In some embodiments, the second slurry further includes a perfluorosulfonic acid resin.

[0062] Optionally, in the second slurry, the mass ratio of the conductive material to the perfluorosulfonic acid resin is 1:(0.15-0.35), preferably 1:(0.25-0.3).

[0063] This application controls the mass ratio of conductive material to perfluorosulfonic acid resin, which is beneficial for constructing proton channels in the catalyst layer, thus facilitating proton transport and serving as both a proton transporter and a binder.

[0064] In some embodiments, the perfluorosulfonic acid resin is added to the slurry as a 5% (w / w) perfluorosulfonic acid resin solution. This application does not impose specific requirements or limitations on the solvent in the perfluorosulfonic acid resin solution. Optionally, the solvent in the perfluorosulfonic acid resin solution is deionized water.

[0065] In some embodiments, the mass-volume concentration of the graphene-based catalyst in the first slurry is 0.1 mg / mL to 3 mg / mL, for example, 0.1 mg / mL, 0.3 mg / mL, 0.6 mg / mL, 0.9 mg / mL, 1.2 mg / mL, 1.5 mg / mL, 1.8 mg / mL, 2.1 mg / mL, 2.4 mg / mL, 2.7 mg / mL or 3.0 mg / mL, preferably 0.3 mg / mL to 1 mg / mL.

[0066] This application controls the concentration of graphene-based catalyst to ensure the efficiency and film formation speed of the graphene layer by spraying, and improves the problem of graphene layer stacking. If the concentration is relatively low, when forming a graphene layer on the proton exchange membrane, not only is the spraying efficiency low, but film formation is also difficult and the swelling phenomenon of the proton exchange membrane is aggravated. If the concentration is relatively high, graphene stacking may occur, thus failing to achieve the effect of conductive support.

[0067] In some embodiments, the mass-volume concentration of the conductive material in the second slurry is 0.1 mg / mL to 3 mg / mL, for example, 0.1 mg / mL, 0.3 mg / mL, 0.6 mg / mL, 0.9 mg / mL, 1.2 mg / mL, 1.5 mg / mL, 1.8 mg / mL, 2.1 mg / mL, 2.4 mg / mL, 2.7 mg / mL or 3.0 mg / mL, preferably 0.3 mg / mL to 1 mg / mL.

[0068] In some embodiments, the mass ratio of the graphene substrate in the first slurry to the mass of the conductive material in the second slurry is (1 to 10):1, for example, 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1 or 10:1, preferably 1:1.

[0069] In some embodiments, the application methods of the first slurry and the second slurry independently include at least one of spraying, scraping, transfer, and sputtering. Preferably, the application method of the first slurry includes ultrasonic spraying, and the application method of the second slurry includes ultrasonic spraying.

[0070] In some embodiments, the dispersion methods of the first slurry and the second slurry each independently include at least one of ultrasonic dispersion and magnetic stirring.

[0071] Optionally, the dispersion time of the first slurry is 1h to 7h, for example 1h, 2h, 3h, 4h, 5h, 6h or 7h, preferably 2h to 3h.

[0072] Optionally, the dispersion time of the second slurry is 1h to 7h, for example 1h, 2h, 3h, 4h, 5h, 6h or 7h, preferably 2h to 3h.

[0073] In some embodiments, the first slurry includes a first solvent. Optionally, the first solvent includes at least one selected from n-propanol, isopropanol, ethanol, n-butanol, tert-butanol, ethylene glycol, and ethoxyethanol.

[0074] In some embodiments, the second slurry includes a second solvent. Optionally, the second solvent includes at least one selected from n-propanol, isopropanol, ethanol, n-butanol, tert-butanol, ethylene glycol, and ethoxyethanol.

[0075] In some embodiments, after the first slurry and the second slurry are applied, a drying process is performed to form the graphene layer and the conductive support layer, respectively.

[0076] Optionally, the drying temperature is 25°C to 80°C, for example, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C or 80°C.

[0077] Optionally, the drying time is 0.5h to 2h, for example, 0.5h, 0.6h, 0.8h, 1.0h, 1.2h, 1.4h, 1.6h, 1.8h or 2.0h.

[0078] Exemplarily, a method for preparing the above-mentioned catalyst layer is provided, comprising:

[0079] To prepare a first slurry, a graphene-based catalyst, a perfluorosulfonic acid resin, and a first solvent are mixed and dispersed to obtain the first slurry. The concentration of the graphene-based catalyst in the first slurry is 0.1 mg / mL to 3 mg / mL, and the mass ratio of the graphene-based catalyst to the perfluorosulfonic acid resin is 1:(0.15 to 0.35).

[0080] To prepare a second slurry, conductive material, perfluorosulfonic acid resin, and a second solvent are mixed and dispersed. The mass ratio of conductive material to perfluorosulfonic acid resin is 1:(0.15~0.35), and the mass ratio of graphene substrate to conductive material in the second slurry is (1~10):1.

[0081] To prepare a catalyst layer, the first slurry is applied to the surface of a substrate and dried to form a graphene layer. A second slurry is applied to the surface of the graphene layer and dried to form a conductive support layer. The first and second slurries are applied alternately to form alternating graphene layers and conductive support layers on the surface of the substrate. The thickness of the conductive support layer is 20 nm to 100 nm, and the thickness of the graphene layer is 10 nm to 50 nm.

[0082] Secondly, this application provides a catalytic layer, such as Figure 1 As shown, the catalyst layer 10 includes alternatingly stacked graphene layers 11 and conductive support layers 12. The graphene layers 11 include a graphene-based catalyst, which includes a graphene substrate and a catalytic material supported on the surface of the graphene substrate.

[0083] In some embodiments, the thickness of each graphene layer is 10nm to 50nm, for example, 10nm, 15nm, 20nm, 23nm, 26nm, 29nm, 32nm, 35nm, 38nm, 41nm, 44nm, 47nm or 50nm.

[0084] In some embodiments, the thickness of each conductive support layer is 20nm to 100nm, for example, 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm or 100nm.

[0085] In some embodiments, the thickness of the catalyst layer is 2 μm to 6 μm, for example, 2.0 μm, 2.3 μm, 2.6 μm, 2.9 μm, 3.2 μm, 3.5 μm, 3.8 μm, 4.1 μm, 4.4 μm, 4.7 μm, 5.0 μm, 5.3 μm, 5.6 μm or 6.0 μm.

[0086] A third aspect of this application provides a membrane electrode comprising a catalytic layer prepared by the method described in the first aspect, or a catalytic layer as described in the second aspect.

[0087] In some embodiments, the membrane electrode includes a frame, a gas diffusion layer, the catalyst layer, and a proton exchange membrane, wherein the catalyst layer and the gas diffusion layer are sequentially stacked on both opposite surfaces of the proton exchange membrane.

[0088] Optionally, the total thickness of the catalyst layer in the membrane electrode is 5 μm to 8 μm, for example, 5.0 μm, 5.3 μm, 5.6 μm, 5.9 μm, 6.2 μm, 6.5 μm, 6.8 μm, 7.1 μm, 7.4 μm, 7.7 μm, or 8.0 μm. It should be noted that the total thickness of the catalyst layer in the membrane electrode refers to the sum of the thicknesses of the cathode catalyst layer and the anode catalyst layer in the membrane electrode.

[0089] A fourth aspect of this application provides a fuel cell, the fuel cell including a membrane electrode assembly as described in the third aspect.

[0090] Unless otherwise specified, all raw materials used in the following examples and comparative examples are commercially available products, and all operating steps and parameters not specifically described are conventional choices made by those skilled in the art.

[0091] In this graphene-based catalyst, the graphene substrate is 8-layer reduced graphene oxide, the catalyst material is Pt, and the graphene-based catalyst is denoted as Pt / G, where G represents the graphene substrate, C represents carbon black, the mass fraction of the perfluorosulfonic acid resin solution is 5%, and the solvent is deionized water.

[0092] Example 1

[0093] Take 25 mg Pt / G, 125 mg perfluorosulfonic acid resin solution and 50 mL isopropanol, and ultrasonically disperse for 2 h to obtain a first slurry with a Pt / G mass concentration of 0.5 mg / mL, and the mass percentage of Pt in Pt / G is 40%.

[0094] Take 15 mg of carbon black with an average particle size of 10 nm (mass ratio G:C = 1:1), 75 mg of perfluorosulfonic acid resin solution and 50 mL of isopropanol, and disperse them by ultrasonication for 2 h to obtain a second slurry with a carbon black mass concentration of 0.3 mg / mL.

[0095] A first slurry was ultrasonically sprayed onto one side of a proton exchange membrane and dried at 70°C to form a 20 nm thick graphene layer. A second slurry was then ultrasonically sprayed onto the graphene layer and dried at 70°C to form a 20 nm thick conductive support layer. The first and second slurries were alternately sprayed to form an anode catalyst layer consisting of alternating graphene and conductive support layers. The Pt loading in the anode catalyst layer was 0.1 mg Pt / cm³. 2 ;

[0096] Using the above method, a first slurry and a second slurry are alternately sprayed onto the other side surface of the proton exchange membrane to form a cathode catalyst layer composed of alternating graphene layers and conductive support layers. The Pt loading in the cathode catalyst layer is 0.2 mg Pt / cm³. 2 The membrane electrode catalytic layer was obtained.

[0097] Example 2

[0098] Take 25 mg Pt / G, 125 mg perfluorosulfonic acid resin solution and 50 mL isopropanol, and ultrasonically disperse for 2 h to obtain a first slurry with a Pt / G mass concentration of 0.5 mg / mL, and the mass proportion of Pt in Pt / G is 70%.

[0099] Take 2.5 mg of carbon black with an average particle size of 10 nm (mass ratio G:C = 3:1), 12.5 mg of perfluorosulfonic acid resin solution and 50 mL of isopropanol, and disperse them by ultrasonication for 2 h to obtain a second slurry with a carbon black mass concentration of 0.05 mg / mL.

[0100] A first slurry was ultrasonically sprayed onto one side of a proton exchange membrane and dried at 50°C to form a 20 nm thick graphene layer. A second slurry was then ultrasonically sprayed onto the graphene layer and dried at 50°C to form a 20 nm thick conductive support layer. The first and second slurries were alternately sprayed to form an anode catalyst layer consisting of alternating graphene and conductive support layers. The Pt loading in the anode catalyst layer was 0.1 mg Pt / cm³. 2 ;

[0101] Using the above method, a first slurry and a second slurry are alternately sprayed onto the other side surface of the proton exchange membrane to form a cathode catalyst layer composed of alternating graphene layers and conductive support layers. The Pt loading in the cathode catalyst layer is 0.2 mg Pt / cm³. 2 The membrane electrode catalytic layer was obtained.

[0102] Example 3

[0103] Take 25 mg Pt / G, 125 mg perfluorosulfonic acid resin solution and 50 mL ethanol, and ultrasonically disperse for 2 h to obtain a first slurry with a Pt / G mass concentration of 0.5 mg / mL, and the mass percentage of Pt in Pt / G is 5%.

[0104] Take 23.75 mg of carbon black with an average particle size of 25 nm (mass ratio G:C = 1:1), 118.75 mg of perfluorosulfonic acid resin solution and 50 mL of ethanol, and ultrasonically disperse for 2 h to obtain a second slurry with a carbon black mass concentration of 0.475 mg / mL.

[0105] A first slurry was ultrasonically sprayed onto one side of a proton exchange membrane and dried at 50°C to form a 50 nm thick graphene layer. A second slurry was then ultrasonically sprayed onto the graphene layer and dried at 50°C to form a 50 nm thick conductive support layer. The first and second slurries were alternately sprayed to form an anode catalyst layer consisting of alternating graphene and conductive support layers. The Pt loading in the anode catalyst layer was 0.1 mg Pt / cm³. 2 ;

[0106] Using the above method, a first slurry and a second slurry are alternately sprayed onto the other side surface of the proton exchange membrane to form a cathode catalyst layer composed of alternating graphene layers and conductive support layers. The Pt loading in the cathode catalyst layer is 0.2 mg Pt / cm³. 2 The membrane electrode catalytic layer was obtained.

[0107] Example 4

[0108] The catalyst layer was prepared according to the method in Example 1, except that the ultrasonic spraying parameters were adjusted to make the thickness of the graphene layer 5 nm.

[0109] Example 5

[0110] The catalyst layer was prepared according to the method of Example 1, except that the ultrasonic spraying parameters were adjusted to make the thickness of the graphene layer 80 nm.

[0111] Example 6

[0112] The catalyst layer was prepared according to the method of Example 1, except that the ultrasonic spraying parameters were adjusted so that the thickness of the conductive support layer was 10 nm.

[0113] Example 7

[0114] The catalyst layer was prepared according to the method of Example 1, except that the ultrasonic spraying parameters were adjusted so that the thickness of the conductive support layer was 150 nm.

[0115] Example 8

[0116] The catalyst layer was prepared according to the method of Example 1, except that the particle size of the carbon black was 5 nm.

[0117] Example 9

[0118] The catalyst layer was prepared according to the method of Example 1, except that the particle size of the carbon black was 60 nm.

[0119] Example 10

[0120] The catalyst layer was prepared according to the method of Example 1, except that the amount of perfluorosulfonic acid resin added to the first slurry was 100 mg.

[0121] Example 11

[0122] The catalyst layer was prepared according to the method of Example 1, except that the amount of perfluorosulfonic acid resin added to the first slurry was 200 mg.

[0123] Example 12

[0124] The catalyst layer was prepared according to the method of Example 1, except that the amount of perfluorosulfonic acid resin added to the second slurry was 30 mg.

[0125] Example 13

[0126] The catalyst layer was prepared according to the method of Example 1, except that the amount of perfluorosulfonic acid resin added to the second slurry was 120 mg.

[0127] Comparative Example 1

[0128] The catalyst layer was prepared according to the method of Example 1, except that the catalyst layer was formed by spraying only the first slurry.

[0129] Comparative Example 2

[0130] The catalyst layer was prepared according to the method of Example 1, except that 25 mg Pt / G, 15 mg carbon black, 200 mg perfluorosulfonic acid resin solution and 100 mL isopropanol were ultrasonically dispersed to obtain a mixed slurry, and the catalyst layer was formed by spraying the mixed slurry.

[0131] Test case

[0132] The membrane electrode catalytic layers prepared using the above examples and comparative examples were subjected to performance testing. The testing methods included:

[0133] The prepared membrane electrode catalytic layer was cut to a size of 6cm×6cm (of which the active area is 5cm×5cm), and hot-pressed with the frame material to obtain a five-in-one membrane electrode. The hot-pressing temperature was 110℃, the hot-pressing pressure was 30kN, and the hot-pressing time was 90s.

[0134] Gas diffusion layers with a size of 5.5cm × 5.5cm are attached to opposite two sides of the five-in-one membrane electrode to obtain a seven-in-one membrane electrode.

[0135] The seven-in-one membrane electrode was tested on a fuel cell fixture with a serpentine flow field. The cell temperature was 75°C, 100% humidified, the hydrogen and air side metering ratios were 1.2 / 2.5 (anode / cathode), and the back pressure was 100kPa / 100kPa (anode / cathode). The test results are shown in Table 1.

[0136] Table 1

[0137]

[0138]

[0139] As can be seen from the table above:

[0140] (1) Compared with Examples 4-5, Example 1 shows that the present application controls the thickness of the graphene layer, which can ensure the loading of the catalytic material and alleviate the stacking of graphene to the greatest extent, thus preserving the good properties of graphene. If the thickness of the graphene layer is relatively low, the concentration of the spray slurry is low, which aggravates the swelling of the proton exchange membrane during the formation of the graphene layer and affects the performance of the membrane electrode. If the thickness of the graphene layer is relatively high, graphene stacking may occur, thereby losing the properties of graphene and stacking to form graphite.

[0141] (2) Compared with Examples 6-7, Example 1 shows that by controlling the thickness of the conductive support layer, this application can effectively ensure the mass transfer between two adjacent graphene layers while ensuring a good support effect. If the thickness of the conductive support layer is relatively low, the support effect of the conductive support layer is poor. If the thickness of the conductive support layer is relatively high, some conductive material may enter the graphene layer and cover the catalytic material on the surface of the graphene substrate, affecting the catalytic performance. Moreover, the thickness of the catalytic layer is relatively thick, resulting in poor mass transfer performance.

[0142] (3) Compared with Examples 8-9, Example 1 controls the particle size of the conductive material, which can provide a good support effect without affecting the catalytic activity of the catalyst layer. If the particle size is relatively small, the formed conductive support layer is too dense, which affects the mass transfer performance and thus hinders the catalytic effect of the catalyst material in the graphene layer. If the particle size is relatively large, the formed conductive support layer is thicker, which leads to a larger catalyst layer thickness under the same catalyst material loading, which is not conducive to the mass transfer of the membrane electrode and fuel cell during discharge.

[0143] (4) Compared with Examples 10-11, it can be seen that by controlling the mass ratio of graphene-based catalyst to perfluorosulfonic acid resin in this application, it is beneficial to construct the proton channel of the catalyst layer, which is beneficial to proton transport and has the functions of both proton transport and binder. If the amount of perfluorosulfonic acid resin added is high, it may coat the catalyst material, thereby blocking the pores and affecting the conductivity of the graphene layer, increasing the contact resistance and mass transfer overpotential of the catalyst layer. If the amount of perfluorosulfonic acid resin added is low, the graphene layer is unstable and easy to fall off, and the proton transport resistance is large, resulting in poor stability and durability.

[0144] (5) Compared with Examples 12-13, Example 1 shows that by controlling the mass ratio of conductive material to perfluorosulfonic acid resin, this application can facilitate the construction of proton channels in the catalyst layer, which is beneficial to proton transport and has the functions of both proton transport and binder.

[0145] (6) Compared with Comparative Examples 1-2, Example 1 shows that the present application uses graphene-based catalyst and conductive material to be coated alternately, and graphene layer and conductive support layer are formed respectively. The conductive material is inserted between adjacent graphene layers to provide support force, avoids stacking between adjacent graphene layers, effectively preserves the properties of graphene, and thus improves the utilization rate of catalytic material in graphene-based catalyst.

[0146] Through the above embodiments and comparative examples, this application employs alternating coating of a first slurry and a second slurry, controlling the effective thickness to provide carbon black support between the graphene sheets. This avoids the stacking of graphene sheets or even their transformation into graphite caused by layer-by-layer coating, maximizing the utilization of graphene's excellent properties. Furthermore, the catalytic material particles loaded on the graphene can be fully exposed to participate in the catalytic reaction, improving catalytic material utilization and membrane electrode performance. Moreover, the conductive material layer between the graphene sheets provides a good mass transport channel for the catalytic layer, reducing mass transfer resistance and further enhancing membrane electrode performance. Simultaneously, the uniform distribution of the conductive material between the graphene sheets not only supports the sheets from stacking but also improves the conductivity of the catalytic layer, reducing contact resistance and contributing to improved membrane electrode performance. Furthermore, the method of this application is simple, and the resulting catalytic layer structure is stable, which is beneficial for membrane electrode performance.

[0147] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0148] The embodiments described above are merely illustrative of several implementation methods of this application, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of this application, and these all fall within the protection scope of this application. Therefore, the protection scope of this invention patent should be determined by the appended claims.

Claims

1. A method for preparing a catalyst layer, characterized in that, The preparation method includes: A first slurry is prepared, the first slurry comprising a graphene-based catalyst, the graphene-based catalyst comprising a graphene substrate and a catalytic material supported on the surface of the graphene substrate; A second slurry is prepared, the second slurry being composed of a conductive material, a perfluorosulfonic acid resin, and a second solvent. The conductive material includes at least one of carbon black and carbon nanotubes, and the particle size of the conductive material is 10 nm to 50 nm. The first slurry and the second slurry are alternately applied to the surface of the substrate to prepare a graphene layer and a conductive support layer, respectively. The graphene layer and the conductive support layer are alternately stacked to obtain the catalyst layer. The conductive material is dispersed in the conductive support layer to support the two adjacent graphene layers. The thickness of each graphene layer is 10nm~50nm, and the thickness of each conductive support layer is 20nm~100nm.

2. The method for preparing the catalyst layer as described in claim 1, characterized in that, The graphene-based catalyst satisfies at least one of the following conditions: (1) The graphene substrate comprises ≤10 graphene layers; (2) The graphene substrate includes at least one of exfoliated graphene, graphene oxide, reduced graphene oxide and doped graphene; (3) The catalytic material includes metal catalytic materials; (4) The mass percentage of the catalytic material in the graphene-based catalyst is 5% to 70%.

3. The method for preparing the catalyst layer as described in claim 2, characterized in that, The catalytic material includes at least one of Pt and Pt alloys.

4. The method for preparing the catalyst layer as described in claim 1, characterized in that, The first slurry also includes perfluorosulfonic acid resin.

5. The method for preparing the catalyst layer as described in claim 4, characterized in that, In the first slurry, the mass ratio of the graphene-based catalyst to the perfluorosulfonic acid resin is 1:(0.15~0.35).

6. The method for preparing the catalyst layer as described in claim 1, characterized in that, In the second slurry, the mass ratio of the conductive material to the perfluorosulfonic acid resin is 1:(0.15~0.35).

7. The method for preparing the catalyst layer according to any one of claims 1-6, characterized in that, The preparation method satisfies at least one of the following conditions: (1) The mass-volume concentration of the graphene-based catalyst in the first slurry is 0.1 mg / mL to 3 mg / mL; (2) The mass-volume concentration of the conductive material in the second slurry is 0.1 mg / mL to 3 mg / mL; (3) The mass ratio of the graphene substrate in the first slurry to the mass of the conductive material in the second slurry is (1~10):1; (4) The application methods of the first slurry and the second slurry independently include at least one of the following: spraying, scraping, transfer and sputtering.

8. A catalyst layer, characterized in that, The catalyst layer includes alternating layers of graphene and a conductive support layer. The graphene layers include a graphene-based catalyst, which includes a graphene substrate and a catalytic material supported on the surface of the graphene substrate. The conductive support layer is composed of a conductive material and a perfluorosulfonic acid resin. The conductive material is dispersed in the conductive support layer to support the two adjacent graphene layers. The conductive material includes at least one of carbon black and carbon nanotubes, and the particle size of the conductive material is 10 nm to 50 nm. The thickness of each graphene layer is 10nm~50nm, and the thickness of each conductive support layer is 20nm~100nm.

9. A membrane electrode, characterized in that, The membrane electrode comprises a catalytic layer prepared by the method described in any one of claims 1-7, or a catalytic layer as described in claim 8.

10. A fuel cell, characterized in that, The fuel cell includes the membrane electrode assembly as described in claim 9.

Citation Information

Patent Citations

  • Catalytic layer with multi-layer structure of fuel cell and preparation method thereof

    CN108063267A