A diaphragm and a secondary battery

By introducing ceramic and adhesive layers into the lithium-ion battery separator and optimizing the pore structure with functional materials, the problems of thermal stability and uneven electrolyte transport at high temperatures were solved, thereby improving the safety and performance of the battery.

CN116581481BActive Publication Date: 2026-11-24SUNWODA MOBILITY ENERGY TECHNOLOGY CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202310766641.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-26
Publication Date
2026-11-24
Estimated Expiration
2043-06-26

AI Technical Summary

Technical Problem

Traditional lithium-ion battery separators have poor thermal stability under high-temperature conditions and insufficient liquid absorption and retention capacity, which limits battery safety and performance. Furthermore, uneven electrolyte transport affects the manufacturing and use of lithium-ion batteries.

Method used

The membrane design incorporates a ceramic layer and an adhesive layer, with a coating porosity of 35-65% and an areal density of 4-15 g/m². It combines functional materials such as kapok, sponge, and coral to control the pore volume ratio at (0.01-0.4):(0.01-0.7):(0.01-0.6), and uses a polyvinylidene fluoride adhesive layer to improve the bonding strength.

Benefits of technology

Significantly improves the thermal stability and electrolyte wettability of the separator, ensures homogeneous electrolyte transport, enhances battery safety and performance, reduces capacity loss and overcharge risk, and achieves high power density and energy density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004308458770000121
    Figure BDA0004308458770000121
  • Figure BDA0004308458770000131
    Figure BDA0004308458770000131
  • Figure BDA0004308458770000141
    Figure BDA0004308458770000141
Patent Text Reader

Abstract

This invention relates to the field of lithium-ion battery technology, and more particularly to a separator and a secondary battery. The separator provided by this invention includes a base film and a coating disposed on at least one surface of the base film. The coating includes a ceramic layer and a binder layer. The ceramic layer includes ceramic particles, a binder, and functional materials. The porosity of the coating of the separator is 35-65%, and the areal density of the coating is 4-15 g / m³. 2 The separator of this invention exhibits excellent thermal stability, with minimal thermal shrinkage in both the MD and TD directions under high-temperature conditions. It also demonstrates good electrolyte absorption and retention capabilities, as well as excellent wettability, ensuring rapid and homogeneous lithium-ion transport during the reaction process. Furthermore, this separator reduces capacity loss and the risk of localized overcharging, thereby protecting the secondary battery. Using the separator of this invention is beneficial for improving the power density, energy density, and safety of secondary batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of secondary battery technology, and in particular to a separator and a secondary battery. Background Technology

[0002] With the advancement of social technology, lithium-ion batteries, as a highly efficient energy storage technology, are widely used in consumer electronics, electric vehicles, and large-scale energy storage equipment. At the same time, the requirements for lithium-ion batteries are becoming increasingly stringent.

[0003] As one of the four main materials in lithium-ion batteries, the separator plays a crucial role. Traditional polypropylene and polyethylene separators can no longer meet the requirements of lithium-ion batteries for high power density, high energy density, high safety, and fast charging, necessitating modifications to traditional basic separators. Furthermore, polyolefin-based separators exhibit poor thermal stability at high temperatures, easily shrinking and potentially causing short circuits during battery operation, leading to a series of safety issues.

[0004] Currently, the development of new coatings mainly focuses on ceramics, which are widely used in lithium-ion battery separators due to their excellent heat resistance. However, their electrolyte absorption and retention capabilities need further improvement. Furthermore, pure ceramic materials cannot guarantee homogeneous electrolyte transport within the separator, leading to safety issues. In coated separators, uneven pore size distribution and uniform pore size in the coating material often cause heterogeneous electrolyte transport during the process, resulting in polarization problems. Good wettability of the electrolyte is crucial for ensuring homogeneous transport within the separator; poor wettability affects lithium-ion battery manufacturing, thus becoming a major production problem.

[0005] In view of this, the present invention is hereby proposed. Summary of the Invention

[0006] The primary objective of this invention is to provide a diaphragm that exhibits excellent thermal stability, good electrolyte absorption and retention capabilities, and excellent electrolyte wettability, thereby facilitating the homogeneous transport of the electrolyte.

[0007] The second objective of this invention is to provide a secondary battery with high power density, high energy density and high safety.

[0008] To achieve the above-mentioned objectives of this invention, the following technical solution is adopted:

[0009] This invention provides a diaphragm comprising a base membrane and a coating disposed on at least one surface of the base membrane. The coating comprises a ceramic layer and an adhesive layer, wherein the ceramic layer comprises ceramic particles, a binder, and functional materials. The porosity of the coating of the diaphragm is 35–65%, and the areal density of the coating is 4–15 g / m³. 2 .

[0010] Furthermore, the functional material includes at least one of kapok, wood, sponge, coral, metal-organic framework material, covalent organic framework material, or carbon material formed from at least one of the aforementioned functional materials.

[0011] Furthermore, in the functional material, the ratio of the pore volume of micropores, the pore volume of mesopores, and the pore volume of macropores is (0.01~0.4):(0.01~0.7):(0.01~0.6).

[0012] Further, in the ceramic layer, the mass ratio of the ceramic particles, the functional material, and the binder is (0.01-0.5):(0.01-0.4):(0.01-0.15).

[0013] Furthermore, the adhesive layer comprises polyvinylidene fluoride.

[0014] Furthermore, the thickness of the ceramic layer is 3 to 6 μm.

[0015] Furthermore, the thickness of the adhesive layer is 3–7 μm.

[0016] Furthermore, the coating of the diaphragm includes additives, including dispersants and / or wetting agents.

[0017] Furthermore, the coating of the diaphragm includes additives, which include dispersants and wetting agents.

[0018] Furthermore, the mass ratio of the dispersant to the wetting agent is 0.5:(0.01 to 0.1).

[0019] The present invention also provides a secondary battery, comprising a positive electrode, a negative electrode, and a separator as described above.

[0020] Another aspect of the present invention provides an electrical device comprising a secondary battery as described above.

[0021] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0022] (1) The diaphragm of the present invention, through the combination of functional materials and ceramic particles, can reduce the degree of thermal shrinkage in the MD and TD directions under high temperature conditions and improve the thermal stability of the diaphragm.

[0023] (2) The diaphragm of the present invention has a ceramic layer and an adhesive layer disposed in the diaphragm coating, and functional materials are added to the ceramic layer. The porosity of the prepared diaphragm coating is 35-65% and the areal density of the coating is 4-15 g / m³. 2 This enhances the diaphragm's ability to absorb and retain electrolyte, significantly improving the diaphragm's wettability to the electrolyte.

[0024] (3) The diaphragm of the present invention provides an excellent environment for the homogeneous transport of electrolyte by adding functional materials to the coating, which can ensure the rapid passage and homogeneous transport of lithium ions during the reaction process. Detailed Implementation

[0025] The technical solution of the present invention will be clearly and completely described below with reference to specific embodiments. However, those skilled in the art will understand that the embodiments described below are some embodiments of the present invention, but not all embodiments, and are only used to illustrate the present invention, and should not be regarded as limiting the scope of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0026] The following is a detailed description of a separator and a secondary battery according to an embodiment of the present invention.

[0027] In some embodiments of the present invention, a diaphragm is provided, comprising a base membrane and a coating disposed on at least one surface of the base membrane, the coating comprising a ceramic layer and an adhesive layer, the ceramic layer comprising ceramic particles, a binder, and functional materials; the porosity of the coating of the diaphragm is 35-65%; the areal density of the coating is 4-15 g / m³. 2 .

[0028] The diaphragm of this invention, through the combination of functional materials and ceramics, can reduce the degree of thermal shrinkage in the MD and TD directions under high-temperature conditions, thereby improving the thermal stability of the diaphragm. The diaphragm coating comprises a ceramic layer and an adhesive layer, with functional materials incorporated into the ceramic layer. The resulting diaphragm coating has a porosity of 35–65% and an areal density of 4–15 g / m³. 2 This enhances the membrane's ability to absorb and retain electrolyte, significantly improving its wettability. Simultaneously, the functional material's abundant porosity, large pore volume, favorable pore size distribution, and channel structure prevent lithium dendrite growth that could lead to membrane puncture, resulting in high safety performance.

[0029] The separator of the present invention can also reduce the risk of capacity reduction and local overcharging, thereby protecting the secondary battery; moreover, the functional materials are characterized by abundant resources, low price and green environmental protection, which is conducive to reducing the cost of the separator.

[0030] In some embodiments of the present invention, the functional material includes at least one of kapok, wood, sponge, coral, metal-organic framework materials, covalent organic framework materials, or carbon materials formed from at least one of the aforementioned functional materials. For example, kapok, wood, sponge, and coral can be obtained by processes such as chopping, crushing, grinding, washing, and drying. Metal-organic framework materials and covalent organic framework materials can be synthesized through chemical methods. In addition, to obtain a functional material with a suitable pore structure, at least one of the aforementioned functional materials can be calcined to obtain a carbon material.

[0031] In some embodiments of the present invention, the ratio of the pore volume of micropores, the pore volume of mesopores, and the pore volume of macropores in the functional material is (0.01-0.4):(0.01-0.7):(0.01-0.6).

[0032] Preferably, in the functional material, the ratio of the pore volume of micropores, mesopores, and macropores is (0.1–0.3):(0.1–0.5):(0.1–0.5). The functional material of this invention simultaneously includes micropores, mesopores, and macropores. By controlling the pore volumes of micropores, mesopores, and macropores in the functional material, and adopting a suitable ratio among the three, the functional material can exhibit good pore size distribution, porosity, and pore structure, thereby improving the wettability of the membrane to the electrolyte and reducing the problem of heterogeneous transport of the electrolyte during transport.

[0033] In some embodiments of the present invention, the mass ratio of the ceramic particles, the functional material, and the binder in the ceramic layer is (0.01–0.5):(0.01–0.4):(0.01–0.15). By controlling the mass ratio of ceramic particles, functional material, and binder within the range specified in the present invention, the present invention facilitates the coordination of the pore structure of the base membrane and the ceramic layer, promotes good electrolyte absorption and retention capacity of the diaphragm, and greatly improves the wettability of the diaphragm to the electrolyte.

[0034] In some embodiments of the present invention, the adhesive layer comprises polyvinylidene fluoride.

[0035] In some embodiments of the present invention, the separator includes a base film, a ceramic layer, and a binder layer that are in sequential contact; the ceramic layer and binder layer are disposed on one side of the base film, or the ceramic layer and binder layer are disposed on both sides of the base film; that is, the separator has a three-layer structure or a five-layer structure. The binder layer can promote tight adhesion between the separator and the positive or negative electrode, which helps to reduce the risk of the separator detaching from the positive or negative electrode during long-cycle charge and discharge, thereby reducing the cycle capacity of the battery.

[0036] In some embodiments of the present invention, the ceramic particles include at least one selected from alumina, boehmite, silicon dioxide, zirconium oxide, magnesium oxide, and titanium oxide. Adding the above-mentioned types of ceramic particles to the separator of the present invention can effectively improve the thermal shrinkage problem of the separator and enhance its thermal stability.

[0037] In some embodiments of the present invention, the thickness of the ceramic layer is 3 to 6 μm. Typically, but not limitingly, the thickness of the ceramic layer is, for example, a range of 3 μm, 4 μm, 5 μm, 6 μm, or any combination thereof. Controlling the thickness of the ceramic layer within the range of the present invention is beneficial for coordinating the pore structure of the ceramic layer and the base membrane, ensuring the air permeability of the diaphragm.

[0038] In some embodiments of the present invention, the thickness of the adhesive layer is 3–7 μm. Typical, but not limiting, for example, the thickness of the adhesive layer is within the range of 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, or any combination thereof. The thickness of the adhesive layer directly affects the bonding strength between the separator and the positive or negative electrode, thereby affecting the battery performance, especially the battery's long-term charge-discharge cycle capability. Controlling the thickness of the adhesive layer within the range of the present invention ensures the bonding ability between the positive and negative electrode and the separator, and reduces the impact on the separator's permeability and heat resistance.

[0039] In some specific embodiments of the present invention, the pore volume of micropores accounts for 20% to 40% of the total pore volume of the functional material; the pore volume of mesopores accounts for 30% to 40% of the total pore volume of the functional material; and the pore volume of macropores accounts for 30% to 40% of the total pore volume of the functional material.

[0040] In some specific embodiments of the present invention, in the structural material of the functional material, the pore size of the micropores is <2nm, the pore size of the mesopores is 2-50nm, and the pore size of the macropores is >50nm.

[0041] In some embodiments of the present invention, the coating of the diaphragm includes additives, which include dispersants and / or wetting agents. During the preparation of the ceramic layer, the additives can disperse and wet the ceramic layer material, ensuring sufficient wetting and uniform dispersion of the ceramic particles, functional materials, and binders in the ceramic layer.

[0042] In some embodiments of the present invention, the diaphragm coating includes additives, including dispersants and wetting agents. In some specific embodiments of the present invention, the contact angle of the diaphragm is less than 11°. Typically, but not limitingly, the contact angle of the diaphragm can be a range of 11°, 10°, 9°, 8°, 7°, 6°, 5°, 4°, 3°, 2°, 1°, or any combination thereof. A contact angle within the range of the present invention facilitates sufficient electrolyte wetting of the diaphragm, improving the overall performance of the diaphragm.

[0043] In some specific embodiments of the invention, the liquid absorption rate of the diaphragm is 175% to 215%. Typically, without limitation, it can be a range of 175%, 180%, 185%, 190%, 195%, 200%, 205%, 210%, 215%, or any combination thereof.

[0044] In some specific embodiments of the invention, the diaphragm undergoes thermal shrinkage of 0.95% to 1.7% in the MD direction at 130°C for 0.5 hours. Typically, and without limitation, the shrinkage can be within the range of 0.95%, 1.0%, 1.15%, 1.25%, 1.35%, 1.45%, 1.55%, 1.65%, 1.7%, or any combination thereof.

[0045] In some specific embodiments of the invention, the diaphragm undergoes thermal shrinkage of 1.05% to 1.85% in the TD direction at 130°C for 0.5 hours. Typically, and without limitation, the shrinkage can be within the range of 1.05%, 1.15%, 1.25%, 1.35%, 1.45%, 1.55%, 1.65%, 1.75%, 1.85%, or any combination thereof.

[0046] In some specific embodiments of the present invention, the dispersant includes at least one of the following: polyoxyethylene dioleate, polytetraethylene glycol monostearate, triethylhexyl phosphate, sodium dodecyl sulfate, methylpentanol, cellulose derivatives, polyacrylamide, glucon, and fatty acid polyethylene glycol esters.

[0047] In some specific embodiments of the present invention, the wetting agent includes at least one of alkyl sulfates, sulfonates, fatty acids, fatty acid ester sulfates, carboxylic acid soaps, phosphate esters, polyoxyethylene alkylphenol ethers, and polyoxyethylene fatty alcohol ethers.

[0048] In some embodiments of the present invention, the mass ratio of the dispersant to the wetting agent is 0.5:(0.01 to 0.1). Typical, but not limiting, examples include mass ratios of 0.5:0.01, 0.5:0.02, 0.5:0.03, 0.5:0.04, 0.5:0.05, 0.5:0.06, 0.5:0.07, 0.5:0.08, 0.5:0.09, 0.5:0.1, or any combination thereof. Controlling the mass ratio of the dispersant to the wetting agent within the range specified in this application is beneficial for obtaining a ceramic layer with uniform texture, thereby obtaining a uniform and stable diaphragm.

[0049] In some embodiments of the present invention, the mass ratio of ceramic particles, functional materials, binders and additives is (0.01-0.5):(0.01-0.4):(0.01-0.15):(0.001-0.05); preferably, the mass ratio of ceramic particles, functional materials, binders and additives is (0.2-0.5):(0.1-0.4):(0.05-0.15):(0.01-0.05).

[0050] The diaphragm of the present invention has a ceramic layer disposed on the surface of a base membrane. The ceramic layer is mainly composed of ceramic particles and functional materials. Appropriate binders, dispersants and wetting agents are used to improve dispersibility and wettability to the base membrane, so that the diaphragm has excellent performance.

[0051] In some embodiments of the present invention, the adhesive includes at least one of polymethyl methacrylate (PMMA), polyimide (PI), polyacrylonitrile (PAN), polyacrylic acid (PAA), carboxymethyl cellulose (CMC), polyvinylidene fluoride (PVDF) oily adhesive, and a water-dispersible emulsion of polytetrafluoroethylene (PTFE).

[0052] In some embodiments of the present invention, the base film is made of at least one of polyethylene (PE), polypropylene (PP), polyvinylidene fluoride (PVDF), polyimide (PI), aramid, polyethylene terephthalate (PET), and polyacrylonitrile (PAN).

[0053] In some embodiments of the present invention, the thickness of the base film is 5 to 20 μm; typically, but not limitingly, for example, the thickness of the base film is a range of 5 μm, 8 μm, 10 μm, 12 μm, 14 μm, 16 μm, 18 μm, 20 μm or any combination thereof.

[0054] In some embodiments of the present invention, a method for preparing the diaphragm is also provided, comprising the following steps:

[0055] Preparation of functional materials: The functional materials are first washed three times with ultrapure water and then three times with washing alcohol. They are then baked in an oven at 60–80°C for 12–24 hours. Next, the baked functional materials are ground in a grinder, first with coarse grinding and then with fine grinding. The coarse grinding pressure is 0.3–0.5 MPa, the coarse grinding speed is 400–1800 r / min, and the coarse grinding time is 5–20 min. The fine grinding pressure is 0.05–0.2 MPa, the fine grinding speed is 2000–6000 r / min, and the fine grinding time is 10–60 min. After the above steps, the ratio of the micropore volume, mesopore volume, and macropore volume of the functional material of this invention is (0.01–0.4):(0.01–0.7):(0.01–0.6).

[0056] Ceramic particles, functional materials, binders, additives and solvents are made into a slurry, which is then coated onto a base film to obtain a ceramic layer. Polyvinylidene fluoride is then sprayed onto the surface of the ceramic layer.

[0057] In some specific embodiments of the present invention, the solvent includes aqueous solvents and / or oil-based solvents; preferably, the solvent includes at least one selected from water, ethanol, glycerol, acetone, and NMP. More preferably, the viscosity of the slurry is 120–240 mPa·s.

[0058] In some embodiments of the present invention, the slurry is coated on one side only, and the polyvinylidene fluoride is coated on one side only; or, the slurry is coated on both sides only, and the polyvinylidene fluoride is coated on both sides only.

[0059] In some embodiments of the present invention, the slurry is coated by roller coating.

[0060] In some embodiments of the present invention, the method of coating polyvinylidene fluoride includes spraying.

[0061] In some embodiments of the present invention, a secondary battery is also provided, comprising a positive electrode, a negative electrode, and the above-described separator.

[0062] The secondary battery of the present invention, by employing the above-mentioned separator, is beneficial to improving the power density, energy density and safety of the secondary battery.

[0063] In some specific embodiments of the present invention, the secondary battery includes a positive electrode material comprising a ternary positive electrode active material. Preferably, the ternary positive electrode active material comprises lithium nickel cobalt manganese oxide and / or lithium nickel cobalt aluminum oxide; more preferably, the lithium nickel cobalt manganese oxide comprises at least one of the lithium nickel cobalt manganese oxide 111 series, lithium nickel cobalt manganese oxide 333 series, lithium nickel cobalt manganese oxide 523 series, lithium nickel cobalt manganese oxide 622 series, and lithium nickel cobalt manganese oxide 811 series; the negative electrode material comprises a negative electrode active material, preferably, the negative electrode active material comprises graphite.

[0064] In some embodiments of the present invention, a method for preparing a lithium-ion battery is also provided, comprising the following steps:

[0065] The positive electrode, negative electrode, and separator are wound and hot-pressed to form a battery cell. The cell then undergoes Hi-pot testing, welding, top sealing, vacuum baking, electrolyte injection, packaging, formation, and capacity testing to produce a lithium-ion battery.

[0066] The present invention will be further described in detail below through specific embodiments.

[0067] Example 1:

[0068] The preparation of the positive electrode sheet includes the following steps:

[0069] The ternary material nickel cobalt manganese oxide (NCM811), polyvinylidene fluoride, and conductive carbon black were added to N-methylpyrrolidone solvent at a mass ratio of 94:3:3 and stirred evenly. The mixture was then coated onto aluminum foil and prepared by drying, cold pressing, and slitting processes to obtain the positive electrode sheet.

[0070] The preparation of the negative electrode sheet includes the following steps:

[0071] Graphite, conductive carbon black, and negative electrode binder (carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR), and polyacrylic acid (PAA)) are added to deionized water at a mass ratio of 95:2.5:2.5, stirred evenly, and coated onto copper foil. The negative electrode sheet is then prepared by drying, cold pressing, and slitting.

[0072] The preparation of the electrolyte includes the following steps:

[0073] An electrolyte was prepared by dissolving lithium hexafluorophosphate in a mixed solution of ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate, with a mass ratio of ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate of 1.2:1.9:0.9; the mass percentage of lithium hexafluorophosphate in the electrolyte was 12.8%.

[0074] The preparation of the diaphragm includes the following steps:

[0075] The coral was first washed three times with ultrapure water, then three times with washing alcohol, and then baked in a 60℃ oven for 24 hours. After baking, the coral was ground in a grinder, first with coarse grinding and then with fine grinding. The coarse grinding pressure was 0.3 MPa, the rotation speed was 800 r / min, and the coarse grinding time was 8 minutes. Then, it underwent fine grinding at a pressure of 0.1 MPa, a rotation speed of 4000 r / min, and a fine grinding time of 15 minutes, resulting in a coral functional material with a micropore:mesopore:macropore ratio of 0.5:0.3:0.2. Next, a 12μm PP membrane was selected as the base membrane. Boehmite powder, coral (micropore:mesopore:macropore ratio = 0.5:0.3:0.2), and PVDF in a ratio of 0.2:0.2:0.15 were prepared into a coating slurry and coated onto the PP base membrane, resulting in a single-sided coating with a thickness of 3μm.

[0076] Example 2

[0077] The preparation method of Example 2 is the same as that of Example 1, except that the ceramic layer is coated on both sides.

[0078] Examples 3-8

[0079] The preparation methods of Examples 3 to 8 are the same as those of Example 1, except that the mass ratio of boehmite:coral:PVDF is different, as detailed in Table 1.

[0080] Examples 9-11

[0081] The preparation methods of Examples 9 to 11 are the same as those of Example 3, except that PVDF is sprayed into the ceramic layer after the ceramic layer is obtained. The thickness of the PVDF adhesive layer is detailed in Table 1.

[0082] Examples 12-13

[0083] The preparation methods of Examples 12 and 13 are the same as those of Example 3, except that the thickness of the ceramic layer is detailed in Table 1.

[0084] Examples 14-15:

[0085] The preparation methods of Examples 14 and 15 are the same as those of Example 3, except that the types of ceramic particles are different, as detailed in Table 1.

[0086] Examples 16-17:

[0087] Examples 16-17: The preparation methods are the same as in Example 3, except that the types of functional materials are different, as detailed in Table 1.

[0088] Examples 18-19:

[0089] The preparation methods of Examples 18 and 19 are the same as those of Example 3, except that the type of binder in the ceramic layer is different, as detailed in Table 1.

[0090] Example 20:

[0091] The preparation method of Example 20 is the same as that of Example 3, except that the coral fine grinding time is 45 min.

[0092] Example 21:

[0093] The preparation method of Example 21 is the same as that of Example 10, except that the coral fine grinding time is 20 min.

[0094] Example 22:

[0095] The preparation method of Example 22 is the same as that of Example 20, except that the coating of the diaphragm includes a resist agent, and polyoxyethylene dioleate dispersant and polyoxyethylene alkylphenol ether wetting agent are added to the slurry, with the ratio of polyoxyethylene dioleate dispersant to polyoxyethylene alkylphenol ether wetting agent being 0.5:0.08.

[0096] Examples 23-24:

[0097] The preparation methods of Examples 23 and 24 are the same as those of Example 22, except that the ratio of polyoxyethylene dioleate dispersant to polyoxyethylene alkylphenol ether wetting agent is different, as detailed in Table 1.

[0098] Example 25:

[0099] The preparation method of Example 25 is the same as that of Example 23, except that the types of additives are different, as detailed in Table 1.

[0100] Comparative Examples 1-3

[0101] The preparation methods of Comparative Examples 1 to 3 are the same as those in Example 1, except that the ratio of boehmite:coral:PVDF in Comparative Example 1 is 0.6:0.2:0.15, the ratio of boehmite:coral:PVDF in Comparative Example 2 is 0.2:0.005:0.15, and the ratio of boehmite:coral:PVDF in Comparative Example 3 is 0.2:0.3:0.25.

[0102] Comparative Example 4

[0103] The preparation method of Comparative Example 4 is the same as that of Example 1, except that the ratio of boehmite to PVDF is 0.2:0.15 and no coral is used.

[0104] Comparative Example 5

[0105] Comparative Example 5 is the same as Example 1, except that the diaphragm is not coated.

[0106] Detailed parameters for each embodiment and comparative example are shown in Table 1.

[0107] Table 1

[0108]

[0109]

[0110]

[0111]

[0112] The basic physical properties of the diaphragms prepared in the examples and comparative examples were tested, and the results are shown in Table 2.

[0113] The thickness testing method was Mahr thickness gauge, with N=20 parallel samples.

[0114] Air permeability test method: Gurley tester, N≥3 parallel samples.

[0115] Heat shrinkage test method: Cut the diaphragm into 100mm×50mm pieces and bake them in a forced-air oven at a certain temperature. Then measure the length after baking. The sample size N≥3.

[0116] Contact angle test method: Refer to GB / T 30447-2013 Standard Method for Measuring Contact Angle of Nanofilms. Sample size: ≥2cm*8cm. Test method: Test the contact angle of the electrolyte on the membrane surface. Test settings: Total time 10.0s, start and pause 0.0s, suction head size 300μL, drop volume 2.0μL. Record the contact angle of the electrolyte droplet on the membrane surface after 10s. Parallel samples N≥3.

[0117] Liquid absorption rate test method: Weigh the cut diaphragm of fixed size using a balance before absorbing the electrolyte, and record the mass of the diaphragm as m1. Then immerse the diaphragm in the electrolyte. After it is fully wetted, take it out and weigh it, and record it as m2. Liquid absorption rate = (m2-m1) / m1*100%, parallel samples N≥3.

[0118] Table 2

[0119]

[0120]

[0121] As shown in Table 2, a comparison between Examples 1-19 and Comparative Example 4 reveals that, under high-temperature conditions, the thermal shrinkage of the diaphragm of the present invention in both the MD and TD directions is significantly improved. The improved thermal stability is due to the fact that both the ceramic particles and functional materials used are highly heat-resistant, exhibiting excellent thermal stability. Furthermore, the liquid absorption rates of Examples 1-19 are significantly higher than those of the diaphragm in Comparative Example 4. This is mainly because the addition of functional materials provides an excellent environment for electrolyte absorption, enhancing the diaphragm's liquid absorption and retention capacity, and further improving its wettability.

[0122] A comparison of Examples 10, 20, and 21 shows that when the pore volume of micropores, mesopores, and macropores in the functional material is within the range of this application, the better the wettability of the prepared diaphragm to the electrolyte and the higher the liquid absorption rate.

[0123] The electrochemical performance of the examples and comparative examples was tested, and the results are shown in Table 3.

[0124] Among them, the cycle performance test: the lithium-ion battery is charged and discharged at 1C rate at 25℃ for 1000 cycles. The battery capacity at 1C rate is compared with the battery capacity before the cycle, and the capacity retention rate after the cycle is calculated.

[0125] Battery gravimetric energy density: Test and calculate the gravimetric energy density of a single battery cell, in Wh / kg.

[0126] Short-circuit safety performance test: After the battery is fully charged to 4.4V in a constant current and constant voltage manner, it is short-circuited for 10 minutes using an external circuit with an internal resistance of <5mΩ.

[0127] Table 3

[0128]

[0129]

[0130] As shown in Table 3, comparing Examples 1-19 and Comparative Example 4, the batteries in Examples 1-19 not only exhibit high gravimetric energy density and high capacity retention, but also showed no short circuits during cell testing. In contrast, the battery in Comparative Example 4 had lower gravimetric energy density and capacity retention, and experienced more short circuits, making it prone to thermal runaway and posing a safety hazard. The introduction of functional materials ensures homogeneous electrolyte transport, achieving high battery safety and high capacity retention.

[0131] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A diaphragm, characterized in that, The coating includes a base film and a coating disposed on at least one surface of the base film, the coating including a ceramic layer and an adhesive layer, the ceramic layer including ceramic particles, an adhesive and a functional material; The porosity of the coating on the diaphragm is 35-65%; The areal density of the coating is 4–15 g / m³. 2 ; In the functional material, the ratio of the pore volume of micropores, the pore volume of mesopores, and the pore volume of macropores is (0.1~0.3):(0.1~0.5):(0.1~0.5). The functional materials include at least one of the following: kapok, wood, sponge, coral, metal-organic framework materials, covalent organic framework materials, or carbon materials formed from at least one of the aforementioned porous materials; The base film is made of at least one of polyethylene, polypropylene, polyvinylidene fluoride, polyimide, aramid, polyethylene terephthalate, and polyacrylonitrile. The thickness of the base film is 5–20 μm; The diaphragm comprises a base membrane, a ceramic layer, and an adhesive layer that are in sequential contact. The contact angle of the diaphragm is less than 11°; The liquid absorption rate of the diaphragm is 175% to 215%.

2. The diaphragm according to claim 1, characterized in that, In the ceramic layer, the mass ratio of the ceramic particles, the functional material, and the binder is (0.01-0.5):(0.01-0.4):(0.01-0.15).

3. The diaphragm according to claim 1, characterized in that, The adhesive layer comprises polyvinylidene fluoride.

4. The diaphragm according to claim 1, characterized in that, The thickness of the ceramic layer is 3–6 μm.

5. The diaphragm according to claim 1, characterized in that, The thickness of the adhesive layer is 3–7 μm.

6. The diaphragm according to claim 1, characterized in that, The coating of the diaphragm includes additives, including dispersants and / or wetting agents.

7. The diaphragm according to claim 1, characterized in that, The coating of the diaphragm includes additives, which include dispersants and wetting agents, wherein the mass ratio of the dispersant to the wetting agent is 0.5:(0.01 to 0.1).

8. A secondary battery, characterized in that, It includes a positive electrode, a negative electrode, and a separator as described in any one of claims 1 to 7.

Citation Information

Patent Citations

  • Nonaqueous electrolyte secondary battery separator

    CN108539108A

  • Separator for non-aqueous secondary batteries, and non-aqueous secondary battery

    CN111492504A

  • Method for producing porous layer, stack, separator for nonaqueous electrolyte secondary battery, and nonaqueous electrolyte secondary battery

    CN113195113A

  • Separator for non-aqueous secondary battery, and non-aqueous secondary battery

    CN113678312A

  • Diaphragm, preparation method thereof and lithium ion battery

    CN113964373A