Halide solid state electrolyte, method of making and use thereof

CN116581367BActive Publication Date: 2026-11-20CHINA FAW CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202211520741.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-30
Publication Date
2026-11-20
Estimated Expiration
2042-11-30

AI Technical Summary

Technical Problem

[0005]本发明的主要目的在于提供一种卤化物固态电解质、其制备方法及应用,以解决现有技术中卤化物电解质无法兼顾良好的湿度稳定性和离子电导率,导致锂离子电池能量密度较低的问题

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116581367B_ABST
    Figure CN116581367B_ABST
Patent Text Reader

Abstract

The application provides a halide solid-state electrolyte, a preparation method and application thereof. The chemical formula of the halide solid-state electrolyte is Li 3‑x Cu x MX 6‑x A x wherein M is selected from In, Sc or Y, X is selected from Cl, Br or I, A is a pseudo-halide anion, and 0.01<=x<=1. The organic-inorganic hybrid lithium ion battery halide solid-state electrolyte of the application introduces a pseudo-halide anion into halogen sites in the halide solid-state electrolyte, greatly reduces the humidity instability caused by halide ions, greatly enhances the humidity stability of the halide electrolyte, and still has a relatively high room-temperature ionic conductivity; therefore, the halide electrolyte is easier to be pressed into a sheet in an environment with relatively high humidity, the assembly of the all-solid-state battery is more convenient, the energy density of the all-solid-state battery can be greatly improved, and the application prospect of the all-solid-state battery is good in large-scale commercialization and practicalization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of lithium-ion battery technology, and more specifically, to a halide solid electrolyte, its preparation method, and its application. Background Technology

[0002] Lithium-ion batteries, as simple and efficient energy storage systems, have received significant attention at all levels of modern energy technology development. However, traditional liquid batteries suffer from the toxicity and flammability of organic electrolytes, and lithium dendrites penetrating the separator can cause internal short circuits, posing safety hazards such as flammability and explosion. Therefore, developing safe, high-performance, and low-cost all-solid-state batteries by replacing the electrolyte and separator in traditional lithium-ion batteries with solid-state electrolytes has become a major challenge in the global energy field. Compared to oxide solid-state electrolytes, sulfide solid-state electrolytes and halide solid-state electrolytes have attracted widespread attention from researchers due to their excellent room-temperature ionic conductivity and low synthesis temperature.

[0003] However, due to the poor air stability of sulfide electrolytes, they easily generate harmful gases such as hydrogen sulfide during use and recycling, thus affecting their practical applications. Halide electrolytes, on the other hand, possess both high ionic conductivity and environmental friendliness, making them a highly promising solid electrolyte material for future commercial production and use. The development of halide electrolytes has gradually emerged in recent years. However, existing halide electrolytes, due to the large amount of metal halides used in their synthesis, exhibit strong hygroscopic and deliquescent properties, resulting in a significant decrease in ionic conductivity. This is a problem faced by the application of halide solid electrolytes.

[0004] Patent CN111106246A discloses a solar cell based on a pseudohalide perovskite containing thiocyanate ions, employing a mixed-cation pseudohalide perovskite FA. x K y Pb(SCN)2I, where x = (0.97~0.99), y = (0.01~0.03), and x+y = 1, is not suitable for lithium-ion batteries and cannot meet the requirement that the electrolyte in the lithium-ion battery system needs to have high lithium-ion conductivity. Summary of the Invention

[0005] The main objective of this invention is to provide a halide solid electrolyte, its preparation method and application, in order to solve the problem that halide electrolytes in the prior art cannot achieve both good humidity stability and ionic conductivity, resulting in low energy density of lithium-ion batteries.

[0006] To achieve the above objectives, according to one aspect of the present invention, a halide solid electrolyte with the chemical formula Li is provided. 3-x Cu x MX6-x A x Where M is selected from In, Sc or Y, X is selected from Cl, Br or I, A is a pseudohalo anion, and 0.01≤x≤1.

[0007] Furthermore, the pseudohalogen anion is selected from SCN. - PF6 - Or BF4 - Preferably, the halide solid electrolyte is Li. 3- x Cu x InCl 6-x SCN x and / or Li 3-x Cu x ScCl 6-x SCN x .

[0008] Furthermore, the humidity stability of the halide solid electrolyte increases with increasing x; preferably, the ionic conductivity of the halide solid electrolyte is 10. -3 ~10 -5 S / cm.

[0009] According to another aspect of the present invention, a method for preparing the above-mentioned halide solid electrolyte is provided, comprising the following steps: step S1, mixing a lithium source, a copper source, a metal halide and a compound containing a pseudohalide anion under an inert atmosphere to obtain a mixed raw material; step S2, vacuum sintering the mixed raw material to obtain a halide solid electrolyte.

[0010] Furthermore, step S1 also includes a step of ball milling the mixed raw materials.

[0011] Furthermore, the ball milling process is carried out at a speed of 500–700 rpm for 12–36 h, with a ball-to-material ratio of (15–25):1.

[0012] Furthermore, the vacuum sintering process is carried out at a temperature of 350–450°C for 8–16 hours.

[0013] Furthermore, the lithium source is one or more of LiCl, LiBr, and LiI; and / or the copper source is CuSCN; and / or the metal halide is one or more of InCl3, ScCl3, and YCl3; and / or the pseudohalide anion compound is one or more of LiSCN, CuSCN, and LiSCN·xH2O.

[0014] According to another aspect of the present invention, the application of the halide solid electrolyte of the present invention in lithium-ion batteries is provided.

[0015] According to another aspect of the present invention, a lithium-ion battery is provided, comprising the halide solid electrolyte of the present invention.

[0016] The organic-inorganic hybrid lithium-ion battery halide solid electrolyte of this invention contains pseudohalogen anions. By introducing pseudohalogen anions into the halogen sites of the halide solid electrolyte, the humidity instability caused by halide ions is significantly reduced, and the humidity stability of the halide electrolyte is greatly enhanced. The room temperature ionic conductivity is still relatively high. As a result, the halide electrolyte is easier to press into sheets in high humidity environments, which facilitates the assembly of all-solid-state batteries and can greatly improve the energy density of all-solid-state batteries. It has good prospects for large-scale commercialization and practical application. Attached Figure Description

[0017] The accompanying drawings, which form part of this application, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an undue limitation of the invention. In the drawings:

[0018] Figure 1 The XRD test results of Li2CuInCl5SCN material according to Embodiment 1 of the present invention are shown;

[0019] Figure 2 The room temperature AC impedance test results of Li2CuInCl5SCN material according to Embodiment 1 of the present invention are shown;

[0020] Figure 3 The sheet-forming effect of Li2CuInCl5SCN material after being placed in air according to Embodiment 1 of the present invention is shown;

[0021] Figure 4 The effect of placing the Li3InCl6 material in air according to Comparative Example 1 is shown; and

[0022] Figure 5 Li is shown in Embodiment 3 according to the present invention. 2.99 Cu 0.01 InCl 5.99 SCN 0.01 Results of AC impedance testing at room temperature for materials. Detailed Implementation

[0023] It should be noted that, unless otherwise specified, the embodiments and features described in this application can be combined with each other. The present invention will now be described in detail with reference to the accompanying drawings and embodiments.

[0024] It should be noted that the room temperature in this invention refers to an ambient temperature of 20–30°C.

[0025] Terminology Explanation:

[0026] Pseudohalo anions: Anions that have properties similar to halide ions, such as ionic radius.

[0027] As described in the background section of this invention, existing technologies suffer from the problem that halide electrolytes cannot simultaneously achieve good humidity stability and ionic conductivity, resulting in low energy density in lithium-ion batteries. To address this issue, in a typical embodiment of this invention, a halide solid electrolyte with the chemical formula Li is provided. 3-x Cu x MX 6-x A x Where M is selected from In, Sc or Y, X is selected from Cl, Br or I, A is a pseudohalo anion, and 0.01≤x≤1.

[0028] The organic-inorganic hybrid lithium-ion battery halide solid electrolyte of this invention uses pseudohalide anions to replace halide ions. Compared with halide ions, the compounds formed by pseudohalide ions are less prone to hygroscopicity and deliquescence, thus significantly reducing the humidity instability caused by halide ions. This results in excellent long-term and humidity stability of the electrolyte, making it easier to form sheets and maintain a thin sheet state. Furthermore, by controlling the amount of pseudohalide anion substitution between 0.01 and 1, the ionic conductivity is maintained within a high range to meet practical application requirements. In addition, Cu is also used. 2+ Ions partially substitute Li + Li is formed by the substitution of lower valence states by higher valence states. + The transport vacancies are beneficial for the internal Li of the material. + The transport properties can be improved, and the ionic conductivity can be appropriately increased. The thin-film electrolyte of this invention, which simultaneously exhibits good humidity stability and ionic conductivity, can be used in the assembly of all-solid-state batteries, thereby increasing the energy density of all-solid-state batteries. X is preferably Cl; the ionic conductivity of the Li3MCl6 system is higher than that of Li3MBr6 and Li3MI6, making doping modification of Cl ions by pseudohalide anion substitution more practically significant.

[0029] In a preferred embodiment, the pseudohalide anion is selected from SCN. - PF6 - Or BF4 - SCN is preferred. - The aforementioned anions possess properties such as ionic radii more similar to halide ions. Replacing halide ions with these anions can improve the humidity stability of the material while maintaining the halide electrolyte's good ionic conductivity and environmental friendliness. Preferably, the halide solid electrolyte is Li. 3-x Cu x InCl 6-x SCN x and / or Li 3-x Cu xScCl 6-x SCN x It can inherit the high ionic conductivity of Li3InCl6 and Li3ScCl6, which is more practical.

[0030] As mentioned above, the introduction of pseudohalogen anions can enhance the humidity stability of halide electrolytes. During the research process, the applicant discovered that in a preferred embodiment, the humidity stability of the halide solid electrolyte increases with increasing x. While increasing the substitution amount x improves air stability and sheet formation, it slightly decreases the ionic conductivity of the material itself. A substitution amount exceeding 1 significantly reduces the ionic conductivity. Therefore, only when the substitution amount is controlled within the range of 0.01 to 1 can the ionic conductivity be maintained at 10. -3 ~10 -5 The conductivity (S / cm) is between 10 and 1000, ensuring the material maintains both good ionic conductivity and humidity stability for practical applications. Preferably, the halide solid electrolyte is monoclinic, belonging to the C2 / m space group, and has an ionic conductivity of 10. -3 ~10 -5 With an S / cm ratio, it performs better as an electrolyte for lithium-ion batteries.

[0031] In another typical embodiment of the present invention, a method for preparing the above-mentioned halide solid electrolyte is also provided, comprising the following steps: Step S1, mixing a lithium source, a copper source, a metal halide and a compound containing pseudohalide anions under an inert atmosphere to obtain a mixed raw material; Step S2, vacuum sintering the mixed raw material to obtain a halide solid electrolyte.

[0032] This invention successfully synthesizes a novel halide solid electrolyte containing pseudohalide anions via solid-state sintering, enriching the existing halide solid electrolyte material system. The preparation method is simple and easy to control, and the resulting halide electrolyte exhibits significantly improved sheet-forming ability, making it easy to press into sheets in higher humidity air for use as an electrolyte material in all-solid-state batteries, thus facilitating the assembly, processing, and recycling of all-solid-state batteries. The preparation process must be carried out under an inert gas atmosphere, such as argon, helium, or nitrogen; otherwise, the raw materials will absorb moisture from the air, which cannot be removed during sintering, leading to synthesis failure.

[0033] To further ensure a more uniform mixing of the raw materials, in a preferred embodiment, step S1 further includes a step of ball milling the mixed raw materials.

[0034] Specifically, in a preferred embodiment, the ball milling process is carried out at a rotation speed of 500-700 rpm for 12-36 hours, and the ball-to-material ratio is (15-25):1.

[0035] Vacuum sintering can be achieved by placing the mixed raw materials in a quartz glass tube, evacuating the quartz glass tube, melting the center of the quartz glass tube at 2000°C, sealing the powder at the bottom of the quartz tube, and then sending it into a muffle furnace for sintering. In a preferred embodiment, the temperature of the vacuum sintering process is 350–450°C, and the time is 8–16 hours, thereby allowing the raw materials to react more fully.

[0036] To further reduce costs, in a preferred embodiment, the lithium source is one or more of LiCl, LiBr, and LiI; and / or the copper source is CuSCN; and / or the metal halide is one or more of InCl3, ScCl3, and YCl3; and / or the pseudohalide anion compound is one or more of LiSCN, CuSCN, and LiSCN·xH2O. The amount of the above raw materials added should conform to the chemical formula of the halide solid electrolyte.

[0037] In another typical embodiment of the present invention, the application of the above-mentioned halide solid electrolyte in lithium-ion batteries is also provided. This is due to the substitution of halide ions with pseudohalide anions and the use of Cu... 2+ Li ions partially substituted + The electrolyte of this invention has excellent long-term stability, humidity stability and room temperature ionic conductivity, and significantly improved sheet formation capability. When applied to lithium-ion batteries, it is beneficial for the assembly, processing and recycling of all-solid-state lithium-ion batteries.

[0038] In another typical embodiment of the present invention, a lithium-ion battery is also provided, comprising the halide solid electrolyte of the present invention, which has high humidity stability and ionic conductivity, and better energy density.

[0039] The present application will be further described in detail below with reference to specific embodiments, which should not be construed as limiting the scope of protection claimed in the present application.

[0040] Example 1

[0041] (1) Weigh LiCl, CuSCN and InCl3 in a molar ratio of 2:1:1 to make a total mass of 1g. Place the weighed sample in a ball mill jar filled with argon gas and ball mill at 600rpm for 24h. During the ball milling process, ensure that the ball-to-material ratio is controlled at 20:1.

[0042] (2) The powder after ball milling is taken out from the ball milling jar and stored in an argon glove box. The powder is placed in a quartz glass tube under argon atmosphere. The quartz glass tube is evacuated and melted in the middle of the quartz glass tube at 2000℃. The powder is then sealed at the bottom of the quartz tube.

[0043] (3) The quartz tube was transferred to a muffle furnace and sintered at 400°C for 12 hours. After naturally cooling to room temperature, the quartz tube was removed and transferred to an argon glove box to remove the material. The material was then ground into powder until uniform, and Li2Cu1InCl5SCN was obtained.

[0044] Example 2

[0045] (1) Weigh LiCl, CuSCN and InCl3 in a molar ratio of 2.5:0.5:1 to make a total mass of 1g. Place the weighed sample in a ball mill jar filled with argon gas and ball mill at 600rpm for 24h. During the ball milling process, ensure that the ball-to-material ratio is controlled at 20:1.

[0046] (2) The powder after ball milling is taken out from the ball milling jar and stored in an argon glove box. The powder is placed in a quartz glass tube under argon atmosphere. The quartz glass tube is evacuated and melted in the middle of the quartz glass tube at 2000℃. The powder is then sealed at the bottom of the quartz tube.

[0047] (3) The quartz tube was transferred to a muffle furnace and sintered at 400℃ for 12 hours. After naturally cooling to room temperature, the quartz tube was removed and transferred to an argon glove box to remove the material. The material was then ground into powder until homogeneous to obtain Li. 2.5 Cu 0.5 InCl 5.5 SCN 0.5 .

[0048] Example 3

[0049] (1) Weigh LiCl, CuSCN and InCl3 in a molar ratio of 2.99:0.01:1 to make a total mass of 1g. Place the weighed sample in a ball mill jar filled with argon gas and ball mill at 600rpm for 24h. The ball-to-material ratio during the ball milling process is controlled at 20:1.

[0050] (2) The powder after ball milling is taken out from the ball milling jar and stored in an argon glove box. The powder is placed in a quartz glass tube under argon atmosphere. The quartz glass tube is evacuated and melted in the middle of the quartz glass tube at 2000℃. The powder is then sealed at the bottom of the quartz tube.

[0051] (3) The quartz tube was transferred to a muffle furnace and sintered at 400℃ for 12 hours. After naturally cooling to room temperature, the quartz tube was removed and transferred to an argon glove box to remove the material. The material was then ground into powder until homogeneous to obtain Li. 2.99 Cu 0.01 InCl 5.99 SCN 0.01 .

[0052] Example 4

[0053] (1) Weigh LiCl, CuBF4 and ScCl3 in a molar ratio of 2:1:1 to make a total mass of 1g. Place the weighed sample in a ball mill jar filled with argon gas and ball mill at 600rpm for 24h. During the ball milling process, ensure that the ball-to-material ratio is controlled at 20:1.

[0054] (2) The powder after ball milling is taken out from the ball milling jar and stored in an argon glove box. The powder is placed in a quartz glass tube under argon atmosphere. The quartz glass tube is evacuated and melted in the middle of the quartz glass tube at 2000℃. The powder is then sealed at the bottom of the quartz tube.

[0055] (3) The quartz tube was transferred to a muffle furnace and sintered at 400°C for 12 hours. After naturally cooling to room temperature, the quartz tube was removed and transferred to an argon glove box to remove the material. The material was then ground into powder until uniform to obtain Li2Cu1ScCl5BF4.

[0056] Example 5

[0057] (1) Weigh LiCl, CuSCN and YCl3 in a molar ratio of 2:1:1 to make a total mass of 1g. Place the weighed sample in a ball mill jar filled with argon gas and ball mill at 600rpm for 24h. During the ball milling process, ensure that the ball-to-material ratio is controlled at 20:1.

[0058] (2) The powder after ball milling is taken out from the ball milling jar and stored in an argon glove box. The powder is placed in a quartz glass tube under argon atmosphere. The quartz glass tube is evacuated and melted in the middle of the quartz glass tube at 2000℃. The powder is then sealed at the bottom of the quartz tube.

[0059] (3) The quartz tube was transferred to a muffle furnace and sintered at 400°C for 12 hours. After naturally cooling to room temperature, the quartz tube was removed and transferred to an argon glove box to remove the material. The material was then ground into powder until uniform to obtain Li2Cu1YCl5SCN.

[0060] Example 6

[0061] (1) Weigh LiCl, CuSCN and InCl3 in a molar ratio of 2:1:1 to make a total mass of 1g. Place the weighed sample in a ball mill jar filled with argon gas and ball mill at 500rpm for 36h. During the ball milling process, ensure that the ball-to-material ratio is controlled at 25:1.

[0062] (2) The powder after ball milling is taken out from the ball milling jar and stored in an argon glove box. The powder is placed in a quartz glass tube under argon atmosphere. The quartz glass tube is evacuated and melted in the middle of the quartz glass tube at 2000℃. The powder is then sealed at the bottom of the quartz tube.

[0063] (3) The quartz tube was transferred to a muffle furnace and sintered at 350°C for 16 hours. After naturally cooling to room temperature, the quartz tube was removed and transferred to an argon glove box to remove the material. The material was then ground into powder until uniform, and Li2Cu1InCl5SCN was obtained.

[0064] Example 7

[0065] (1) Weigh LiCl, CuSCN and InCl3 in a molar ratio of 2:1:1 to make a total mass of 1g. Place the weighed sample in a ball mill jar filled with argon gas and ball mill at 700rpm for 12h. During the ball milling process, ensure that the ball-to-material ratio is controlled at 15:1.

[0066] (2) The powder after ball milling is taken out from the ball milling jar and stored in an argon glove box. The powder is placed in a quartz glass tube under argon atmosphere. The quartz glass tube is evacuated and melted in the middle of the quartz glass tube at 2000℃. The powder is then sealed at the bottom of the quartz tube.

[0067] (3) The quartz tube was transferred to a muffle furnace and sintered at 450°C for 8 hours. After naturally cooling to room temperature, the quartz tube was removed and transferred to an argon glove box to remove the material. The material was then ground into powder until uniform, and Li2Cu1InCl5SCN was obtained.

[0068] Comparative Example 1

[0069] LiCl and InCl3 were weighed in a molar ratio of 3:1 to make a total mass of 1g. The weighed sample was placed in a ball mill jar filled with argon gas and ball milled at 600rpm for 24h. During the ball milling process, the ball-to-material ratio was controlled at 20:1.

[0070] After ball milling, the powder is removed from the ball mill jar and stored in an argon glove box. The powder is then placed in a quartz glass tube under an argon atmosphere. The quartz glass tube is then evacuated and melted in the middle at 2000℃, sealing the powder at the bottom of the quartz tube.

[0071] The quartz tube was transferred to a muffle furnace and sintered at 400°C for 12 hours. After naturally cooling to room temperature, the quartz tube was removed and transferred to an argon glove box to remove the material. The material was then ground into powder until homogeneous to obtain Li3InCl6.

[0072] Comparative Example 2

[0073] (1) Weigh LiCl, CuSCN and InCl3 in a molar ratio of 1:2:1 to make a total mass of 1g. Place the weighed sample in a ball mill jar filled with argon gas and ball mill at 600rpm for 24h. During the ball milling process, ensure that the ball-to-material ratio is controlled at 20:1.

[0074] (2) The powder after ball milling is taken out from the ball milling jar and stored in an argon glove box. The powder is placed in a quartz glass tube under argon atmosphere. The quartz glass tube is evacuated and melted in the middle of the quartz glass tube at 2000℃. The powder is then sealed at the bottom of the quartz tube.

[0075] (3) The quartz tube was transferred to a muffle furnace and sintered at 400°C for 12 hours. After naturally cooling to room temperature, the quartz tube was removed and transferred to an argon glove box to remove the material. The material was then ground into powder until uniform, and Li1Cu2InCl4SCN2 was obtained.

[0076] test:

[0077] The halide solid electrolyte material of Example 1 was subjected to XRD and room temperature AC impedance testing; the XRD results are as follows: Figure 1 As shown, this result indicates that the Li2Cu1InCl5SCN synthesized in Example 1 has the same space group structure as Li3InCl6, belonging to the monoclinic crystal system, space group C2 / m; the AC impedance test results are as follows. Figure 2 As shown. After being placed in an air environment for a period of time, 40mg of the material was placed in a 10mm diameter tableting mold and pressed into a tablet at 300MPa for 1 minute. The tablet was successfully removed, and the tablet appearance was as shown. Figure 3 As shown, the sheet has a thickness of 0.2 mm. The sheet formation effect of Examples 2 to 7 is similar to that of Example 1.

[0078] The halide solid electrolyte material of Comparative Example 1 was transferred to the same air environment as in Example 1 and observed for the same period of time. It was found that it had become hygroscopic and viscous, and could not be pressed into sheets. Figure 4 As shown.

[0079] The halide solid electrolyte material of Example 3 was subjected to room temperature AC impedance testing, and the results are as follows: Figure 5 As shown.

[0080] The ionic conductivity of Examples 1 to 7 and Comparative Examples 1 to 2 is shown in Table 1.

[0081] Test method:

[0082] Room temperature AC impedance testing, ionic conductivity: impedance / gain-phase analyzer.

[0083] Table 1

[0084] Ionic conductivity S / cm Example 1 <![CDATA[2.0×10 -5 ]]> Example 2 <![CDATA[6.0×10 -4 ]]> Example 3 <![CDATA[2.0×10 -3 ]]> Example 4 <![CDATA[1.9×10 -5 ]]> Example 5 <![CDATA[1.9×10 -5 ]]> Example 6 <![CDATA[1.8×10 -5 ]]> Example 7 <![CDATA[1.8×10 -5 ]]> Comparative Example 1 <![CDATA[3.0×10 -3 ]]> Comparative Example 2 <![CDATA[2.0×10 -6 ]]>

[0085] As can be seen from the above, compared with the comparative examples, the organic-inorganic hybrid lithium-ion battery halide solid electrolytes of the various embodiments of the present invention significantly reduce the humidity instability caused by halide ions by introducing pseudohalo anions into the halogen sites of the halide solid electrolyte, greatly enhancing the humidity stability of the halide electrolyte. At the same time, by controlling the amount of pseudohalo anion substitution, a high room temperature ionic conductivity can be achieved. As a result, the halide electrolyte is easier to press into sheets in high humidity environments, which facilitates the assembly of all-solid-state batteries and can greatly improve the energy density of all-solid-state batteries.

[0086] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A halide solid electrolyte, characterized in that, The chemical formula of the halide solid electrolyte is Li 3-x Cu x MX 6- x A x Where M is selected from In, Sc or Y, X is selected from Cl, Br or I, A is a pseudohalo anion, and 0.01≤x≤1.

2. The halide solid electrolyte according to claim 1, characterized in that, The pseudohalogen anion is selected from SCN. - PF6 - Or BF4 - .

3. The halide solid electrolyte according to claim 2, characterized in that, The halide solid electrolyte is Li 3-x Cu x InCl 6-x SCN x and / or Li 3-x Cu x ScCl 6-x SCN x .

4. The halide solid electrolyte according to claim 1 or 2, characterized in that, The humidity stability of the halide solid electrolyte increases with increasing x.

5. The halide solid electrolyte according to claim 4, characterized in that, The ionic conductivity of the halide solid electrolyte is 10. -3 ~10 -5 S / cm.

6. The method for preparing the halide solid electrolyte according to any one of claims 1 to 5, characterized in that, Includes the following steps: Step S1: Under an inert atmosphere, a lithium source, a copper source, a metal halide, and a compound containing pseudohalide anions are mixed to obtain a mixed raw material; Step S2: Vacuum sinter the mixed raw materials to obtain the halide solid electrolyte.

7. The preparation method according to claim 6, characterized in that, Step S1 further includes a step of ball milling the mixed raw materials.

8. The preparation method according to claim 7, characterized in that, The ball milling process is carried out at a speed of 500-700 rpm for 12-36 hours, with a ball-to-material ratio of (15-25):

1.

9. The preparation method according to claim 6, characterized in that, The vacuum sintering process is carried out at a temperature of 350~450℃ for 8~16 hours.

10. The preparation method according to claim 6, characterized in that, The lithium source is one or more of LiCl, LiBr, and LiI; and / or the copper source is CuSCN; and / or the metal halide is one or more of InCl3, ScCl3, and YCl3; and / or the pseudohalide-containing anion compound is one or more of LiSCN, CuSCN, and LiSCN·xH2O.

11. The application of the halide solid electrolyte according to any one of claims 1 to 5 in lithium-ion batteries.

12. A lithium-ion battery, characterized in that, Includes the halide solid electrolyte according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Solar cell based on thiocyanate ion-containing pseudohalide perovskite

    CN111106246A

  • Anion-modified solid lithium battery and preparation method

    CN109546227A

  • Modified microcrystalline glassy sulfide solid-state degradation substance as well as preparation method and application thereof

    CN115312844A